WO2003016362A1 - Ethylene polymerization process - Google Patents
Ethylene polymerization process Download PDFInfo
- Publication number
- WO2003016362A1 WO2003016362A1 PCT/US2002/026314 US0226314W WO03016362A1 WO 2003016362 A1 WO2003016362 A1 WO 2003016362A1 US 0226314 W US0226314 W US 0226314W WO 03016362 A1 WO03016362 A1 WO 03016362A1
- Authority
- WO
- WIPO (PCT)
- Prior art keywords
- reactor
- ethylene
- catalyst
- polymer
- polymerization
- Prior art date
Abstract
Description
Claims