JP2005105455A - Woven fabric - Google Patents
Woven fabric Download PDFInfo
- Publication number
- JP2005105455A JP2005105455A JP2003339196A JP2003339196A JP2005105455A JP 2005105455 A JP2005105455 A JP 2005105455A JP 2003339196 A JP2003339196 A JP 2003339196A JP 2003339196 A JP2003339196 A JP 2003339196A JP 2005105455 A JP2005105455 A JP 2005105455A
- Authority
- JP
- Japan
- Prior art keywords
- woven fabric
- warp
- dyeing
- weft
- fabric
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
本発明は織物に関する。より詳細には、通気性、すべり性に優れ、かつ、目ズレの生じにくい裏地用途に好適な織物に関する。 The present invention relates to a fabric. More specifically, the present invention relates to a woven fabric that is excellent in breathability and slipperiness and suitable for lining applications that are less likely to cause misalignment.
従来から、衣料に清涼性を付与するために、高い通気性を有する織物、例えば、織目が粗く、比較的薄地の織物等が用いられていた。清涼性の高い衣料として、和服では、絡み織り組織からなる織物(以下、絡み織物、と称する)が用いられていた。
上衣や裏地に通気性を付与するために、特定構造の絡み織物を用いることが知られている(例えば、特許文献1参照)。しかし、裏地に用いられる織物には、目ズレが生じにくく、すべり性に優れることが必要であるが、絡み織物でこれらの性能を全て満足することは困難であった。特に必要とされる通気性レベルを得るためにはトータルカバーファクターが1800以下とする必要があるが、目ズレの発生が顕著となる。特許文献1では、絡み織物を有撚糸で構成することにより目ズレが改善されることが開示されているが、その効果は充分ではなく、裏地用途に必要なすべり性が低下する問題が発生する。
In order to impart breathability to an upper garment or a lining, it is known to use a woven fabric having a specific structure (see, for example, Patent Document 1). However, the woven fabric used for the lining needs to be free from misalignment and excellent in slipperiness, but it has been difficult to satisfy all of these performances with the entangled fabric. In particular, in order to obtain the required air permeability level, the total cover factor needs to be 1800 or less, but the occurrence of misalignment becomes significant. In Patent Document 1, it is disclosed that the misalignment is improved by configuring the entangled fabric with twisted yarn, but the effect is not sufficient, and the problem that the slipperiness necessary for the lining use is reduced occurs. .
本発明は通気性、すべり性に優れ、かつ、目ズレの生じにくい織物を提供することを目的とするものである。 An object of the present invention is to provide a woven fabric that is excellent in air permeability and slipperiness and is less likely to cause misalignment.
発明者は前記課題を解決するために、絡み織物の構成要件例えば繊維素材並びにその形態、形状、織物密度等と目ズレとの関連について詳細に検討した結果、特定の織物密度とすることにより目ズレが大きく改善されることを見出し、本発明に到達したものである。
すなわち、本発明は下記の通りである。
1.トータルカバーファクターが1000〜1800であり、経糸カバーファクター(A)と緯糸カバーファクター(B)の比(A/B)が0.7〜1.6である絡み織からなることを特徴とする織物。
2.経糸及び又は緯糸が、実質的に無撚のマルチフィラメント糸であることを特徴とする上記1記載の織物。
3.上記1又は2記載の織物で構成された裏地。
In order to solve the above-mentioned problems, the inventor has studied in detail the structural requirements of the entangled fabric, for example, the relationship between the fiber material and its form, shape, fabric density, etc. and misalignment. The inventors have found that the deviation is greatly improved and have reached the present invention.
That is, the present invention is as follows.
1. A woven fabric comprising a woven fabric having a total cover factor of 1000 to 1800 and a ratio (A / B) of warp cover factor (A) to weft cover factor (B) of 0.7 to 1.6 .
2. 2. The woven fabric according to 1 above, wherein the warp and / or weft is a substantially untwisted multifilament yarn.
3. A lining composed of the woven fabric according to 1 or 2 above.
本発明の織物は通気性、すべり性に優れ、かつ、目ズレの生じにくいものであり、裏地用途に好適に用いることができる。 The woven fabric of the present invention is excellent in breathability and slipperiness and hardly causes misalignment, and can be suitably used for lining applications.
本発明について、以下具体的に説明する。
本発明でいう絡み織物とは、和装業界では良く知られている織物素材組織であり、地経糸と絡み経糸とが一組となり、絡み経糸が緯糸一本または数本ごとにその位置を変えて組織し、緯糸と緯糸の間に絡み目を作った織物である。例えば、実教出版株式会社発行の繊維工学2織物の89ページから102ページに示されているものである。図1に最も基本となる紗の組織を表す図を示す。これは、地経糸aと絡み経糸bを、緯糸c1本ごとにその位置を変えて組織し、緯糸と緯糸の間に絡み目dを作った織物である。
The present invention will be specifically described below.
The entangled woven fabric referred to in the present invention is a fabric material structure well known in the Japanese clothing industry, and a pair of ground warp and entangled warp is used, and the position of the entwined warp is changed by one or several wefts. It is a woven fabric that is textured and has a tangled line between the wefts. For example, it is shown in pages 89 to 102 of the textile engineering 2 fabric issued by Jikkyo Publishing Co., Ltd. FIG. 1 shows a diagram representing the most basic cocoon structure. This is a woven fabric in which a ground warp a and an entangled warp b are organized by changing the position of each weft c, and an entangled d is formed between the weft and the weft.
絡み織の組織としては、紗・絽・紗と絽を組み合わせた変則絽(ほら絽)等があり、絡む1組の経糸本数によって、2本からみ・3本からみ・4本からみ等がある。本発明ではこれらを組み合わせたものを目的に応じて使用することができる。特に薄地化、柔軟性、すべり性を得るには2本からみが好適である。また、防透け性を重要視する裏地の組織として、絽組織の3本絽、5本絽、等又は紗と絽を組み合わせた変則絽が好適であり、目的に応じて適宜選定することができる。また、織物構造でストライプ柄を出す手段として、緯は絽組織、絽と紗の組み合わせた変則絽、繊度違いで、経は空き羽、繊度違い、等を使用することができ、裏地には経ストライプ柄が好適である。 As the woven fabric structure, there are irregular cocoons (紗) that combine cocoons, cocoons, cocoons and cocoons, and there are two, three, four, etc., depending on the number of warps that are involved. In the present invention, a combination of these can be used according to the purpose. In particular, two strands are suitable for thinning, flexibility and slipperiness. Further, as the lining structure that places importance on the see-through property, a three-row cocoon, five-fold cocoon, etc., or an irregular cocoon combining cocoon and cocoon is suitable and can be appropriately selected according to the purpose. . In addition, as a means of producing a striped pattern in a woven structure, we can use a weave structure, an irregular wrinkle with a combination of wrinkles and wrinkles, a different fineness, a warp, an empty feather, a different fineness, etc. A stripe pattern is preferred.
本発明の織物は次式で計算されるトータルカバーファクター(TC)が1000〜1800であることを特徴とする。1000未満では目ずれを抑えることが困難であり、且つ縫い目滑脱性が著しく低下する。1800を越えると裏地織物としての高通気性及び軽量性、柔軟性に乏しい傾向にある。さらに好ましくは1100〜1600であり、特に好ましくは1200〜1500である。
TC=(経糸の繊度:dtex)0.5×経糸密度(本/2.54cm)+(緯糸の繊度:dtex)0.5×緯糸密度(本/2.54cm)
The woven fabric of the present invention is characterized in that the total cover factor (TC) calculated by the following formula is 1000 to 1800. If it is less than 1000, it is difficult to suppress misalignment, and the slippage of the seam is significantly reduced. When it exceeds 1800, it tends to be poor in air permeability, lightness and flexibility as a lining fabric. More preferably, it is 1100-1600, Most preferably, it is 1200-1500.
TC = (fineness of warp: dtex) 0.5 × warp density (main / 2.54 cm) + (fineness of weft: dtex) 0.5 × weft density (main / 2.54 cm)
本発明の織物はまた、経糸カバーファクター(A)と緯糸カバーファクター(B)の比(A/B)が0.7〜1.6であることを特徴とする。0.7未満では目ずれを抑えることが困難であり、1.6を超えると目ずれを抑えることが困難、且つ織物表面のすべり性に欠ける。さらに好ましくは0.9〜1.45である。
A=(経糸の繊度:dtex)0.5×経糸密度(本/2.54cm)
B=(緯糸の繊度:dtex)0.5×緯糸密度(本/2.54cm)
本発明における経糸及び又は緯糸が実質的に無燃のマルチフィラメント糸とは、撚数が
500T/m未満をいう。撚を付与することで目ずれを抑制することは可能であるが、500T/m以上にすると生地のすべり性が悪くなり、ソフトな風合いを阻害するため好ましくない。
The woven fabric of the present invention is also characterized in that the ratio (A / B) of the warp cover factor (A) to the weft cover factor (B) is 0.7 to 1.6. If it is less than 0.7, it is difficult to suppress misalignment, and if it exceeds 1.6, it is difficult to suppress misalignment, and the fabric surface lacks slipperiness. More preferably, it is 0.9-1.45.
A = (fineness of warp: dtex) 0.5 × warp density (line / 2.54 cm)
B = (fineness of weft: dtex) 0.5 × weft density (line / 2.54 cm)
The multifilament yarn in which the warp and / or the weft is substantially non-flammable in the present invention means a twist number of less than 500 T / m. It is possible to suppress misalignment by imparting twist, but if it is 500 T / m or more, the slipperiness of the fabric is deteriorated and the soft texture is hindered.
本発明の織物は、経方向及び/又は緯方向にストレッチ性を有する方が、縫い目での応力集中が軽減して、縫い目滑脱性が向上するとともに着用時の圧迫感を軽減する効果がある。経方向及び/又は緯方向にストレッチ性を得るための手段として、公知のポリエステル系長繊維の仮撚加工糸、ニットデニット糸、押し込み加工糸及び潜在捲縮性ポリエステル系繊維等の糸使いや、或いは染色加工工程で付与することができる。前記染色加工工程での緯ストレッチ性付与方法としては、特許第3338029号に開示されているように、キュプラレーヨン繊維、ビスコースレーヨン繊維、アセテート繊維などのセルロース系繊維は原糸を打ち込んだ精練前の織物に水を付与した後、製織後の生機織物幅に対して、5〜15%の幅入れした状態で、熱処理を100℃〜210℃で行うことにより緯伸びが5〜12%もった裏地を得ることができる。5〜15%の幅入れ熱処理方法については、緯糸がポリエステル系長繊維の原糸を用いた場合と同様な方法であるが、異なるのは幅入れ熱処理前の生機織物にあらかじめ水を付与しておくことが重要である。 If the fabric of the present invention has stretch properties in the warp direction and / or the weft direction, the stress concentration at the seam is reduced, the seam slippage is improved, and the feeling of pressure at the time of wearing is reduced. As means for obtaining stretch properties in the warp direction and / or the weft direction, known polyester yarns such as false twisted yarns, knitted knitted yarns, indented yarns and latent crimped polyester fibers can be used. Alternatively, it can be applied in the dyeing process. As a method for imparting weft stretchability in the dyeing process, as disclosed in Japanese Patent No. 3338029, cellulosic fibers such as cupra rayon fiber, viscose rayon fiber, and acetate fiber are used before scouring the raw yarn. After water was applied to the woven fabric, the weft elongation was increased to 5 to 12% by carrying out the heat treatment at 100 to 210 ° C. with a width of 5 to 15% of the width of the woven fabric after weaving. Lining can be obtained. The 5 to 15% width-filling heat treatment method is the same as the case where the weft yarn is a polyester long fiber, but the difference is that water is applied to the raw fabric before the width-filling heat treatment. It is important to keep
本発明に用いられる素材としては、キュプラレーヨン繊維、ビスコースレーヨン繊維、アセテート繊維などのセルロース系繊維糸や、ポリトリメチレンテレフタレート系繊維、ポリエチレンテレフタレート系繊維、ポリブチレンテレフタレート系繊維等のポリエステル系繊維、ポリアミド繊維などの合成繊維が挙げられ、キュプラレーヨン繊維が好ましい。
繊維の形態は、長さ方向に均一なものや太細のあるものでもよい。繊維の断面形状は、丸型、三角、L型、T型、Y型、W型、八葉型、偏平(扁平度1.3〜4程度のもので、W型、I型、ブ−メラン型、波型、串団子型、まゆ型、直方体型等がある)、ドッグボーン型等の多角形型、多葉型、中空型や不定形なものでもでもよい。
本発明の糸の形態としては、フィラメント糸で交絡、混繊、等公知の手段で糸段階で混用し、さらに経糸および/または緯糸において一本〜数本交互で混用してもよい。
Examples of the material used in the present invention include cellulose fiber yarns such as cupra rayon fiber, viscose rayon fiber and acetate fiber, and polyester fibers such as polytrimethylene terephthalate fiber, polyethylene terephthalate fiber, and polybutylene terephthalate fiber. And synthetic fibers such as polyamide fibers, with cupra rayon fibers being preferred.
The shape of the fiber may be uniform or thick in the length direction. The cross-sectional shape of the fiber is round, triangular, L-shaped, T-shaped, Y-shaped, W-shaped, Yaba-shaped, flat (flatness of about 1.3-4, W-shaped, I-shaped, Boomerang The shape may be a polygonal shape such as a dog shape, a multi-leaf shape, a hollow shape, or an indeterminate shape.
As a form of the yarn of the present invention, a filament yarn may be mixed at a yarn stage by a known means such as entanglement and blending, and one to several yarns may be used alternately in warp and / or weft.
織物の形態としては、経糸と緯糸の繊維素材の組み合わせに何ら制限はなく、裏地に使用される対象服の種類や使用される部位、要求性能の内容(水洗濯かドライクリーニングか)などによって適宜選定される。例えば、安価でイージケア性(水洗濯しても寸法変化が小さくシワになりにくい)や着用頻度の高い衣服の裏地に用いられる場合は、 経糸にポリエステル系繊維100%で、緯糸にポリエステル系繊維の原糸100%又はポリエステル系長繊維の仮撚加工糸100%或いは潜在捲縮発現性ポリトリメチレンフトレート繊維よりなる組み合わせのポリエステル系繊維100%からなる裏地が好ましい。一方、実用時の快適性(吸放湿性能や制電性)やドレープ性が要求される高価な衣服の場合には、経/緯ともにセルロース系繊維の組み合わせよりなるセルロース系繊維100%の裏地であることが好ましい。 As for the form of the woven fabric, there are no restrictions on the combination of warp and weft fiber materials, depending on the type of clothing to be used for the lining, the part to be used, the content of the required performance (water washing or dry cleaning), etc. Selected. For example, when it is used for the lining of clothes that are inexpensive and easy-care (small dimensional change is less likely to wrinkle even when washed with water) and is frequently used, 100% polyester fiber for warp and polyester fiber for weft A backing made of 100% raw yarn or 100% polyester continuous fiber false twisted yarn or 100% polyester fiber in combination of latent crimped polytrimethylene phthalate fibers is preferred. On the other hand, in the case of expensive clothes that require practical comfort (moisture absorption / release performance and anti-static properties) and drapeability, the lining is made of 100% cellulosic fibers made of a combination of cellulosic fibers in both the length and the length. It is preferable that
本発明の絡み織物を製織する方法としては絡み綜絖を装備した普通織機、レピア織機、エアージェットルーム、ウオータージェットルーム、グリッパー織機(弾丸織機)、多相織機が挙げられる。しかし、これらに限定されるものではなく、絡み綜絖以外を装備して絡み織物を製織できる装置を具備した織機であれば良く例えば、スルザーテキスタイル社製パワーレノを装備したグリッパー織機がある。
地組織の筬への経糸通し方は1羽毎に空き羽にすれば経糸よろけが解消され、好適である。絡み綜絖として糸綜絖や金属綜絖を用いることができるが、金属綜絖が製織性、織物欠点、織物経品位共に良好で且つ、防目ずれ性に好適である。金属綜絖が防目ずれ性に対して良好になる理由として、経糸が絡む時に経糸が均一な張力になっており、安定した経糸張力バランスによって緯糸把持が強固になるためと推測している。
Examples of the method for weaving the entangled fabric of the present invention include a normal loom equipped with an entanglement raft, a rapier loom, an air jet loom, a water jet loom, a gripper loom (bullet loom), and a multiphase loom. However, the present invention is not limited to these, and any loom equipped with a device capable of weaving the woven fabric by equipping other than the entanglement can be used. For example, there is a gripper loom equipped with a power leno manufactured by Sulzer Textile.
It is preferable that the warp threading of the ground structure is made to be an empty wing for each wing, so that the warp warpage is eliminated. As the entanglement kite, a yarn kite or a metal kite can be used. However, the metal kite has good weaving properties, fabric defects, and fabric warp quality, and is suitable for preventing slippage. It is assumed that the reason why the metal wrinkles are good in terms of anti-seizure property is that when the warp is entangled, the warp has a uniform tension, and the weft grip is strengthened by a stable warp tension balance.
本発明において、原糸の総繊度は、経糸では33d〜110dtexが好ましく、より好ましくは33〜56dtexのものが用いられ、緯糸では56〜167dtexが好ましく、より好ましくは84〜110dtexである。しかし、これらに限定されるものではない。単糸繊度は0.11〜3.5dtexの範囲が好ましく、さらに好ましくは0.22〜2.34dtexの範囲である。
本発明の絡み織物の目付量は本発明の目的を達成するためには、35〜90g/m2であることが好ましく、更に好ましくは35〜80g/m2、最も好ましくは40〜70g/m2である。30g/m2未満では防目ずれ性に劣る傾向がみられ、90g/m2を越えると裏地織物として軽量性に不足する傾向にある。
In the present invention, the total fineness of the raw yarn is preferably 33d to 110 dtex for warp yarn, more preferably 33 to 56 dtex, and more preferably 56 to 167 dtex for weft yarn, and more preferably 84 to 110 dtex. However, it is not limited to these. The single yarn fineness is preferably in the range of 0.11 to 3.5 dtex, and more preferably in the range of 0.22 to 2.34 dtex.
To achieve the purpose of the mass per unit area according to the present invention tangled fabric of the present invention is preferably 35~90g / m 2, more preferably 35~80g / m 2, most preferably 40~70g / m 2 . If it is less than 30 g / m 2 , the tendency of inferior eye-proofing tends to be inferior, and if it exceeds 90 g / m 2 , it tends to be insufficient in light weight as a woven fabric.
本発明の絡み織物の通気量は100cc/cm2/sec以上である事が好ましく、更に好ましくは150cc/cm2/sec以上、最も好ましくは200cc/cm2/sec以上であり、100cc/cm2/sec未満では本発明の目的である裏地織物として適さないことがある。
本発明の生機精練は一般的に用いられているオープンソーパー型連続精練機、液流型染色機、浴中懸垂型連続精練機、ソフサ精練機などの使用が好ましい。精練が終了した後は、裏地の一般的な加工工程である染色、仕上げの工程が適用される。ポリエステル系繊維100%で風合いをよりソフトする場合には、染色前にアルカリ減量を行っても差し支えない。
The air permeability of the woven fabric of the present invention is preferably 100 cc / cm 2 / sec or more, more preferably 150 cc / cm 2 / sec or more, most preferably 200 cc / cm 2 / sec or more, and 100 cc / cm 2. If it is less than / sec, it may not be suitable as the lining fabric that is the object of the present invention.
For the raw machine scouring of the present invention, it is preferable to use a generally used open soap type continuous scouring machine, liquid flow type dyeing machine, suspension-type continuous scouring machine in bath, and softener scouring machine. After the scouring is completed, a dyeing and finishing process, which is a general processing process for the lining, is applied. When softening the texture with 100% polyester fiber, it is possible to reduce the alkali before dyeing.
本発明の織物がポリエステル系繊維100%よりなる場合の染色加工には、ポリエステル系繊維で構成されている従来の加工方法が適用され、液流型染色機、ビーム染色機、ジッカー染色機、ウインス染色機などが使用されるが、染色品の品位、コスト面からは、液流染色機が好ましい。染色後の仕上げ加工についても、染色加工同様にポリエステル系繊維を用いた裏地の製造で汎用される加工が適用される。ただ、最終仕上工程でシワを除去するためのピンテンター等による幅だし熱処理で幅出しする割合が大きくとるとストレッチ性を有する織物場合は、伸びの少ない裏地となってしまうので注意が必要である。 For the dyeing process when the woven fabric of the present invention is made of 100% polyester fiber, a conventional processing method composed of polyester fiber is applied, and a liquid flow dyeing machine, beam dyeing machine, zicker dyeing machine, wins Although a dyeing machine or the like is used, a liquid dyeing machine is preferable from the viewpoint of the quality and cost of the dyed product. As for the finishing process after dyeing, a process widely used in the production of a lining using polyester fibers is applied as in the dyeing process. However, it should be noted that if the ratio of width-developing by a pin tenter or the like for removing wrinkles in the final finishing process is large, a stretched woven fabric will become a lining with little elongation.
又、表面が平滑でストレッチ性を発現させるためには、例えば、生機をリラックス処理し幅入れさせた後、染色を行い、仕上げ処理を兼ねたファイナルセットを行うことが好ましい。リラックス処理に使用する機械としてはU型ソフサー又はオープンソーパーを用いるのが表面性とストレッチ性発現の面からより好ましい。U型ソフサー又はオープンソーパーにより拡布状態で精練する場合の温度は80〜105℃が好ましく、より好ましくは90〜100℃である。経及び緯の両方向にストレッチを発現させるためには、引き続き液流染色機によるリラックス処理を行なうことが好ましい。リラックス処理する場合の温度は95〜130℃が好ましく、より好ましくは100〜120℃である。 Moreover, in order to express the stretch property with a smooth surface, for example, it is preferable to perform a final set that also serves as a finishing process after dyeing and dyeing the raw machine after relaxing the width. As the machine used for the relaxation treatment, it is more preferable to use a U-type softer or an open soaper in terms of surface properties and expression of stretch properties. The temperature when scouring in an expanded state with a U-type softer or an open soaper is preferably 80 to 105 ° C, more preferably 90 to 100 ° C. In order to develop the stretch in both the warp and weft directions, it is preferable to perform a relaxing process with a liquid dyeing machine. The temperature for the relaxation treatment is preferably 95 to 130 ° C, more preferably 100 to 120 ° C.
染色前に中間セットを入れることが表面平滑性を達成するためにより好ましい。中間セットの温度は150〜190℃が好ましい。150℃未満では、セット性が不十分であり、190℃を超えると、ストレッチ性が低下することがある。中間セット時の幅設定は、染色上がりの幅が目標とする仕上げ幅にできるだけ近くなるよう適宜選択することが好ましい。前記仕上工程で、付加的に仕上げ剤として帯電防止剤、撥水剤、吸汗剤などを付与することもできる。また、織物表面の光沢、平滑性、風合いを改善するために、仕上げ剤付与後にカレンダー処理などを適用することもできる。 It is more preferable to put an intermediate set before dyeing in order to achieve surface smoothness. The temperature of the intermediate set is preferably 150 to 190 ° C. If it is less than 150 degreeC, set property is inadequate, and if it exceeds 190 degreeC, stretch property may fall. The width setting at the time of intermediate setting is preferably selected as appropriate so that the width after dyeing is as close as possible to the target finishing width. In the finishing step, an antistatic agent, a water repellent, a sweat absorbing agent, or the like can be additionally provided as a finishing agent. Moreover, in order to improve the gloss, smoothness, and texture of the fabric surface, calendering or the like can be applied after applying the finishing agent.
セルロース系繊維/ポリエステル系繊維よりなる交織裏地の場合の染色加工では、まず前記と同様な方法で精練した後、緯糸であるポリエステル繊維の染色を行う。次いで、セルロース系繊維の染色を行う。この場合、ポリエステル系繊維を染色した染色機と同機を用いて染色しても良いし、またコールドパッドバッチ法やパッドスチーム法やジッカー法による別の染色機を用いて染色することができる。染色終了後の仕上げ加工では、通常のセルロース繊維の加工で実施されている洗濯収縮率、湿摩擦堅牢度を向上させるための樹脂加工を付与することもできる。又、表面が平滑で緯ストレッチ性を発現させるためには、ポリエステル系繊維100%よりなる裏地と同様な加工を実施すればよい。 In the dyeing process in the case of an union lining made of cellulosic fibers / polyester fibers, first, scouring is performed in the same manner as described above, and then polyester fibers that are wefts are dyed. Next, the cellulosic fibers are dyed. In this case, it may be dyed by using the same dyeing machine as that used for dyeing polyester fibers, or by using another dyeing machine such as a cold pad batch method, a pad steam method or a zicker method. In the finishing process after the completion of dyeing, a resin process for improving the washing shrinkage rate and the fastness to wet friction, which is carried out in normal cellulose fiber processing, can also be imparted. Further, in order to develop a weft stretch property with a smooth surface, the same processing as that of a lining made of 100% polyester fiber may be performed.
セルロース系繊維100%よりなる裏地の染色加工には、織物に付着している紡糸オイルや経糸糊油剤などを除去する目的で精練される。精練工程で用いられる処理液としては、水または界面活性剤とアルカリを含む水溶液が良い。織物の精練で一般的に用いられているオープンソーパー型連続精練機、液流型染色機、浴中懸垂型連続精練機、ソフサ精練機など特に限定されるものでない。生産性や加工時のシワ発生を考慮すればオープンソーパー型連続精練機やジッカー染色機の使用が好ましい。 In the dyeing process of the lining made of 100% cellulosic fibers, scouring is performed for the purpose of removing the spinning oil and warp glue oil adhering to the fabric. The treatment liquid used in the scouring process is preferably water or an aqueous solution containing a surfactant and an alkali. There is no particular limitation such as an open soap type continuous scouring machine, a liquid flow type dyeing machine, a suspension type continuous scouring machine in bath, and a soft scouring machine generally used for scouring fabrics. In consideration of productivity and generation of wrinkles during processing, it is preferable to use an open soap type continuous scouring machine or a zicker dyeing machine.
精練処理織物は、セルロース系繊維を用いた裏地の一般的な加工が随意付加した裏地に仕上げられる。その一つである染色方法は特に限定されるものでなく、液流染色法、ジッカー染色法、ビーム染色法、コールドパッドバッチ染色法、パッドスチーム染色法、パッドロール染色法、等の中から経、緯糸に用いられるセルロース系繊維の種類によって用いる染料及び染色方法を適宜選定すればよい。経糸がポリエステル系繊維で緯糸がセルロース系繊維の場合も上記と同様の染色機を用いることができるが、ポリエステル系繊維を染色した染色機と同機を用いてセルロース系繊維を染色してもよいし、また、コールドパッドバッチ法やパッドスチーム法、ジッカー法による別の染色機を用いてセルロース系繊維の染色を行うことができる。染色終了後の仕上げ加工では、通常セルロース繊維の加工で汎用されている洗濯収縮率、湿摩擦堅牢度を向上させるための樹脂加工を付与することが好ましい。この仕上げ工程のところで、仕上げ剤として帯電防止剤、撥水剤、吸汗剤などを付与してもかまわない。また、織物表面の光沢、平滑性、風合いを改善するために、仕上げ剤付与後にカレンダー加工を施すことができる。 The scoured woven fabric is finished into a lining optionally added with general processing of the lining using cellulosic fibers. One of the dyeing methods is not particularly limited, and liquid dyeing method, zicker dyeing method, beam dyeing method, cold pad batch dyeing method, pad steam dyeing method, pad roll dyeing method, etc. The dye and dyeing method used may be appropriately selected depending on the type of cellulosic fiber used for the weft. When the warp is a polyester fiber and the weft is a cellulosic fiber, the same dyeing machine as described above can be used. However, the cellulosic fiber may be dyed using the same machine as that for dyeing the polyester fiber. In addition, cellulosic fibers can be dyed using another dyeing machine using a cold pad batch method, a pad steam method, or a zicker method. In the finishing process after the completion of dyeing, it is preferable to provide a resin process for improving the washing shrinkage and the fastness to wet friction that are generally used in the processing of cellulose fibers. In this finishing step, an antistatic agent, a water repellent, a sweat absorbing agent or the like may be added as a finishing agent. Moreover, in order to improve the gloss, smoothness, and texture of the fabric surface, calendering can be performed after applying the finishing agent.
以下実施例により本発明を詳細に説明するが、本発明はこれら実施例に限定されるものではない。なお、実施例中の数値は及び製品の特徴の判定基準は以下の評価法で実施した。
(1)織物の防目ずれ性評価
当業界に5年以上従事したことのある経験者5人がモニターとなり、官能評価を行い、下記の4段階の判定を行った。
◎:極めて防目ずれ性に優れている。
○:概ね防目ずれ性に優れている。
△:やや防目ずれに劣っている。
×:防目ずれ性に劣る。
EXAMPLES The present invention will be described in detail below with reference to examples, but the present invention is not limited to these examples. In addition, the numerical value in an Example and the judgment criteria of the characteristic of a product were implemented with the following evaluation methods.
(1) Evaluation of anti-slip property of woven fabric Five experienced persons who have been engaged in this industry for more than 5 years became monitors, and sensory evaluation was performed, and the following four steps were judged.
(Double-circle): It is very excellent in eye-proof shift.
○: It is generally excellent in misalignment resistance.
(Triangle | delta): It is inferior to some misalignment.
×: Inferior in anti-glare property.
(2)織物のすべり性の評価
当業者に5年以上従事したことのある経験者5人がモニターとなり、手で触ったときの官能評価を下記4段階の判定を行った。
◎:すべり感がきわめて良好。
○:すべり感が良好。
△:すべり感が若干わるい。
×:すべり感がわるい。
(3)織物の通気量
JIS−L1096 8.27.2A法(フラジール形法)により測定した。
(2) Evaluation of slipperiness of fabrics Five experienced persons who have been engaged in the art for 5 years or more became monitors, and the sensory evaluation when touched by hand was judged in the following four stages.
(Double-circle): A slip feeling is very favorable.
○: Good sliding feeling.
Δ: Slightly uncomfortable feeling.
X: A slippery feeling is bad.
(3) Aeration rate of woven fabric Measured by JIS-L1096 8.27.2A method (Fragile type method).
[実施例1〜3、比較例1〜2]
トータルカバーファクターが約1500であり、経糸カバーファクターと緯糸カバーファクターの比を変更するため適宜設計を変更して、経糸に56dtex/30fの実質的無撚のキュプラレーヨン繊維を各種筬に1羽2本入れとして準備し、金属絡み綜絖を搭載した石川製作所製レピア織機にて、緯糸に84dtex/45fの実質的無撚のキュプラレーヨン繊維を密度違いで打ち込んで、図1に示す紗組織の絡み織生機を得た。
この生機にオープンソーパー型連続精練機を用いて糊抜き精練を行った。引き続きコールドパットバッチ染色法で染色した後、仕上げ加工を行い、表1の織物を得た。
得られた織物の結果は表1に示すように、実施例は防目ずれ性、通気性に優れ、良好な風合いを持つ織物裏地に最適なものであった。
[Examples 1-3, Comparative Examples 1-2]
The total cover factor is about 1500, and the design is appropriately changed to change the ratio of the warp cover factor to the weft cover factor, and 56 dtex / 30f substantially untwisted cupra rayon fiber is used for each warp. Prepared as a main case, and with a rapier weaving machine manufactured by Ishikawa Seisakusho equipped with a metal twine, 84 dtex / 45f of substantially untwisted cupra rayon fiber was driven into the weft yarn with different densities, and the twine of twine structure shown in FIG. I got a living machine.
Paste scouring was performed on this raw machine using an open soap type continuous scouring machine. Subsequently, after dyeing by the cold pad batch dyeing method, finishing was performed to obtain the woven fabric shown in Table 1.
As shown in Table 1, the results of the obtained woven fabric were excellent in slip prevention and breathability, and were optimum for a woven fabric lining having a good texture.
[実施例4〜6、比較例3〜4]
経糸カバーファクターと緯糸カバーファクターの比を1.0一定にし、トータルカバーファクターを種々変更するために、適宜設計を変更して、経糸に56dtex/30fの実質的無撚のキュプラレーヨン繊維を、実施例5〜6及び比較例4は筬に1羽2本入れとし、実施例4、比較例3は筬に1羽2本入れとして1羽毎に空き羽にして経糸を準備し、金属絡み綜絖を搭載した石川製作所製レピア織機にて、緯糸に84dtex/45fの実質的無撚のキュプラレーヨン繊維を密度違いで打ち込んで、図1に示す紗組織の絡み織生機を得た。この生機にオープンソーパー型連続精練機を用いて糊抜き精練を行った。引き続きコールドパットバッチ染色法で染色した後、仕上げ加工を行い、表2の織物を得た。
得られた織物の結果は表2に示すように、実施例は防目ずれ性、通気性に優れ、良好な風合いを持つ織物裏地に最適なものであった。
[Examples 4-6, Comparative Examples 3-4]
In order to keep the ratio of the warp cover factor to the weft cover factor constant at 1.0, and to change the total cover factor in various ways, the design was changed as appropriate to implement a substantially untwisted cupra rayon fiber of 56 dtex / 30f on the warp. In Examples 5 to 6 and Comparative Example 4, two wings are put in a cocoon, and in Example 4 and Comparative Example 3, two wings are put in a cocoon and each wing is emptied and a warp is prepared. In the rapier weaving machine manufactured by Ishikawa Seisakusho, 84 dtex / 45f of substantially untwisted cupra rayon fibers were driven into the weft yarns with different densities to obtain a knotted tissue weaving machine shown in FIG. Paste scouring was performed on this raw machine using an open soap type continuous scouring machine. Subsequently, after dyeing by the cold pad batch dyeing method, finishing was performed to obtain the woven fabric shown in Table 2.
As shown in Table 2, the results of the obtained woven fabric were excellent in anti-slip properties and breathability, and were optimum for a woven fabric lining having a good texture.
[実施例7〜9、比較例5〜6]
経糸に撚数1500T/m、緯糸に1200T/mの撚を付与した以外は、実施例1〜3、比較例1〜2と同じ方法で、表3の織物を得た。得られた織物の結果は表3に示すように、実施例7〜9の織物ではすべり性がやや低下する傾向にあるが、防目ずれ性、通気性に優れ、織物裏地に好適なものであった。
[Examples 7 to 9, Comparative Examples 5 to 6]
A woven fabric shown in Table 3 was obtained in the same manner as in Examples 1 to 3 and Comparative Examples 1 and 2, except that a twist of 1500 T / m was applied to the warp and a twist of 1200 T / m was applied to the weft. As shown in Table 3, the results of the obtained woven fabrics have a tendency for slipperiness to be slightly lowered in the woven fabrics of Examples 7 to 9, but they are excellent in slip prevention and breathability and are suitable for woven fabric lining. there were.
本発明の織物は、特に裏地用途に好適に用いることができる。 The fabric of the present invention can be suitably used particularly for lining applications.
a:地経糸
b:絡み経糸
c:緯糸
d:絡み目
a: Ground warp b: Tangle warp c: Weft d: Tangle
Claims (3)