JP3386222B2 JP05824594A JP5824594A JP3386222B2 JP 3386222 B2 JP3386222 B2 JP 3386222B2 JP 05824594 A JP05824594 A JP 05824594A JP 5824594 A JP5824594 A JP 5824594A JP 3386222 B2 JP3386222 B2 JP 3386222B2
Authority
JP
Japan
Prior art keywords
pigment
coating film
coated
titanium dioxide
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP05824594A
Other languages
Japanese (ja)
Other versions
JPH07241520A (en
Inventor
英造 新美
孝一 高橋
東 柳田
和広 木村
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Paint Co Ltd
Nippon Paint Holdings Co Ltd
Original Assignee
Nippon Paint Co Ltd
Nippon Paint Holdings Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Paint Co Ltd, Nippon Paint Holdings Co Ltd filed Critical Nippon Paint Co Ltd
Priority to JP05824594A priority Critical patent/JP3386222B2/en
Publication of JPH07241520A publication Critical patent/JPH07241520A/en
Application granted granted Critical
Publication of JP3386222B2 publication Critical patent/JP3386222B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Links

Landscapes

  • Application Of Or Painting With Fluid Materials (AREA)

Description

【発明の詳細な説明】 【0001】 【産業上の利用分野】本発明は、自動車およびその部品
類、自転車、家電製品などを対象とする工業塗装に有用
な意匠塗膜形成方法に係り、詳しくは、彩度が高く、濁
りがなく、着色下地の色感を再現するパール調光輝感を
与える意匠性に優れた複層塗膜の形成方法に関する。 【0002】 【従来の技術】従来、塗膜にパール調光輝感を与える塗
料成分として鱗片状雲母の表面に二酸化チタンの薄膜を
コーティングしたシルバおよび干渉雲母チタンが用いら
れている。塗膜の形成は該雲母顔料を含む塗料を着色し
た下地塗膜上に塗布し、さらにクリヤーコートを形成す
る3コート系の複層塗膜形成法によって行われている。 【0003】この種のシルバおよび干渉雲母チタンを含
む塗料系の塗装技術としては、例えば粒子サイズが5〜
25μm の二酸化チタン被覆雲母顔料を含むラッカーを
塗装し、更にクリヤラッカーを塗装する真珠光沢顔料に
よるラッカー塗装方法(特開昭58−166964号公報)、マ
ンセルカラーチャートでN−4〜N−8のカラーベース
上に6〜13%(樹脂固形分比)の主として二酸化チタ
ンからなる金属酸化物で被覆した雲母を含む透明なパー
ル塗膜を塗装し、さらにトップクリヤーコートを塗装す
る被覆方法(特開昭61−37423 号公報) 、着色下地塗膜
上にチタナイズドマイカ顔料を含有する低隠蔽塗料を上
塗りする場合、チタナイズドマイカ顔料としてその顔料
干渉色が着色下地塗膜の色相と同系統のものを用いる塗
装仕上げ方法(特開昭59−160571号公報)等が提案され
ている。 【0004】これら二酸化チタン被覆雲母顔料の基材と
しては、優れた光輝性を得るために表面が平滑で薄片状
の天然白雲母が選択的に使用されている。ところが、天
然白雲母には不純物として微量の鉄分、泥土等が含まれ
ており、これら成分が被覆した水酸化チタンを焼成して
TiO2 に転化させる際に酸化されて淡黄色や微黄褐色
を呈する現象を惹起する。このような現象が発生する
と、白雲母特有の純粋な白色性が阻害され、シェード部
において底濁りの視感を与える。 【0005】このような問題を解消するために、被覆基
材を透明性の高い薄片状硫酸バリウム単結晶とした二酸
化チタン被覆硫酸バリウム顔料からなる真珠様光沢組成
物とその製造方法が本出願人の一人によって開発されて
いる(特公昭47−24930 号公報) 。 【0006】 【発明が解決しようとする課題】上記の二酸化チタン被
覆薄片状硫酸バリウム顔料は、二酸化チタン被覆雲母顔
料に比べて透明感に優れるうえに、純粋な単結晶である
ため着色原因となる不純物が含まれていない。したがっ
て、上述した二酸化チタン被覆雲母顔料を用いる際の色
相上の問題は解消されるものの、光輝感が乏しい難点が
あった。 【0007】本発明者らは、上記のような二酸化チタン
被覆雲母顔料および二酸化チタン被覆薄片状硫酸バリウ
ム顔料に固有の欠点を解決すべく鋭意研究を重ねた結
果、これら二酸化チタン被覆雲母顔料と二酸化チタン被
覆薄片状硫酸バリウム顔料を特定範囲の量比で配合して
塗料化し、これを一定の明度および彩度を有する着色下
地塗装面に塗布し、更に上面にクリヤー塗膜を形成する
と、両顔料成分が個々の欠点を相互に補完し合って着色
下地の色相を示すパール調光輝感が発現する事実を確認
した。 【0008】本発明は前記の知見に基づいて開発された
もので、その目的は、彩度が高くてシェード部での底濁
り感がなく、着色下地の色調を再現する優れたパール調
光輝感を与える意匠塗膜形成方法を提供することにあ
る。 【0009】 【課題を解決するための手段】上記の目的を達成するた
めの本発明による意匠塗膜形成方法は、下記 (1)〜(3)
の塗膜形成工程を順次に施すことを構成上の特徴とす
る。 (1)マンセル表示系における明度が3以上で、彩度が2
以上の着色下地層塗膜形成工程 (2)重量比(P1/P2)で95/5〜50/50の範囲にあ
る二酸化チタン被覆薄片状硫酸バリウム顔料(P1)と二酸
化チタン被覆雲母顔料(P2)からなる組成の光輝性顔料
を、樹脂固形分100重量部当たり3〜10重量部含有
する光輝層塗膜形成工程、および (3)クリヤー塗膜形成工程 【0010】本発明の意匠塗膜形成対象となる被塗物
は、鉄、アルミニウム、銅もしくはこれらの合金を含む
金属類を始めとして、ガラス、セメント、コンクリート
などの無機材料、ポリエチレン、ポリプロピレン、エチ
レン−酢酸ビニル共重合体、ポリアミド、ポリアクリ
ル、ポリエステル、エチレン−ポリビニルアルコール共
重合体、塩化ビニル、塩化ビニリデン、ポリカーボネー
ト、ポリウレタン等の樹脂成形品および各種FRPなど
のプラスチック材料、木材、繊維材料が該当する。な
お、これら被塗基材に予め適宜なアンダーコートやプレ
コート処理を施すことは任意である。 【0011】塗装は被塗物に直接塗布することもできる
が、例えば自動車の塗装等においては、通常、表面化成
処理後に電着塗料などによる下塗り塗装を施し、塗膜が
硬化した後に塗膜を形成する。塗装方法としては、霧化
式塗装やロールコーター式塗装が使用されるが、特に霧
化式塗装法によるエアスプレー塗装、静電塗装などが好
適に用いられる。 【0012】被塗物には、まず一般的にカラー中塗り塗
料と称される着色下地塗膜を形成する。カラー中塗り塗
料に使用される顔料は、塗料用に常用される有機系、無
機系の各種着色顔料および体質顔料が使用可能である。
着色顔料としては、例えば有機系のアゾレーキ系顔料、
不溶性アゾ系顔料、縮合アゾ系顔料、フタロシアニン系
顔料、インジゴ系顔料、ペリノン系顔料、ペリレン系顔
料、ジオキサジン系顔料、キナクリドン系顔料、イソイ
ンドリノン系顔料、金属錯体顔料など、無機系の黄鉛、
黄色酸化鉄、ベンガラ、カーボンブラック、二酸化チタ
ンなど、体質顔料として炭酸カルシウム、硫酸バリウ
ム、クレー、タルクなどが用いられる。また、塗膜形成
用のビヒクルとなる樹脂としては、アクリル樹脂、ポリ
エステル樹脂、アルキド樹脂などの基本樹脂にアミノ樹
脂や(ブロック)ポリイソシアネートなどの架橋剤を混
合した系が挙げられる。このほか、常温乾燥により硬化
することができる2液型ポリウレタン樹脂やシリコーン
樹脂なども用いられる。形成する着色下地塗膜の乾燥膜
厚は、25〜50μm 、好ましくは30〜40μm の範
囲である。 【0013】この工程で形成する着色下地塗膜は、着色
顔料とビヒクル樹脂との配合比率を制御して、塗膜の色
相がマンセル表示系で明度が3以上、彩度が2以上にな
るように調整する。明度が3未満になると白ぼけ感が生
じたり色むらが発生するようになり、また彩度が2を下
廻ると底濁り感が増大するようになって、いずれの場合
も着色下地の色調を効果的に再現するパール調光輝感を
発現することができなくなる。特に好ましい着色下地塗
膜の色相は、マンセル表示系の明度が6以上、彩度が4
以上である。 【0014】着色下地塗膜面には、二酸化チタン被覆薄
片状硫酸バリウム顔料と二酸化チタン被覆雲母顔料を配
合した光輝性顔料を含む塗料をドライオンウエットによ
り塗装して光輝層塗膜を形成する。工程によっては、ウ
エットオンウエットによることも可能である。 【0015】光輝性塗料を構成する二酸化チタン被覆薄
片状硫酸バリウム顔料(P1)は、薄片状硫酸バリウム単結
晶粉末の表面に二酸化チタンが薄層としてコーティング
された被覆組成を有するもので、次のようにして調製す
ることができる。硫酸塩濃度が0.5〜0.001mol/
l の可溶性硫酸塩溶液にバリウム塩濃度が0.5〜0.
001mol/l の可溶性バリウム塩溶液を加え、常温から
沸点まで酸性pH領域の条件下で反応させて大きさが5
〜100μm 、厚さが0.05〜1μm 程度の薄片状硫
酸バリウムの単結晶を生成する。例えば、塩酸によりp
H3に調整し、40℃に加温した硫酸アンモニウムの
0.01モル溶液10l に、40℃に加温した塩化バリ
ウムの0.02モル溶液5.5l を加えて反応させる
と、長径5〜100μm 、短径5〜30μm の薄片アス
ペクト性状を備えるやや変形した硫酸バリウムの菱形結
晶は生成する。好ましくは、長径10〜40μm 、短径
5〜30μm である。 【0016】得られた薄片状硫酸バリウムを水洗し、分
級したのち純水に懸濁させ、硫酸チタニル、四塩化チタ
ンその他の水溶性チタン化合物あるいは錯化合物を加え
て熱もしくはアルカリにより加水分解する。この加水分
解により薄片状硫酸バリウムの表面に付着した水酸化チ
タンを水洗後の焼成処理することにより、二酸化チタン
として薄層被覆される。この工程では、着色を妨げない
範囲で、錫やジルコニウム等の金属酸化物を添加しても
よい。このようにして、真珠光沢と干渉性をもつパール
光輝感の二酸化チタン被覆薄片状硫酸バリウム顔料が得
られる。 【0017】一方、二酸化チタン被覆雲母顔料(P2)とし
ては雲母微粉末に二酸化チタンが薄層でコーティングさ
れた真珠光沢を発するものが用いられ、上記の二酸化チ
タン被覆薄片状硫酸バリウム顔料と併用して配合され
る。二酸化チタン被覆薄片状硫酸バリウム顔料(P1)と二
酸化チタン被覆雲母顔料(P2)の配合比率は、重量比(P1/
P2) として95/5〜50/50の範囲に設定する。二
酸化チタン被覆雲母顔料の配合比率が前記範囲を下廻る
と光輝感が減退し、また前記範囲を越えると底濁り感が
強まって着色下地塗膜の色相が濁るようになる。より好
ましい配合重量比(P1/P2) は、80/20〜50/50
の範囲である。 【0018】二酸化チタン被覆薄片状硫酸バリウム顔料
と二酸化チタン被覆雲母顔料を配合した組成の光輝性顔
料は、ビヒクル成分に混合して光輝性塗料を作製する。
ビヒクルとなる樹脂としては、アクリル樹脂、ポリエス
テル樹脂、アルキド樹脂、シリコン樹脂、フッ素樹脂な
どの基体樹脂にアミノ樹脂や(ブロック)ポリイソシア
ネートなどの架橋剤と混合して使用されるが、これら樹
脂は1種に限らず2種以上を組み合わせて使用すること
もできる。このほか、常温乾燥により硬化することがで
きる2液型ポリウレタン樹脂やシリコーン樹脂なども用
いられる。 【0019】ビヒクル樹脂に対する光輝性顔料の添加量
は、樹脂固形分100重量部当たり3〜10重量部、好
ましくは4〜8重量部である。この添加量が3重量部を
下廻ると干渉色および光輝感が低下し、10重量部を越
えると光輝感が強すぎて白ぼけしたり、着色下地色の再
現化が減退する。形成する光輝層塗膜の厚さは、乾燥膜
厚として10〜30μm の範囲が好適である。 【0020】上記の光輝性塗料には、微小樹脂粒からな
る架橋重合体微粒子を加えてもよく、この添加は粘性を
制御し、塗膜の外観を改善するために有効に機能する。
該架橋重合体微粒子は、例えばエチレン性不飽和単量体
を架橋性の共重合単量体と水性媒体中でサスペンジョン
重合または乳化重合させ、得られた微小樹脂粒子分散液
を溶媒置換、共沸、遠心分離乾燥などにより水を除去す
る方法、脂肪酸炭化水素などの低SP有機溶媒またはエ
ステル、ケトン、アルコールなどの高SP有機溶媒のよ
うにモノマーは溶解するが重合体は溶解しない非水性有
機溶媒中で、エチレン性不飽和単量体と架橋性共重合体
とを共重合させ、得られた微小樹脂粒子(共重合体)を
分散させる方法(NAD法または沈殿析出法と称され
る)などにより製造される。このほか、特開昭58−1
29066号公報に記載のある両イオン性基を有する水
溶性樹脂を使用する方法を採用してもよい。 【0021】添加する架橋重合体微粒子は、平均粒径が
0.01〜10μm の範囲にあることが好ましく、例え
ば日本ペイント(株)製のAZS797、AZS597
などが好適に使用される。配合量は、樹脂固形分100
重量部に対して、好ましくは0.1〜20重量部、より
好ましくは0.5〜10重量部とする。 【0022】このほか、光輝性塗料には従来の塗料組成
物に常用されている各種の添加剤を任意に配合すること
ができる。添加剤としては、例えば酸化ポリエチレンワ
ックスおよびポリアマイドワックス等の沈降防止剤、ド
デシルベンゼンスルホン酸等の硬化触媒、ベンゾトリア
ゾール系の紫外線吸収剤、ベンゾフェノール系の酸化防
止剤、シリコーンや有機高分子等の表面調整剤、タレ止
め剤、増粘剤などが挙げられる。これらの成分は、通
常、塗膜形成用樹脂100重量部に対し5重量部以下の
配合量で塗料や塗膜の性能を改善することができる。 【0023】なお、上塗り塗料は有機溶媒型が一般的で
あるが、これに限られるものではなく非水分散液型、水
溶液型、水分散液型など各種の形態として塗料構成する
ことができる。製造時の固形分は、30〜70重量%が
好ましい。塗装に際しては、有機溶剤、水等の溶媒で塗
装適性粘度に希釈して用いるが、塗装時の固形分は10
〜50重量%が好ましい。 【0024】ついで、光輝性塗膜面にクリヤー塗料をウ
エットオンウエット方式で塗布し、クリヤー塗膜を形成
する。クリヤー塗料としては、光輝性塗料に用いたビヒ
クル樹脂と同様の一般に常用される透明性樹脂が使用さ
れる。光輝性塗膜とクリヤー塗膜は、2コート1ベーク
方式により同時に硬化させて複合塗膜を形成する。形成
するクリヤー塗膜の好ましい乾燥膜厚は、30〜60μ
m である。 【0025】 【作用】本発明の意匠塗膜形成方法は、一定以上の色相
を有する着色下地塗膜面に、光輝性顔料成分を含む塗料
を塗布して光輝性塗膜を形成し、更にクリヤー塗膜を形
成する工程からなるが、特に光輝性顔料として特定比率
範囲で配合された二酸化チタン被覆薄片状硫酸バリウム
と二酸化チタン被覆雲母顔料からなる組成の光輝性顔料
成分を選択使用したところに目的の作用効果をもたらす
主要な構成要素がある。すなわち、光輝性顔料の基材と
なる硫酸バリウムの屈折率は1.64で他方の基材とな
る雲母の屈折率1.54〜1.59に近似している。こ
のため、二酸化チタン被覆薄片状硫酸バリウム顔料は、
塗膜内部で高度な透明度を示し、そのうえ基材が単結晶
であって不純物が含有されていないため顔料自体に濁り
がない。一方、二酸化チタン被覆雲母顔料は、二酸化チ
タン被覆薄片状硫酸バリウム顔料が引き起こす光輝感の
弱化現象を補完するために機能する。 【0026】このような顔料成分の相互補完機能は、二
酸化チタン被覆薄片状硫酸バリウム(P1)と二酸化チタン
被覆雲母顔料(P2)を重量比(P1/P2) で95/5〜50/
50の範囲に設定した場合に効果的に発揮され、着色下
地塗膜の明度および彩度の低下を最小限に留めた状態
で、底濁り感、白ぼけ感および色むら等を伴うことなく
着色下地の色相を鮮明に再現するパール調光輝感を発現
する。したがって、常に意匠性に優れる光輝性塗膜を形
成することが可能となる。 【0027】 【実施例】以下、本発明の実施例を比較例と対比して具
体的に説明する。各例で適用した二酸化チタン被覆薄膜
状硫酸バリウム顔料(P1)、二酸化チタン被覆雲母顔料(P
2)および塗膜形成樹脂等は下記の市販品とした。なお、
表1〜7における前記成分の表示は各成分の前に示した
記号によった。配合量は固形分の重量部で示した。 【0028】二酸化チタン被覆薄片状硫酸バリウム顔料
(P1); (P1a) 日本光研工業(株)製、“ジェネスター710
1”(シルバー色) (P1b) 日本光研工業(株)製、“ジェネスター720
1”(干渉ゴールド) 二酸化チタン被覆雲母顔料(P2); (P2a) メルクジャパン社製、“イリオジン103WII”
(シルバー色) (P2b) メルクジャパン社製、“イリオジン205WII”
(干渉ゴールド) 酸化鉄被覆雲母顔料(P3:比較例用) ; (P3)メルクジャパン社製、“NPラセットWII” 塗膜形成樹脂; アクリル樹脂は、スチレン/メチルメタアクリレート/
エチルアクリレート・ヒドロキシエチルメタアクリレー
ト/メタアクリル酸の共重合体、数平均分子量2000
0、水酸基価45、酸価15、固形分50%。メラミン
樹脂は三井東圧化学(株)製、“ユーバン20SE”
(固形分60%) を用いた。 【0029】実施例1〜16、比較例1〜17 リン酸亜鉛で化成処理した厚さ0.8mmのダル鋼板基材
に、カチオン電着塗料〔日本ペイント(株)製、“パワ
ートップU−50”〕を乾燥塗膜が25μm になるよう
に塗装したのち、160℃で30分間焼付けた。この電
着塗膜面にポリエステル/メラミン樹脂系の中塗塗料
〔日本ペイント(株)製、“オルガS−90シーラー”
ブルー、エロー、グリーン、レッド、ブルーグリーン、
エンジ〕を乾燥塗膜が40μm になるようにエアスプレ
ー塗装し、140℃で30分間焼付けして試験板を作製
した。形成した着色下地塗膜につき、マンセル色票と合
わせてそれぞれ色相を測定した(表1〜7の上部欄外に
表示)。 【0030】二酸化チタン被覆薄片状硫酸バリウム顔料
(P1)と二酸化チタン被覆雲母顔料(P2)を所定の重量比(P
1/P2) で、樹脂固形分100重量部に対する光輝性顔料
の配合量を各表の含有量で示した割合に配合し、これを
塗料形成樹脂〔アクリル樹脂/メラミン樹脂=80/20(固
形分) 〕に混合して光輝性塗料を調製した。この光輝性
塗料を、フォードカップ#4で20℃、12〜15秒と
なるように溶剤(トルエン/キシレン/酢酸エチル/酢
酸ブチル=70/15/10/5)で粘度調整し、乾燥塗膜が15
μm になるように試験片の着色下地塗膜面に塗装した。
塗装は静電塗装機〔ランズバーグゲマ社製、Auto
REA〕を用い霧化圧2.8kg/cm2でおこない、塗装中
のブースの雰囲気は温度25℃、湿度75%に保持し
た。 【0031】塗装後3分間セッティングを施したのち、
アクリル/メラミン樹脂系クリヤー塗料〔日本ペイント
(株)製、“スーパーラック0−100”〕を乾燥膜厚
が約35μm になるようウエットオンウエットにより塗
装した。ついで、約10分間室温でセッティングしたの
ち、140℃で30分間焼付けた。 【0032】形成した塗膜につき、下記の基準でCIE
(L* , a* , b* )表示系における色相の光学測定、
および目視観察による底濁り感、白ぼけ感、光輝感、色
むらを判定評価した。その結果を、着色下地塗膜の中塗
色相毎に、光輝性塗料の二酸化チタン被覆薄片状硫酸バ
リウム顔料(P1)および二酸化チタン被覆雲母顔料(P2)の
種類、配合比(P1/P2) 、樹脂固形分100重量部に対す
る光輝性顔料の含有量(重量部)と対比させて表1〜7
に示した。なお、表6および表7は、着色下地層塗膜の
明度または彩度が本発明の要件範囲を外れる例である。 【0033】CIE(L* , a* , b* )表示系におけ
る色相の測定;変角分光測色計〔村上色彩研究所製、G
CMS−3型、D65光源、2度視野〕を用い、図1に示
すように塗膜形成した測定試料に対し垂線から45°の
角度で光源を照明し、その照明角度の正反射方向から光
源側に15°(ハイライト方向の受光点H)および11
0°(シェード方向の受光点S)の角度で同時に受光し
た。これを明度−彩度のL* a * b * 表色系により測色
し、明度(L* )、彩度(C* ) を測定した。C*
{(a* )2+(b* )21/2 により計算した。表中のΔL*
およびΔC* は、着色下地塗膜との差である。 【0034】目視判定評価の基準;目視観察による判定
評価の基準は、下記によった。 底濁り感:◎全くなし ○殆どなし □若干あり △あ
り ×強い 白ぼけ感:◎全くなし ○殆どなし □若干あり △あ
り ×強い 光輝感 :◎非常に強い ○強い □やや弱い △弱い
×なし 色むら :◎非常に強い ○強い □やや弱い △弱い
×なし 【0035】 【表1】 表注:S部はシェード部、H部はハイライト部を示す
(以下、同じ)。 【0036】 【表2】【0037】 【表3】【0038】 【表4】【0039】 【表5】【0040】 【表6】【0041】 【表7】 【0042】表1〜7の結果から、本発明により形成さ
れた実施例による意匠塗膜は相対的にΔL* およびΔC
* の幅が小さくなり、底濁り感、白ぼけ感が少なく、か
つ色むらのない優れた光輝性を保持している。これに対
し、本発明の要件を外れる比較例群は底濁り感、白ぼけ
感、光輝感および色むらの少なくとも1つの性能におい
て劣っており、実施例塗膜のような着色下地の色感を明
確に再現するパール調光輝感を発現させることができな
かった。 【0043】なお、本発明の好ましい態様は、以下のと
おりである。 (1)着色下地層塗膜を焼付硬化後、光輝性塗膜とクリヤ
ー塗膜をウエットオンウエット方式で形成する意匠塗膜
形成方法。 (2)光輝性塗膜中の二酸化チタン被覆薄片状硫酸バリウ
ム(P1)と二酸化チタン被覆雲母顔料(P2)の重量比(P1/P
2) が80/20〜50/50である意匠性塗膜形成方
法。 (3)光輝層塗膜中の光輝性顔料を樹脂固形分100重量
部当たり4〜8重量部とする意匠性塗膜形成方法。 (4)着色下地層塗膜のマンセル表示系における明度が6
以上、彩度が4以上である意匠性塗膜形成方法。 (5)光輝層塗膜中の二酸化チタン被覆薄片状硫酸バリウ
ム顔料(P1)の粒度が、長径5〜100μm 、短径5〜3
0μm である意匠性塗膜形成方法。 (6)着色下地層塗膜/光輝層塗膜/クリヤー塗膜の乾燥
膜厚が25〜50μm /10〜30μm /30〜60μ
m である意匠性塗膜形成方法。 (7)光輝層塗膜の樹脂がアクリル樹脂、ポリエステル樹
脂、アルキド樹脂、シリコン樹脂、フッ素樹脂から選ば
れた少なくとも1種の熱硬化性樹脂とアミノ樹脂および
/または(ブロック)ポリイソシアネートからなる架橋
剤の組合せである意匠性塗膜の形成方法。 (8)着色下地層塗膜を化成処理後、電着塗装された電着
塗膜層の上に形成する意匠性塗膜形成方法。 【0044】 【発明の効果】以上のとおり、本発明に係る意匠塗膜形
成方法に従えば、一定の色相を有する着色下地層塗膜面
に、特定配合比率の酸化チタン被覆薄片状硫酸バリウム
顔料と二酸化チタン被覆雲母顔料を含む光輝性塗膜、お
よびクリヤー塗膜を形成する工程を順次に施すことによ
り、濁りや色むらのない状態で着色下地の色感を再現す
るパール調光輝感の複層塗膜を得ることが可能となる。
したがって、優れた意匠性が要求される自動車車体の外
面塗装をはじめ、各種の被塗基材に対し高品位の複層塗
膜を形成する目的に極めて有用である。
Description: BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to a method for forming a design coating film useful for industrial coating of automobiles and parts thereof, bicycles, home electric appliances and the like. The present invention relates to a method for forming a multi-layer coating film having high chroma, no turbidity, and excellent esthetic properties giving a pearlescent luster that reproduces the color of a colored base. 2. Description of the Related Art Conventionally, silver and interference mica titanium having a thin film of titanium dioxide coated on the surface of flaky mica have been used as a paint component for imparting a pearlescent luster to a coating film. The coating film is formed by a three-coat multi-layer coating method in which a paint containing the mica pigment is applied on a colored undercoat film and a clear coat is formed. [0003] As a coating technique of a paint containing this kind of silver and interference mica titanium, for example, a particle size of 5 to 5 is used.
Lacquer coating method using pearlescent pigment (Japanese Patent Application Laid-Open No. 58-166964), in which a lacquer containing 25 μm titanium dioxide-coated mica pigment is applied, and then a clear lacquer is applied. A coating method in which a transparent pearl coating containing mica coated with a metal oxide mainly composed of titanium dioxide of 6 to 13% (resin solid content ratio) on a color base is applied, and a top clear coat is applied (Japanese Patent Application Laid-Open No. No. 61-37423), when a low concealment paint containing a titanized mica pigment is overcoated on a colored undercoat film, a titanized mica pigment whose pigment interference color is the same as the hue of the colored undercoat film is used. A paint finishing method to be used (JP-A-59-160571) and the like have been proposed. As a base material of these titanium dioxide-coated mica pigments, flaky natural muscovite having a smooth surface is selectively used in order to obtain excellent glitter. However, trace amounts as a natural muscovite impurity iron, are included mud, etc., of a pale yellow or slightly yellowish brown oxidized when by calcining titanium hydroxide which these components are coated is converted to TiO 2 Cause the phenomenon to be exhibited. When such a phenomenon occurs, pure whiteness peculiar to muscovite is disturbed, and the shade portion gives a sense of bottom turbidity. In order to solve such a problem, a pearl-like luster composition comprising a titanium dioxide-coated barium sulfate pigment in which the coated substrate is a highly transparent flaky barium sulfate single crystal and a method for producing the same have been proposed by the present applicant. (Japanese Patent Publication No. 47-24930). The above flaky barium sulfate pigment coated with titanium dioxide is excellent in transparency as compared with the mica pigment coated with titanium dioxide, and is a pure single crystal, which causes coloring. Contains no impurities. Therefore, although the problem of hue at the time of using the above-mentioned titanium dioxide-coated mica pigment is solved, there is a problem that luster is poor. The present inventors have conducted intensive studies to solve the above-mentioned drawbacks inherent in the titanium dioxide-coated mica pigment and the titanium dioxide-coated flaky barium sulfate pigment. As a result, these titanium dioxide-coated mica pigments and Titanium-coated flaky barium sulfate pigment is formulated into a paint by mixing it in a specific range of the amount ratio, and this is applied to a colored undercoating surface having a certain lightness and saturation, and then a clear coating film is formed on the upper surface. It was confirmed that the components complemented each other's disadvantages and developed a pearlescent luster that indicates the hue of the colored base. The present invention has been developed on the basis of the above findings, and has as its object to provide an excellent pearlescent luster that reproduces the color tone of a colored base without having a high saturation and no turbidity in a shade portion. And to provide a method for forming a design coating film. Means for Solving the Problems [0009] The method for forming a design coating film according to the present invention for achieving the above object includes the following (1) to (3).
The film forming process is sequentially performed. (1) The brightness in the Munsell display system is 3 or more and the saturation is 2
Above colored underlayer coating film forming step (2) Titanium dioxide-coated flaky barium sulfate pigment (P1) and titanium dioxide-coated mica pigment (P2) in weight ratio (P1 / P2) in the range of 95/5 to 50/50. A) a bright layer coating film containing 3 to 10 parts by weight per 100 parts by weight of resin solid content of a bright pigment having a composition comprising: (3) a clear film forming step; The object to be coated includes metals including iron, aluminum, copper or alloys thereof, glass, cement, inorganic materials such as concrete, polyethylene, polypropylene, ethylene-vinyl acetate copolymer, polyamide, poly Acrylic, polyester, ethylene-polyvinyl alcohol copolymer, vinyl chloride, vinylidene chloride, polycarbonate, polyurethane and other resin molded products and various FRP Plastic material, wood, fiber material is appropriate. It is optional to apply an appropriate undercoat or precoat treatment to these substrates in advance. The coating can be applied directly to the object to be coated. For example, in the case of coating an automobile, an undercoating such as an electrodeposition paint is usually applied after a surface chemical conversion treatment, and the coating is cured after the coating is cured. Form. As a coating method, an atomization type coating or a roll coater type coating is used. In particular, an air spray coating, an electrostatic coating or the like by the atomization type coating method is suitably used. First, a colored base coat generally called a color intermediate coat is formed on an object to be coated. As the pigment used for the color intermediate coating, various types of organic and inorganic coloring pigments and extenders commonly used for coatings can be used.
As the color pigment, for example, an organic azo lake pigment,
Inorganic graphite such as insoluble azo pigment, condensed azo pigment, phthalocyanine pigment, indigo pigment, perinone pigment, perylene pigment, dioxazine pigment, quinacridone pigment, isoindolinone pigment, metal complex pigment, etc. ,
Calcium carbonate, barium sulfate, clay, talc and the like are used as extenders such as yellow iron oxide, red iron oxide, carbon black and titanium dioxide. Examples of the resin serving as a vehicle for forming a coating film include a system in which a basic resin such as an acrylic resin, a polyester resin, or an alkyd resin is mixed with a crosslinking agent such as an amino resin or (block) polyisocyanate. In addition, a two-component polyurethane resin or silicone resin that can be cured by drying at room temperature is also used. The dry film thickness of the colored undercoat film to be formed is in the range of 25 to 50 μm, preferably 30 to 40 μm. The colored undercoating film formed in this step is controlled such that the hue of the coating film is 3 or more in Munsell display system and 2 or more in saturation by controlling the mixing ratio of the coloring pigment and the vehicle resin. Adjust to When the lightness is less than 3, a blurred feeling or uneven color is generated, and when the saturation is less than 2, the sense of bottom turbidity increases. It is not possible to express a pearlescent brightness that can be effectively reproduced. Particularly preferred hue of the colored undercoat film is Munsell display system having a lightness of 6 or more and a chroma of 4
That is all. On the surface of the colored undercoat film, a paint containing a glitter pigment obtained by mixing a flaky barium sulfate pigment coated with titanium dioxide and a mica pigment coated with titanium dioxide is applied by dry-on-wet to form a glitter layer coating film. Depending on the process, it is also possible to use wet-on-wet. The titanium dioxide-coated flaky barium sulfate pigment (P1) constituting the glittering paint has a coating composition in which titanium dioxide is coated as a thin layer on the surface of a flaky barium sulfate single crystal powder. It can be prepared as follows. Sulfate concentration of 0.5 to 0.001 mol /
l of soluble sulfate solution having a barium salt concentration of 0.5 to 0.1.
001 mol / l of a soluble barium salt solution was added, and the mixture was allowed to react under a condition of an acidic pH range from room temperature to the boiling point to obtain a solution having a size of 5%.
A single crystal of flaky barium sulfate having a thickness of about 100 μm and a thickness of about 0.05 to 1 μm is produced. For example, p
H3, 10 l of a 0.01 mol solution of ammonium sulfate heated to 40 DEG C. and 5.5 l of a 0.02 mol solution of barium chloride heated at 40 DEG C. were reacted to give a long diameter of 5-100 .mu.m. A slightly deformed rhombic crystal of barium sulfate having a flaky aspect with a minor axis of 5 to 30 μm is formed. Preferably, the major axis is 10 to 40 μm and the minor axis is 5 to 30 μm. The obtained flaky barium sulfate is washed with water, classified, suspended in pure water, and added with titanyl sulfate, titanium tetrachloride or another water-soluble titanium compound or complex compound, and hydrolyzed by heat or alkali. Titanium hydroxide adhered to the surface of the flaky barium sulfate by this hydrolysis is subjected to a baking treatment after washing with water, so that a thin layer is coated as titanium dioxide. In this step, a metal oxide such as tin or zirconium may be added as long as coloring is not hindered. In this way, a titanium dioxide-coated flaky barium sulfate pigment having pearl luster and interference and having pearl luster is obtained. On the other hand, as the mica pigment coated with titanium dioxide (P2), a mica fine powder coated with a thin layer of titanium dioxide to give a pearly luster is used, and is used in combination with the above-mentioned flaky barium sulfate pigment coated with titanium dioxide. Mixed. The compounding ratio of the titanium dioxide-coated flaky barium sulfate pigment (P1) and the titanium dioxide-coated mica pigment (P2) is the weight ratio (P1 /
P2) is set in the range of 95/5 to 50/50. If the blending ratio of the titanium dioxide-coated mica pigment falls below the above range, the glitter will decrease, and if it exceeds the range, the sense of bottom turbidity will increase and the hue of the colored undercoat film will become cloudy. More preferred weight ratio (P1 / P2) is 80/20 to 50/50.
Range. A brilliant pigment having a composition obtained by mixing a flaky barium sulfate pigment coated with titanium dioxide and a mica pigment coated with titanium dioxide is mixed with a vehicle component to prepare a brilliant paint.
As the vehicle resin, a base resin such as an acrylic resin, a polyester resin, an alkyd resin, a silicon resin, and a fluororesin is used by mixing with a crosslinking agent such as an amino resin or a (block) polyisocyanate. Not only one kind but also two or more kinds can be used in combination. In addition, a two-component polyurethane resin or silicone resin that can be cured by drying at room temperature is also used. The amount of the glitter pigment added to the vehicle resin is 3 to 10 parts by weight, preferably 4 to 8 parts by weight, per 100 parts by weight of the resin solids. When the addition amount is less than 3 parts by weight, the interference color and the brilliant feeling are reduced, and when the added amount is more than 10 parts by weight, the brilliant feeling is too strong to be blurred or the reproduction of the colored base color is reduced. The thickness of the bright layer coating film to be formed is preferably in the range of 10 to 30 μm as a dry film thickness. [0020] Crosslinked polymer fine particles consisting of fine resin particles may be added to the above-mentioned brilliant paint, and this addition effectively functions to control the viscosity and improve the appearance of the coating film.
The crosslinked polymer fine particles are, for example, suspension polymerization or emulsion polymerization of an ethylenically unsaturated monomer and a crosslinkable comonomer in an aqueous medium, and the resulting fine resin particle dispersion is solvent-exchanged, azeotropic. Non-aqueous organic solvents in which monomers dissolve but polymers do not dissolve like low SP organic solvents such as fatty acid hydrocarbons or high SP organic solvents such as esters, ketones, alcohols, etc. In which an ethylenically unsaturated monomer and a crosslinkable copolymer are copolymerized to disperse the obtained fine resin particles (copolymer) (referred to as NAD method or precipitation method) It is manufactured by In addition, JP-A-58-1
A method using a water-soluble resin having a zwitterionic group described in 29066 may be adopted. The added crosslinked polymer fine particles preferably have an average particle size in the range of 0.01 to 10 μm. For example, AZS797 and AZS597 manufactured by Nippon Paint Co., Ltd.
Are preferably used. The compounding amount is 100 resin solids.
The amount is preferably 0.1 to 20 parts by weight, more preferably 0.5 to 10 parts by weight with respect to parts by weight. In addition, various additives commonly used in conventional coating compositions can be arbitrarily added to the glittering coating. Examples of additives include anti-settling agents such as oxidized polyethylene wax and polyamide wax, curing catalysts such as dodecylbenzene sulfonic acid, benzotriazole-based ultraviolet absorbers, benzophenol-based antioxidants, silicone and organic polymers. Surface conditioners, anti-sagging agents, thickeners and the like. These components can generally improve the performance of paints and coatings in amounts of 5 parts by weight or less based on 100 parts by weight of the resin for forming a coating. The top coat is generally of an organic solvent type, but is not limited thereto, and can be formed in various forms such as a non-aqueous dispersion type, an aqueous solution type and an aqueous dispersion type. The solid content at the time of production is preferably 30 to 70% by weight. At the time of coating, it is diluted with a solvent such as an organic solvent or water to a coating-suitable viscosity and used.
~ 50% by weight is preferred. Next, a clear coating is applied to the surface of the bright coating film by a wet-on-wet method to form a clear coating film. As the clear paint, a commonly used transparent resin similar to the vehicle resin used for the glitter paint is used. The bright coating film and the clear coating film are simultaneously cured by a two-coat one-bake method to form a composite coating film. The preferred dry film thickness of the clear coating film to be formed is 30 to 60 μm.
m. According to the method for forming a design coating film of the present invention, a coating containing a glittering pigment component is applied to the surface of a colored undercoating film having a certain hue or more to form a glittering coating film, and further, a clear coating film is formed. It consists of the step of forming a coating film, but the purpose is to use a glittering pigment component composed of flaky barium sulfate coated with titanium dioxide and a mica pigment coated with titanium dioxide, particularly blended as a glittering pigment in a specific ratio range. There are major components that have the effect of That is, the refractive index of barium sulfate, which is the base material of the bright pigment, is 1.64, which is close to the refractive index of mica, which is the other base material, of 1.54 to 1.59. For this reason, flaky barium sulfate pigment coated with titanium dioxide,
The pigment has high transparency inside the coating film, and since the base material is single crystal and contains no impurities, the pigment itself is not turbid. On the other hand, the mica pigment coated with titanium dioxide functions to complement the phenomenon of weakening of the glitter caused by the flaky barium sulfate pigment coated with titanium dioxide. The function of complementing the pigment components is to provide a titanium dioxide-coated flaky barium sulfate (P1) and a titanium dioxide-coated mica pigment (P2) in a weight ratio (P1 / P2) of 95/5 to 50/50.
Effective when set to a range of 50, with no reduction in lightness and saturation of the colored base coating film, with no turbidity, blurring, uneven color, etc. It develops a pearlescent luster that clearly reproduces the hue of the base. Therefore, it is possible to always form a glittering coating film having excellent design properties. EXAMPLES Examples of the present invention will be specifically described below in comparison with comparative examples. The titanium dioxide-coated thin film barium sulfate pigment (P1) and titanium dioxide-coated mica pigment (P
2) and the film-forming resin were the following commercially available products. In addition,
The designation of the components in Tables 1 to 7 is in accordance with the symbol shown before each component. The amount was shown in parts by weight of the solid content. Flaky barium sulfate pigment coated with titanium dioxide
(P1); (P1a) Nippon Koken Kogyo Co., Ltd., “Genestar 710
1 "(silver color) (P1b) Nippon Koken Kogyo Co., Ltd.," Genestar 720
1 "(interference gold) Mica pigment coated with titanium dioxide (P2); (P2a)" Iriodin 103WII "manufactured by Merck Japan
(Silver color) (P2b) “Iriodin 205WII” manufactured by Merck Japan
(Interference Gold) Mica pigment coated with iron oxide (P3: for comparative example); (P3) “NP Lassett WII” film-forming resin manufactured by Merck Japan; acrylic resin is styrene / methyl methacrylate /
Ethyl acrylate / hydroxyethyl methacrylate / methacrylic acid copolymer, number average molecular weight 2000
0, hydroxyl value 45, acid value 15, solid content 50%. Melamine resin manufactured by Mitsui Toatsu Chemicals, "Uban 20SE"
(Solid content 60%). Examples 1 to 16 and Comparative Examples 1 to 17 A 0.8 mm-thick dull steel plate base material chemically treated with zinc phosphate was coated with a cationic electrodeposition paint [Nippon Paint Co., Ltd., “Power Top U- 50 "] was applied so that the dry coating film became 25 µm, and baked at 160 ° C for 30 minutes. A polyester / melamine resin intermediate coating [Nippon Paint Co., Ltd., “Olga S-90 Sealer”]
Blue, yellow, green, red, blue green,
Was spray-coated with air so that the dry coating film had a thickness of 40 μm, and baked at 140 ° C. for 30 minutes to prepare a test plate. The hue of each of the formed colored undercoat films was measured together with the Munsell color chart (displayed in the upper margin of Tables 1 to 7). Flaky barium sulfate pigment coated with titanium dioxide
(P1) and titanium dioxide-coated mica pigment (P2) in a predetermined weight ratio (P
1 / P2), the blending amount of the brilliant pigment with respect to 100 parts by weight of the resin solid content was blended in the ratio shown in the content of each table, and this was mixed with the paint forming resin [acrylic resin / melamine resin = 80/20 (solid )) To prepare a glittering paint. The viscosity of this glitter paint is adjusted with a solvent (toluene / xylene / ethyl acetate / butyl acetate = 70/15/10/5) in a Ford cup # 4 at 20 ° C. for 12 to 15 seconds. Is 15
The test piece was coated on the colored undercoat film surface so as to have a thickness of μm.
Coating is performed by an electrostatic coating machine [Auto manufactured by Randsburg Gema, Auto
REA] at an atomization pressure of 2.8 kg / cm 2 , and the booth atmosphere during coating was maintained at a temperature of 25 ° C. and a humidity of 75%. After setting for 3 minutes after painting,
An acrylic / melamine resin-based clear coating (“Super Rack 0-100”, manufactured by Nippon Paint Co., Ltd.) was applied by wet-on-wet so that the dry film thickness was about 35 μm. Then, after setting at room temperature for about 10 minutes, baking was performed at 140 ° C. for 30 minutes. The coating film thus formed was subjected to CIE according to the following criteria.
(L * , a * , b * ) optical measurement of hue in display system,
In addition, the feeling of bottom turbidity, the feeling of white blur, the feeling of glitter, and the unevenness of color by visual observation were evaluated. The results are shown for each intermediate coating hue of the colored base coat, the type, blending ratio (P1 / P2) of titanium dioxide-coated flaky barium sulfate pigment (P1) and titanium dioxide-coated mica pigment (P2) of glittering paint, and Tables 1 to 7 in comparison with the content (parts by weight) of the brilliant pigment based on 100 parts by weight of the solid content
It was shown to. Tables 6 and 7 are examples in which the brightness or the saturation of the colored underlayer coating film falls outside the required range of the present invention. Measurement of hue in CIE (L * , a * , b * ) display system; goniospectrocolorimeter [G
The CMS-3 type, D65 light source, 2 degree field of view] is used to illuminate the light source at an angle of 45 ° from the perpendicular to the coating-formed measurement sample as shown in FIG. 15 ° (light receiving point H in the highlight direction) and 11
Light was received simultaneously at an angle of 0 ° (light receiving point S in the shade direction). The color was measured using a lightness-chroma L * a * b * color system, and lightness (L * ) and chroma (C * ) were measured. C * was calculated by {(a *) 2 + ( b *) 2} 1/2. ΔL * in the table
And ΔC * are the differences from the colored base coat. Criteria for Evaluation by Visual Evaluation; The criteria for evaluation by visual observation were as follows. Bottom turbidity: ◎ None 殆 ど Almost none □ Somewhat △ Yes × Strong white blur: ◎ Nothing ○ Almost no □ Somewhat □ Somewhat △ Yes × Strong glitter: ◎ Very strong ○ Strong □ Somewhat weak △ Weak × No Color shading: ◎ Very strong ○ Strong □ Slightly weak △ Weak × None [Table 1] Table Note: S part shows shade part, H part shows highlight part (the same applies hereinafter). [Table 2] [Table 3] [Table 4] [Table 5] [Table 6] [Table 7] From the results shown in Tables 1 to 7, it can be seen from the results that the design coating films according to the examples formed according to the present invention have relatively ΔL * and ΔC.
The width of * is small, the feeling of turbidity and blurring is small, and excellent brightness without color unevenness is maintained. On the other hand, the comparative example group which does not satisfy the requirements of the present invention is inferior in at least one of performances of bottom turbidity, white blur, brilliantness and color unevenness, and shows the color sensation of a colored base such as the coating film of the example. It was not possible to develop a pearlescent luster that clearly reproduced. The preferred embodiments of the present invention are as follows. (1) A design coating film forming method in which a glittering coating film and a clear coating film are formed by a wet-on-wet method after baking and curing the colored underlayer coating film. (2) The weight ratio of titanium dioxide-coated flaky barium sulfate (P1) and titanium dioxide-coated mica pigment (P2) in the glittering coating film (P1 / P
2) A method for forming a decorative coating film, wherein is 80/20 to 50/50. (3) A method for forming a decorative coating film in which the glitter pigment in the glitter layer coating film is 4 to 8 parts by weight per 100 parts by weight of the resin solid content. (4) The lightness of the colored underlayer coating film in the Munsell display system is 6
As described above, a method for forming a decorative coating film having a saturation of 4 or more. (5) The particle size of the titanium dioxide-coated flaky barium sulfate pigment (P1) in the bright layer coating film is 5 to 100 μm in major axis and 5 to 3 in minor axis.
0 μm. (6) The dried film thickness of the colored underlayer coating film / bright layer coating film / clear coating film is 25 to 50 μm / 10 to 30 μm / 30 to 60 μm.
m. (7) Crosslinking wherein the resin of the bright layer coating film is at least one thermosetting resin selected from acrylic resin, polyester resin, alkyd resin, silicone resin, and fluororesin, and amino resin and / or (block) polyisocyanate. A method for forming a decorative coating film, which is a combination of agents. (8) A method for forming a decorative coating film in which a colored underlayer coating film is subjected to a chemical conversion treatment and then formed on the electrodeposited coating film layer which has been electrodeposited. As described above, according to the design coating film forming method according to the present invention, a titanium oxide-coated flaky barium sulfate pigment coated with a specific blending ratio is coated on the colored underlayer coating film surface having a fixed hue. A pearlescent luster that reproduces the color sensation of a colored base without turbidity or color unevenness by sequentially performing the process of forming a luminous coating containing mica pigment coated with titanium dioxide and titanium dioxide, and a clear coating. It is possible to obtain a layer coating film.
Therefore, it is extremely useful for the purpose of forming a high-quality multilayer coating film on various substrates to be coated, such as the exterior surface coating of an automobile body requiring excellent design properties.

【図面の簡単な説明】 【図1】実施例における色相測定法を示した説明図であ
る。
BRIEF DESCRIPTION OF THE DRAWINGS FIG. 1 is an explanatory diagram showing a hue measuring method in an example.

───────────────────────────────────────────────────── フロントページの続き (72)発明者 柳田 東 東京都立川市一番町6丁目1番地2 日 本光研工業株式会社内 (72)発明者 木村 和広 東京都立川市一番町6丁目1番地2 日 本光研工業株式会社内 (56)参考文献 特開 平5−163447(JP,A) 特開 平5−169019(JP,A) 特開 昭61−123673(JP,A) 特開 平5−311098(JP,A) 特開 昭58−21455(JP,A) 特開 平3−32784(JP,A) 特開 昭59−215857(JP,A) 特開 昭63−205177(JP,A) 特開 昭63−232882(JP,A) (58)調査した分野(Int.Cl.7,DB名) B05D 5/06 B05D 1/38 B05D 7/24 301 B05D 7/24 303 ──────────────────────────────────────────────────の Continuing on the front page (72) Inventor Yanagita Higashi 6-1, Ichibancho, Tachikawa-shi, Tokyo Nippon Koken Kogyo Co., Ltd. (72) Inventor Kazuhiro Kimura 6, Ichibancho, Tachikawa-shi, Tokyo No. 1 in Nihon Koken Kogyo Co., Ltd. (56) References JP-A-5-163447 (JP, A) JP-A-5-169019 (JP, A) JP-A-61-123673 (JP, A) JP-A-5-311098 (JP, A) JP-A-58-21455 (JP, A) JP-A-3-32784 (JP, A) JP-A-59-215857 (JP, A) JP-A-63-205177 (JP, A) JP, A) JP-A-63-232882 (JP, A) (58) Fields investigated (Int. Cl. 7 , DB name) B05D 5/06 B05D 1/38 B05D 7/24 301 B05D 7/24 303

Claims (1)

(57)【特許請求の範囲】 【請求項1】 下記 (1)〜(3) の塗膜形成工程を順次に
施すことを特徴とする意匠塗膜形成方法。 (1)マンセル表示系における明度が3以上で、彩度が2
以上の着色下地層塗膜形成工程 (2)重量比(P1/P2)で95/5〜50/50の範囲にあ
る二酸化チタン被覆薄片状硫酸バリウム顔料(P1)と二酸
化チタン被覆雲母顔料(P2)からなる組成の光輝性顔料
を、樹脂固形分100重量部当たり3〜10重量部含有
する光輝層塗膜形成工程、および (3)クリヤー塗膜形成工程
(57) [Claims] [Claim 1] A method for forming a design coating film, which comprises sequentially performing the following coating film forming steps (1) to (3). (1) The brightness in the Munsell display system is 3 or more and the saturation is 2
Above colored underlayer coating film forming step (2) Titanium dioxide-coated flaky barium sulfate pigment (P1) and titanium dioxide-coated mica pigment (P2) in weight ratio (P1 / P2) in the range of 95/5 to 50/50. And (3) a clear coating film-forming step in which a glitter pigment having a composition of 3 to 10 parts by weight per 100 parts by weight of resin solid content is contained.
JP05824594A 1994-03-03 1994-03-03 Design film formation method Expired - Lifetime JP3386222B2 (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP05824594A JP3386222B2 (en) 1994-03-03 1994-03-03 Design film formation method

Applications Claiming Priority (1)

Application Number Priority Date Filing Date Title
JP05824594A JP3386222B2 (en) 1994-03-03 1994-03-03 Design film formation method

Publications (2)

Publication Number Publication Date
JPH07241520A JPH07241520A (en) 1995-09-19
JP3386222B2 true JP3386222B2 (en) 2003-03-17

Family

ID=13078742

Family Applications (1)

Application Number Title Priority Date Filing Date
JP05824594A Expired - Lifetime JP3386222B2 (en) 1994-03-03 1994-03-03 Design film formation method

Country Status (1)

Country Link
JP (1) JP3386222B2 (en)

Families Citing this family (6)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JP3834350B2 (en) * 1996-03-14 2006-10-18 株式会社きもと Light reflecting material
JP4026696B2 (en) * 1998-02-27 2007-12-26 パイロットインキ株式会社 Magnetic display device
JP4958090B2 (en) * 2004-01-20 2012-06-20 関西ペイント株式会社 MULTILAYER COATING FORMATION METHOD AND COATED ARTICLE
JP4789508B2 (en) * 2005-05-25 2011-10-12 トヨタ自動車株式会社 Method for producing silver-colored pearlescent pigment
JP2012170909A (en) * 2011-02-22 2012-09-10 Kansai Paint Co Ltd Multi-layered coating film forming method
JP2012170910A (en) * 2011-02-22 2012-09-10 Kansai Paint Co Ltd Multi-layered coating film forming method

Also Published As

Publication number Publication date
JPH07241520A (en) 1995-09-19

Similar Documents

Publication Publication Date Title
JPH0811219B2 (en) Paint finish method
JP6468554B2 (en) Multi-layer coating formation method
JP3386222B2 (en) Design film formation method
JP3123697B2 (en) Coating
JP4031562B2 (en) Glittering paint composition and method for forming glittering composite coating film
JP4170806B2 (en) Multilayer coating film forming method, multilayer coating film and article
JP2004358329A (en) Method for forming bright metallic coating film
JP2011251253A (en) Method of forming multilayer coating film
JPH09323064A (en) Formation of bright coating film and coated material
JP3159884B2 (en) Paint composition and coating film forming method
JP4063358B2 (en) Method for repairing laminated coating film and coating composition for repair
JPH08170034A (en) Metallic coating composition and formation of film
JP2829813B2 (en) Metallic coating composition and method for forming metallic coating film
JP4314469B2 (en) LAMINATED COATING FORMATION METHOD, LAMINATED COATING AND COATED PRODUCT
JP4290837B2 (en) Method for forming metallic coating film
JP3370204B2 (en) Bright coating film forming method
JPS62210081A (en) Method for applying pearl gloss pigment-containing paint
JPH10296170A (en) Formation of plural-layer coating film
JPH08155384A (en) Double layered coated film-forming method
JP2005144338A (en) Coating method
JPH101625A (en) Coating material composition, formation of coated film and coated material
JP4638771B2 (en) White pearl coating film forming method and laminated coating film
JPH05311098A (en) Metallic coating composition and formation of multilayer coating film
JPH0716534A (en) Formation of double-layered film
JPH04200778A (en) Method for forming mat film

Legal Events

Date Code Title Description
R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20090110

Year of fee payment: 6

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20090110

Year of fee payment: 6

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20100110

Year of fee payment: 7

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20110110

Year of fee payment: 8

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20110110

Year of fee payment: 8

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20120110

Year of fee payment: 9

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20120110

Year of fee payment: 9

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20130110

Year of fee payment: 10

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20130110

Year of fee payment: 10

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20140110

Year of fee payment: 11

R250 Receipt of annual fees

Free format text: JAPANESE INTERMEDIATE CODE: R250

EXPY Cancellation because of completion of term