Surface hardened pt alloy member for decoration

Info

Publication number
JPS59143032A
JPS59143032A JP1708683A JP1708683A JPS59143032A JP S59143032 A JPS59143032 A JP S59143032A JP 1708683 A JP1708683 A JP 1708683A JP 1708683 A JP1708683 A JP 1708683A JP S59143032 A JPS59143032 A JP S59143032A
Authority
JP
Japan
Prior art keywords
alloy member
dispersed
hardened
alloy
hard
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP1708683A
Other languages
Japanese (ja)
Other versions
JPS621469B2 (en
Inventor
Masaki Morikawa
正樹 森川
Hideaki Yoshida
秀昭 吉田
Toshiharu Hiji
臂 利玄
Fukuhisa Matsuda
松田 福久
Kazuhiro Nakada
一博 中田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsubishi Metal Corp
Original Assignee
Mitsubishi Metal Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsubishi Metal Corp filed Critical Mitsubishi Metal Corp
Priority to JP1708683A priority Critical patent/JPS59143032A/en
Publication of JPS59143032A publication Critical patent/JPS59143032A/en
Publication of JPS621469B2 publication Critical patent/JPS621469B2/ja
Granted legal-status Critical Current

Abstract

PURPOSE:To provide a titled alloy member having extremely high surface hardness and excellent wear resistance by forming a surface-hardened layer consisting of the texture dispersed therein with hard CrB on the surface of a Pt- Cr alloy member consisting of a specific compsn. CONSTITUTION:The surface of a Pt alloy member having the compsn. contg. 0.5-15wt% Cr, further contg. either one or both of 0.5-25% Pd and 0.5-15% >=1 kind among Cu, Ag, Ni, Co, Fe, Au and Ir according to need and the balance consisting of Pt and unavoidable impurities is subjected to a boriding treatment, then the B diffused and intruded from the surface reacts with the Cr solutionized mainly in the base, thereby forming hard CrB. A surface-hardened layer having extremely high hardness of about 1,000-1,500Hv dispersed with hard CrB is formed on the surface of the above-mentioned Pt alloy member and the beautiful decorative metallic gloss is maintained semipermanently.

Description

【発明の詳細な説明】 この発明は、著しく高い表面硬さを有し、したがって実
用に際してはすぐれた耐摩性を発揮する指輪やネックレ
スなどの装飾用pt合金部材に関するものである。
DETAILED DESCRIPTION OF THE INVENTION The present invention relates to decorative PT alloy members such as rings and necklaces that have extremely high surface hardness and therefore exhibit excellent wear resistance in practical use.

周知のように、PtはAuと同様に金属の中で最も安定
した金属であり、しかも美麗な金属光沢を長期に亘って
保持するほか、きわめて柔軟にして展延性にもすぐれ、
かつ細工が容易であることと相まって、Auと同様に装
飾用材料として広く用いられている。
As is well known, Pt, like Au, is the most stable metal among metals, retains a beautiful metallic luster for a long time, and is extremely flexible and malleable.
Coupled with the fact that it is easy to work with, it is widely used as a decorative material like Au.

また、ptはきわめて軟質であるため傷がつきゃすく、
したがってこれにCu、 kg、 Ni、 Co、 F
i’e、 Au。
Also, since PT is extremely soft, it is easily scratched.
Therefore, Cu, kg, Ni, Co, F
i'e, Au.

あるいはIrなどの金属を合金成分として含有させて適
度の強度をもたせたPt合金が、950プラチナ、85
0プラチナなどとして実用に供されている。
Alternatively, Pt alloys containing metals such as Ir as alloy components to give appropriate strength are 950 platinum and 85 platinum.
It is put into practical use as 0 platinum.

しかし、これらのpt金合金おいても、装飾品として身
につけた場合には、傷が容易につくものであり、比較的
早期に金属光沢が劣化するものである。
However, even when these PT gold alloys are worn as accessories, they are easily scratched and their metallic luster deteriorates relatively quickly.

さらに近年ダイヤカット法といわれる鋭い切込みによる
鮮明な模様を施した指輪やネックレスなどが普及してき
たが、従来のpt金合金は軟質のたメニエッソカ摩耗し
、模様が不鮮明になることがしばしば問題となっておシ
、これらの点がらも硬質なpt金合金要求が強まってい
る。
Furthermore, in recent years, rings and necklaces with clear patterns created by sharp cuts called the diamond cutting method have become popular, but conventional PT gold alloys are soft and often wear out, causing the patterns to become unclear. In view of these points, the demand for hard PT gold alloys is increasing.

一般に、pt合金部材を装飾品として身にっけたときK
、その表面に傷がつかないためには、pt合金部材の表
面硬さがHv(ビッカース硬さ)、4o○以上、好まし
くはHv:500以上がよいとされており、例えば腕時
計の文字盤ガラスの硬さはおよそHv:500であるか
ら%Hv:500以上の硬さをもったpt金合金できれ
ば、この文字盤ガラスでも傷がつかないpt合金製時計
が提供できることになる。
Generally, when wearing PT alloy members as accessories, K
In order to prevent scratches on the surface of the PT alloy member, it is said that the surface hardness of the PT alloy member should be Hv (Vickers hardness) of 4o○ or more, preferably Hv: 500 or more. Since the hardness of %Hv:500 is approximately Hv:500, if a PT gold alloy with a hardness of %Hv:500 or higher can be made, it will be possible to provide a PT alloy watch that will not be scratched even with this dial glass.

しかしながら、種々のpt金合金熱机理を施したり、あ
るいはさらに加工硬化を利用したりしても、得られる硬
さは精々Hv:350どまりであって、上記のような要
求を満足する硬質のpt合金部材は得られていないのが
現状である。
However, even if various PT gold alloys are subjected to thermal mechanics or work hardening is used, the hardness obtained is at most Hv: 350, and it is difficult to obtain a hard PT that satisfies the above requirements. Currently, alloy members are not available.

そこで、本発明者等は、上述のような観点から、硬質゛
、特に高い表面硬さを有するpt合金部材を得べく研究
を行なった結果、pt合金部材を、重量%で、Cr、0
,5〜15%を含有し、さらに必要に応じてPd、05
〜25%と、Cu、 Ag、 Ni、 Co、 Fe 
Therefore, from the above-mentioned viewpoint, the present inventors conducted research to obtain a PT alloy member having hardness, particularly high surface hardness.
, 5 to 15%, and optionally Pd, 05%.
~25%, Cu, Ag, Ni, Co, Fe
.

Au、および行のうちの1種または2種以上、05〜1
5%のいずれが、または両方を含有し、残9がptと不
可避不純物からなる組成を有するもので構成し、このp
t合金部材の表面にほう化処理を施すと、表面よシ拡散
侵入したBが主として素地に固溶しているCrと反応し
てきわめて硬質のほう化クロムを形成することがら、前
記pt合金部材の表面には硬質のほう化クロムが分散し
た組織を有する表面硬化層が形成されるようになり、こ
の表面硬化層はHv: 1000−1500の著しく高
い硬さをもつことがら、この結果の表面硬化pt合金部
材はきわめてすぐれた耐摩性を示し、半永久的に美麗な
金属光沢を保持するようになるという知見を得たのであ
る。
Au, and one or more of the rows, 05-1
5% contains one or both, and the remaining 9 consists of pt and unavoidable impurities, and this p
When the surface of the PT alloy member is subjected to boriding treatment, the B that has diffused into the surface reacts mainly with Cr dissolved in the base material to form extremely hard chromium boride. A hardened surface layer having a structure in which hard chromium boride is dispersed is formed on the surface of the It was discovered that the hardened PT alloy member exhibits extremely excellent wear resistance and retains a beautiful metallic luster semi-permanently.

この発明は、上記知見にもとづいてなされたものであっ
て、重量%で、 Cr:0.5〜15%。
This invention was made based on the above-mentioned knowledge, and includes: Cr: 0.5 to 15% by weight.

を含有し、さらに必要に応じて、 Pd:0.5〜25%と、 Cu + Ag + N1+ Co + Fe + A
u + および工rのうちの1種または2種以上゛o5
〜15%。
and, if necessary, Pd: 0.5 to 25%, Cu + Ag + N1+ Co + Fe + A
One or more of u + and k r゛o5
~15%.

のいずれか、または両方を含有し、残りがptと不可避
不純物からなる組成を有するpt合金部材の表面に、硬
質のほう化クロムが分散した組織を有する表面硬化層を
形成してなる装飾用表面硬化pt合金部材に特徴を有す
るものである。
A decorative surface formed by forming a hardened surface layer having a structure in which hard chromium boride is dispersed on the surface of a PT alloy member having a composition containing either or both of the above and the remainder consisting of PT and unavoidable impurities. This is characterized by a hardened PT alloy member.

つぎに、この発明のpt合金部拐において、成分組成範
囲を上記の通りに限定した理由を説明する。
Next, the reason why the composition range of the PT alloy of the present invention is limited as described above will be explained.

(a)Cr Cr成分には、素地に固溶して、これを強化するほか、
部材にほう化処理を施すと、硬質のほう化クロムを形成
して、その表面硬さを高めて耐摩性を著しく向」ニさせ
る作用があるが、その含有量が05%未満では所望の高
硬度をもった表面硬化層を形成することができず、一方
15%を越えて含有させると、部材自体の塑性加工性に
劣化傾向が現われるようになり、しかも表面硬化層によ
り一層の硬さ向上効果も期待できないことから、その含
有量を05〜15%と定めた。
(a) Cr The Cr component has a solid solution in the base material to strengthen it.
When a material is subjected to boriding treatment, it forms hard chromium boride, which increases its surface hardness and significantly improves wear resistance. However, if the content is less than 0.5%, the desired high It is not possible to form a surface hardening layer with hardness, and on the other hand, if the content exceeds 15%, the plastic workability of the component itself tends to deteriorate, and furthermore, the hardness is further improved by the surface hardening layer. Since no effect could be expected, its content was set at 05 to 15%.

(b)  pa Pd成分には、pt合金部材の延性を向上させる作用が
めるので、特に延性が要求される場合に必要に応じて含
有されるが、その含有量が0.5%未満では所望の靭性
向上効果が得られず、一方25%を越えて含有させると
、耐食性が低下するようになることから、その含有量を
05〜25%と定めた。
(b) pa The Pd component has the effect of improving the ductility of the PT alloy member, so it is included as necessary when particularly ductility is required, but if the content is less than 0.5%, the desired content cannot be achieved. The effect of improving toughness cannot be obtained, and if the content exceeds 25%, the corrosion resistance will decrease, so the content was set at 05 to 25%.

(c)  Cu、 Ag、 Ni+ Co、 Fe、 
Au、およびIrこれらの成分には、 pt合金部材を
強化する作用があるので、特に強度が要求される場合に
必要に応じて含有されるが、その含有量が05%未満で
は所望の強化をはかることができず、一方15%を越え
て含有させると、延性が低下するようになって塑性加工
が困難になることから、その含有量を05〜15%と定
めた。
(c) Cu, Ag, Ni+ Co, Fe,
Au and Ir These components have the effect of strengthening the PT alloy member, so they are included as necessary when particularly strong strength is required, but if their content is less than 0.5%, the desired strengthening cannot be achieved. On the other hand, if the content exceeds 15%, the ductility decreases and plastic working becomes difficult, so the content was set at 05 to 15%.

つぎに、この発明のpt合金部材を実施例により具体的
に説明する。
Next, the PT alloy member of the present invention will be specifically explained with reference to Examples.

実施例 TIGアークを用い、銅製水冷るつぼ内で、必要な合金
化金属と電解ptを溶解して、それぞれ第1表に示され
る成分組成をもったpt合金溶湯:logづつを調製し
た後、金型に鋳造してボタン状とし、ついで、これに表
面研磨を施して平面:lOB×厚さ:1mの寸法を有す
る試験片とし、この試験片に、予め黒鉛るつぼ内で加熱
溶融して800℃に保持しである溶融フラックス(組成
Example Using a TIG arc, necessary alloying metals and electrolytic PT were melted in a water-cooled copper crucible to prepare molten PT alloys (logs) each having the composition shown in Table 1. It is cast into a mold to form a button shape, and then its surface is polished to obtain a test piece having dimensions of flat surface: 1 OB x thickness: 1 m. Holds the molten flux (composition).

重量楚で、B4C: 80%、 H3POs : 10
%。
Weight: B4C: 80%, H3POs: 10
%.

Na2B4O7: 10%)中に8時間浸漬のほう化処
理を施した後、大気中に取出すことによって本発明pt
合全全部材〜27および比較Pt合金部材1〜8をそれ
ぞれ製造した。
The present invention's pt
Combined total members ~27 and comparative Pt alloy members 1~8 were manufactured, respectively.

ついで、この結果得られた各種の部材の表面最高硬さく
ビッカース硬さ)を測定した。これらの結果を第1表に
示した。なお、第1表にはほう化処理前の表面最高硬さ
も示した。
Then, the maximum surface hardness (Vickers hardness) of the various members obtained as a result was measured. These results are shown in Table 1. Furthermore, Table 1 also shows the maximum surface hardness before the boriding treatment.

なお、比較ptt金部材1〜8は、いずれも従来公知の
pt金合金ほう化処理を施したものである。
The comparative PTT gold members 1 to 8 were all subjected to a conventionally known PT gold alloy boriding treatment.

第1表に示される結果から、本発明ptt金部材]〜2
7は、いずれもほう化処理によシ表面硬さが一段と向上
し、Hv:500以上のきわめて高い表面硬さをもつの
に対して、Crを含有しない比較ptt金部材1〜8に
おいては、はう化処理を施しても硬質のほう化クロムが
分散した組織を有する表面硬化層の形成がないので、そ
の表面硬さはほとんど変らないことが明らかである。
From the results shown in Table 1, the PTT gold member of the present invention]~2
In contrast to the comparative PTT gold members 1 to 8, which do not contain Cr, the surface hardness of PTT gold members 1 to 8, which do not contain Cr, has a much higher surface hardness of Hv: 500 or more. It is clear that even if the fertilizing treatment is carried out, the surface hardness remains almost unchanged since no hardened surface layer having a structure in which hard chromium boride is dispersed is formed.

上述のように、この発明のptt金部材は、硬質のほう
化クロムが分散した組織の表面硬化層を有するので、こ
れを装飾用として使用した場合には著しく長期に亘って
原形を保持し、美的価値を損なうことがないなど工業上
有用な特性を有するのである。
As mentioned above, the PTT gold member of the present invention has a hardened surface layer with a structure in which hard chromium boride is dispersed, so when it is used for decoration, it retains its original shape for an extremely long period of time. It has industrially useful properties such as not impairing its aesthetic value.

出願人  三菱金属株式会社Applicant: Mitsubishi Metals Corporation

Claims (4)

【特許請求の範囲】[Claims] (1)  Cr: 0.5〜15%を含有し、残9がp
tと不可避不純物からなる組成(以上重量%)を有する
pt合金部材の表面に、硬質のほう化クロムが分散した
組織を有する表面硬化層を形成してなる装飾用表面硬化
pt合金部材。
(1) Cr: Contains 0.5 to 15%, the balance 9 is p
A surface hardened PT alloy member for decoration, comprising a surface hardened layer having a structure in which hard chromium boride is dispersed, on the surface of a PT alloy member having a composition (the above weight %) consisting of T and unavoidable impurities.
(2)  Cr: 0.5〜15%を含有し、さらにP
d05〜25%を含有し、残りがptと不可避不純物か
らなる組成(以上重量%)を有するpi合金部材の表面
に、硬質のほう化クロムが分散した組織を有する表面硬
化層を形成してなる装飾用表面硬化pt合金部材。
(2) Cr: Contains 0.5 to 15%, and further contains P
A hardened surface layer having a structure in which hard chromium boride is dispersed is formed on the surface of a Pi alloy member having a composition (weight%) containing d05 to 25% and the remainder consisting of PT and unavoidable impurities. Decorative surface hardened PT alloy parts.
(3)  Cr: 0.5〜15tybを含有し、さら
にCu、 Ag 。 iJl、 Co、 Fe 、Au + およびIrのう
ちの1種または2種以上、05〜15%を含有し、残り
がptと不可避不純物からなる組成(以上重量%)を有
゛するpt合金部材の表面に、硬質のほう化クロムが分
散した組織を有する表面硬化層を形成してなる装飾用表
面硬化pt合金部材。
(3) Cr: Contains 0.5 to 15 tyb, and further contains Cu and Ag. A PT alloy member containing 05 to 15% of one or more of Co, Fe, Au + and Ir, with the remainder consisting of PT and unavoidable impurities (weight %). A decorative surface-hardened PT alloy member formed with a surface-hardened layer having a structure in which hard chromium boride is dispersed.
(4)  Cr: O,,5〜15%を含有し、さらに
Pd:0.5〜25%と、Cu、 Ag 、 Ni 、
 Co、 F’e、 Au、および工rのうちの1種ま
たは2種以上  05〜コ、5饅とを含有し、残りがp
tと不可避不純物からなる組成(以上重量%)を有する
pt合金部材の表面に、硬質のほう化クロムが分散した
組織を有する表面硬化層を形成してなる装飾用表面硬化
pt合金部材。
(4) Contains Cr: O, 5-15%, further contains Pd: 0.5-25%, Cu, Ag, Ni,
Contains one or more of Co, F'e, Au, and 05 to 5, and the rest is p.
A surface hardened PT alloy member for decoration, comprising a surface hardened layer having a structure in which hard chromium boride is dispersed, on the surface of a PT alloy member having a composition (the above weight %) consisting of T and unavoidable impurities.
JP1708683A 1983-02-04 1983-02-04 Surface hardened pt alloy member for decoration Granted JPS59143032A (en)