[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JPS5957675A - Two-piece solid golf ball - Google Patents

Two-piece solid golf ball

Info

Publication number
JPS5957675A
JPS5957675A JP57169144A JP16914482A JPS5957675A JP S5957675 A JPS5957675 A JP S5957675A JP 57169144 A JP57169144 A JP 57169144A JP 16914482 A JP16914482 A JP 16914482A JP S5957675 A JPS5957675 A JP S5957675A
Authority
JP
Japan
Prior art keywords
weight
parts
hardness
golf ball
tensile strength
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP57169144A
Other languages
Japanese (ja)
Other versions
JPH0145378B2 (en
Inventor
幹生 山田
矢吹 芳計
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sumitomo Rubber Industries Ltd
Original Assignee
Sumitomo Rubber Industries Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Rubber Industries Ltd filed Critical Sumitomo Rubber Industries Ltd
Priority to JP57169144A priority Critical patent/JPS5957675A/en
Publication of JPS5957675A publication Critical patent/JPS5957675A/en
Publication of JPH0145378B2 publication Critical patent/JPH0145378B2/ja
Granted legal-status Critical Current

Abstract

(57)【要約】本公報は電子出願前の出願データであるた
め要約のデータは記録されません。
(57) [Summary] This bulletin contains application data before electronic filing, so abstract data is not recorded.

Description

【発明の詳細な説明】 本発明はツウーピーヌンリソドコルフボールに関する。[Detailed description of the invention] TECHNICAL FIELD The present invention relates to a two-piece ball.

糸巻きゴルフボールの耐久性の悪さを改良すみために開
発されたツウ−ピースソリッドゴルフボールは一体成形
したソリッドコアとそれを被覆するカバーから構成され
る。カバーのね質としては、機械的強度に優れ、特に打
撃時の面1カット性と適度の弾力性に優れているという
理由から、エチレンの共重合体に金属イオンを化学結合
させたアイオノマー樹脂が天然ゴム等のかわりに利用さ
れるよう番こなっている。
A two-piece solid golf ball, which was developed to improve the poor durability of thread-wound golf balls, is composed of an integrally molded solid core and a cover covering the solid core. The material used for the cover is an ionomer resin, which is made by chemically bonding metal ions to an ethylene copolymer, because it has excellent mechanical strength, particularly good ability to cut one side when struck, and moderate elasticity. It is being used in place of natural rubber, etc.

しかしながら従来のこの種のソウ−ピースソリッドゴル
フボールも反撥弾性Cインパクト時のボール初速度)と
記入性、特に低温耐久性OJ点でなお改良すべき余地が
あり、本発明はこのような観点からなされたものであっ
てその要旨は、基材ゴム100重量部、不飽和脂肪酸の
金属塩10〜60重量部、酸化亜鉛40〜70重量部お
よび架橋剤1〜5重量部含有する組成物を加熱硬化して
得られるソリッドコアを、ショアーD硬度65似上−引
張強度250〜300 kq/C1nおよび脆化温度−
100−−110℃、M I (Mel t Inde
x ) = Q。
However, there is still room for improvement in the conventional saw-piece solid golf balls of this type in terms of repulsion (C), ball initial velocity at impact), write-in performance, and especially low-temperature durability (OJ). The gist is that a composition containing 100 parts by weight of base rubber, 10 to 60 parts by weight of a metal salt of an unsaturated fatty acid, 40 to 70 parts by weight of zinc oxide, and 1 to 5 parts by weight of a crosslinking agent is heated. The solid core obtained by hardening has a Shore D hardness of 65 or higher, a tensile strength of 250 to 300 kq/C1n, and a embrittlement temperature.
100--110℃, MI (Melt Inde
x ) = Q.

7〜2.0、融点88℃のアイオノマー樹脂40〜45
重量部、ンヨアーD硬度65以上、引張強度275〜3
20 kq10r+および脆化温度−100〜−1]O
℃、MI=2.3〜3,0、融点90℃のアイオノマー
樹脂40〜45重量部、ショアー1)硬度60〜64、
引張強度200〜230 kq/anおよび脆化温度−
70〜−80℃、M I == 8〜12、融びンヨア
ーD硬度60〜64.引張強度190〜220 kQ/
cmおよび脆化温度−75〜−85℃、MI−4,s 
−’ s、 o、融点94℃のアイオノマー樹脂5〜1
0型開部を主材とするカバーで被mして成るツウーピー
ヌソリッドコルフボールに存する。
7-2.0, ionomer resin 40-45 with a melting point of 88°C
Part by weight, Hardness D: 65 or more, Tensile strength: 275-3
20 kq10r+ and embrittlement temperature -100 to -1]O
°C, MI = 2.3-3.0, 40-45 parts by weight of ionomer resin with melting point 90 °C, Shore 1) Hardness 60-64,
Tensile strength 200-230 kq/an and embrittlement temperature -
70 to -80°C, M I == 8 to 12, melting yore D hardness 60 to 64. Tensile strength 190-220 kQ/
cm and embrittlement temperature -75 to -85°C, MI-4,s
-'s, o, ionomer resin 5 to 1 with melting point of 94°C
This consists of a two-upine solid Corfu ball that is covered with a cover whose main material is a 0-type opening.

本発明に用いる基材ゴムとしてはポリブタジェンコム、
スチレンブタジェンコム、天然コム、ハイスチレン樹脂
等が例示されろか、ポリブタジェンコム、就中ンヌ1,
4−ホリブタシエンコムが好ましい。
The base rubber used in the present invention is polybutadiene com,
Examples include styrene butadiene com, natural comb, high styrene resin, etc. Polybutadiene com, among others Nnu 1,
4-Hoributashiencom is preferred.

不発明に用いる不飽和脂肪酸の金属塩としては伏素原子
数3〜8の不飽和脂肪酸−例えばアクリル酸、メタクリ
ル酸等の亜鉛塩、マグネ/ラム塩等が例示されるが、特
にアクリル酸亜鉛および/またはメタクリル酸亜鉛が好
ましい。
Examples of the metal salts of unsaturated fatty acids used in the invention include unsaturated fatty acids having 3 to 8 atom atoms, such as zinc salts of acrylic acid, methacrylic acid, magne/rum salts, etc., but especially zinc acrylate. and/or zinc methacrylate are preferred.

不飽和脂肪酸の金属塩は基材コム100重量部に対して
10〜60重量部使用する。該金属、塩が10重量部よ
りも少ないと十分な硬さが得られず、インパクト時のボ
ールの初速度も小さくなり、また60重量部以上になる
とボールが硬くなり丁きて初速度が低下する。
The metal salt of unsaturated fatty acid is used in an amount of 10 to 60 parts by weight based on 100 parts by weight of the base comb. If the amount of the metal or salt is less than 10 parts by weight, sufficient hardness will not be obtained and the initial velocity of the ball at impact will be low; if it is more than 60 parts by weight, the ball will become hard and bunch, reducing the initial velocity. do.

酸化亜鉛は重量調整剤として使用するもので、その配合
量は通常法材ゴム100重量部に対して40〜70重量
部とする。
Zinc oxide is used as a weight adjuster, and its amount is usually 40 to 70 parts by weight per 100 parts by weight of the rubber material.

重量調整剤としては他の常套の充填剤、例えば硫酸バリ
ウム、FA酸カルシウム、シリカ等を適宜防用してもよ
い。
Other conventional fillers, such as barium sulfate, calcium FA acid, silica, etc., may be used as appropriate weight adjusters.

ソリッドコアに最適硬度を何方するために使用する架橋
剤としてはジクミルパーオキサイドOJような過酸化物
および7ゾビスイソブチルニトリルのようなアゾ化合物
が例示されるが、特にジクミルパーオキサイドが好まし
い。
Examples of crosslinking agents used to obtain the optimum hardness for the solid core include peroxides such as dicumyl peroxide OJ and azo compounds such as 7zobisisobutylnitrile, with dicumyl peroxide being particularly preferred. .

架橋剤の配合量は基材ゴム100重量部に対して通常1
〜5重量部であり、この範囲1外0J架橋剤を使用する
と最適硬度のコアはKR黄(tい。
The amount of crosslinking agent is usually 1 part by weight per 100 parts by weight of the base rubber.
~5 parts by weight, and when using 0J crosslinking agent outside this range, the core of optimum hardness is KR yellow (t).

」二記成分を配合して得られろコア用組成物は常套の混
練機、例えばバンバリーミキサ−やロール等を用いて湿
練し、常法によって約140〜]70℃でプレス成形し
て規格θ〕一体成形ソリッドコアとする。
The core composition obtained by blending the two components is wet-kneaded using a conventional kneading machine, such as a Banbury mixer or a roll, and then press-molded at about 140 to 70°C by a conventional method to form a standard. θ] One-piece solid core.

一体成形ソリッドコアを被覆するカバーは、アイオノマ
ー樹脂を主材とし、必要により着色等の目的で無機充填
剤、例えば二酸化チタン、酸化亜鉛等を適宜配合させて
もよい。
The cover covering the integrally molded solid core is mainly made of an ionomer resin, and may contain an appropriate inorganic filler such as titanium dioxide, zinc oxide, etc. for the purpose of coloring, if necessary.

不発明に使用するアイオノマー樹脂はモノオレフィンと
不飽和モノまたはジカルボン酸およびそれらのエステル
から成る群から選択される少なくとも1種との重合体に
交叉金属結合を付与した熱可塑性樹脂、好ましくはモノ
オレフィンと炭素原子数3〜8の不飽和モノまたはジカ
ルボン酸およびそれらOJエヌテルから成る群から選択
されろ少なくとも1腓との重合体C不飽和モノまたはジ
カルボン酸および/またはそれらのエヌテル4〜30重
量係含有)に交叉金属結合を併有した熱可塑凶。
The ionomer resin used in the invention is a thermoplastic resin, preferably a monoolefin, in which a cross-metallic bond is added to a polymer of a monoolefin and at least one selected from the group consisting of unsaturated mono- or dicarboxylic acids and esters thereof. and at least one polymer selected from the group consisting of unsaturated mono- or dicarboxylic acids having 3 to 8 carbon atoms and their A thermoplastic resin containing cross-metallic bonding.

樹lIi¥−から選ばれる下記4種のタイプの混合梢脂
である。
The following four types of mixed tree resin are selected from the following.

即ち、ショアーD硬度65以上、引張強度250〜30
0 kg/cm および脆化温度−100〜−]]0℃
、M I = 0.7〜2,0、融点88℃の特性を有
するアイオノマー樹脂(以下、アイオノマー樹脂Iとい
う)、40〜45重置部、ショアーD硬度65以上、引
張強度275〜320 kglorrおよび脆化温度−
100〜−110℃、M I : 2.3〜3.3、融
点90℃の特性を有するアイオノマー樹脂C以下、アイ
オノマー樹脂■という)40〜45重量部、ショアーD
硬度60〜64、引張強度200〜230 kq/cm
 および脆化温度−70〜−80℃、Ml−8〜12、
融点96℃の特性を有するアイオノマー樹脂C以下、ア
イオノマー樹脂■といつ)5〜10重量部およびショア
ーD硬度60〜64、引張強度190〜220 kq/
αおよび脆化温度−75、、−85℃、MI==4.5
〜8.0、融点94℃の特性を有するアイオノマー樹脂
C以下、アイオノマー樹脂■という)5〜lO重量部か
ら成る混合樹脂である。
That is, Shore D hardness is 65 or more, tensile strength is 250-30
0 kg/cm and embrittlement temperature -100~-]]0℃
, M I = 0.7-2,0, an ionomer resin having the characteristics of a melting point of 88°C (hereinafter referred to as ionomer resin I), a 40-45 overlapping part, a Shore D hardness of 65 or more, a tensile strength of 275-320 kglorr, and Brittle temperature -
100 to -110°C, MI: 2.3 to 3.3, melting point 90°C Ionomer resin C (hereinafter referred to as ionomer resin ■) 40 to 45 parts by weight, Shore D
Hardness 60-64, tensile strength 200-230 kq/cm
and embrittlement temperature -70 to -80°C, Ml -8 to 12,
Ionomer resin C or below, ionomer resin ■ having the characteristics of a melting point of 96°C, 5 to 10 parts by weight, Shore D hardness 60 to 64, tensile strength 190 to 220 kq/
α and embrittlement temperature -75, -85°C, MI==4.5
It is a mixed resin consisting of 5 to 10 parts by weight of ionomer resin (hereinafter referred to as ionomer resin (hereinafter referred to as ionomer resin)) having the characteristics of ionomer resin C and melting point of 8.0°C and 94°C.

アイオノマー樹脂I= II、■および■の配合割合が
上舵範囲をはすれると本発明の所期の目的は達成し雛い
。アイオノマー樹脂■が40重置部以下ではボール初速
度が低下し、耐久性も低下し、また45重量部以上にな
ると低温耐久性が悪化する。アづオノマー樹脂■が40
重量部以下ではボが 成型性が悪化し、融着力が低下する。アイオノマー樹脂
■が5重量部以下では融着力が低下し、また10重量部
以上になるとボール初速度が低下する。アイオノマー樹
脂■が5重量部以下では成型性が悪化し、また10重量
部以上になるとポール初速度が低下する。
When the blending proportions of ionomer resin I=II, ■ and ■ are out of the upper rudder range, the intended object of the present invention is achieved. If the amount of ionomer resin (2) is less than 40 parts by weight, the initial velocity of the ball will be lowered and the durability will be lowered, and if it is more than 45 parts by weight, the low temperature durability will be deteriorated. Azuonomer resin ■ is 40
If the amount is less than 1 part by weight, the moldability will deteriorate and the fusion strength will decrease. If the amount of the ionomer resin (2) is less than 5 parts by weight, the fusing strength will be reduced, and if it is more than 10 parts by weight, the initial velocity of the ball will be reduced. If the amount of the ionomer resin (2) is less than 5 parts by weight, the moldability will deteriorate, and if it is more than 10 parts by weight, the initial velocity of the pole will decrease.

カバーをソリッドコアに被覆する方法は特に限定的では
ないが、通常は予め半球殻状に成形した2枚のカバーで
ソリッドコアを包み、約170℃で2分間加圧成形する
。また、カバー用組成物を射出成形してソリッドコアを
包みこんでもよい。
The method of covering the solid core with the cover is not particularly limited, but usually the solid core is wrapped with two covers that have been previously formed into a hemispherical shell shape, and the solid core is press-molded at about 170° C. for 2 minutes. Alternatively, the cover composition may be injection molded to enclose the solid core.

以上のようにして得られろソウ−ピースソリッドゴルフ
ボールは、従来の同種の製品においては不十分だった反
撥弾性(初速塵)および耐久性、特に低温耐久性並びに
打撃時のフィーリングの悪さを改良したゴルフボールで
ある。
The Sou-Piece solid golf ball obtained as described above has improved repulsion (initial velocity dust) and durability, especially low-temperature durability and poor feel when hitting, which were insufficient in conventional products of the same type. This is an improved golf ball.

以下、本発明を実施例によって説明する。Hereinafter, the present invention will be explained by examples.

実施例1および比較例1〜6 表−1の配合処方によるコア用組成物をモールド内で1
50°仁30分間加圧成形して直径37゜1 mノ〃0
ノコアを製造した。
Example 1 and Comparative Examples 1 to 6 The core composition according to the formulation shown in Table 1 was placed in a mold.
Pressure molded at 50° for 30 minutes to create a diameter of 37°1 m no.0
Manufactured by Nokoa.

得られたコアを、表−1の配合処方によるカッく−を用
い常法によって被覆してヌモール@Iイズツーピーヌゴ
ルフボールを製造した。
The obtained core was coated with a coating according to the formulation shown in Table 1 in a conventional manner to produce a Numol@I is two pine golf ball.

得られたボールの物性を表−1に示す。Table 1 shows the physical properties of the obtained ball.

表−1 1″デユポン製サーリン1605(シヨアD硬度67、
引張強度296 kglorr 、脆化温度−106℃
 1.MI=2.8、融点90℃)デュポン社製ザーリ
ン1.706(ショアーD硬度66、引張強度275 
kqlolt 、脆化温度−105°C,、MI=0.
7、融点88℃)31テュポン社製サーリン1555 
 (ンヨアーD硬度62、引張強度214 kqlo)
!、脆化温度−75℃ 、、、M1=IQ、融点96℃
)4′デュポン社製ザーリン1557(/コアー1)硬
度63、引張強度204 kQ/C〃t 、脆化1FI
A度−80°C、、MI=5.0、融点94°C)5ゝ
ツル一テンパー社製スイングロボットを用いて測定(ヘ
ッドヌピード451±Q、 3 m 7秒、ボール温度
25℃)。
Table-1 1″ Dupont Surlyn 1605 (Shore D hardness 67,
Tensile strength 296 kglorr, embrittlement temperature -106℃
1. MI=2.8, melting point 90°C) DuPont ZARLIN 1.706 (Shore D hardness 66, tensile strength 275
kqlolt, embrittlement temperature -105°C, MI=0.
7. Melting point 88℃) 31 Surlyn 1555 manufactured by Typhon
(Nyoar D hardness 62, tensile strength 214 kqlo)
! , embrittlement temperature -75°C, M1=IQ, melting point 96°C
) 4' DuPont ZARLIN 1557 (/core 1) Hardness 63, Tensile strength 204 kQ/C〃t, Brittleness 1FI
A degree -80°C, MI=5.0, melting point 94°C) Measured using a swing robot manufactured by Tsuruichi Temper Co., Ltd. (Head Nupedo 451±Q, 3 m 7 seconds, ball temperature 25°C).

6ゝ実施例1によるボールの耐衝撃回数を100とした
ときの相対値。
6. Relative value when the number of impact resistance of the ball according to Example 1 is set to 100.

71実施例1によるボールの耐衝撃回数を100とした
ときの相対値。
71 Relative value when the number of impact resistance of the ball according to Example 1 is set to 100.

Claims (1)

【特許請求の範囲】 ■、基材ゴム100重量部、不飽和脂肪酸の金属塩10
〜60重量部、酸化亜鉛40〜70重量部および架橋側
1〜5重量部含有する組成物を加熱硬化して得られるソ
リッドコアを、ショアーD硬度65以上、引張強度25
0〜300kg/cノrt2および脆化温度−100〜
−110℃、MI−07〜2.0、融点約88℃のアイ
オノマー樹脂40〜45重量部、ショアーD硬度65以
上、引張強度275〜320 kq/cnrおよび脆化
温度−100〜−1]0℃、M I : 2.3〜3.
3、融点90℃のアイオノマー杉」脂40〜45重量部
、ショアーD硬度60〜64、引張強度200〜230
 kglonおよび脆化温度−70〜−80℃、M I
 = 3〜12、融点96℃のアイオノマー樹脂5〜1
0重量部およびショアーD硬度60〜64、引張強度1
90〜2201cq/cm および脆化温度−75−−
85℃、M 1−4.5〜8.0、融点94℃のアイオ
ノマー樹脂5〜10重量部を主材とするカバーで被覆し
て成るツウ−ピースソリッドゴルフボール。 2、  基材−fムがシス1,4−ポリブタジェンゴム
である第1項記載のソリッドゴルフボール。 3、不飽和脂肪酸の金属塩がアクリル酸亜鉛および/ま
たはメタクリル酸亜鉛である第1項記載のソリッドゴル
フボール。 4、  架a剤がジクミルパーオキサイドである第1項
記載のソリッドゴルフボール。
[Claims] (1) 100 parts by weight of base rubber, 10 parts by weight of metal salt of unsaturated fatty acid
A solid core obtained by heating and curing a composition containing ~60 parts by weight, 40 to 70 parts by weight of zinc oxide, and 1 to 5 parts by weight of the crosslinked side has a Shore D hardness of 65 or more and a tensile strength of 25.
0~300kg/cnort2 and embrittlement temperature -100~
-110°C, MI-07 to 2.0, 40 to 45 parts by weight of ionomer resin with melting point of about 88°C, Shore D hardness of 65 or more, tensile strength of 275 to 320 kq/cnr, and embrittlement temperature of -100 to -1]0 °C, MI: 2.3-3.
3. Ionomer cedar fat with melting point of 90°C 40-45 parts by weight, Shore D hardness 60-64, tensile strength 200-230
kglon and embrittlement temperature -70~-80℃, MI
= 3-12, ionomer resin with melting point of 96°C 5-1
0 parts by weight and Shore D hardness 60-64, tensile strength 1
90-2201 cq/cm and embrittlement temperature -75--
A two-piece solid golf ball coated with a cover whose main material is 5 to 10 parts by weight of an ionomer resin having a temperature of 85°C, M 1-4.5 to 8.0, and a melting point of 94°C. 2. The solid golf ball according to item 1, wherein the base material is cis-1,4-polybutadiene rubber. 3. The solid golf ball according to item 1, wherein the metal salt of unsaturated fatty acid is zinc acrylate and/or zinc methacrylate. 4. The solid golf ball according to item 1, wherein the cross-linking agent is dicumyl peroxide.
JP57169144A 1982-09-27 1982-09-27 Two-piece solid golf ball Granted JPS5957675A (en)