[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JPH079050B2 - Connecting rod for internal combustion engine - Google Patents

Connecting rod for internal combustion engine

Info

Publication number
JPH079050B2
JPH079050B2 JP3674892A JP3674892A JPH079050B2 JP H079050 B2 JPH079050 B2 JP H079050B2 JP 3674892 A JP3674892 A JP 3674892A JP 3674892 A JP3674892 A JP 3674892A JP H079050 B2 JPH079050 B2 JP H079050B2
Authority
JP
Japan
Prior art keywords
connecting rod
weight
cap
rod body
aluminum alloy
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP3674892A
Other languages
Japanese (ja)
Other versions
JPH0570879A (en
Inventor
治男 椎名
良一 村樫
雅己 星
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Honda Motor Co Ltd
Original Assignee
Honda Motor Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority claimed from JP18476186A external-priority patent/JPS6342343A/en
Application filed by Honda Motor Co Ltd filed Critical Honda Motor Co Ltd
Priority to JP3674892A priority Critical patent/JPH079050B2/en
Publication of JPH0570879A publication Critical patent/JPH0570879A/en
Publication of JPH079050B2 publication Critical patent/JPH079050B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【産業上の利用分野】本発明は内燃機関用コンロッド、
特に、桿部を有するコンロッド本体と、そのコンロッド
本体にボルトにより締結されるキャップとを備えた内燃
機関用コンロッドに関する。
BACKGROUND OF THE INVENTION The present invention relates to a connecting rod for an internal combustion engine,
In particular, the present invention relates to a connecting rod for an internal combustion engine that includes a connecting rod body having a rod portion and a cap fastened to the connecting rod body by a bolt.

【0002】[0002]

【従来の技術】従来、この種コンロッドとして、粉末冶
金法の適用により大量のSi、Fe、Mn等を添加した
高強度アルミニウム合金より構成されたものが知られて
いる。
2. Description of the Related Art Heretofore, as this type of connecting rod, one made of a high-strength aluminum alloy to which a large amount of Si, Fe, Mn or the like has been added by applying a powder metallurgy method is known.

【0003】[0003]

【発明が解決しようとする課題】しかしながら、従来の
コンロッド用高強度アルミニウム合金(以下、公知合金
と称す)には次に述べるような諸問題点がある。 (a) 公知合金は微細金属組織を有するので、強度的
には優れているが、クリープ特性が劣るため、高温下で
常時圧縮応力を受けるキャップのボルト締結部では、長
時間の使用に伴いクリープ縮みが増加し、その結果、ボ
ルト締結力が減少したり、極端な場合にはボルト締結部
の破壊に至るおそれがある。 (b) 公知合金は大量のSi、Fe、Mn等の添加に
より熱膨脹係数の低下およびヤング率の向上を狙ってい
るが、工業材料としての生産性および靱性を考慮する
と、熱膨脹係数は約18×10-6/℃、ヤング率は約1
0000kg/mm2 が限界である。
However, the conventional high-strength aluminum alloy for connecting rod (hereinafter referred to as a known alloy) has the following problems. (A) Since the known alloy has a fine metal structure and therefore is excellent in strength, it has poor creep characteristics. Therefore, at the bolt fastening portion of the cap that is constantly subjected to compressive stress at high temperatures, creep occurs with long-term use. The shrinkage increases, and as a result, the bolt fastening force may be reduced, or in extreme cases, the bolt fastening portion may be broken. (B) The known alloy aims to lower the coefficient of thermal expansion and improve the Young's modulus by adding a large amount of Si, Fe, Mn, etc. However, considering the productivity and toughness as an industrial material, the coefficient of thermal expansion is about 18 ×. 10 -6 / ℃, Young's modulus is about 1
The limit is 0000 kg / mm 2 .

【0004】アルミニウム合金よりコンロッドを構成
し、それを鋼製クランクシャフトと組合せた場合、それ
らの間のクリアランス、圧入代等を決定するに当り、ア
ルミニウム合金の熱膨脹係数が鋼のそれに接近していれ
ば設計上の自由度が増すことになるが、公知合金ではこ
のような要求を満たすことができない。そのため、コン
ロッドのクランクピン孔とクランクシャフトのクランク
ピンとの間のクリアランスは温度の上昇に伴い大幅に増
大する。
When a connecting rod is made of aluminum alloy and is combined with a steel crankshaft, the coefficient of thermal expansion of the aluminum alloy should be close to that of steel when determining the clearance between them and the press-fitting margin. Although the degree of freedom in design increases, the known alloy cannot meet such requirements. Therefore, the clearance between the crankpin hole of the connecting rod and the crankpin of the crankshaft greatly increases as the temperature rises.

【0005】またヤング率は、荷重を受けた時のコンロ
ッドの弾性域における変位、歪を左右する重要なフアク
タであり、コンロッドの小型化を図るためにはヤング率
を十分に大きくする必要があるが、公知合金ではこのよ
うな要求を満たすことができない。 (c) 公知合金は、それに析出する初晶Si、共晶S
i、金属間化合物等が非常に微細であるため、摺動摩耗
量が比較的多く、その結果高面圧、高速摺動下では耐久
性に乏しいといった問題があり、コンロッド構成材料と
して満足すべきものではない。
The Young's modulus is an important factor that influences the displacement and strain of the connecting rod in the elastic region when a load is applied, and it is necessary to sufficiently increase the Young's modulus in order to downsize the connecting rod. However, known alloys cannot meet such requirements. (C) Known alloys include primary crystal Si and eutectic S that precipitate on the alloy.
Since i and intermetallic compounds are extremely fine, there is a relatively large amount of sliding wear, and as a result, there is a problem that durability is poor under high surface pressure and high-speed sliding. is not.

【0006】本発明は前記諸問題を解決し得る前記内燃
機関用コンロッドを提供することを目的とする。
An object of the present invention is to provide a connecting rod for an internal combustion engine which can solve the above problems.

【0007】[0007]

【課題を解決するための手段】本発明は、桿部を有する
コンロッド本体と、そのコンロッド本体にボルトにより
締結されるキャップとを備えた内燃機関用コンロッドに
おいて、前記コンロッド本体は、 12.0重量%≦Si≦28.0重量%、 0.8重量%≦Cu≦5.0重量%、 0.3重量%≦Mg≦3.5重量%、 2.0重量%≦Fe≦10.0重量%、 0.5重量%≦Mn≦2.9重量% および不可避不純物を含む残部Alよりなる急冷凝固ア
ルミニウム合金粉末を用いた高強度アルミニウム合金よ
り構成され、前記キャップは、前記急冷凝固アルミニウ
ム合金粉末を用いた高強度アルミニウム合金マトリック
スに、Al23 粒子、SiC粒子、Si3 4 粒子お
よび金属Si粒子から選択される少なくとも一種の硬質
粒子を1.5重量%以上、15.0重量%以下分散させ
た複合材より構成されていることを特徴とする。
The present invention provides a connecting rod for an internal combustion engine comprising a connecting rod body having a rod portion and a cap fastened to the connecting rod body by a bolt, wherein the connecting rod body has a weight of 12.0. % ≤ Si ≤ 28.0 wt%, 0.8 wt% ≤ Cu ≤ 5.0 wt%, 0.3 wt% ≤ Mg ≤ 3.5 wt%, 2.0 wt% ≤ Fe ≤ 10.0 wt% %, 0.5 wt% ≤ Mn ≤ 2.9 wt% and the balance Al containing unavoidable impurities, and is composed of a high strength aluminum alloy using a rapidly solidified aluminum alloy powder, and the cap is the rapidly solidified aluminum alloy powder. 1. In a high-strength aluminum alloy matrix using 1., at least one hard particle selected from Al 2 O 3 particles, SiC particles, Si 3 N 4 particles, and metallic Si particles. It is characterized by being composed of a composite material in which 5% by weight or more and 15.0% by weight or less are dispersed.

【0008】[0008]

【作用】急冷凝固アルミニウム合金粉末の組成を前記の
ように特定すると、優れた高温強度、耐摩耗性およびヤ
ング率を有し、また熱膨脹係数の低下を図ると共に耐応
力腐食割れ特性を改善された高強度アルミニウム合金、
したがってコンロッド本体およびキャップのマトリック
スを構成することができる。
When the composition of the rapidly solidified aluminum alloy powder is specified as described above, it has excellent high-temperature strength, wear resistance and Young's modulus, and also has a low thermal expansion coefficient and improved stress corrosion cracking resistance. High strength aluminum alloy,
Therefore, the matrix of the connecting rod body and the cap can be constructed.

【0009】また急冷凝固アルミニウム合金は一般に難
加工性であるが、前記のように各化学成分の含有量を特
定することによって、熱間押出し加工性、熱間鍛造加工
性等の熱間塑性加工性を向上させてコンロッド本体およ
びキャップの生産性を良好にすることができる。
Further, the rapidly solidified aluminum alloy is generally difficult to work, but by specifying the content of each chemical component as described above, hot plastic workability such as hot extrusion workability and hot forging workability is obtained. It is possible to improve productivity and improve productivity of the connecting rod body and the cap.

【0010】各化学成分および硬質粒子の含有理由およ
び含有量の限定理由は以下の通りである。 (a) Siについて Siは、急冷凝固アルミニウム合金粉末より形成される
コンロッド本体およびキャップのマトリックスにおける
耐摩耗性、ヤング率および熱伝導率を向上し、また熱膨
脹係数を低下する効果を有する。ただし、12.0重量
%を下回ると前記効果を得ることができず、一方、2
8.0重量%を上回ると、熱間押出し加工および熱間鍛
造加工において成形性が悪化し、コンロッド本体等に割
れを生じ易くなる。 (b) Cuについて Cuは、熱処理においてコンロッド本体等を強化する効
果を有する。ただし、0.8重量%を下回ると前記効果
を得ることができず、一方、5.0重量%を上回ると、
熱間鍛造加工性が低下し、またコンロッド本体等の耐応
力腐食割れ特性が悪化する。 (c) Mgについて Mgは、Cuと同様に熱処理においてコンロッド本体等
を強化する効果を有する。ただし、0.3重量%を下回
ると前記効果を得ることができず、一方、3.5重量%
を上回ると、熱間鍛造加工性が低下し、またコンロッド
本体等の耐応力腐食割れ特性が悪化する。 (d) Feについて Feは、コンロッド本体等の高温強度およびヤング率を
向上させる効果を有する。ただし、2.0重量%を下回
ると、コンロッド本体等における高温強度の向上を期待
することができず、一方、10.0重量%を上回ると高
速熱間鍛造加工が事実上不可能となる。 (e) Mnについて Mnは、特にFe≧4重量%の範囲において、熱間鍛造
加工性を向上させ、またコンロッド本体等の高温強度お
よび耐応力腐食割れ特性を改善する効果を有する。ただ
し、0.5重量%を下回ると、前記効果を得ることがで
きず、一方、2.9重量%を上回ると、却って熱間鍛造
加工性が悪化する等、悪影響が現れる。 (f) 硬質粒子について 前記のように特定された4種の硬質粒子は、キャップの
マトリックスに分散することによりその結晶の転位を固
着して高温下におけるキャップのクリープ特性を改善
し、また熱膨脹係数を低下し、さらにヤング率および耐
摩耗性を向上する効果を有する。ただし、急冷凝固アル
ミニウム合金粉末に対する硬質粒子の含有量が1.5重
量%を下回ると、キャップの耐摩耗性が改善されず、ま
たヤング率の向上および熱膨脹係数の減少の程度も低く
なり、一方、15.0重量%を上回ると、熱間鍛造加工
性が低下し、またキャップの疲労強度および機械加工性
がそれぞれ著しく低下する。
The reasons for containing each chemical component and the hard particles and the reasons for limiting the content are as follows. (A) About Si Si has the effects of improving the wear resistance, Young's modulus and thermal conductivity of the matrix of the connecting rod body and cap formed from the rapidly solidified aluminum alloy powder, and reducing the coefficient of thermal expansion. However, if it is less than 12.0% by weight, the above effect cannot be obtained, while 2
If it exceeds 8.0% by weight, the formability is deteriorated in the hot extrusion process and the hot forging process, and the connecting rod body or the like is likely to be cracked. (B) Regarding Cu Cu has the effect of strengthening the connecting rod body and the like during heat treatment. However, if less than 0.8% by weight, the above effect cannot be obtained, while if more than 5.0% by weight,
Hot forgeability deteriorates and stress corrosion cracking resistance of the connecting rod body deteriorates. (C) About Mg Like Mg, Mg has the effect of strengthening the connecting rod body and the like during heat treatment. However, if it is less than 0.3% by weight, the above effect cannot be obtained, while if it is 3.5% by weight.
If it exceeds the range, the hot forgeability deteriorates and the stress corrosion cracking resistance of the connecting rod body and the like deteriorates. (D) About Fe Fe has the effect of improving the high temperature strength and Young's modulus of the connecting rod body and the like. However, if it is less than 2.0% by weight, improvement in high temperature strength in the connecting rod body or the like cannot be expected, while if it exceeds 10.0% by weight, high speed hot forging becomes practically impossible. (E) About Mn Mn has the effect of improving hot forgeability and improving high-temperature strength and stress corrosion cracking resistance of the connecting rod body and the like, particularly in the range of Fe ≧ 4 wt%. However, if it is less than 0.5% by weight, the above effect cannot be obtained, while if it exceeds 2.9% by weight, adverse effects such as deterioration of hot forgeability rather occur. (F) Hard Particles The four kinds of hard particles specified as described above are dispersed in the cap matrix to fix crystal dislocations, improve the creep characteristics of the cap at high temperature, and increase the thermal expansion coefficient. And also has the effect of improving Young's modulus and wear resistance. However, when the content of the hard particles in the rapidly solidified aluminum alloy powder is less than 1.5% by weight, the wear resistance of the cap is not improved, and the Young's modulus is improved and the coefficient of thermal expansion is also decreased. If it exceeds 15.0% by weight, the hot forgeability is deteriorated, and the fatigue strength and machinability of the cap are remarkably deteriorated.

【0011】[0011]

【実施例】図1は、内燃機関用コンロッド1を示し、そ
のコンロッド1は桿部2を有するコンロッド本体3と、
そのコンロッド本体3にボルト4により締結されるキャ
ップ5とを備えている。
1 shows a connecting rod 1 for an internal combustion engine, which connecting rod 1 has a connecting rod body 3 having a rod portion 2,
The connecting rod body 3 is provided with a cap 5 that is fastened with bolts 4.

【0012】前記急冷凝固アルミニウム合金粉末におけ
る各化学成分の含有量は、コンロッド本体3およびキャ
ップ5のマトリックスにおいて、特に耐応力腐食割れ特
性および熱間鍛造加工性を良好にするためには下記に限
定される。
The content of each chemical component in the rapidly solidified aluminum alloy powder is limited to the following in the matrix of the connecting rod body 3 and the cap 5 in order to particularly improve stress corrosion cracking resistance and hot forgeability. To be done.

【0013】 14.0重量%≦Si≦18.0重量% 2.0重量%≦Cu≦5.0重量% 0.3重量%≦Mg≦1.5重量% 3.0重量%≦Fe≦6.0重量% 0.5重量%≦Mn≦2.5重量% 前記複合材より、熱的影響を受けるキャップ5を構成す
る場合、このキャップ5についてはヤング率、熱膨脹係
数、クリープ特性および機械加工性が問題となるので、
前記硬質粒子の含有量は9.0重量%以上、13.0重
量%以下が好ましい。その理由は、9.0重量%を下回
ると、クリープ特性改善効果が減少傾向となり、一方、
13.0重量%を上回ると機械加工性が低下する傾向に
あるからである。
14.0 wt% ≦ Si ≦ 18.0 wt% 2.0 wt% ≦ Cu ≦ 5.0 wt% 0.3 wt% ≦ Mg ≦ 1.5 wt% 3.0 wt% ≦ Fe ≦ 6.0% by weight 0.5% by weight ≦ Mn ≦ 2.5% by weight When the cap 5 to be thermally affected is composed of the composite material, the cap 5 has Young's modulus, coefficient of thermal expansion, creep characteristics and mechanical properties. Since workability is a problem,
The content of the hard particles is preferably 9.0% by weight or more and 13.0% by weight or less. The reason is that if it is less than 9.0% by weight, the creep property improving effect tends to decrease, while
This is because if it exceeds 13.0% by weight, the machinability tends to decrease.

【0014】また鋼製クランクシャフトとの摺動摩耗が
問題となる場合には、その鋼の種類にもよるが、硬質粒
子の含有量は2.0重量%以上、4.0重量%以下が好
ましい。その理由は、2.0重量%を下回るとキャップ
5の摩耗量が増える傾向にあり、一方、4.0重量%を
上回るとクランクシャフトの摩耗量が増える傾向にある
からである。
When sliding wear with a steel crankshaft poses a problem, the content of hard particles should be 2.0% by weight or more and 4.0% by weight or less, depending on the type of the steel. preferable. The reason is that if it is less than 2.0% by weight, the amount of wear of the cap 5 tends to increase, while if it exceeds 4.0% by weight, the amount of wear of the crankshaft tends to increase.

【0015】キャップ5を製造する場合は、例えば急冷
凝固アルミニウム合金粉末と硬質粒子とを混合して混合
粉末を得、次いでその混合粉末に冷間静水圧プレス成形
法(CIP法)等を適用して圧粉体を得、その後圧粉体
に熱間押出し加工を施すものである。
When the cap 5 is manufactured, for example, rapidly solidified aluminum alloy powder and hard particles are mixed to obtain a mixed powder, and then the cold isostatic pressing method (CIP method) or the like is applied to the mixed powder. To obtain a green compact, and then subject the green compact to hot extrusion processing.

【0016】この場合、急冷凝固アルミニウム合金粉末
の粒度は、325メッシュ以下のものを、45重量%以
上、70重量%以下とする。その理由は、前記粒度の粉
末が45重量%を下回ると疲労強度が低下し、一方、7
0重量%を上回るとクリープ特性が悪化するからであ
る。
In this case, the particle size of the rapidly solidified aluminum alloy powder is not less than 325 mesh and not less than 45% by weight and not more than 70% by weight. The reason is that if the powder having the above particle size is less than 45% by weight, the fatigue strength decreases, while
This is because if it exceeds 0% by weight, the creep characteristics deteriorate.

【0017】また硬質粒子の粒径は、疲労強度を損なわ
ずに耐摩耗性を向上し、またクリープ特性を改善するた
めには、5μm以上、74μm以下が好ましい。その理
由は5μmを下回ると、取扱い性が悪くなり、一方、7
4μmを上回ると、疲労強度が低下する傾向にあるから
である。
The particle size of the hard particles is preferably 5 μm or more and 74 μm or less in order to improve wear resistance without impairing fatigue strength and improve creep characteristics. The reason for this is that if the thickness is less than 5 μm, the handling becomes poor, while
This is because if it exceeds 4 μm, the fatigue strength tends to decrease.

【0018】コンロッド本体3を、硬質粒子を含まない
前記高強度アルミニウム合金より構成する理由は、コン
ロッド本体3は疲労強度が優先して要求されるため硬質
粒子を含まない方が有利であるからである。これに対
し、キャップ5はコンロッド本体3に比べて疲労強度の
要求は少ないが、ボルト締結部の面圧が高く、クリープ
縮みを減少させる必要があるので硬質粒子を含む複合材
より構成する。
The reason why the connecting rod body 3 is made of the above-mentioned high-strength aluminum alloy containing no hard particles is that the connecting rod body 3 is preferentially required to have fatigue strength, and therefore it is advantageous not to contain hard particles. is there. On the other hand, the cap 5 is less required to have fatigue strength than the connecting rod body 3, but the surface pressure of the bolt fastening portion is high and it is necessary to reduce creep shrinkage, so that the cap 5 is made of a composite material containing hard particles.

【0019】次に、キャップ5を構成する複合材の製造
方法およびその複合材についての各種試験結果について
説明する。
Next, a method of manufacturing the composite material forming the cap 5 and various test results of the composite material will be described.

【0020】急冷凝固アルミニウム合金粉末として、S
i 17.2重量%、Cu 2.5重量%、Mg 0.
6重量%、Fe 4.3重量%、Mn 1.8重量%お
よび不可避不純物を含む残部Alよりなる粉末を、アト
マイズ法を適用して、冷却速度103 〜104 ℃/sec
の条件の下に製造する。
As the rapidly solidified aluminum alloy powder, S
i 17.2% by weight, Cu 2.5% by weight, Mg 0.
A powder consisting of 6 wt%, Fe 4.3 wt%, Mn 1.8 wt% and the balance Al containing inevitable impurities was subjected to an atomizing method to cool at a rate of 10 3 to 10 4 ° C / sec.
Manufactured under the conditions of.

【0021】急冷凝固アルミニウム合金粉末に、表1に
示す含有量にて各種硬質粒子を配合し、以下に述べる各
工程を経て複合材(1)〜(12)を製造する。
Various hard particles are added to the rapidly solidified aluminum alloy powder in the amounts shown in Table 1, and composite materials (1) to (12) are manufactured through the following steps.

【0022】即ち、急冷凝固アルミニウム合金粉末と各
硬質粒子とをV型ブレンダにて混合した後、各混合粉末
に冷間静水圧プレス成形法(CIP法)、または金型圧
縮成形法を適用して密度比75%の圧粉体を得る。
That is, after the rapidly solidified aluminum alloy powder and each hard particle are mixed in a V-type blender, a cold isostatic pressing method (CIP method) or a die compression molding method is applied to each mixed powder. To obtain a green compact having a density ratio of 75%.

【0023】冷間静水圧プレス成形法においては、ゴム
製チューブ内に混合粉末を入れ、1.5〜3.0ton /
cm2 程度の静水圧下で成形を行い、金型圧縮成形法にお
いては、金型内に混合粉末を入れて、常温大気中で1.
5〜3.0ton /cm2 程度の圧力下で成形を行う。各圧
粉体を、炉内温度400℃の均熱炉内に設置して4時間
保持し、次いで各圧粉体に熱間押出し加工を施して直径
18mm、長さ450mmの丸棒状に成形された複合材
(1)〜(12)を得る。
In the cold isostatic press molding method, the mixed powder is put in a rubber tube to obtain 1.5 to 3.0 ton /
Molding is carried out under hydrostatic pressure of about cm 2 , and in the mold compression molding method, the mixed powder is put into the mold, and the mixture is allowed to stand at room temperature in air.
Molding is performed under a pressure of about 5 to 3.0 ton / cm 2 . Each green compact is placed in a soaking furnace with a furnace temperature of 400 ° C and held for 4 hours, and then each green compact is subjected to hot extrusion processing to be formed into a round bar shape with a diameter of 18 mm and a length of 450 mm. The composite materials (1) to (12) are obtained.

【0024】この場合の押出し方法は、直接押出し(前
方押出し)、間接押出し(後方押出し)のいずれでもよ
いが、押出し比は5以上を必要とする。押出し比が5以
下では、強度のばらつきが大きくなるので好ましくな
い。
The extrusion method in this case may be either direct extrusion (forward extrusion) or indirect extrusion (rear extrusion), but an extrusion ratio of 5 or more is required. When the extrusion ratio is 5 or less, variations in strength increase, which is not preferable.

【0025】[0025]

【表1】 比較のため、前記と同様の手法により表2に示す比較材
(1)〜(3)を製造する。
[Table 1] For comparison, comparative materials (1) to (3) shown in Table 2 are manufactured by the same method as described above.

【0026】[0026]

【表2】 なお、比較材(1)は、複合材(1)〜(12)におけ
るマトリックスと同一組成であり、また比較材(2)は
鋳造材であるJIS AC8Cに相当し、さらに比較材
(3)は複合材である。
[Table 2] The comparative material (1) has the same composition as the matrix of the composite materials (1) to (12), the comparative material (2) corresponds to JIS AC8C which is a casting material, and the comparative material (3) is It is a composite material.

【0027】表3は、複合材(1)〜(12)および比
較材(1),(2)の熱膨脹係数(×10-6、20〜2
00℃)およびヤング率(200℃、kg/mm2 )を示
す。
Table 3 shows the thermal expansion coefficients (× 10 −6 , 20 to 2) of the composite materials (1) to (12) and the comparative materials (1) and (2).
00 ° C.) and Young's modulus (200 ° C., kg / mm 2 ) are shown.

【0028】[0028]

【表3】 表3から明らかなように、複合材(1)〜(12)は比
較材(1),(2)に比べて、熱膨脹係数が低下し、ま
たヤング率が向上しており、これはマトリックスにAl
2 3 等の硬質粒子が分散していることに起因する。
[Table 3] As is clear from Table 3, the composite materials (1) to (12) have a lower coefficient of thermal expansion and a higher Young's modulus than the comparative materials (1) and (2). Al
This is due to the dispersion of hard particles such as 2 O 3 .

【0029】表4は、複合材(1)〜(12)および比
較材(3)に対して応力腐食割れ試験(JIS H87
11)を行った場合の結果を示す。
Table 4 shows the stress corrosion cracking test (JIS H87) for the composite materials (1) to (12) and the comparative material (3).
The result when 11) is performed is shown.

【0030】応力腐食割れ試験は、縦80mm、横10m
m、厚さ2mmのテストピースを、それに対する負荷応力
をσ0.2 ×0.9(ただし、σ0.2 は、各複合材(1)
〜(12)および比較材(3)の0.2%耐力)とし
て、液温30℃、濃度3.5%のNaCl水溶液中に2
8日間浸漬することにより行われ、耐応力腐食割れ特性
の優劣はテストピースにおけるクラックの発生の有無に
より判断する。
The stress corrosion cracking test is 80 mm long and 10 m wide.
A test piece with a thickness of 2 mm and a load of σ 0.2 × 0.9 (where σ 0.2 is the composite material (1)
~ (12) and the 0.2% proof stress of the comparative material (3)), 2 in a NaCl solution with a liquid temperature of 30 ° C and a concentration of 3.5%.
It is carried out by immersing for 8 days, and the superiority or inferiority of the stress corrosion cracking resistance property is judged by the presence or absence of cracks in the test piece.

【0031】[0031]

【表4】 表4から明らかなように、複合材(1)〜(12)は比
較材(3)に比べて耐応力腐食割れ特性が優れており、
これは主としてMnの含有に起因する。
[Table 4] As is clear from Table 4, the composite materials (1) to (12) are superior in stress corrosion cracking resistance property to the comparative material (3),
This is mainly due to the inclusion of Mn.

【0032】表5は、複合材(2),(5),(8)お
よび比較材(1)に対して摺動摩耗試験を行った場合の
結果を示す。
Table 5 shows the results when a sliding wear test was conducted on the composite materials (2), (5), (8) and the comparative material (1).

【0033】摺動摩耗試験は、縦10mm、横10mm、厚
さ5mmのテストピースを、速度2.5m/sec で回転す
る直径135mmのJIS S50C製円盤に圧力200
kg/cm2 を以て押圧し、また潤滑油を5cc/min の条件
で滴下し、摺動距離18kmに亘って行われたもので、摩
耗量はテストピースにおける試験前後の重量差(g)を
求めることにより測定される。
In the sliding wear test, a test piece having a length of 10 mm, a width of 10 mm and a thickness of 5 mm was applied to a JIS S50C disc having a diameter of 135 mm rotating at a speed of 2.5 m / sec and a pressure of 200.
It was performed over a sliding distance of 18 km by pressing with kg / cm 2 and lubricating oil dropped under the condition of 5 cc / min, and the wear amount is the weight difference (g) before and after the test in the test piece. It is measured by

【0034】[0034]

【表5】 表5から明らかなように、複合材(2),(5),
(8)は比較材(1)に比べて、優れた耐摩耗性を有し
ており、これはマトリックスにAl2 3 、SiC、S
3 4 といった硬質粒子が分散していることに起因す
る。
[Table 5] As is clear from Table 5, composite materials (2), (5),
Compared with the comparative material (1), (8) has excellent wear resistance, which is due to Al 2 O 3 , SiC, S in the matrix.
This is because hard particles such as i 3 N 4 are dispersed.

【0035】表6は、複合材(2),(5),(8)お
よび比較材(1)に対してクリープ試験を行った場合の
結果を示す。
Table 6 shows the results when the creep test was conducted on the composite materials (2), (5), (8) and the comparative material (1).

【0036】クリープ試験は、直径10mm、平行部の長
さ40mmのテストピースに、170℃にて12kg/mm2
の圧縮力を100時間に亘って付与することにより行わ
れ、クリープ縮み量はテストピースの試験前後の長さの
比(%)を求めることによって測定される。
The creep test was carried out on a test piece having a diameter of 10 mm and a parallel portion length of 40 mm at 12 kg / mm 2 at 170 ° C.
Is applied for 100 hours, and the amount of creep shrinkage is measured by determining the ratio (%) of the length of the test piece before and after the test.

【0037】[0037]

【表6】 表6から明らかなように、複合材(2),(5),
(8)は、比較材(1)に比べてクリープ縮み量が減少
しており、これはマトリックスにAl2 3 、SiC、
Si3 4 といった硬質粒子が分散していることにより
マトリックスの結晶の転位が固着されることに起因す
る。
[Table 6] As is clear from Table 6, composite materials (2), (5),
The creep shrinkage of (8) is smaller than that of the comparative material (1). This is because Al 2 O 3 , SiC, and
This is because the dislocations of the crystal of the matrix are fixed due to the dispersion of hard particles such as Si 3 N 4 .

【0038】なお、鋳造材である比較材(2)のクリー
プ縮み量は0.04%であり、複合材(2),(5),
(8)のそれは鋳造材に略匹敵する。
The creep shrinkage of the comparative material (2), which is a cast material, is 0.04%, and the composite materials (2), (5),
That of (8) is almost comparable to cast material.

【0039】表7は、コンロッド1における直径45mm
のクランクピン孔6の寸法変化と温度との関係を示す。
Table 7 shows a diameter of the connecting rod 1 of 45 mm.
The relationship between the dimensional change of the crank pin hole 6 and the temperature is shown.

【0040】実施例コンロッド1は、そのコンロッド本
体3を前記マトリックス材、したがって比較材(1)よ
り構成され、またキャップ5を複合材(3)より構成さ
れている。比較例コンロッド1は、そのコンロッド本体
3およびキャップ5を比較材(1)より構成されてい
る。両コンロッド1において、キャップ5はコンロッド
本体3にボルト4により締結される。
In the connecting rod 1 of the embodiment, the connecting rod body 3 is made of the matrix material, that is, the comparative material (1), and the cap 5 is made of the composite material (3). In the comparative connecting rod 1, the connecting rod body 3 and the cap 5 are made of the comparative material (1). In both connecting rods 1, the cap 5 is fastened to the connecting rod body 3 with bolts 4.

【0041】[0041]

【表7】 表7から明らかなように、複合材(3)より構成される
キャップ5を備えた実施例コンロッド1は、比較材
(1)より構成された比較例コンロッド1に比べて温度
上昇に伴うクランクピン孔6の直径変化量が少なく、こ
れにより機関運転時におけるクランクピンとクランクピ
ン孔6間のクリアランス変化を抑制することができる。
これはマトリックスに10重量%のAl2 3 粒子を分
散させたことによりキャップ5の熱膨脹係数の低下が図
られていることに起因する。
[Table 7] As is clear from Table 7, the example connecting rod 1 provided with the cap 5 made of the composite material (3) has a higher crankshaft temperature than the comparative example connecting rod 1 made of the comparative material (1). The amount of change in the diameter of the hole 6 is small, so that the change in clearance between the crankpin and the crankpin hole 6 during engine operation can be suppressed.
This is because the coefficient of thermal expansion of the cap 5 is lowered by dispersing 10% by weight of Al 2 O 3 particles in the matrix.

【0042】[0042]

【発明の効果】本発明によれば、前記のように特定され
た構成材料を用いることによって、優れた高温強度、耐
摩耗性およびヤング率を有し、また熱膨脹係数の低下を
図ると共に耐応力腐食割れ特性を改善された生産性の良
いコンロッド本体およびキャップを備え、特にキャップ
の高温下におけるクリープ特性を改善した内燃機関用コ
ンロッドを提供することができる。
According to the present invention, by using the constituent materials specified as described above, it has excellent high temperature strength, wear resistance and Young's modulus, and also aims to reduce the coefficient of thermal expansion and stress resistance. It is possible to provide a connecting rod for an internal combustion engine, which includes a connecting rod main body and a cap with improved corrosion cracking characteristics and high productivity, and in particular, has improved creep characteristics of the cap at high temperatures.

【図面の簡単な説明】[Brief description of drawings]

【図1】内燃機関用コンロッドの要部破断正面図であ
る。
FIG. 1 is a fragmentary front view of a connecting rod for an internal combustion engine.

【符号の説明】[Explanation of symbols]

1 コンロッド、 2 桿部、 3 コンロッド本体、 4 ボルト、 5 キャップ 1 connecting rod, 2 rod part, 3 connecting rod body, 4 bolts, 5 cap

───────────────────────────────────────────────────── フロントページの続き (56)参考文献 特開 昭60−121250(JP,A) 特開 昭60−50138(JP,A) 特開 昭61−104043(JP,A) ─────────────────────────────────────────────────── ─── Continuation of front page (56) References JP-A-60-121250 (JP, A) JP-A-60-50138 (JP, A) JP-A-61-104043 (JP, A)

Claims (1)

【特許請求の範囲】[Claims] 【請求項1】 桿部(2)を有するコンロッド本体
(3)と、そのコンロッド本体(3)にボルト(4)に
より締結されるキャップ(5)とを備えた内燃機関用コ
ンロッドにおいて、前記コンロッド本体(3)は、 12.0重量%≦Si≦28.0重量%、 0.8重量%≦Cu≦5.0重量%、 0.3重量%≦Mg≦3.5重量%、 2.0重量%≦Fe≦10.0重量%、 0.5重量%≦Mn≦2.9重量% および不可避不純物を含む残部Alよりなる急冷凝固ア
ルミニウム合金粉末を用いた高強度アルミニウム合金よ
り構成され、前記キャップ(5)は、前記急冷凝固アル
ミニウム合金粉末を用いた高強度アルミニウム合金マト
リックスに、Al 2 3 粒子、SiC粒子、Si3 4
粒子および金属Si粒子から選択される少なくとも一種
の硬質粒子を1.5重量%以上、15.0重量%以下分
散させた複合材より構成されていることを特徴とする内
燃機関用コンロッド。
1. A connecting rod body having a rod portion (2).
(3) and the bolt (4) on the connecting rod body (3)
A cap for internal combustion engine having a cap (5) tightened by
In the connecting rod body, the connecting rod body (3) has: 12.0 wt% ≦ Si ≦ 28.0 wt%, 0.8 wt% ≦ Cu ≦ 5.0 wt%, 0.3 wt% ≦ Mg ≦ 3.5 % By weight, 2.0% by weight ≤ Fe ≤ 10.0% by weight, 0.5% by weight ≤ Mn ≤ 2.9% by weight, and a rapid solidification alloy consisting of the balance Al containing unavoidable impurities.
A high-strength aluminum alloy made of aluminum alloy powder
The cap (5) is made up of
High strength aluminum alloy mat using minium alloy powder
Licks, Al 2O3Particles, SiC particles, Si3NFour
Particles and at least one selected from metallic Si particles
Hard particles of 1.5% by weight or more and 15.0% by weight or less
Characterized by being composed of dispersed composite materials
Connecting rod for fuel engine.
JP3674892A 1986-08-06 1992-02-24 Connecting rod for internal combustion engine Expired - Fee Related JPH079050B2 (en)