WO2021042939A1 - Dispositif électronique, couvercle de batterie, et son procédé de fabrication - Google Patents

Dispositif électronique, couvercle de batterie, et son procédé de fabrication Download PDF

Info

Publication number
WO2021042939A1
WO2021042939A1 PCT/CN2020/107928 CN2020107928W WO2021042939A1 WO 2021042939 A1 WO2021042939 A1 WO 2021042939A1 CN 2020107928 W CN2020107928 W CN 2020107928W WO 2021042939 A1 WO2021042939 A1 WO 2021042939A1
Authority
WO
WIPO (PCT)
Prior art keywords
mold
glass sheet
battery cover
electronic device
manufacturing
Prior art date
Application number
PCT/CN2020/107928
Other languages
English (en)
Chinese (zh)
Inventor
邹攀
Original Assignee
Oppo广东移动通信有限公司
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Oppo广东移动通信有限公司 filed Critical Oppo广东移动通信有限公司
Publication of WO2021042939A1 publication Critical patent/WO2021042939A1/fr

Abstract

La présente invention concerne un dispositif électronique (100), un couvercle de batterie (110), et son procédé de fabrication. Le procédé de fabrication comprend les étapes consistant : à recouvrir un premier moule (210) en utilisant une feuille en verre (300), la feuille en verre (300) et une rainure (211) définissant une cavité étanche (201) ; à recouvrir la feuille en verre (300) en utilisant un second moule (220), une protubérance (221) faisant face à la rainure (211), et la protubérance (221) effectuant un contact avec la feuille en verre (300) ; à chauffer le premier moule (210), le second moule (220) et la feuille en verre (300) ; à mettre sous vide la cavité étanche (201), la feuille en verre (300) se déformant lorsque la pression d'air à l'intérieur de la cavité étanche (201) baisse, et la protubérance (221) se déplaçant progressivement dans la rainure (211) ; et la feuille en verre (300) se déformant en une forme prédéterminée.
PCT/CN2020/107928 2019-09-03 2020-08-07 Dispositif électronique, couvercle de batterie, et son procédé de fabrication WO2021042939A1 (fr)

Applications Claiming Priority (2)

Application Number Priority Date Filing Date Title
CN201910829327.2 2019-09-03
CN201910829327.2A CN112448072A (zh) 2019-09-03 2019-09-03 电子设备、电池盖、及其制造方法

Publications (1)

Publication Number Publication Date
WO2021042939A1 true WO2021042939A1 (fr) 2021-03-11

Family

ID=74734063

Family Applications (1)

Application Number Title Priority Date Filing Date
PCT/CN2020/107928 WO2021042939A1 (fr) 2019-09-03 2020-08-07 Dispositif électronique, couvercle de batterie, et son procédé de fabrication

Country Status (2)

Country Link
CN (1) CN112448072A (fr)
WO (1) WO2021042939A1 (fr)

Citations (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0848407A2 (fr) * 1996-12-04 1998-06-17 Matsushita Electric Works, Ltd. Lampe fluorescente compacte intégralement moulée
CN106231829A (zh) * 2016-08-03 2016-12-14 南昌欧菲光学技术有限公司 电子产品、玻璃外壳及其制造设备和方法
CN108401044A (zh) * 2016-01-04 2018-08-14 广东欧珀移动通信有限公司 手机后盖
CN108437344A (zh) * 2018-04-24 2018-08-24 东莞市裕鼎纳米科技有限公司 一种具有纳米纹理的塑胶外壳及其制造方法
CN208539941U (zh) * 2018-05-25 2019-02-22 Oppo广东移动通信有限公司 壳体和电子装置
CN110040945A (zh) * 2019-03-13 2019-07-23 深圳市东方碳素实业有限公司 一种热弯手机玻璃盖板的制作方法
CN110040946A (zh) * 2019-03-13 2019-07-23 深圳市东方碳素实业有限公司 一种热弯手机玻璃盖板的成型工艺
CN110191604A (zh) * 2019-06-27 2019-08-30 Oppo广东移动通信有限公司 壳体组件及其制备方法、电子设备
CN110255870A (zh) * 2019-06-27 2019-09-20 Oppo广东移动通信有限公司 热弯设备及壳体的热弯成型方法

Family Cites Families (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
DE102009036164B4 (de) * 2009-05-28 2011-06-09 Schott Ag Verfahren zum Biegen und thermischen Vorspannen von Strahlenschutzglas
TW201806890A (zh) * 2016-08-26 2018-03-01 關鍵應用科技股份有限公司 3d玻璃製造方法
CN107867793A (zh) * 2017-10-31 2018-04-03 广东欧珀移动通信有限公司 曲面玻璃盖板、曲面玻璃盖板的制备方法及移动终端
CN207685130U (zh) * 2017-12-06 2018-08-03 李宝轮 一种曲面玻璃成型装置

Patent Citations (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
EP0848407A2 (fr) * 1996-12-04 1998-06-17 Matsushita Electric Works, Ltd. Lampe fluorescente compacte intégralement moulée
CN108401044A (zh) * 2016-01-04 2018-08-14 广东欧珀移动通信有限公司 手机后盖
CN106231829A (zh) * 2016-08-03 2016-12-14 南昌欧菲光学技术有限公司 电子产品、玻璃外壳及其制造设备和方法
CN108437344A (zh) * 2018-04-24 2018-08-24 东莞市裕鼎纳米科技有限公司 一种具有纳米纹理的塑胶外壳及其制造方法
CN208539941U (zh) * 2018-05-25 2019-02-22 Oppo广东移动通信有限公司 壳体和电子装置
CN110040945A (zh) * 2019-03-13 2019-07-23 深圳市东方碳素实业有限公司 一种热弯手机玻璃盖板的制作方法
CN110040946A (zh) * 2019-03-13 2019-07-23 深圳市东方碳素实业有限公司 一种热弯手机玻璃盖板的成型工艺
CN110191604A (zh) * 2019-06-27 2019-08-30 Oppo广东移动通信有限公司 壳体组件及其制备方法、电子设备
CN110255870A (zh) * 2019-06-27 2019-09-20 Oppo广东移动通信有限公司 热弯设备及壳体的热弯成型方法

Also Published As

Publication number Publication date
CN112448072A (zh) 2021-03-05

Similar Documents

Publication Publication Date Title
CN107197063A (zh) 一种手机盖板及其制备方法和移动终端
US10035723B2 (en) Glass housing, manufacturing equipment and method thereof
WO2020199438A1 (fr) Verre en 3d et procédé de fabrication s'y rapportant, moule et ébauche en verre en 3d
CN107278385B (zh) 一种终端外壳及终端
CN102950697B (zh) 一种uv转印模内转印装饰方法
US20180037486A1 (en) Glass housing, electronic device having the same, manufacturing apparatus and method thereof
CN112092407B (zh) 一种贴膜方法及贴膜装置
CN106541669A (zh) 3d玻璃装饰膜加工设备及方法
WO2020200174A1 (fr) Procédé et système de préparation de feuille de verre incurvée, plaque de couverture en verre et dispositif électronique
WO2021042940A1 (fr) Dispositif électronique, couvercle de batterie et son procédé de fabrication
CN112265350A (zh) 一种膜片贴合工艺
WO2021042939A1 (fr) Dispositif électronique, couvercle de batterie, et son procédé de fabrication
CN104889874A (zh) 一种蓝宝石抛光用吸附垫及其制备方法
TWI529061B (zh) 複合材料的製造方法
CN206201645U (zh) 3d玻璃装饰膜加工设备
CN112976551B (zh) 壳体基体母板、壳体基体及制备方法、壳体、模具、电子设备
KR101932258B1 (ko) 모바일기기의 곡면형 디스플레이 패널 화면 보호필름 및 그 제조방법
CN114478001A (zh) 壳体组件及其制备方法和电子设备
CN111355832A (zh) 不等厚壳体、其加工方法及终端设备
CN112123741B (zh) 一种轻薄3d全包塑胶手机壳加工系统及其加工工艺
KR102068069B1 (ko) 장식시트를 가지는 곡면 글라스 성형방법
CN112944786B (zh) 一种表面触感曲面玻璃门体及其制作工艺
KR102005919B1 (ko) 곡면글라스 성형지그 및 이를 포함하는 곡면글라스 제조장치
CN212581753U (zh) 负压成型设备
US20200017391A1 (en) Protection film for a terminal curved surface and manufacture method thereof

Legal Events

Date Code Title Description
121 Ep: the epo has been informed by wipo that ep was designated in this application

Ref document number: 20861749

Country of ref document: EP

Kind code of ref document: A1

NENP Non-entry into the national phase

Ref country code: DE

122 Ep: pct application non-entry in european phase

Ref document number: 20861749

Country of ref document: EP

Kind code of ref document: A1