[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JPH0245578A - Paint composition - Google Patents

Paint composition

Info

Publication number
JPH0245578A
JPH0245578A JP63195885A JP19588588A JPH0245578A JP H0245578 A JPH0245578 A JP H0245578A JP 63195885 A JP63195885 A JP 63195885A JP 19588588 A JP19588588 A JP 19588588A JP H0245578 A JPH0245578 A JP H0245578A
Authority
JP
Japan
Prior art keywords
pigment
coating
coat
titanium black
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP63195885A
Other languages
Japanese (ja)
Other versions
JPH0822982B2 (en
Inventor
Takahiko Hamada
孝彦 浜田
Katsumi Yamamoto
勝美 山本
Hajime Ishihara
肇 石原
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nippon Paint Co Ltd
Original Assignee
Nippon Paint Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nippon Paint Co Ltd filed Critical Nippon Paint Co Ltd
Priority to JP63195885A priority Critical patent/JPH0822982B2/en
Publication of JPH0245578A publication Critical patent/JPH0245578A/en
Publication of JPH0822982B2 publication Critical patent/JPH0822982B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Abstract

PURPOSE:To obtain a top-coating paint composition for household furniture, electrical appliance, car, etc., required to have good appearance by adding mica, flaky pigment having metallic luster and titanium black pigment at specific ratios to a resin composition composed of a thermosetting film-forming resin, a crosslinking agent and a solvent. CONSTITUTION:The objective composition can be produced by compounding (A) a thermosetting resin composition composed of a thermosetting film-forming resin, a crosslinking agent and a solvent with (B) an interference mica and/or a flaky pigment having metallic luster and (C) a titanium black pigment. The weight ratio of the solid pigment of the components B+C in the composition is 2-40% and the ratio of the component C to the components B+C is 0.5-35wt.%.

Description

【発明の詳細な説明】 産業上の利用分野 本発明は塗料組成物、特に美観を必要とする什器・家庭
用電気製品・自動車などの上塗り塗料組成物に関する。
DETAILED DESCRIPTION OF THE INVENTION Field of the Invention The present invention relates to a coating composition, and particularly to a top coating composition for furniture, household electrical appliances, automobiles, etc. that require aesthetic appearance.

従  来  技  術 従来自動車なとの上塗り塗料には、酸化チタン・酸化鉄
などの顔料によるソリ・ソドカラーとアルミニウム粉な
どの金属粉を用いたメタリ・ツクカラーによる表面仕上
げか代表的である、後者の一例としては、例えば、特公
昭411−3 Q +l 115号にはアクリル樹脂系
メタリ・ツクベースコートを含む2コート1ベーク仕上
けが紹介されている。
Conventional technology Conventional top coat paints for automobiles include surface finishes using solid color using pigments such as titanium oxide and iron oxide, and metallic color using metal powder such as aluminum powder. As an example, a two-coat, one-bake finish including an acrylic resin-based metallic base coat is introduced in Japanese Patent Publication No. 411-3 Q+l 115.

しかしながら近時、自動車・家電製品なとの分野に於て
、外観や色相なとの差別fヒが従来以上に強く求められ
るようになりつつ−hす、例えば、特開昭61−374
23号には、特定の色相を有する下地、色の上にコーテ
ィングマイカ層池を積層してメタリック塗膜に無い光輝
感を発揮させるマイカカラー仕上げが提示されている。
However, recently, in the fields of automobiles and home appliances, there has been a stronger demand for discrimination based on appearance and hue than ever before.
No. 23 proposes a mica color finish in which a coating mica layer is laminated on a base and color having a specific hue to exhibit a sense of brilliance not found in metallic coatings.

しかし従来の塗料で表現できる塗膜の色、外観には限界
があり、例えばシルク調の外観を有する塗膜や、濃色系
の光輝性塗膜は従来知られている顔料を単純に組み合わ
せただけでは得られない。例えば、シルク調の外観を得
べく、カーボンブラックに干渉マイカを組み合わせて塗
膜を作成した場合、塗色としては仏味が残り、目的とす
るシルク調も得られず、結局、これまでの塗料ではこの
ようなものは実用的に提示されるに至っていない。
However, there are limits to the color and appearance of paint films that can be expressed with conventional paints; for example, paint films with a silk-like appearance or dark glittering paint films are created by simply combining conventionally known pigments. You can't get it by yourself. For example, when creating a paint film by combining carbon black and interference mica in order to obtain a silk-like appearance, the paint color retains a Buddha-like appearance and the desired silk-like appearance cannot be obtained. However, something like this has not yet been presented in practical terms.

発明が解決しようとする問題点 そこで従来得られていないような意匠性に1量れたシル
ク調の塗膜、光輝感のあるマイカカラー塗膜を与えうる
塗料組成物を提供することか本発明目的である、 問題を解決するための手段 本発明の目的は、熱硬化型フィルム形成性樹脂、架橋剤
、および溶剤からなる熱硬化型の樹脂組5!j、物に <A)干渉マイカ、金属鱗片状顔料あるいはそれらの組
み合わせと、 (B)チタンブラ・ツク顔料 とを分散含有せしめてなり、(A)+ (B)の顔料固
形分重量比か2〜4096であり、且つ、(B)を(A
)+ (B)の1]、5〜35重量%の割合で存在せし
めた塗料組成物により達成せられる。
Problems to be Solved by the Invention Therefore, an object of the present invention is to provide a coating composition that can provide a silk-like coating film and a mica color coating film with a glittering appearance and a high degree of design, which have not been previously available. An object of the present invention is to provide a thermosetting resin set 5 consisting of a thermosetting film-forming resin, a crosslinking agent, and a solvent. j, the material contains <A) interference mica, metal scale pigment, or a combination thereof, and (B) titanium black pigment dispersed therein, and the pigment solid content weight ratio of (A) + (B) is 2. ~4096, and (B) is (A
) + (B) 1] is present in a coating composition in a proportion of 5 to 35% by weight.

本発明で用いられる干渉マイカは酸化チタン・酸化鉄・
クロム酸等の単独または二つ以上の組み合わせ系て表面
をコートされたマイカ粒子であって、パール塗装用等に
通常使用されている任意のものとすることができる。具
(本例としては、例えば、エクステリアマ−リンブライ
)・ホワイト(マール社(Mearl Corpora
tion )製品、酸化チタンコート)・エクステリア
マ−リンハイライトブルー(同社製品、酸1ヒチタンコ
ート)・エクステリアマーリンラセ・ソト(同社製品、
酸、rヒ鉄コート、酸(ヒチタンコート)・ハールクレ
イスSME−11fl−“)(日本充所・′m製品、酸
化チタンコート) バール7レイスSMBQO−9(日
本充所(m製品、酸(ヒチタンコート)パールグしイス
S M C5112−’1ci9 (日本充所1…製品
、酸rヒ鉄、酸化千タンコート)等か挙けられる。
The interference mica used in the present invention is titanium oxide, iron oxide,
Any mica particles whose surface is coated with chromic acid or the like alone or in combination of two or more, which are commonly used for pearl coatings, etc., can be used. (In this example, for example, Exterior Marlin Bly) / White (Mearl Corpora
tion) products, titanium oxide coat), Exterior Marlin Highlight Blue (the company's product, acid 1 titanium coat), Exterior Marlin Lase Soto (the company's product,
Acid, r arsenate coat, acid (hititanium coat), HARCLACE SME-11fl-") (Nihon Jyusho, 'm product, titanium oxide coat) Bar 7 Wraith SMBQO-9 (Nippon Jyusho (m product, acid) (Hititanium coat) Pearl steel chair S M C5112-'1ci9 (Nippon Jusho 1... product, acid r arsenate, 1,000 tananium oxide coat), etc.

金属Qgi−状顔料としてはアルミ箔が代表的であり、
例えば、東洋アルミニウム製造側のアルペースト713
flN、アルペースト51−231、アルペースl−5
2−509などが使用可能のものとして例示される。
Aluminum foil is a typical metal Qgi-like pigment,
For example, Toyo Aluminum Manufacturing's Alpaste 713
flN, Alpaste 51-231, Alpace l-5
2-509 etc. are exemplified as usable ones.

上記干渉マイカ、および/′または金属鱗片状顔料に組
み合わして使用するチタンブラック顔料は、いわゆる低
次酸化チタンと称せられる、二酸化チタンを除く千タン
酸(ヒ杓からなる黒色系顔料であって、還元度により多
彩な色目のらのか提供せられ、所望により選択・使用せ
られる。
The titanium black pigment used in combination with the above-mentioned interference mica and/or metal flake pigment is a black pigment consisting of 1,000 tanoic acid excluding titanium dioxide, called so-called lower titanium oxide. Various colors are available depending on the degree of reduction, and can be selected and used as desired.

組成式で示せば、例えは、Ti01Ti203、Ti3
O5、Ti4O7、TizoO31等が挙げられ、これ
らは−服代; Ti02−、 (ただしXは0<x<2
を満尾する実数)で表すことかできる。真木的には、黒
色酸化チタンM−1・黒色酸化チタンS1(何れら石原
産業(m製品)・チタンブラック粉末13R・チタンブ
ラック10S(何れも三菱金属(m製品)等が挙げられ
る。
In terms of compositional formula, for example, Ti01Ti203, Ti3
O5, Ti4O7, TizoO31, etc. are mentioned, and these are -clothing cost; Ti02-, (where X is 0<x<2
can be expressed as a full real number). Maki's examples include black titanium oxide M-1, black titanium oxide S1 (all manufactured by Ishihara Sangyo (m products)), titanium black powder 13R, and titanium black 10S (all manufactured by Mitsubishi Metals (m products)).

なお、所望により、本発明の目的達成に支障の無い範[
川内において、前記以外の着色顔料・木質顔料・防錆顔
料・耐チッピング性頷科等を前記の顔料混合系に適当量
併用することは可t1ヒである。
In addition, if desired, the range [
In Kawauchi, it is possible to use appropriate amounts of coloring pigments, wood pigments, rust-preventive pigments, chipping-resistant pigments, etc. other than those mentioned above in combination with the above-mentioned pigment mixture system.

このような顔料混合系は、熱硬(上型フィルム形成性樹
脂、架橋剤および溶剤からなる熱硬化型の樹脂組成物に
分散含有せしめられる、熱硬化型フィルム形成性I厨指
としては、51+Mアルコールと多塩基酸から成るポリ
エステル樹脂、およびこれを油等で変性したアルキF 
I5(指、あるいは(メタ)アクリル酸、(メタ)アク
リル酸エステルからなるアクリル樹脂等、通常塗料分野
て゛熱硬化型のバインダー樹脂として用いられるものが
好都合に使用され、これに架橋剤としてメラミン樹脂や
プロ・ツクイソシアネート等か組み合わせられる。
Such a pigment mixture system is dispersed in a thermosetting resin composition consisting of a thermosetting resin, a crosslinking agent, and a solvent. Polyester resin consisting of alcohol and polybasic acid, and Alki-F modified with oil etc.
It is convenient to use acrylic resins made of I5 (acrylic acid, (meth)acrylic acid, (meth)acrylic acid esters, etc., which are usually used as thermosetting binder resins in the paint field, and melamine resin as a crosslinking agent). It can be combined with pro-tsukiisocyanate, etc.

次に、(A >干渉マイカ、金属鱗片状顔nあるいはそ
れらの組み合わせと、(B)チタンブラック顔料とのき
計量(A)+ (B)の顔料固形分重量比は、塗料組成
物の固形分全重量に対し2〜4096であることが必要
であり、2重量%より少ない場合には、目的とする外観
・色相を得難いし、一方40重量%を超える場合には、
顔料過剰により塗面にツヤヒケを生じたり、十分な塗膜
性能の維持が困難となり好ましくない。
Next, when (A > interference mica, metal scale face n, or a combination thereof and (B) titanium black pigment, the pigment solid content weight ratio of (A) + (B) is the solid content of the coating composition. It is necessary to have a content of 2 to 4096 based on the total weight. If it is less than 2% by weight, it will be difficult to obtain the desired appearance and hue, while if it exceeds 40% by weight,
Excess pigment causes glossy sink marks on the coated surface and makes it difficult to maintain sufficient coating performance, which is undesirable.

またチタンブラック顔料(B)は干渉マイカ、金属鱗片
状顔料(A)およびチタンブラック顔料(B)の合計量
の115〜359もとすべきで、0.5°6よりも少な
くなるとシルキー感がなくなり、また35°6よりも多
くなると黒のソリ・ソド色に近くなり、光輝感がなくな
るため、いずれも好ましくなく、意匠性かなくなること
か確かめられている8 干渉マイカやアルミ箔等の鱗片状顔料は、予め適当な溶
剤で分散したペーストとじて、またはそのまま直接塗料
液に攪拌等をしながら混合するのみて均一に分散できる
、一方、チタンブラ・ツク顔料は例えば、予め、1重用
する熱硬「ヒ型アクリル崩脂ワニスの一部に均一に分散
させた後、残りのアクリル樹脂やメラミン樹脂などを添
加して溶解し、分散液を調整する。
In addition, the titanium black pigment (B) should be 115 to 359 of the total amount of interference mica, metal flake pigment (A), and titanium black pigment (B), and if it is less than 0.5°6, a silky feeling will occur. Moreover, if it exceeds 35°6, the color becomes close to black, and the shine disappears, so both are unfavorable and it has been confirmed that the design quality will be lost. 8. Scales of interference mica, aluminum foil, etc. Titanium black pigments can be dispersed uniformly by making a paste that has been dispersed in advance with an appropriate solvent, or by directly mixing it with the paint liquid while stirring. After uniformly dispersing it in a portion of hard acrylic fat-soluble varnish, the remaining acrylic resin, melamine resin, etc. are added and dissolved to prepare a dispersion liquid.

従って、塗料組成物を調整する場合、先ずチタンブラッ
ク顔料の分散液を調整しておき、これに鱗片状顔料をそ
のまま直接または溶剤ペーストの形で適宜混合せしめれ
ば、好適に調整できる。
Therefore, when preparing a coating composition, first a dispersion of titanium black pigment is prepared, and the flaky pigment is suitably mixed therein either directly or in the form of a solvent paste.

本発明の塗料組成物は、熱硬化型塗料を塗装される各種
の被塗物に仕上げ用上塗りとして適用せられ、特有の美
観効果を発揮するか、持に美観を必要とする什器・家庭
用電気製品・自動車などの上塗りとして有用である。そ
の中て代表的塗装系として自動車なとを対象とした2コ
ーl〜1ベーク塗装系が挙げられ、この2コー1−1ヘ
ーク塗装系のベースコートとして本塗料組成物は特に有
用である。
The coating composition of the present invention can be applied as a finishing top coat to various objects to be coated with thermosetting paints, and can exhibit a unique aesthetic effect, or can be used for fixtures and home use that require a particularly aesthetic appearance. It is useful as a top coat for electrical products, automobiles, etc. Among these, representative coating systems include 2 coat 1 to 1 bake coating systems for automobiles, and the present coating composition is particularly useful as a base coat for these 2 coat 1-1 bake coating systems.

ここで2コート1ベーク塗装系とは、上塗り塗料に関す
る塗装系の−ってあって、自動車等の金属被塗物の場合
には先ず、通常、化成処理をし、電着プライマー(乾燥
膜厚、通常15〜3011、 )か適用され、次に中塗
塗料が適用され、(乾燥膜厚、通常35〜40μ)乾燥
焼付を行い、所望により本所で表面を平滑にする等の前
段階を経た後に、この2コート1ベーク塗装系が適用せ
られる、 すなわち、これは、先ず初めに顔料汁の多いベース コ
ートを塗装し、次いでその」二に透明クリヤー または
顔料分の少ないカラークリヤーであるト・・ノブコート
をウェット・オン  ウニ’7トで適用し、−度に焼付
硬化せしめてベースコート塗膜層(乾燥膜厚、通常10
〜211μ)とクリヤーまたはカラークリヤー層(乾燥
膜厚、通常25〜40μ)とを形成せしめる工程からな
るもめである。
Here, the 2-coat, 1-bake coating system refers to a coating system related to topcoat paints, and in the case of metal objects such as automobiles, a chemical conversion treatment is usually performed first, followed by an electrodeposition primer (dry film thickness). , usually 15-3011) is applied, then an intermediate coating is applied (dry film thickness, usually 35-40μ), dry baking is performed, and if desired, the surface is smoothed at the main office, etc. Later on, this two-coat, one-bake coating system is applied, i.e., first a pigment-rich base coat is applied, followed by a second coat, either a transparent clear or a low-pigment color clear.・Apply Knob Coat wet-on-unit and bake harden it to form a base coat layer (dry film thickness, usually 10
~211μ) and a clear or color clear layer (dry film thickness, usually 25 to 40μ).

本発明による塗料組成物を被塗面に適用した場合、これ
までの塗料では得ることのできなかった落ち着いたシル
キー調の、意匠性に優れた塗膜か得られ、特に自動車・
末完電気製品・什器等の塗装において、従来品との差別
1ヒが可能となり、大幅な商品価値の向上につながる5
以下実施例に基づいて詳細の説明を行う、特にことわり
ない限り、部および?6は重置による。
When the coating composition according to the present invention is applied to a surface to be coated, a coating film with a calm silky tone and excellent design properties, which could not be obtained with conventional coatings, can be obtained.
When painting finished electrical appliances, fixtures, etc., it becomes possible to differentiate it from conventional products, leading to a significant increase in product value5.
Detailed explanations will be given below based on Examples, unless otherwise specified. 6 is due to overlapping.

実施例 1 干渉マイカ(マール社製、エクステリアマリーンブライ
トホワイト)2部1部にhルエン20部を加えて均一に
分散させた。
Example 1 20 parts of h-luene was added to 2 parts and 1 part of interference mica (manufactured by Marl Corporation, Exterior Marine Bright White) and uniformly dispersed.

これとは別にチタンブラ・ツク顔料く三菱3属(中震、
チタンブラック粉末13R)20部を予め熱硬化型アク
リル(M脂ワニス(三井東圧+t4f製、アルマテック
スNT−u−448、樹脂固形分48%)  166.
7部に同容量の2mmφカラスピースと混ぜ、デイスパ
ーで60分間分散せしめた液にメラミン樹脂ワニス(大
日本インキ(中震、スーツく−ベッカミンJ −820
−60、樹脂固形分60%)を加えてデイスパーにて3
0分間攪拌し、濾過し、ガラスピーズを除去した。この
チタンブラ・ツク顔料分散ワニスに、先に調整した干渉
マイカペーストをカロ疋、均一に攪拌して塗料液とした
、実施例 2〜8 実施例1と同じ原料を使用し、但し実施例1の各原料の
配合量を第1表に示した通りの各配合量に代える以外は
、実施例1と同様方法で各塗料液を調整した。
Apart from this, there are three types of Mitsubishi including titanbura and Tsuku pigments (medium shock,
166. 20 parts of titanium black powder 13R) was previously mixed with thermosetting acrylic (M fat varnish (Mitsui Toatsu + T4F, Almatex NT-U-448, resin solid content 48%).
Mix 7 parts with the same volume of 2mmφ crow pieces and disperse for 60 minutes using a disperser.
-60, resin solids content 60%) was added and 3
Stir for 0 minutes, filter and remove glass beads. Examples 2 to 8 The same raw materials as in Example 1 were used, except that the previously prepared interference mica paste was added to this titanium black pigment-dispersed varnish and stirred uniformly to form a coating liquid. Each coating liquid was prepared in the same manner as in Example 1, except that the amounts of each raw material were changed to those shown in Table 1.

実施例 9 実施例2の干渉マイカをアルミ箔顔料(東洋アルミニウ
ム(掬製、アルペースト713ON、固型分65%)に
代える以外は、実施例2と同じ配合と方法で塗料液を調
整した。
Example 9 A coating liquid was prepared using the same formulation and method as in Example 2, except that the interference mica in Example 2 was replaced with an aluminum foil pigment (Alpaste 713ON, manufactured by Toyo Aluminum Co., Ltd., manufactured by Kiki, solid content 65%).

比較例 1 干渉マイカ(マール社製、エクステリアマ−リンブライ
トホワイト)20部にトルエン20部を加えて攪拌し、
均一に分散させた、 これとは別に熱硬化型アクリル(M脂ワニス(アルマテ
ックスNT−電J −40>  166.7部およびメ
ラミン樹1指フェス(スーパーベッカミン、工826−
60) 33.3部を加えてデイスパーにて30分間攪
拌しな。このワニスに、先に調整した干渉マイカペース
トを加え、均一に攪拌して塗料液とした。
Comparative Example 1 20 parts of toluene was added to 20 parts of interference mica (manufactured by Marl Corporation, Exterior Marlin Bright White) and stirred.
Separately, thermosetting acrylic (M resin varnish (Almatex NT-Den J-40) > 166.7 parts and melamine resin 1-finger fest (Super Beckamine, Engineering 826-
60) Add 33.3 parts and stir with a disper for 30 minutes. The previously prepared interference mica paste was added to this varnish and stirred uniformly to form a coating liquid.

比較例 2 チタンブラック顔料(チタンブラック粉末13R)20
部に、熱硬化型アクリル樹脂ワニス(アルマテックスN
 T −11−448>  !66.7部、および°メ
ラミン樹脂ワニス(スーパーベッカミンJ−1126−
60) 33.3部を加えて、同容量(約200m1 
)の2朋φガラスピーズを入れ、デイスパーにて60分
間攪拌し、濾過によりカラスピースを除去し、塗料液を
調整した (  以  下、余  白  ) 塗装試験板の作製 音鋼板(長さ 500■、巾3011順、厚さ 0.8
1)をリン酸亜鉛処理剤(日本ペイント(作製、グラノ
ヂン5D51]00)で常法により前処理した後、カチ
オン電着塗料(日本ペイント(作製、パワートップU−
30、エポキシウレタン・カチオン樹脂系)で常法によ
り電着塗装を行い、乾燥膜厚20μの電着塗膜を形成せ
しめた。次いで中塗塗料(日本ペイント(作製、オルガ
P−2グレー、ポリエステルメラミン樹脂系)を常法に
より塗布し、乾燥膜735μの中塗塗膜を形成せしめた
Comparative example 2 Titanium black pigment (Titanium black powder 13R) 20
Thermosetting acrylic resin varnish (Almatex N)
T-11-448>! 66.7 parts, and °Melamine resin varnish (Super Beckamine J-1126-
60) Add 33.3 parts to make the same volume (approx. 200ml)
) and stirred with a disper for 60 minutes, removed the glass pieces by filtration, and adjusted the paint solution (see below for margins) Preparation of painted test plate Sound steel plate (length 500cm) , width 3011 order, thickness 0.8
1) was pretreated with a zinc phosphate treatment agent (manufactured by Nippon Paint Co., Ltd., Granodin 5D51] 00) in a conventional manner, and then treated with a cationic electrodeposition paint (manufactured by Nippon Paint Co., Ltd., Power Top U-
No. 30, epoxy urethane/cationic resin system) was electrocoated using a conventional method to form an electrocoated film with a dry thickness of 20 μm. Then, an intermediate coating (manufactured by Nippon Paint, Olga P-2 Gray, polyester melamine resin system) was applied by a conventional method to form an intermediate coating film with a dry film thickness of 735 μm.

この上に前記第1表に示した各塗料液を塗料用シンナー
(日本ペイン+−+m製、ニツペ298)でうすめ(#
4フォート力・ツブで13秒’2n’C)、スフ。
On top of this, dilute each paint solution shown in Table 1 above with paint thinner (Nippon Paint +-+M, Nizpe 298).
13 seconds '2n'C) with 4 fort power and Tsubu, Sufu.

1/−カン(H本うンズ°バーグI+@、R,13A、
)、ズルキャ・7No、+;)で静電噴Wr塗装(第1
回と第2回の間C,こ1分間フラ・ノシュオフして2回
塗り重ね)を行い、塗膜を形成せしめた(乾燥膜厚に換
算し5μ〉、二の?裔つェット・オン・ウニ・ソトて゛
クリヤー塗料(日本ペイント(作製、スーパーラ・ツク
0−28L、アクリル・メラミン樹脂系)を塗装し14
0 ’Cで20分間焼付を行い、乾燥全膜厚110μの
塗膜を形成せしめた、それぞれ各実施例、比較例に対応
した塗装試験板を作製した。
1/-Kan (H book Unsberg I+@, R, 13A,
), Zurkya 7No, +;) electrostatic spray Wr coating (first
Between the first and second coats (C), the coating was applied for 1 minute and then coated twice) to form a coating film (converted to a dry film thickness of 5μ). Painted with Uni Sototen clear paint (manufactured by Nippon Paint, Super La Tsuk 0-28L, acrylic/melamine resin system) 14
Coated test plates corresponding to each of the Examples and Comparative Examples were prepared by baking at 0'C for 20 minutes to form a coating film with a total dry film thickness of 110μ.

この塗装試験板についての試験を行った5試験結果 比較例3と比べ、実施例1〜1oは、シルキー調の落ち
着いた色相が与えれな、 特許出願代理友 弁理士  伊  藤  武  雄
Five test results were conducted on this coated test board. Compared to Comparative Example 3, Examples 1 to 1o had a silky, muted hue.

Claims (1)

【特許請求の範囲】 熱硬化型フィルム形成性樹脂、架橋剤、および溶剤から
なる熱硬化型の樹脂組成物に (A)干渉マイカ、金属鱗片状顔料あるいはそれらの組
み合わせと、 (B)チタンブラック顔料 とを分散含有せしめてなり、(A)+(B)の顔料固形
分重量比が2〜40%であり、且つ、(B)を(A)+
(B)の0.5〜35重量%の割合で存在せしめること
を特徴とする塗料組成物。
[Scope of Claims] A thermosetting resin composition comprising a thermosetting film-forming resin, a crosslinking agent, and a solvent, and (A) interference mica, metal scale pigment, or a combination thereof, and (B) titanium black. (A) + (B) has a pigment solid content weight ratio of 2 to 40%, and (B) is dispersed in (A) +
A coating composition characterized in that (B) is present in a proportion of 0.5 to 35% by weight.
JP63195885A 1988-08-05 1988-08-05 Paint composition Expired - Lifetime JPH0822982B2 (en)