JPS6055046A - Propylene copolymer composition - Google Patents
Propylene copolymer compositionInfo
- Publication number
- JPS6055046A JPS6055046A JP16315383A JP16315383A JPS6055046A JP S6055046 A JPS6055046 A JP S6055046A JP 16315383 A JP16315383 A JP 16315383A JP 16315383 A JP16315383 A JP 16315383A JP S6055046 A JPS6055046 A JP S6055046A
- Authority
- JP
- Japan
- Prior art keywords
- propylene
- butene
- film
- random copolymer
- weight
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
Description
【発明の詳細な説明】 本発明はプロピレン共重合体組成物に関する。[Detailed description of the invention] The present invention relates to propylene copolymer compositions.
プロピレンホモポリマーフィルムは透明性にすぐれるほ
か腰が強い等の利点を有している反面、低温衝撃強度が
小さい、ヒートシール温度が高いという欠点がある。Although propylene homopolymer film has advantages such as excellent transparency and strong stiffness, it has disadvantages such as low low-temperature impact strength and high heat sealing temperature.
このような欠点を改良したフィルムとしてプロピレン−
エチレンランダム共m 合体フイルムカ提案されている
が、このフィルムは低温衝撃強度の改善はされているも
ののヒートシール温度が高いという点は十分には改善さ
れていない。このヒートシール温度を低くするためには
、エチレンを大量に共重合させればよいが、この場合は
副生物の発生が避けられず工業的な製造法としては好ま
しくない。さらに、エチレンの代りにブテン−1を用い
たプロピレン−ブテン−1ランダム共重合体フィルムも
知られているが、このフィルムは低温衝撃強度が小さい
ものであり、ブテン−1を大意に共重合させる必要があ
るため、得られる共重合体が軟質化してフィルムの腰が
弱くなるという欠点がある。Propylene is a film that improves these drawbacks.
An ethylene random composite film has been proposed, but although the low-temperature impact strength of this film has been improved, the high heat-sealing temperature has not been sufficiently improved. In order to lower the heat-sealing temperature, a large amount of ethylene may be copolymerized, but in this case, the generation of by-products is unavoidable, and this is not preferred as an industrial production method. Furthermore, a propylene-butene-1 random copolymer film using butene-1 instead of ethylene is also known, but this film has low low-temperature impact strength and requires extensive copolymerization of butene-1. This has the disadvantage that the resulting copolymer becomes soft and the film becomes stiff.
また、ポリプロピレンフィルムに対する消費者の要求は
次第に高度化され、したがって、ボリプ四ピレンフィル
ムに対するフィルム物性の評fllli4極めて厳格で
ある。fcとえば、ヒートシール温度を改良することが
できても引張弾性率、低温衝撃強度が劣る場合は、その
フィルムは総合的計価としては不合格とされる。In addition, consumer demands for polypropylene films have become increasingly sophisticated, and therefore, evaluations of film physical properties for polypropylene films have become extremely strict. For example, if the heat-sealing temperature can be improved but the tensile modulus and low-temperature impact strength are inferior, the film will be rejected in terms of comprehensive evaluation.
このような実情に鑑み、本発明者らはプロピレンホモポ
リマーの利点をそのま′、1巳有し、がっ該ポリマーの
前記欠点を解消した樹脂組成物を開発すべく検討した結
果、特定のプロピレン−エチレンランダム共重合体、’
: l)ν定のプロピレン−ブテン−1ランダム共重合
体とを所定の割合で重合させた樹脂組成物が上記目的を
満足さ刊ることを見出し、この知見に基いて本発明を完
成したのである。In view of these circumstances, the present inventors conducted research to develop a resin composition that possesses one of the advantages of propylene homopolymer and eliminates the disadvantages of this polymer. Propylene-ethylene random copolymer,'
We have discovered that a resin composition obtained by polymerizing a propylene-butene-1 random copolymer with a constant v constant at a predetermined ratio satisfies the above object, and based on this knowledge, we have completed the present invention. be.
本発明It 、プロピレン−エチレンランダム共重合体
(エチレン含有iiO,3〜6.11jjNd%) 9
8〜45重祭%とプロピレン−ブテン−1ランダム共重
合体(ブテン−1含有傾、0.5〜15重岨%)2〜5
5重量%より2zるプロピレン共重合体組成物である。Invention It, propylene-ethylene random copolymer (ethylene-containing iiO, 3 to 6.11jjNd%) 9
8-45 weight percent and propylene-butene-1 random copolymer (butene-1 content gradient, 0.5-15 weight percent) 2-5
This is a propylene copolymer composition containing 5% by weight or more.
本発明に用いるプロピレン−エチレンランダム共重合体
はエチレン含有社がa、S〜6.0重量%、好ましく
tj: o、s〜4.o重ni%であることが必要であ
る。エチレン含イT I?tが0.3重り一%未満であ
ると、低温衝撃強度が十分でなく、また(S、[]重i
t%を越えると、フィルムを製fat シlc ’46
合に腰が弱いものとなる。The propylene-ethylene random copolymer used in the present invention preferably has an ethylene content of a, S to 6.0% by weight.
tj: o, s~4. It is necessary that the amount is o weight ni%. Ethylene-containing T I? When t is less than 0.3% by weight, the low-temperature impact strength is insufficient, and (S, []weight i
If it exceeds t%, the film will be made fat Silc '46
If this happens, your back will become weak.
次に、プロピレン−ブテン−1ランダム共重合体はブテ
ン−1含有量が0゜5〜15重量%、好ましくは0.6
〜10重量%であることが必要である。Next, the propylene-butene-1 random copolymer has a butene-1 content of 0.5 to 15% by weight, preferably 0.6%.
~10% by weight is required.
ブテン−1含有址が0.3重量%未満であると、ヒート
シール性の改良効果が不十分であり、15重量%を越え
ると、フィルムを製造した場合に腰の強さが低下するば
かシでなく、高価なブテン−1を多量に使用することと
なり経済的でない。If the butene-1 content is less than 0.3% by weight, the effect of improving heat sealing properties will be insufficient, and if it exceeds 15% by weight, the stiffness will decrease when the film is produced. However, a large amount of expensive butene-1 is used, which is not economical.
上記の共重合体はいずれも常法により製造することがで
き、たとえばチーグラーナック触媒、担持型チタン系触
媒などを用いてスラリー重合、溶液重合、気相重合など
によシ製造することができる(t¥j開昭53−799
84号、同55−9051*同55−98210号、同
56−22307号1%公昭46−51478号、同4
9−1t543号など参照)。All of the above copolymers can be produced by conventional methods, such as slurry polymerization, solution polymerization, gas phase polymerization, etc. using Zieglernack catalysts, supported titanium catalysts, etc. t¥j Kaisho 53-799
No. 84, No. 55-9051 * No. 55-98210, No. 56-22307 1% Kosho No. 46-51478, No. 4
9-1t543, etc.).
本発明のプロピレン共重合体組成物は、プロピレン−エ
チレンランダム共重合体98〜45重量%、好ましくは
95〜50重量%とプロピレン−ブテン−1ランダム共
重合体2〜55重量%、好ましくは5〜50重量%を配
合してなるものである。ここでプロピレン−エチレンラ
ンダム共重合体の配合量が98重社%を越えると、低温
ヒートシール性の改良効果が不十分となり、また45重
量%未満であると、低温衝撃強度が不足するほかフィル
ムを製造した場合に、腰の強さが不十分なものとなる。The propylene copolymer composition of the present invention comprises 98-45% by weight, preferably 95-50% by weight of propylene-ethylene random copolymer and 2-55% by weight, preferably 5% by weight of propylene-butene-1 random copolymer. ~50% by weight. If the amount of the propylene-ethylene random copolymer exceeds 98% by weight, the effect of improving low-temperature heat sealability will be insufficient, and if it is less than 45% by weight, the low-temperature impact strength will be insufficient and the film will If manufactured, the strength of the waist will be insufficient.
これら共重合体の配合は公知の方法によって行なえばよ
く、たとえば乾湿・融混併用法、多段溶融混合法、単純
溶融混合法などにより混合し、さらにバンバリー文キサ
−、フニーダー。These copolymers may be blended by a known method, such as a combined dry/wet/melt blending method, a multi-stage melt blending method, a simple melt blending method, etc.
押出機、二軸混練押出機等を用いて混練すればよい。得
られた配合物は既知の製膜機によりフィルムとすること
ができる。The kneading may be carried out using an extruder, a twin-screw kneading extruder, or the like. The resulting formulation can be made into a film using known film-forming machines.
本発明のプロピレン共重合体組成物は透明性にすぐれ、
腰が強い上に低温衝撃強度と代温ヒートシール性が良好
であり、しかも両者のバランスがとれているため、包装
用フィルムの素材として極めて有用なものである。The propylene copolymer composition of the present invention has excellent transparency,
In addition to being strong, it has good low-temperature impact strength and thermostatic heat-sealing properties, and has a good balance between the two, making it extremely useful as a material for packaging films.
次に、本発明を実施例により詳しく説明する。Next, the present invention will be explained in detail with reference to examples.
製造例
(1) プロピレン−ブテン−1ランダム共重合体内容
積201の攪拌機付重合反応器内にn−へブタン8t、
三塩化チタン1.21およびジエチルアルミニウムクロ
ライド6.01を入れた。次いで、温度60°C1圧力
6.0kl?/ crl aO下でプロピレンとブテン
−1の混合ガスを供給して重合を行なった。ブテン−1
を重合系内の組成が一定となるように一定量づつ供給し
つつ内圧が6.0kg/dGとなるように制御した。Production example (1) Propylene-butene-1 random copolymer 8 tons of n-hebutane,
1.21 parts of titanium trichloride and 6.0 parts of diethylaluminum chloride were charged. Next, the temperature is 60°C and the pressure is 6.0kl? Polymerization was carried out by supplying a mixed gas of propylene and butene-1 under an atmosphere of /crl aO. Butene-1
was supplied in a constant amount at a time so that the composition within the polymerization system remained constant, and the internal pressure was controlled to be 6.0 kg/dG.
重合反応終了後、重合スラリーにn−ブタノール100
1を加え触媒を分解したのち、溶媒可溶分を分離除去し
、得られた粉末を乾燥した。After the polymerization reaction is complete, add 100% n-butanol to the polymerization slurry.
1 was added to decompose the catalyst, the solvent-soluble components were separated and removed, and the resulting powder was dried.
(2) プロピレン−エチレンランダム共重合体ブテン
−1の代りにエチレンを供給したこと以外は上記(11
と同様に行なった。(2) Propylene-ethylene random copolymer (11) except that ethylene was supplied instead of butene-1.
I did the same thing.
実施例1〜6および比較例1〜6
プロピレン−エチレンランダム共重合体トフロビレンー
ブテンー1ランダム共重合体をそれぞれ所定量の割合で
配合し、押出機より押出してベレットを得た。次に、3
5■の製膜機を用いて厚さ50μのフィルムを製造した
。Examples 1 to 6 and Comparative Examples 1 to 6 Propylene-ethylene random copolymer and toflopylene-butene-1 random copolymer were each blended in predetermined amounts and extruded from an extruder to obtain pellets. Next, 3
A film with a thickness of 50 μm was produced using a 5-inch film forming machine.
得られたフィルムの物性について測定17た結果を第1
表に示す。表中の引張弾性率はフィルムの腰の強さを、
フィルムインバク) IJ伶撃強度を示すものである。The physical properties of the obtained film were measured 17 times.
Shown in the table. The tensile modulus in the table indicates the stiffness of the film,
(Film impact) This shows the IJ impact strength.
/
@1 引張5Ll’J=I JIs−z1yo2に準拠
・2 ヒートシール温度 ヒートシーラーによ#)フィ
ルム同士を所定の温度で2 kg/CIIの荷重をかけ
、2秒間圧着して得
た幅25酵の試料を剥離速度
200 w/min 、剥離角度180゜で剥離を行な
って舟た剥離抵抗
力が3ooy/25簡のときの温度
・i フィルムイン/9ト フィルムをリング状に固定
し、1インチの衝撃頭を持つ振子で
前記リング状のフィルムを打抜
き、それに要したエネルギーを
測定した。使用機器は東洋精機
製作所フィルムイン/9トテス
タである。/ @1 Tensile 5Ll'J=I Based on JIs-z1yo2 ・2 Heat sealing temperature Using a heat sealer, the width 25 obtained by applying a load of 2 kg/CII to each other at the specified temperature and pressing them together for 2 seconds The fermentation sample was peeled at a peeling speed of 200 w/min and a peeling angle of 180°, and the temperature when the peeling resistance was 3ooy/25cm was determined. The ring-shaped film was punched out using a pendulum with an inch impact head, and the energy required for punching was measured. The equipment used is Toyo Seiki Seisakusho Film In/9 Tester.
特許出願人 出光石油化学株式会礼 9−Patent applicant: Idemitsu Petrochemical Co., Ltd. 9-
Claims (1)
レン含有量0.3〜6.0重j1%)98〜45重量−
とプロピレン−ブテン−1ランダム共重合体(ブテン−
1含有蒙0.5〜15重量%)2〜55重Ili%よシ
なるプロピレン共重合体組成物〇1. Purpyrene-ethylene random co-merge (ethylene content 0.3-6.0 wt j1%) 98-45 wt.
and propylene-butene-1 random copolymer (butene-1)
Propylene copolymer composition containing 0.5 to 15% by weight) and 2 to 55% by weight