[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JPH04335223A - Information recording medium - Google Patents

Information recording medium

Info

Publication number
JPH04335223A
JPH04335223A JP3135524A JP13552491A JPH04335223A JP H04335223 A JPH04335223 A JP H04335223A JP 3135524 A JP3135524 A JP 3135524A JP 13552491 A JP13552491 A JP 13552491A JP H04335223 A JPH04335223 A JP H04335223A
Authority
JP
Japan
Prior art keywords
recording layer
layer
depth
dye
thickness
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Withdrawn
Application number
JP3135524A
Other languages
Japanese (ja)
Inventor
Mitsuru Sawano
充 沢野
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Fujifilm Holdings Corp
Original Assignee
Fuji Photo Film Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Fuji Photo Film Co Ltd filed Critical Fuji Photo Film Co Ltd
Priority to JP3135524A priority Critical patent/JPH04335223A/en
Publication of JPH04335223A publication Critical patent/JPH04335223A/en
Withdrawn legal-status Critical Current

Abstract

PURPOSE:To obtain the recording medium which is high in both of a modulation degree and reflectivity and is excellent in tracking property as well by providing specific relations between the depth of prepits and the film thickness of a recording layer and between the depth of pregrooves and the film thickness of the recording layer. CONSTITUTION:The following relation is provided between the depth of the prepits 8 and the film thickness of the recording layer 2: 0.15lambda<=nsdp- nd tp<=0.24l. The following relation is provided between the depth of the pregrooves and the film thickness of the recording layer 2: 0.02lambda<=nsdg- nd tg<=0.08lambda, where, ns is the refractive index of the substrate 1; nd is the refractive index of the recording layer 2; dp is the depth of the prepits; tp is the difference between the film thickness of the recording layer in the bottom of the prepits and the film thickness in the inter-prepit part; dg is the depth of the pregrooves; tg is the difference between the film thickness of the recording layer in the bottom of the pregrooves and the film thickness in the inter- pregroove part; lambda is the wavelength of a reproducing laser.

Description

【発明の詳細な説明】[Detailed description of the invention]

【0001】0001

【産業上の利用分野】本発明は、光により情報の記録が
可能な情報記録媒体に関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to an information recording medium on which information can be recorded using light.

【0002】0002

【従来の技術】近年において、レーザー光等の高エネル
ギー密度のビームを用いる情報記録媒体が開発され、実
用化されている。この情報記録媒体は光ディスクと称さ
れ、ビデオ・ディスク、オーディオ・ディスク、さらに
は大容量静止画像ファイルおよび大容量コンピュータ用
ディスク・メモリーとして使用されうるものである。こ
れらの情報記録媒体のうちで、音楽等のオーディオ再生
用としてコンパクトディスク(CD)が広く実用化され
ている。
2. Description of the Related Art In recent years, information recording media using high energy density beams such as laser beams have been developed and put into practical use. This information recording medium is called an optical disk, and can be used as a video disk, an audio disk, a large-capacity still image file, and a large-capacity computer disk memory. Among these information recording media, compact discs (CDs) are widely used for audio reproduction of music and the like.

【0003】一般のDRAW(Direct Read
 After Write 、書き込み可能)型の情報
記録媒体は、基本構造としてプラスチック、ガラス等か
らなる円盤状の透明基板と、この上に設けられたBi、
Sn、In、Te等の金属または半金属、あるいはシア
ニン色素等の色素類からなる記録層とを有する。記録媒
体への情報の書き込みは、たとえばレーザービームを記
録媒体に照射することにより行なわれ、記録層の照射部
分がその光を吸収して局所的に温度上昇する結果、ピッ
ト形成等の物理的変化あるいは化学的変化を生じてその
光学的特性を変えることにより情報が記録される。光デ
ィスクからの情報の読み取りもまた、レーザービームを
光ディスクに照射することにより行なわれ、記録層の光
学的特性の変化に応じた反射光または透過光を検出する
ことにより情報が再生される。
General DRAW (Direct Read)
The basic structure of an After Write (writable) type information recording medium is a disc-shaped transparent substrate made of plastic, glass, etc., and a Bi provided on this.
It has a recording layer made of a metal or metalloid such as Sn, In, Te, etc., or a dye such as a cyanine dye. Information is written on a recording medium by, for example, irradiating the recording medium with a laser beam, and the irradiated portion of the recording layer absorbs the light and locally increases in temperature, resulting in physical changes such as pit formation. Alternatively, information can be recorded by causing chemical changes to change its optical properties. Information is also read from an optical disk by irradiating the optical disk with a laser beam, and the information is reproduced by detecting reflected or transmitted light depending on changes in the optical characteristics of the recording layer.

【0004】前記情報再生用の光ディスクであるコンパ
クトディスク(CD)は、一般にCDフォーマット信号
等のEFM(Eight to Fourteen M
odulation)デジタルオーディオ信号情報を有
する孔(ピット)が予め形成されているプラスチックの
円盤状透明基板と、この上に設けられたAl等の反射性
薄膜および保護膜とから構成されている。CDからの情
報の読み取りは、レーザービームを光ディスクに照射す
ることにより行なわれ、ピットの有無による反射率の変
化によってCDフォーマット信号等が読み取られる。こ
のようなCDは、CD規格に基づいて、CDを1.2〜
1.4m/秒の定線速度で回転させて記録することによ
り、信号面内径45mmおよび信号面外径116mmの
範囲内で、トラックピッチ1.6μmにて最大74分の
記録時間を有することが要求されている。従来において
、このようなオーディオ用CDは上記のように予め基板
にピットが形成された再生専用のものである。また最近
では、音楽情報の代わりに、各種文書、静止画像などの
情報が予め記録されたCD−ROM(Read Onl
y Memory)も実用化されている。このような光
ディスクは、当然情報の記録、編集等ができないとの欠
点を有している。従って、DRAW(Direct R
ead After Write 、書き込み可能)型
CDの開発が行なわれており一部実用化されている。
[0004] Compact discs (CDs), which are optical discs for information reproduction, generally contain EFM (Eight to Fourteen M) such as CD format signals.
It is composed of a plastic disc-shaped transparent substrate in which holes (pits) containing digital audio signal information are formed in advance, and a reflective thin film such as Al and a protective film provided thereon. Information from a CD is read by irradiating the optical disc with a laser beam, and CD format signals and the like are read by changes in reflectance depending on the presence or absence of pits. Based on the CD standard, such CDs have a CD rating of 1.2~
By rotating and recording at a constant linear speed of 1.4 m/sec, it is possible to have a maximum recording time of 74 minutes at a track pitch of 1.6 μm within the range of a signal surface inner diameter of 45 mm and a signal surface outer diameter of 116 mm. requested. Conventionally, such audio CDs are play-only CDs with pits formed in advance on the substrate as described above. In addition, recently, instead of music information, CD-ROMs (Read Only) have been pre-recorded with information such as various documents and still images.
y Memory) has also been put into practical use. Such optical discs naturally have the disadvantage that information cannot be recorded or edited. Therefore, DRAW (Direct R
Ead After Write (writable) type CDs are being developed and some have been put into practical use.

【0005】上記DRAW型CDは、記録した情報を市
販のCDプレーヤーで再生できることが要求されている
。CDプレーヤーで再生を行なうためには、光ディスク
に高い反射率を有することが必要であることから、高反
射率の光ディスクが望まれる。前記色素記録層も金属記
録層も、反射率は一般に30〜40%程度と低いため、
塗布により容易に記録層を形成することができる色素の
方が金属に比べて製造上の利点を有する。従って、基板
上に色素記録層および反射層が積層されたDRAW型C
Dが検討されている。このようなDRAW型CDの例と
して、ポリカーボネート基板上に色素記録層、Auの反
射層および保護層がこの順で積層された構造の光ディス
クが日経エレクトロニクス(107頁、1989年 1
月23日発行)に記載されている。
[0005] The DRAW type CD is required to be able to play recorded information on a commercially available CD player. Since it is necessary for an optical disc to have a high reflectance in order to play it on a CD player, an optical disc with a high reflectance is desired. Since the reflectance of both the dye recording layer and the metal recording layer is generally as low as about 30 to 40%,
Dyes that can be easily coated to form a recording layer have manufacturing advantages over metals. Therefore, DRAW type C in which a dye recording layer and a reflective layer are laminated on a substrate.
D is being considered. As an example of such a DRAW type CD, an optical disc having a structure in which a dye recording layer, an Au reflective layer, and a protective layer are laminated in this order on a polycarbonate substrate is published by Nikkei Electronics (p. 107, 1989, 1).
published on the 23rd of May).

【0006】このようなDRAW型CDは(従来のDR
AW型光ディスクもそうであるが)、一般に、基板の内
周側に番地情報などの記録情報としてのピットが形成さ
れたプリピット領域とプリピット領域より外周側には情
報を記録するためのレーザーを案内するプリグルーブが
基板上に設けられたプリグルーブ領域(記録領域)を有
する。また、最近では、再生用CDとDRAW型CDの
両方の機能を一枚のディスクで持つような光ディスクが
提案されている(特開平2−42652号公報)。すな
わち、再生用CDの外周側に上記基板上にプリグルーブ
を有する記録可能領域を設け、内周側に音楽等の情報が
入ったROM領域、すなわち再生専用領域、を有する光
ディスクである。これにより、他の人と同じ情報(音楽
やプログラム)を共有しながら且つ同じディスクに使用
者がデーターやメモを記録することが可能となる。
[0006] Such a DRAW type CD (conventional DR
(The same is true for AW type optical discs), generally there is a pre-pit area where pits are formed for recording information such as address information on the inner circumference side of the substrate, and a laser for recording information is guided on the outer circumference side of the pre-pit area. A pregroove for recording has a pregroove area (recording area) provided on the substrate. Furthermore, recently, an optical disc has been proposed that has the functions of both a playback CD and a DRAW type CD in a single disc (Japanese Patent Laid-Open No. 2-42652). That is, it is an optical disc having a recordable area having a pregroove on the substrate on the outer circumference side of a CD for reproduction, and a ROM area containing information such as music, that is, a reproduction-only area on the inner circumference side. This allows the user to record data and memos on the same disc while sharing the same information (music and programs) with other people.

【0007】このようなROM領域と記録可能領域を有
する光ディスクの作成方法は、上記特開平2−4265
2号公報によれば、基板の再生専用領域(ROM領域)
より外周側に当たる、基板の直径80〜117mmの範
囲のグルーブ上に色素塗布液を塗布して色素記録層を形
成している。そして再生専用領域と記録層上に反射層を
形成している。すなわち、プリピットからなる再生専用
領域領域には記録層を形成せず、プリグルーブ領域にの
み記録層を設けている。このような記録層の形成は、記
録層用の色素塗布液を再生専用領域に塗布することによ
り行なわれるが、再生専用領域まで塗布すると、プリピ
ットが塗布液により埋められるため、プリピットの実質
的な深さが予定の深さより浅くなって変調度が低下し、
再生信号を殆ど読むことができなくなる。従って、上記
のように色素記録層をプリグルーブ領域にのみに設ける
ようにされている。
A method for creating an optical disc having such a ROM area and a recordable area is disclosed in the above-mentioned Japanese Patent Application Laid-Open No. 2-4265.
According to Publication No. 2, the read-only area (ROM area) of the board
A dye recording layer is formed by coating a dye coating liquid on a groove having a diameter of 80 to 117 mm on the substrate, which is closer to the outer circumferential side. A reflective layer is formed on the read-only area and the recording layer. That is, a recording layer is not formed in the read-only area consisting of pre-pits, but a recording layer is provided only in the pre-groove area. Formation of such a recording layer is carried out by applying a dye coating liquid for the recording layer to the read-only area. However, if the dye coating liquid for the recording layer is applied to the read-only area, the pre-pits are filled with the coating liquid, so the actual pre-pits are The depth becomes shallower than the planned depth and the modulation degree decreases,
It becomes almost impossible to read the reproduced signal. Therefore, as described above, the dye recording layer is provided only in the pregroove area.

【0008】しかしながら、上記特開平2−42652
号公報に記載されているような、再生専用領域に色素記
録層を設けず、記録可能領域にのみ色素記録層を設けた
情報記録媒体においては、色素記録層が設けられた部分
と色素記録層が設けられていない部分との境界部で、そ
の境界を再現性よく形成することはが困難である。ある
いは、境界部に当たる色素記録層の端部で、膜厚が不均
一となり易いとの問題、また円環状に形成される色素記
録層の偏心が生じ易いとの問題がある。このため、再生
時に、この境界部でフォーカシングが外れるとのエラー
が発生し易い。さらに、実際上、再生専用領域とその外
周側の記録可能領域との二つの領域に分かれた情報記録
媒体。しか製造することができない。すなわち、再生専
用領域の内周側にプリグルーブの記録可能領域を設けた
り、再生専用領域と記録可能領域とを混在させて設けた
りすることが困難である。また、再生専用領域にアプリ
ケーションソフトを予め記録しておくことや、そのソフ
トの利用方法などが制限される。
However, the above-mentioned Japanese Patent Application Laid-Open No. 2-42652
In an information recording medium that does not provide a dye recording layer in the read-only area and only provides a dye recording layer in the recordable area, as described in the publication, the portion where the dye recording layer is provided and the dye recording layer It is difficult to form a boundary with good reproducibility at a boundary with a portion where no Alternatively, there is a problem that the film thickness tends to become non-uniform at the end portion of the dye recording layer corresponding to the boundary portion, and a problem that eccentricity of the dye recording layer formed in an annular shape tends to occur. Therefore, during playback, errors such as loss of focus at this boundary are likely to occur. Furthermore, the information recording medium is actually divided into two areas: a read-only area and a recordable area on the outer circumference side. can only be manufactured. That is, it is difficult to provide a pregroove recordable area on the inner circumferential side of the read-only area or to provide a mix of the read-only area and the recordable area. Furthermore, there are restrictions on pre-recording application software in the reproduction-only area and on how to use the software.

【0009】[0009]

【発明が解決しようとする課題】本出願人は、上記問題
を解決するため、プリピットからなる再生専用領域およ
びプリグルーブからなる記録可能領域の全域に色素記録
層を形成して、上記欠点のない情報記録媒体を既に出願
している。特願平2−264786号には、プリピット
(およびプリグルーブ)が塗布液により埋められること
を考慮して、基板に形成されるプリピットの深さを予め
深く作成して再生信号が小さくならないように設計した
基板を用いることが記載されている。また、特願平2−
191257号には、プリピット(およびプリグルーブ
)が塗布液により埋められることがないように色素塗布
液を塗布できる、改良された塗布方法が記載されている
[Problems to be Solved by the Invention] In order to solve the above-mentioned problems, the present applicant formed a dye recording layer over the entire read-only area consisting of pre-pits and the recordable area consisting of pre-grooves, thereby eliminating the above-mentioned drawbacks. An application has already been filed for information recording media. Japanese Patent Application No. 2-264786 discloses that in consideration of the fact that pre-pits (and pre-grooves) are filled with a coating liquid, the pre-pits formed on the substrate are made deep in advance so that the reproduced signal does not become small. It is described that a designed board is used. In addition, the patent application Hei 2-
No. 191,257 describes an improved coating method that allows the dye coating solution to be applied so that the pre-pits (and pre-grooves) are not filled with the coating solution.

【0010】色素記録層の形成方法として、上記特願平
2−191257号の方法に従えば、プリピットの底部
の膜厚と間部の膜厚を、あるいはプリグルーブの底部の
膜厚と間部の膜厚を、ほぼ均一に形成することができる
。勿論、従来の方法では均一に膜を形成することは出来
ない。上記形成方法を利用しても、プリピットおよびプ
リグルーブの形状(特に深さ)は同じでないため、色素
層のプリピットおよびプリグルーブへの埋まり方は一様
でない場合が多い。従って、それぞれの色素層の埋まり
方を考慮してプリグルーブとプリピットの深さを決定す
ることが必要があるが、このような決定方法は知られて
いない。このため、実験的に、深さが異なったプリピッ
トおよびプリグルーブを、且つ深さを種々の組み合わせ
で形成して基板を作成し、これに色素層形成を繰り返す
ことによって好ましい基板を選択する必要がある。また
色素を変更した場合、膜の均一形成のためその色素に合
った溶剤組成を調製しなければならないとの問題がある
。一方、特願平2−264786号の基板に形成される
プリピットの深さを予め深く作成しておく方法でも、や
はり色素塗布液が変更した場合、その埋まり方、膜厚の
均一性が異なるため実験が必要であり、また上記のよう
にプリピット(およびプリグルーブ)の深さにより埋ま
る程度が異なるとの問題もある。
As a method for forming the dye recording layer, according to the method disclosed in Japanese Patent Application No. 2-191257, the film thickness at the bottom of the pre-pits and the film thickness at the space between the pre-pits, or the film thickness at the bottom of the pre-groove and the film thickness at the space between the pre-pits is adjusted. It is possible to form a film with a substantially uniform thickness. Of course, it is not possible to form a uniform film using conventional methods. Even if the above formation method is used, the shapes (particularly the depths) of the pre-pits and pre-grooves are not the same, so the way the pigment layer is filled into the pre-pits and pre-grooves is often uneven. Therefore, it is necessary to determine the depths of pre-grooves and pre-pits in consideration of how each dye layer is filled, but such a determining method is not known. Therefore, it is necessary to experimentally create a substrate by forming pre-pits and pre-grooves with different depths and in various combinations of depths, and then select a preferable substrate by repeating the formation of a dye layer on this. be. Furthermore, when the dye is changed, there is a problem in that a solvent composition suitable for the dye must be prepared in order to form a uniform film. On the other hand, even with the method of preparing the pre-pits to be formed on the substrate deep in advance as described in Japanese Patent Application No. 2-264786, if the dye coating liquid is changed, the filling method and the uniformity of the film thickness will differ. Experiments are required, and as mentioned above, there is also the problem that the degree of filling varies depending on the depth of the pre-pits (and pre-grooves).

【0011】従って、本発明は、再生専用領域と記録可
能領域とを有し、両方の領域で高い変調度の再生信号を
得ることができ且つトラッキング特性にも優れた情報記
録媒体を提供することを目的とする。また、本発明は、
簡易に製造することができる再生専用領域と記録可能領
域とを有する情報記録媒体を提供することを目的とする
Therefore, it is an object of the present invention to provide an information recording medium that has a read-only area and a recordable area, can obtain a reproduced signal with a high degree of modulation in both areas, and has excellent tracking characteristics. With the goal. Moreover, the present invention
It is an object of the present invention to provide an information recording medium having a read-only area and a recordable area that can be easily manufactured.

【0012】0012

【課題を解決するための手段】前記目的は、表面に、プ
リピットからなる再生専用領域とプリグルーブからなる
記録可能領域とが設けられた円盤状基板の上に、レーザ
ーによる情報の記録が可能な記録層および反射層が、こ
の順で設けられた情報記録媒体において、該プリピット
の深さと該記録層の膜厚との関係が下記式(I):  
    0.15λ≦ns dp −nd Δtp ≦
0.24λ      (I)を満足し、且つ 該プリグルーブの深さと該記録層の膜厚との関係が下記
式(II):       0.02λ≦ns dg −nd Δtg
 ≦0.08λ      (II)[但し、ns は
基板の屈折率を表わし、nd は記録層の屈折率を表わ
し、dp はプリピットの深さ(nm)を表わし、Δt
p はプリピット底部の記録層の膜厚とプリピット間部
の記録層の膜厚との差(nm)を表わし、dg はプリ
グルーブの深さ(nm)を表わし、Δtg はプリグル
ーブ底部の記録層の膜厚とプリグルーブ間部の記録層の
膜厚との差(nm)を表わし、そしてλは再生時に使用
するレーザーの波長を表わす。]を満足することを特徴
とする情報記録媒体により達成することができる。
[Means for Solving the Problems] The object is to provide a disc-shaped substrate having a read-only area consisting of pre-pits and a recordable area consisting of pre-grooves on its surface, on which information can be recorded by laser. In an information recording medium in which a recording layer and a reflective layer are provided in this order, the relationship between the depth of the pre-pits and the thickness of the recording layer is expressed by the following formula (I):
0.15λ≦ns dp −nd Δtp ≦
0.24λ (I), and the relationship between the depth of the pregroove and the thickness of the recording layer is expressed by the following formula (II): 0.02λ≦ns dg −nd Δtg
≦0.08λ (II) [However, ns represents the refractive index of the substrate, nd represents the refractive index of the recording layer, dp represents the depth of prepits (nm), and Δt
p represents the difference (nm) between the thickness of the recording layer at the bottom of the pre-pits and the thickness of the recording layer between the pre-pits, dg represents the depth of the pre-groove (nm), and Δtg represents the thickness of the recording layer at the bottom of the pre-groove. represents the difference (nm) between the film thickness of the recording layer and the film thickness of the recording layer between the pregrooves, and λ represents the wavelength of the laser used during reproduction. This can be achieved by an information recording medium that satisfies the following.

【0013】上記本発明の情報記録媒体の好ましい態様
は以下の通りである。
Preferred embodiments of the information recording medium of the present invention are as follows.

【0014】1)該記録層が、色素からなる層であるこ
とを特徴とする上記情報記録媒体。
1) The above-mentioned information recording medium, wherein the recording layer is a layer made of a dye.

【0015】2)該式(I)が下記式 (III): 
     0.17λ≦ns dp −nd Δtp 
≦0.22λ       (III)[但し、ns 
、nd 、dp 、Δtp およびλは、上記定義と同
じ意味を表わす]を満足する特徴とする上記情報記録媒
体。
2) The formula (I) is the following formula (III):
0.17λ≦ns dp −nd Δtp
≦0.22λ (III) [However, ns
, nd, dp, Δtp and λ have the same meanings as defined above].

【0016】3)該式(II)が下記式(IV):  
    0.03λ≦ns dg −nd Δtg ≦
0.06λ      (IV)[但し、ns 、nd
 、dg 、Δtg およびλは、上記定義と同じ意味
を表わす]を満足する特徴とする上記情報記録媒体。
3) The formula (II) is the following formula (IV):
0.03λ≦ns dg −nd Δtg ≦
0.06λ (IV) [However, ns, nd
, dg, Δtg and λ have the same meanings as defined above].

【0017】4)上記dp が、80〜300nmの範
囲にあることを特徴とする上記情報記録媒体。
4) The above information recording medium, wherein the dp is in the range of 80 to 300 nm.

【0018】5)上記dg が、10〜230nmの範
囲にあることを特徴とする上記情報記録媒体。
5) The above-mentioned information recording medium, wherein the above-mentioned dg is in a range of 10 to 230 nm.

【0019】6)上記Δtp が、0〜120nmの範
囲にあることを特徴とする上記情報記録媒体。
6) The above-mentioned information recording medium, wherein the above-mentioned Δtp is in a range of 0 to 120 nm.

【0020】7)上記Δtg が、0〜110nmの範
囲にあることを特徴とする上記情報記録媒体。
7) The above-mentioned information recording medium, wherein the above-mentioned Δtg is in a range of 0 to 110 nm.

【0021】8)該記録層が、金属および/または金属
化合物からなる相変化型の記録層であることを特徴とす
る上記情報記録媒体。
8) The information recording medium described above, wherein the recording layer is a phase change type recording layer made of a metal and/or a metal compound.

【0022】9)上記反射層の上に、さらに保護層が形
成されていることを特徴とする上記情報記録媒体。
9) The information recording medium described above, further comprising a protective layer formed on the reflective layer.

【0023】10)上記再生専用領域の情報が、CDフ
ォーマットのEFM信号であることを特徴とする情報記
録媒体。
10) An information recording medium characterized in that the information in the read-only area is an EFM signal in CD format.

【0024】[0024]

【発明の効果】上記のようにプリピットの深さと記録層
の膜厚が上記式(I)を満足し、且つプリグルーブの深
さと記録層の膜厚が上記式(II)を満足するように作
成された再生専用領域と記録可能領域とを有する情報記
録媒体は、両方の領域で再生信号の変調度が高く、且つ
トラッキング特性にも優れたものである。すなわち、上
記本発明よれば、例えば、新しい基板を使用する場合は
、既に作成された基板のプリピットおよびプリグルーブ
の深さを測定することにより、プリピットおよびプリグ
ルーブ底部での記録層の膜厚を上記式を満足するように
塗布形成すれば、上記特性の優れた情報記録媒体を容易
に製造することができる。また、例えば色素塗布液を変
える場合は、プリピットおよびプリグルーブの寸法が既
知の基板に色素塗布液を塗布、成膜し、色素記録層のプ
リピットおよびプリグルーブへの埋まり方、すなわち各
部の膜厚を測定し、次に上記式を満足するようにプリピ
ットおよびプリグルーブの深さを有する基板を作成し、
その基板に色素記録層を形成することにより上記情報記
録媒体を容易に製造することができる。また、相変化型
の金属記録層の場合も、それ自体では反射率が低く、高
反射率を得るには記録層の上に反射層を設けることが必
要であることから、プリピットからなる再生専用領域と
プリグルーブからなる記録可能領域とを有する光ディス
クとした場合、本発明のプリピット、プリグルーブおよ
び記録層の膜厚の関係を利用した媒体とすることにより
、容易に高い変調度の再生信号を得ることができ且つト
ラッキング特性にも優れた情報記録媒体を容易に得るこ
とができる。
[Effects of the Invention] As described above, the depth of the pre-pit and the thickness of the recording layer satisfy the above formula (I), and the depth of the pre-groove and the thickness of the recording layer satisfy the formula (II) above. The created information recording medium having a read-only area and a recordable area has a high degree of modulation of a reproduced signal in both areas, and also has excellent tracking characteristics. That is, according to the present invention, for example, when using a new substrate, the thickness of the recording layer at the bottom of the pre-pits and pre-grooves can be determined by measuring the depth of the pre-pits and pre-grooves of the already created substrate. By coating and forming in a manner that satisfies the above formula, it is possible to easily manufacture an information recording medium having excellent properties as described above. In addition, for example, when changing the dye coating liquid, the dye coating liquid is applied to a substrate with known pre-pit and pre-groove dimensions, and a film is formed. Then, create a substrate with pre-pit and pre-groove depths that satisfy the above formula,
The above information recording medium can be easily manufactured by forming a dye recording layer on the substrate. In addition, in the case of a phase-change metal recording layer, the reflectance itself is low, and in order to obtain a high reflectance it is necessary to provide a reflective layer on top of the recording layer. In the case of an optical disc having a recordable area consisting of a region and a pregroove, it is possible to easily reproduce a reproduced signal with a high degree of modulation by using the relationship between the film thickness of the prepit, pregroove, and recording layer of the present invention. It is possible to easily obtain an information recording medium with excellent tracking characteristics.

【0025】[発明の詳細な記述]本発明の情報記録媒
体は、円盤状基板の上に色素からなる記録層および反射
層が、この順で形成された基本構造を有する。
[Detailed Description of the Invention] The information recording medium of the present invention has a basic structure in which a recording layer made of a dye and a reflective layer are formed in this order on a disk-shaped substrate.

【0026】添付図面を参照しながら本発明の情報記録
媒体の構成について説明する。図1は、本発明の情報記
録媒体の一例を示す半断面斜視図である。図1で示され
る情報記録媒体は、円盤状基板1、基板上に設けられた
記録層2、記録層上に設けられた反射層3、そして反射
層上に設けられた保護層4からなる構成を有している。 上記情報記録媒体は、内周側基板上に記録信号としてプ
リピットが設けられた再生専用領域5、そして外周側基
板上にプリレグルーブが形成された情報の記録が可能な
記録可能領域6が設けられている。再生専用領域と記録
可能領域はそれぞれ二つ以上設けられても良く、例えば
、再生専用領域5の内周側に記録可能領域が設けられて
も、記録可能領域6の外側に再生専用領域が設けられて
も良い。なお、一般に基板の内周縁近傍および外周縁近
傍は、ピットやグルーブが形成されていないプレーンな
面である(図示せず)。
The structure of the information recording medium of the present invention will be explained with reference to the accompanying drawings. FIG. 1 is a half-sectional perspective view showing an example of the information recording medium of the present invention. The information recording medium shown in FIG. 1 includes a disc-shaped substrate 1, a recording layer 2 provided on the substrate, a reflective layer 3 provided on the recording layer, and a protective layer 4 provided on the reflective layer. have. The above-mentioned information recording medium has a read-only area 5 in which prepits are provided as recording signals on the inner substrate, and a recordable area 6 in which information can be recorded in which pre-reg grooves are formed on the outer substrate. There is. Two or more read-only areas and two or more recordable areas may be provided. For example, even if a recordable area is provided on the inner circumferential side of the read-only area 5, a read-only area may be provided outside the recordable area 6. It's okay to be beaten. Note that, in general, the vicinity of the inner peripheral edge and the vicinity of the outer peripheral edge of the substrate are plain surfaces on which pits and grooves are not formed (not shown).

【0027】図2は、上記図1の再生専用領域と記録可
能領域との境界部近傍の部分拡大断面図である。円盤状
基板1の表面は、情報が記録されたプリピット8からな
る再生専用領域5、および記録(または再生)用のレー
ザーを案内するプリグルーブ9からなる記録可能領域6
から成っている。色素記録層2は、再生専用領域5およ
び記録可能領域6の全面に形成されている。色素記録層
を全て覆うように反射層3が設けられ、そして反射層上
に保護層4が形成されている。
FIG. 2 is a partially enlarged sectional view of the vicinity of the boundary between the read-only area and the recordable area in FIG. The surface of the disc-shaped substrate 1 includes a read-only area 5 consisting of pre-pits 8 on which information is recorded, and a recordable area 6 consisting of pre-grooves 9 for guiding a laser for recording (or reproduction).
It consists of The dye recording layer 2 is formed on the entire surface of the read-only area 5 and the recordable area 6. A reflective layer 3 is provided to completely cover the dye recording layer, and a protective layer 4 is formed on the reflective layer.

【0028】次に、本発明のプリピットの深さと記録層
の膜厚との関係、およびプリグルーブの深さと記録層の
膜厚との関係について説明する。
Next, the relationship between the depth of the pre-pit and the thickness of the recording layer and the relationship between the depth of the pre-groove and the thickness of the recording layer according to the present invention will be explained.

【0029】図3は、本発明のプリピットの深さと記録
層の膜厚の関係を示すプリピットの半径方向の断面図で
ある。円盤状基板1の表面にプリピット8(再生専用領
域5内)が形成され、そしてその表面に記録層2が、プ
リピットの形状に沿うように形成されている。記録層上
には反射層および保護層が設けられているがここでは図
示しない。dp は、プリピットの深さ(nm)であり
、tp は記録層のプリピット底部における膜厚(nm
)であり、そしてtbpはプリピット間部における膜厚
(nm)である。そして、記録層のプリピット底部にお
ける膜厚tp とプリピット間部における膜厚tbpと
の差が、下記式(I)中のΔtp (=tp −tbp
)に当たる。
FIG. 3 is a radial cross-sectional view of the prepits showing the relationship between the depth of the prepits and the thickness of the recording layer according to the present invention. Pre-pits 8 (within the read-only area 5) are formed on the surface of the disc-shaped substrate 1, and a recording layer 2 is formed on the surface so as to follow the shape of the pre-pits. A reflective layer and a protective layer are provided on the recording layer, but are not shown here. dp is the depth (nm) of the prepit, and tp is the film thickness (nm) at the bottom of the prepit of the recording layer.
), and tbp is the film thickness (nm) between prepits. Then, the difference between the film thickness tp at the bottom of the prepits of the recording layer and the film thickness tbp between the prepits is expressed as Δtp (=tp −tbp
).

【0030】本発明では、上記プリピットの深さと記録
層(好ましくは色素記録層)の膜厚の関係が下記式(I
)を満足する。       0.15λ≦ns dp −nd Δtp
 ≦0.24λ      (I)ns は基板1の屈
折率を表わし、nd は記録層の屈折率を表わしそして
λは再生時に使用するレーザーの波長を表わす。プリピ
ット部においては反射率が0の場合が信号の強度が大き
く好ましく、一般にそれには位相差を1/4λにすれば
良い。しかしながら、この位相差によってトラッキング
を制御するためのプッシュプル信号も生成しなくてはな
らず、この信号は同一ディスク内にあるプリグルーブの
信号強度とほぼ等しいことが必要である。このため、本
発明者等が検討を重ねたところ位相差{上記の(ns 
dp−nd Δtp )に当たる}が上記(I)式の範
囲にあることが、プリピット領域で高い変調度の信号が
得られ、且つトラッキングも良好となることが明らかに
なった。
In the present invention, the relationship between the depth of the prepits and the thickness of the recording layer (preferably the dye recording layer) is expressed by the following formula (I
) is satisfied. 0.15λ≦ns dp −nd Δtp
≦0.24λ (I)ns represents the refractive index of the substrate 1, nd represents the refractive index of the recording layer, and λ represents the wavelength of the laser used during reproduction. In the prepit portion, it is preferable that the reflectance is 0 because the signal strength is large, and generally the phase difference may be set to 1/4λ. However, it is also necessary to generate a push-pull signal for controlling tracking based on this phase difference, and this signal needs to be approximately equal to the signal strength of the pregroove within the same disc. For this reason, the inventors of the present invention have repeatedly studied and found that the phase difference {the above (ns
dp-nd Δtp ) is within the range of the above formula (I), it has become clear that a signal with a high modulation degree can be obtained in the pre-pit region and tracking can also be good.

【0031】図4は、本発明のプリグルーブの深さと記
録層の膜厚との関係を示すプリグルーブの半径方向の断
面図である。円盤状基板1の表面にプリグルーブ9(記
録可能領域6内)が形成され、そしてその表面に記録層
2がプリグルーブの形状に沿うように形成されている。 記録層上には反射層および保護層が設けられているがこ
こでは図示しない。dg は、プリグルーブの深さ(n
m)であり、tg は記録層のプリグルーブ底部におけ
る膜厚(nm)であり、そしてtbgはプリグルーブ間
部(ランド部)における膜厚(nm)である。そして記
録層のプリグルーブ底部における膜厚tgとプリグルー
ブ間部における膜厚tbgとの差が下記式(I)中のΔ
tg (=tg−tbg)に当たる。
FIG. 4 is a radial cross-sectional view of the pregroove of the present invention showing the relationship between the depth of the pregroove and the thickness of the recording layer. A pregroove 9 (inside the recordable area 6) is formed on the surface of the disc-shaped substrate 1, and a recording layer 2 is formed on the surface so as to follow the shape of the pregroove. A reflective layer and a protective layer are provided on the recording layer, but are not shown here. dg is the pregroove depth (n
m), tg is the film thickness (nm) at the bottom of the pregroove of the recording layer, and tbg is the film thickness (nm) at the part between the pregrooves (land part). Then, the difference between the film thickness tg at the bottom of the pregroove of the recording layer and the film thickness tbg between the pregrooves is expressed as Δ in the following formula (I).
This corresponds to tg (=tg-tbg).

【0032】本発明では、上記プリグルーブの深さと記
録層(好ましくは色素記録層)の膜厚の関係が下記式(
II)を満足する。       0.02λ≦ns dg −nd Δtg
 ≦0.08λ      (II)ns は基板1の
屈折率を表わし、nd は記録層の屈折率を表わしそし
てλは再生時に使用するレーザーの波長を表わす。プリ
グルーブ部においては、未記録状態では反射率が高い(
例えばCDのように)ことが好ましく、それには位相差
を0すれば良い。しかしながら、この位相差によってト
ラッキングを制御するためのプッシュプル信号も生成し
なくてはならず、この信号は同一ディスク内にあるプリ
ピットの信号強度とほぼ等しいことが必要である。この
ため、本発明者等が検討を重ねたところ、位相差{上記
の(ns dp −nd Δtp )に当たる}が上記
(II)式の範囲にあることが、プリグルーブの領域で
高い反射率の信号が得られ、且つトラッキングも良好と
なることが明らかになった。
In the present invention, the relationship between the depth of the pregroove and the thickness of the recording layer (preferably the dye recording layer) is expressed by the following formula (
II) is satisfied. 0.02λ≦ns dg −nd Δtg
≦0.08λ (II) ns represents the refractive index of the substrate 1, nd represents the refractive index of the recording layer, and λ represents the wavelength of the laser used during reproduction. In the pre-groove area, the reflectance is high in the unrecorded state (
For example, a CD) is preferable, and the phase difference may be set to 0 for that purpose. However, it is also necessary to generate a push-pull signal for controlling tracking based on this phase difference, and this signal needs to be approximately equal in signal strength to the signal intensity of prepits in the same disk. Therefore, after repeated studies by the present inventors, the fact that the phase difference {which corresponds to (ns dp - nd Δtp ) above} is within the range of formula (II) above is the reason for the high reflectance in the pregroove region. It became clear that a signal could be obtained and tracking was also good.

【0033】上記式(I)はさらに下記式 (III)
:      0.17λ≦ns dp −nd Δt
p ≦0.22λ       (III)[但し、n
s 、nd 、dp 、Δtp およびλは、上記定義
と同じ意味を表わす]を満足することが好ましく、上記
式(II)はさらに下記式(IV):      0.
03λ≦ns dg −nd Δtg ≦0.06λ 
     (IV)[但し、ns 、nd 、dg 、
Δtg およびλは、上記定義と同じ意味を表わす]を
満足することが好ましい。
The above formula (I) is further transformed into the following formula (III)
: 0.17λ≦ns dp −nd Δt
p ≦0.22λ (III) [However, n
s , nd , dp , Δtp and λ have the same meanings as defined above], and the above formula (II) preferably satisfies the following formula (IV): 0.
03λ≦ns dg −nd Δtg ≦0.06λ
(IV) [However, ns, nd, dg,
Δtg and λ have the same meanings as defined above].

【0034】また、上記dp (プリピット底部の深さ
)は、80〜300nmの範囲にあることが好ましく、
上記dg (プリグルーブ底部の深さ)は、10〜23
0nmの範囲にあることが好ましい。さらに上記Δtp
 (プリピット底部とプリピット間部とにおける膜厚)
の差は、0〜120nmの範囲にあることが好ましく、
上記Δtg (プリグルーブ底部とプリグルーブ間部と
における膜厚)が、0〜110nmの範囲にあることが
好ましい。ns (基板の屈折率)はプラスチック基板
の場合は一般に1,4〜1.7にあり、例えばポリカー
ボネート基板の場合は1.58である。、nd (色素
記録層の屈折率)は一般に1.4〜4.0にあり、例え
ばインドレニン系シアニン色素の場合は2.0〜3.5
にある。
[0034] Furthermore, the above dp (depth of the bottom of the pre-pit) is preferably in the range of 80 to 300 nm,
The above dg (depth of the bottom of the pregroove) is 10 to 23
It is preferably in the range of 0 nm. Furthermore, the above Δtp
(Film thickness at the bottom of the pre-pits and between the pre-pits)
The difference is preferably in the range of 0 to 120 nm,
The above Δtg (film thickness at the bottom of the pregroove and the area between the pregrooves) is preferably in the range of 0 to 110 nm. ns (refractive index of the substrate) is generally between 1.4 and 1.7 for plastic substrates, for example 1.58 for polycarbonate substrates. , nd (refractive index of the dye recording layer) is generally between 1.4 and 4.0, for example, in the case of indolenine cyanine dyes, it is between 2.0 and 3.5.
It is in.

【0035】本発明の情報記録媒体の作成は、例えば、
ある寸法のプリピットおよびプリグルーブを有する基板
に色素記録層を塗布、成膜し、色素記録層のプリピット
およびプリグルーブへの埋まり方、すなわち各部の膜厚
を測定し、次に上記式を満足するようにプリピットおよ
びプリグルーブの深さを有する基板を作成し、それから
製造を行なう。あるいは、既に作成された基板のプリピ
ットおよびプリグルーブの深さを測定することにより、
プリピットおよびプリグルーブ底部での膜厚を上記式を
満足するように塗布方法を変えて形成し、塗布方法の確
立後、製造を行えば良い。
[0035] The information recording medium of the present invention can be created by, for example,
A dye recording layer is coated and formed on a substrate having pre-pits and pre-grooves of a certain size, and the way the dye recording layer is filled into the pre-pits and pre-grooves, that is, the film thickness at each part, is measured, and then the above formula is satisfied. A substrate having pre-pit and pre-groove depths as described above is prepared, and then manufacturing is performed. Alternatively, by measuring the depth of pre-pits and pre-grooves in already created substrates,
The coating method may be changed so that the film thickness at the bottom of the pre-pits and pre-grooves satisfies the above formula, and after the coating method is established, manufacturing may be performed.

【0036】本発明の情報記録媒体は、たとえば以下に
述べるような方法により製造することができる。
The information recording medium of the present invention can be manufactured, for example, by the method described below.

【0037】本発明の円盤状基板は、従来の情報記録媒
体の基板として用いられている各種の材料から任意に選
択することができる。本発明の基板材料として、例えば
ガラス;ポリカーボネート;ポリメチルメタクリレート
等のアクリル樹脂;ポリ塩化ビニル、塩化ビニル共重合
体等の塩化ビニル系樹脂;エポキシ樹脂;アモルファス
ポリオレフィンおよびポリエステルなどを挙げることが
でき、所望により併用してもよい。なお、これらの材料
はフィルム状としてまたは剛性のある基板として使うこ
とができる。上記材料の中で、耐湿性、寸法安定性およ
び価格などの点からポリカーボネートが好ましい。
The disc-shaped substrate of the present invention can be arbitrarily selected from various materials used as substrates of conventional information recording media. Examples of the substrate material of the present invention include glass; polycarbonate; acrylic resin such as polymethyl methacrylate; vinyl chloride resin such as polyvinyl chloride and vinyl chloride copolymer; epoxy resin; amorphous polyolefin and polyester. They may be used together if desired. Note that these materials can be used in the form of a film or as a rigid substrate. Among the above materials, polycarbonate is preferred in terms of moisture resistance, dimensional stability, cost, and the like.

【0038】記録層が設けられる側の基板表面には、平
面性の改善、接着力の向上、感度の向上および記録層の
変質の防止の目的で、下塗層が設けられてもよい。下塗
層の材料としてはたとえば、ポリメチルメタクリレート
、アクリル酸・メタクリル酸共重合体、スチレン・無水
マレイナト共重合体、ポリビニルアルコール、N−メチ
ロールアクリルアミド、スチレン・ビニルトルエン共重
合体、クロルスルホン化ポリエチレン、ニトロセルロー
ス、ポリ塩化ビニル、塩素化ポリオレフィン、ポリエス
テル、ポリイミド、酢酸ビニル・塩化ビニル共重合体、
エチレン・酢酸ビニル共重合体、ポリエチレン、ポリプ
ロピレン、ポリカーボネート等の高分子物質;およびシ
ランカップリング剤などの有機物質を挙げることができ
る。
An undercoat layer may be provided on the surface of the substrate on which the recording layer is provided for the purpose of improving planarity, adhesion, sensitivity, and preventing deterioration of the recording layer. Examples of materials for the undercoat layer include polymethyl methacrylate, acrylic acid/methacrylic acid copolymer, styrene/maleinate anhydride copolymer, polyvinyl alcohol, N-methylolacrylamide, styrene/vinyltoluene copolymer, and chlorosulfonated polyethylene. , nitrocellulose, polyvinyl chloride, chlorinated polyolefin, polyester, polyimide, vinyl acetate/vinyl chloride copolymer,
Examples include polymeric substances such as ethylene/vinyl acetate copolymer, polyethylene, polypropylene, and polycarbonate; and organic substances such as silane coupling agents.

【0039】下塗層は、たとえば上記物質を適当な溶剤
に溶解または分散して塗布液を調製したのち、この塗布
液をスピンコート、ディップコート、エクストルージョ
ンコートなどの塗布法により基板表面に塗布することに
より形成することができる。下塗層の層厚は一般に0.
005〜20μmの範囲にあり、好ましくは0.01〜
10μmの範囲である。
The undercoat layer is prepared by, for example, dissolving or dispersing the above-mentioned substance in a suitable solvent to prepare a coating solution, and then applying this coating solution to the substrate surface by a coating method such as spin coating, dip coating, or extrusion coating. It can be formed by The thickness of the undercoat layer is generally 0.
It is in the range of 0.005 to 20 μm, preferably 0.01 to 20 μm.
The range is 10 μm.

【0040】本発明の円盤状基板(または下塗層)上に
は、アドレス信号等の情報あるいは音楽情報等を表わす
プリピットおよびトラッキング用のグルーブ(プリグル
ーブ)が形成されている。上記ポリカーボネートなどの
樹脂材料を使用する場合は、樹脂材料を射出成形あるい
は押出成形などにより直接基板上にプリピットおよびプ
リグルーブが設けられることが好ましい。
Pre-pits and tracking grooves (pre-grooves) representing information such as address signals or music information are formed on the disc-shaped substrate (or undercoat layer) of the present invention. When using a resin material such as the above-mentioned polycarbonate, it is preferable that pre-pits and pre-grooves are provided directly on the substrate by injection molding or extrusion molding of the resin material.

【0041】またプリグルーブ等の形成を、プレグルー
ブ層を設けることにより行なってもよい。プリグルーブ
層の材料としては、アクリル酸のモノエステル、ジエス
テル、トリエステルおよびテトラエステルのうちの少な
くとも一種のモノマー(またはオリゴマー)と光重合開
始剤との混合物を用いることができる。プリグルーブ層
の形成は、まず精密に作られた母型(スタンパー)上に
上記のアクリル酸エステルおよび重合開始剤からなる混
合液を塗布し、さらにこの塗布液層上に基板を載せたの
ち、基板または母型を介して紫外線の照射により液層を
硬化させて基板と液相とを固着させる。次いで、基板を
母型から剥離することによりプリグルーブ層の設けられ
た基板が得られる。プリグルーブ層の層厚は一般に0.
05〜100μmの範囲にあり、好ましくは0.1〜5
0μmの範囲である。
[0041] Pregroove and the like may also be formed by providing a pregroove layer. As the material for the pregroove layer, a mixture of at least one monomer (or oligomer) of acrylic acid monoester, diester, triester, and tetraester and a photopolymerization initiator can be used. The pregroove layer is formed by first coating a mixture of the above-mentioned acrylic ester and polymerization initiator on a precisely made matrix (stamper), and then placing the substrate on top of this coating layer. The liquid layer is cured by irradiation with ultraviolet rays through the substrate or the matrix, thereby fixing the substrate and the liquid phase. Next, by peeling the substrate from the mother mold, a substrate provided with a pregroove layer is obtained. The thickness of the pregroove layer is generally 0.
In the range of 0.05 to 100 μm, preferably 0.1 to 5
It is in the range of 0 μm.

【0042】円盤状基板の上には、記録層が設けられる
。記録層として色素記録層を形成する場合、本発明に使
用される色素としては、例えば、インドレニン系色素、
イミダゾキノキサリン系色素、インドリジン系色素など
のシアニン系色素、フタロシアニン系色素、ナフタロシ
アニン系色素、ピリリウム系・チオピリリウム系色素、
アズレニウム系色素、スクワリリウム系色素、Ni,C
rなどの金属錯塩系色素、ナフトキノン系・アントラキ
ノン系色素、インドフェノール系色素、インドアニリン
系色素、トリフェニルメタン系色素、トリアリルメタン
系色素、メロシアン系色素、オキソノール系色素、アミ
ニウム系・ジインモニウム系色素およびニトロソ化合物
を挙げることができる。
A recording layer is provided on the disk-shaped substrate. When forming a dye recording layer as a recording layer, examples of dyes used in the present invention include indolenine dyes,
Cyanine dyes such as imidazoquinoxaline dyes, indolizine dyes, phthalocyanine dyes, naphthalocyanine dyes, pyrylium/thiopyrylium dyes,
Azulenium pigment, squalirium pigment, Ni, C
Metal complex dyes such as r, naphthoquinone/anthraquinone dyes, indophenol dyes, indoaniline dyes, triphenylmethane dyes, triallylmethane dyes, merocyan dyes, oxonol dyes, aminium/diimmonium dyes Mention may be made of dyes and nitroso compounds.

【0043】色素層の形成は、上記色素、さらに所望に
より結合剤、金属錯塩系色素またはアミニウム系・ジイ
ンモニウム系色素(クエンチャー)を溶剤に溶解して塗
布液を調製し、次いでこの塗布液を基板表面に塗布して
塗膜を形成したのち乾燥することにより行なうことがで
きる。
To form the dye layer, a coating solution is prepared by dissolving the above dye, and optionally a binder, a metal complex dye, or an aminium/diimmonium dye (quencher) in a solvent. This can be done by coating the surface of the substrate to form a coating film and then drying it.

【0044】上記色素塗布液調製用の溶剤としては、酢
酸エチル、酢酸ブチル、セロソルブアセテートなどのエ
ステル、メチルエチルケトン、シクロヘキサノン、メチ
ルイソブチルケトンなどのケトン、ジクロルメタン、1
,2−ジクロルエタン、クロロホルムなどのハロゲン化
炭化水素、テトラヒドロフラン、エチルエーテル、ジオ
キサンなどのエーテル、エタノール、n−プロパノール
、イソプロパノール、n−ブタノールなどのアルコール
、ジメチルホルムアミドなどのアミド、2、2、3、3
−テトラフロロプロパノール等フッ素系溶剤などを挙げ
ることができる。なお、これらの非炭化水素系有機溶剤
は、50容量%以内である限り、脂肪族炭化水素溶剤、
脂環族炭化水素溶剤、芳香族炭化水素溶剤などの炭化水
素系溶媒を含んでいてもよい。塗布液中にはさらに酸化
防止剤、UV吸収剤、可塑剤、潤滑剤など各種の添加剤
を目的に応じて添加してもよい。
Examples of the solvent for preparing the dye coating solution include esters such as ethyl acetate, butyl acetate, and cellosolve acetate, ketones such as methyl ethyl ketone, cyclohexanone, and methyl isobutyl ketone, dichloromethane,
, halogenated hydrocarbons such as 2-dichloroethane and chloroform, ethers such as tetrahydrofuran, ethyl ether and dioxane, alcohols such as ethanol, n-propanol, isopropanol and n-butanol, amides such as dimethylformamide, 2, 2, 3, 3
- Fluorinated solvents such as tetrafluoropropanol can be mentioned. In addition, these non-hydrocarbon organic solvents may include aliphatic hydrocarbon solvents, as long as the amount is within 50% by volume.
It may also contain hydrocarbon solvents such as alicyclic hydrocarbon solvents and aromatic hydrocarbon solvents. Various additives such as antioxidants, UV absorbers, plasticizers, and lubricants may be further added to the coating liquid depending on the purpose.

【0045】結合剤を使用する場合に結合剤としては、
例えばゼラチン、ニトロセルロース、酢酸セルロース等
のセルロース誘導体、デキストラン、ロジン、ゴムなど
の天然有機高分子物質;およびポリエチレン、ポリプロ
ピレン、ポリスチレン、ポリイソブチレン等の炭化水素
系樹脂、ポリ塩化ビニル、ポリ塩化ビニリデン、ポリ塩
化ビニル・ポリ酢酸ビニル共重合体等のビニル系樹脂、
ポリアクリル酸メチル、ポリメタクリル酸メチル等のア
クリル樹脂、ポリビニルアルコール、塩素化ポリオレフ
ィン、エポキシ樹脂、ブチラール樹脂、ゴム誘導体、フ
ェノール・ホルムアルデヒド樹脂等の熱硬化性樹脂の初
期縮合物などの合成有機高分子物質を挙げることができ
る。塗布方法としては、スプレー法、スピンコート法、
ディップ法、ロールコート法、ブレードコート法、ドク
ターロール法、スクリーン印刷法などを挙げることがで
きる。色素層の材料として結合剤を併用する場合に、結
合剤に対する色素の比率は一般に0.01〜99%(重
量比)の範囲にあり、好ましくは1.0〜95%(重量
比)の範囲にある。
[0045] When a binder is used, the binder includes:
For example, cellulose derivatives such as gelatin, nitrocellulose, and cellulose acetate, natural organic polymer substances such as dextran, rosin, and rubber; and hydrocarbon resins such as polyethylene, polypropylene, polystyrene, and polyisobutylene, polyvinyl chloride, polyvinylidene chloride, Vinyl resins such as polyvinyl chloride and polyvinyl acetate copolymers,
Synthetic organic polymers such as initial condensates of acrylic resins such as polymethyl acrylate and polymethyl methacrylate, polyvinyl alcohol, chlorinated polyolefins, epoxy resins, butyral resins, rubber derivatives, and thermosetting resins such as phenol/formaldehyde resins. Can list substances. Application methods include spray method, spin coating method,
Examples include a dip method, a roll coating method, a blade coating method, a doctor roll method, and a screen printing method. When a binder is used in combination as a material for the dye layer, the ratio of the dye to the binder is generally in the range of 0.01 to 99% (weight ratio), preferably in the range of 1.0 to 95% (weight ratio). It is in.

【0046】プリピットおよびプリグルーブの底部と間
部との膜厚をほぼ同じように形成する方法は、特願平2
−191257号明細書に記載された方法を利用するこ
とができる。色素塗布液の溶剤として、使用する色素の
良溶剤(好ましくは、色素溶液の塗布温度において使用
する色素を2重量%以上溶解し得る溶剤)と、使用する
色素の貧溶剤(好ましくは、色素溶液の塗布温度におい
て使用する色素を2重量%以上溶解しない溶剤)との混
合物であることが好ましい。その際に、該良溶剤と該貧
溶剤とは相溶性であり、上記塗布温度において該貧溶剤
の蒸発速度が該良溶剤の蒸発速度よりも大きくないこと
が必要である。上記色素塗布液をスピンコート法により
基板上に塗布するに際しては、それ自体公知の装置及び
方法を使用して行なうことができる。上記色素溶液を、
一般に0〜100℃、特に5〜80℃、更に特に10〜
60℃の温度で塗布することが好ましい。基板の回転数
は、色素溶液を塗布するときは、一般に10〜1000
r.p.m.、特に100〜500r.p.m.にする
ことが好ましく、色素塗膜を乾燥するときは、一般に3
00〜10000r.p.m.、特に500〜7000
r.p.m.、更に特に700〜4000r.p.m.
にすることが好ましい。
[0046] A method for forming the film thickness at the bottom and the intervening part of pre-pits and pre-grooves to be almost the same is disclosed in Japanese Patent Application No.
The method described in Japanese Patent No.-191257 can be used. The solvent for the dye coating solution is a good solvent for the dye to be used (preferably a solvent that can dissolve 2% by weight or more of the dye to be used at the coating temperature of the dye solution) and a poor solvent for the dye to be used (preferably a dye solution). It is preferable to use a mixture with a solvent that does not dissolve 2% by weight or more of the dye used at the coating temperature. In this case, it is necessary that the good solvent and the poor solvent are compatible, and that the evaporation rate of the poor solvent is not greater than the evaporation rate of the good solvent at the above coating temperature. When applying the dye coating liquid onto the substrate by a spin coating method, a device and method known per se can be used. The above dye solution,
Generally 0-100°C, especially 5-80°C, more especially 10-80°C
Preferably, it is applied at a temperature of 60°C. The rotation speed of the substrate is generally 10 to 1000 when applying the dye solution.
r. p. m. , especially from 100 to 500 r. p. m. When drying the pigment coating, it is generally
00~10000r. p. m. , especially 500-7000
r. p. m. , more particularly from 700 to 4000 r. p. m.
It is preferable to

【0047】また、記録層として金属からなる相変化型
記録層を形成する場合、記録層材料としては、Te、G
e、Sn、O、In、Se、Tl、Co、Sb、Se、
AgおよびZnを挙げることができる。これらの中で、
Te、Sn、In、Se、Ge、SbおよびSeが好ま
しい。これらは単独でも二種以上組み合せて使用しても
良い。相変化型記録層は、たとえば上記金属を真空蒸着
、スパッタリングまたはイオンプレーティングすること
により基板の上に形成することができる。例えば、In
・Sb・Teからなる記録層の膜厚は15〜25nmが
好ましい。相変化型記録層を設ける場合は、記録層が相
変化以上の変化、例えばピットの形成等を起こさせない
ように、記録層の上下にAl2 O3などの酸化膜の層
を形成することが好ましい。記録層上のAl2 O3 
層の膜厚は80〜120nmが好ましく、記録層の下の
Al2 O3 層の膜厚は50〜200nmが好ましい
Further, when forming a phase change type recording layer made of metal as the recording layer, the recording layer material may be Te, G
e, Sn, O, In, Se, Tl, Co, Sb, Se,
Mention may be made of Ag and Zn. Among these,
Te, Sn, In, Se, Ge, Sb and Se are preferred. These may be used alone or in combination of two or more. The phase change recording layer can be formed on the substrate, for example, by vacuum evaporation, sputtering or ion plating of the above metals. For example, In
- The thickness of the recording layer made of Sb.Te is preferably 15 to 25 nm. When a phase change type recording layer is provided, it is preferable to form layers of oxide films such as Al2O3 above and below the recording layer to prevent the recording layer from undergoing changes beyond phase change, such as the formation of pits. Al2O3 on recording layer
The thickness of the layer is preferably 80 to 120 nm, and the thickness of the Al2O3 layer below the recording layer is preferably 50 to 200 nm.

【0048】上記記録層と基板との間に、塩素化ポリオ
レフィン、ニトロセルロースあるいは弗素樹脂からなる
中間層を設けても良い。
An intermediate layer made of chlorinated polyolefin, nitrocellulose or fluororesin may be provided between the recording layer and the substrate.

【0049】上記基板上および記録層上には反射層が設
けられる。反射層の材料である光反射性物質はレーザー
光に対する反射率が高い物質であり、その例としては、
Mg、Se、Y、Ti、Zr、Hf、V、Nb、Ta、
Cr、Mo、W、Mn、Re、Fe、Co、Ni、Ru
、Rh、Pd、Ir、Pt、Cu、Ag、Au、Zn、
Cd、Al、Ga、In、Si、Ge、Te、Pb、P
o、Sn、Biなどの金属および半金属を挙げることが
できる。これらのうちで好ましいものはAl、Au、C
rおよびNiである。これらの物質は単独で用いてもよ
いし、あるいは二種以上の組合せでまたは合金として用
いてもよい。反射層は、たとえば上記光反射性物質を真
空蒸着、スパッタリングまたはイオンプレーティングす
ることにより基板の上に形成することができる。 反射層の層厚は一般には10〜300nmの範囲にある
A reflective layer is provided on the substrate and the recording layer. The light reflective material that is the material of the reflective layer is a material that has a high reflectance to laser light, examples of which are:
Mg, Se, Y, Ti, Zr, Hf, V, Nb, Ta,
Cr, Mo, W, Mn, Re, Fe, Co, Ni, Ru
, Rh, Pd, Ir, Pt, Cu, Ag, Au, Zn,
Cd, Al, Ga, In, Si, Ge, Te, Pb, P
Mention may be made of metals and metalloids such as O, Sn, Bi, etc. Among these, preferred are Al, Au, and C.
r and Ni. These substances may be used alone, or in combination of two or more or as an alloy. The reflective layer can be formed on the substrate, for example, by vacuum deposition, sputtering, or ion plating of the light reflective material described above. The thickness of the reflective layer is generally in the range of 10 to 300 nm.

【0050】また、反射層の上には、記録層などを物理
的および化学的に保護する目的で保護層が設けられるこ
とが好ましい。この保護層は、基板の記録層が設けられ
ていない側にも耐傷性、耐湿性を高める目的で設けられ
てもよい。保護層に用いられる材料の例としては、Si
O、SiO2 、MgF2、SnO2 、Si3 N4
 等の無機物質;熱可塑性樹脂、熱硬化性樹脂、UV硬
化性樹脂等の有機物質を挙げることができる。
Further, it is preferable that a protective layer is provided on the reflective layer for the purpose of physically and chemically protecting the recording layer and the like. This protective layer may also be provided on the side of the substrate where the recording layer is not provided for the purpose of increasing scratch resistance and moisture resistance. Examples of materials used for the protective layer include Si
O, SiO2, MgF2, SnO2, Si3 N4
and organic substances such as thermoplastic resins, thermosetting resins, and UV curable resins.

【0051】保護層は、たとえばプラスチックの押出加
工で得られたフィルムを接着層を介して記録層(反射層
)上および/または基板上にラミネートすることにより
形成することができる。あるいは真空蒸着、スパッタリ
ング、塗布等の方法により設けられてもよい。また、熱
可塑性樹脂、熱硬化性樹脂の場合には、これらを適当な
溶剤に溶解して塗布液を調製したのち、この塗布液を塗
布し、乾燥することによっても形成することができる。 UV硬化性樹脂の場合には、そのままもしくは適当な溶
剤に溶解して塗布液を調製したのちこの塗布液を塗布し
、UV光を照射して硬化させることによっても形成する
ことができる。これらの塗布液中には、更に帯電防止剤
、酸化防止剤、UV吸収剤等の各種添加剤を目的に応じ
て添加してもよい。記録層上に直接保護層形成材料を塗
布する場合は、該記録層を保護層の塗布液の溶解作用か
ら守るため記録層上にポリブタジエンなどを塗布(その
際溶剤としては記録層を溶解しない溶剤を用いる)する
ことにより中間層を設けることが好ましい。中間層は、
金属等の薄膜を蒸着により設けてもよい。保護層の層厚
は一般には0.1〜100μmの範囲にある。
The protective layer can be formed, for example, by laminating a film obtained by extrusion of plastic onto the recording layer (reflection layer) and/or the substrate via an adhesive layer. Alternatively, it may be provided by methods such as vacuum deposition, sputtering, and coating. In the case of a thermoplastic resin or a thermosetting resin, it can also be formed by dissolving these in an appropriate solvent to prepare a coating liquid, then applying this coating liquid and drying it. In the case of a UV curable resin, it can also be formed by preparing a coating liquid as it is or by dissolving it in an appropriate solvent, applying this coating liquid, and curing it by irradiating it with UV light. Various additives such as antistatic agents, antioxidants, and UV absorbers may be further added to these coating liquids depending on the purpose. When coating the protective layer forming material directly on the recording layer, coat polybutadiene or the like on the recording layer to protect the recording layer from the dissolving action of the coating liquid for the protective layer (in this case, use a solvent that does not dissolve the recording layer). It is preferable to provide the intermediate layer by using The middle class is
A thin film of metal or the like may be provided by vapor deposition. The thickness of the protective layer is generally in the range of 0.1 to 100 μm.

【0052】さらに、記録層上に保護層を形成するの代
わりに、記録層上にプラスチックのフィルムを基板の内
周及び外周にて融着して設けることにより記録層を保護
してもよい。
Furthermore, instead of forming a protective layer on the recording layer, the recording layer may be protected by providing a plastic film on the recording layer by welding it to the inner and outer peripheries of the substrate.

【0053】本発明において、情報記録媒体は上述した
構成からなる単板であってもよいが、あるいは更に上記
構成を有する二枚の基板を記録層が内側となるように向
い合わせ、接着剤等を用いて接合することにより、貼合
せタイプの記録媒体を製造することもできる。あるいは
また、二枚の円盤状基板のうちの少なくとも一方に上記
構成を有する基板を用いて、リング状内側スペーサとリ
ング状外側スペーサとを介して接合することにより、エ
アーサンドイッチタイプの記録媒体を製造することもで
きる。本発明の情報記録媒体は上記のような方法で製造
することができる。
In the present invention, the information recording medium may be a single substrate having the above-described structure, or alternatively, two substrates having the above-described structure may be placed facing each other so that the recording layer is on the inside, and an adhesive or the like is applied to the medium. A laminated type recording medium can also be manufactured by bonding using. Alternatively, an air sandwich type recording medium is manufactured by using a substrate having the above structure as at least one of two disc-shaped substrates and joining them via a ring-shaped inner spacer and a ring-shaped outer spacer. You can also. The information recording medium of the present invention can be manufactured by the method described above.

【0054】情報記録および再生方法は、上記情報記録
媒体を用いて、例えば次のように行なわれる。まず、情
報記録媒体を定線速度(CDフォーマットの場合は1.
2〜1.4m/秒)または定角速度にて回転させながら
、基板側から半導体レーザー光などの記録用の光を照射
する。この光の照射により、記録層にピット(孔)が形
成されることにより、基板表面に変形、変質が起こるこ
とにより、あるいは記録層に変色、会合状態の変化等に
より、屈折率が変化することによって情報が記録される
と考えられる。記録光としては550nm〜850nm
の範囲の発振波長を有する半導体レーザービームが用い
られる。
The information recording and reproducing method is carried out using the above information recording medium, for example, as follows. First, the information recording medium is moved at a constant linear velocity (1.
Recording light such as semiconductor laser light is irradiated from the substrate side while rotating at a constant angular velocity (2 to 1.4 m/sec) or at a constant angular velocity. Irradiation of this light causes pits (holes) to be formed in the recording layer, resulting in deformation and alteration of the substrate surface, or by discoloration of the recording layer, changes in the state of association, etc., and the refractive index changes. It is thought that information is recorded by. Recording light is 550nm to 850nm
A semiconductor laser beam having an oscillation wavelength in the range of is used.

【0055】上記のように記録された情報の再生は、情
報記録媒体を上記と同一の定線速度で回転させながら半
導体レーザー光を基板側から照射して、その反射光を検
出することにより行なうことができる。なお、レーザー
光の照射は、フレキシブルディスクなどの場合、記録層
側から行なうこともある。
Reproduction of the information recorded in the above manner is carried out by irradiating semiconductor laser light from the substrate side while rotating the information recording medium at the same constant linear velocity as above, and detecting the reflected light. be able to. Incidentally, in the case of a flexible disk, etc., the laser beam irradiation may be performed from the recording layer side.

【0056】[0056]

【実施例】以下に、本発明の実施例および比較例を記載
する。ただし、これらの各例は本発明を制限するもので
はない。
[Examples] Examples and comparative examples of the present invention will be described below. However, these examples do not limit the invention.

【0057】[実施例1] 円盤状のポリカーボネート基板;(1) 寸法:外径が
120mm、内径が15mm、厚さが1.2mm、屈折
率が1.58 (2) 直径44〜47mm領域:トラックピッチが1
.6μm、プリグルーブの半値幅が0.8μm、深さが
37nmの溝が形成、 (3) 直径47〜70mm領域:トラックピッチが1
.6μm、プリピットの半値幅が0.6μm、深さが1
10nmの凹部が形成、 (4) 直径70〜116mm領域:トラックピッチが
1.6μm、プリグルーブの半値幅が0.8μm、深さ
が37nmの溝が形成、 を光ディスクの基板として用意した。
[Example 1] Disc-shaped polycarbonate substrate; (1) Dimensions: outer diameter 120 mm, inner diameter 15 mm, thickness 1.2 mm, refractive index 1.58 (2) Diameter 44-47 mm region: track pitch is 1
.. 6 μm, pre-groove half-value width of 0.8 μm, and a groove with a depth of 37 nm. (3) Diameter 47-70 mm region: Track pitch is 1
.. 6μm, pre-pit half width 0.6μm, depth 1
A concave portion of 10 nm was formed. (4) A region with a diameter of 70 to 116 mm: a groove with a track pitch of 1.6 μm, a pregroove half width of 0.8 μm, and a depth of 37 nm was prepared as a substrate for an optical disk.

【0058】下記の色素A(屈折率:2.8):色素AThe following dye A (refractive index: 2.8): Dye A

【0059】[0059]

【化1】[Chemical formula 1]

【0060】3.25gと 下記の色素B: 色素B[0060] 3.25g Dye B below: Dye B

【0061】[0061]

【化2】[Case 2]

【0062】0.325gとを、2,2,3,3−テト
ラフロロ−1−プロパノール75ml、エチルセルソル
ブ20mlおよびテトラクロロエタン5mlからなる混
合溶剤に、超音波1時間の付与により溶解して色素記録
層塗布液を調製した。
0.325 g was dissolved in a mixed solvent consisting of 75 ml of 2,2,3,3-tetrafluoro-1-propanol, 20 ml of ethyl cellosolve, and 5 ml of tetrachloroethane by applying ultrasonic waves for 1 hour to record the dye. A layer coating solution was prepared.

【0063】上記円盤状のポリカーボネート基板の内周
側から、上記塗布液をスピンコート法により回転数20
0rpm の速度で5秒間塗布した後、1秒間に50r
pmづつ2000rpmまで速度を上昇させ、2000
rpmで30秒間保持することにより乾燥させ、層厚が
下記のような色素記録層を形成した。   (1) 直径47〜70mm領域のプリピット底部
:  125nm  (2) 直径47〜70mm領域
のプリピット間部:  120nm  (3) 直径7
0〜116mm領域のプリグルーブ底部:  125n
m  (4) 直径70〜116mm領域のプリグルー
ブ間部:  120nm
[0063] The coating solution was applied from the inner peripheral side of the disc-shaped polycarbonate substrate by spin coating at a rotation speed of 20.
After applying for 5 seconds at a speed of 0 rpm, apply at a speed of 50 rpm per second.
Increase the speed by pm to 2000 rpm, 2000
It was dried by holding at rpm for 30 seconds to form a dye recording layer having the thickness shown below. (1) Bottom of prepits in diameter 47-70mm region: 125nm (2) Part between prepits in diameter 47-70mm region: 120nm (3) Diameter 7
Pregroove bottom in 0-116mm area: 125n
m (4) Area between pregrooves in diameter 70-116mm region: 120nm

【0064】上記色素記録層上
、直径42〜118mmの領域に、AuをDCスパッタ
リング(Ar圧力:2Pa、電力:200W)して膜厚
が100nmの反射層を形成した。
A reflective layer having a thickness of 100 nm was formed on the dye recording layer by DC sputtering (Ar pressure: 2 Pa, power: 200 W) in an area having a diameter of 42 to 118 mm.

【0065】さらに、反射層上に、紫外線硬化型樹脂(
商品名:3070、スリーボンド(株)製)をスピンコ
ート法により回転数200rpm の速度で塗布した後
回転数1500rpmで30秒間レベレングさせ、次い
で紫外線(高圧水銀灯200W/cm)を10秒照射す
ることにより硬化させ、層厚2μm(外周端面の層厚2
〜10μm)の保護層を形成した。
Furthermore, on the reflective layer, an ultraviolet curing resin (
Product name: 3070, manufactured by Three Bond Co., Ltd.) was applied by spin coating at a rotation speed of 200 rpm, leveled at a rotation speed of 1500 rpm for 30 seconds, and then irradiated with ultraviolet rays (high pressure mercury lamp 200 W/cm) for 10 seconds. Cured, layer thickness 2 μm (layer thickness 2 μm on outer peripheral end surface)
A protective layer of ~10 μm) was formed.

【0066】このようにして、基板、色素記録層、反射
層および保護層からなる情報記録媒体を製造した。
In this manner, an information recording medium consisting of a substrate, a dye recording layer, a reflective layer and a protective layer was manufactured.

【0067】[実施例2]実施例1において、円盤状の
ポリカーボネート基板としてプリピットの深さを110
nmから105nmに変え、プリグルーブの深さを37
nmから25nmに変えたものを使用した以外は実施例
1と同様にして下記の膜厚の記録層を有する情報記録媒
体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  120nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
0nm
[Example 2] In Example 1, the pre-pit depth was set to 110 mm as a disc-shaped polycarbonate substrate.
Changed the pregroove depth from 37 nm to 105 nm.
An information recording medium having a recording layer having the following thickness was manufactured in the same manner as in Example 1 except that the thickness was changed from nm to 25 nm. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 120 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
0nm

【0068】[実施例3]実施例1において、円
盤状のポリカーボネート基板としてプリピットの深さを
110nmから115nmに変え、プリグルーブの深さ
を37nmから40nmに変えたものを使用した以外は
実施例1と同様にして下記の膜厚の記録層を有する情報
記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  120nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
0nm
[Example 3] Example 1 except that a disk-shaped polycarbonate substrate was used in which the pre-pit depth was changed from 110 nm to 115 nm and the pre-groove depth was changed from 37 nm to 40 nm. An information recording medium having a recording layer having the thickness shown below was manufactured in the same manner as in Example 1. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 120 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
0nm

【0069】[実施例4]実施例1において、円
盤状のポリカーボネート基板としてプリピットの深さを
110nmから90nmに変えたものを使用した以外は
実施例1と同様にして下記の膜厚の記録層を有する情報
記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  120nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
0nm
[Example 4] A recording layer having the following film thickness was prepared in the same manner as in Example 1, except that a disk-shaped polycarbonate substrate was used in which the pre-pit depth was changed from 110 nm to 90 nm. An information recording medium having the following was manufactured. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 120 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
0nm

【0070】[実施例5]実施例1において、円
盤状のポリカーボネート基板としてプリグルーブの深さ
を37nmから50nmに変えたものを使用した以外は
実施例1と同様にして下記の膜厚の記録層を有する情報
記録媒体を製造した。
[Example 5] The following film thickness was recorded in the same manner as in Example 1, except that a disk-shaped polycarbonate substrate was used with the pregroove depth changed from 37 nm to 50 nm. An information recording medium having layers was manufactured.

【0071】[比較例1]実施例1において、円盤状の
ポリカーボネート基板としてプリピットの深さを110
nmから170nmに変え、プリグルーブの深さを37
nmから80nmに変えたものを使用した以外は実施例
1と同様にして下記の膜厚の記録層を有する情報記録媒
体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  120nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
0nm
[Comparative Example 1] In Example 1, the prepit depth was set to 110 mm as a disc-shaped polycarbonate substrate.
Change the pregroove depth from 37 nm to 170 nm.
An information recording medium having a recording layer having the following thickness was manufactured in the same manner as in Example 1 except that the thickness was changed from nm to 80 nm. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 120 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
0nm

【0072】[比較例2]実施例1において、円
盤状のポリカーボネート基板としてプリピットの深さを
110nmから80nmに変え、プリグルーブの深さを
37nmから50nmに変えたものを使用した以外は実
施例1と同様にして下記の膜厚の記録層を有する情報記
録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  120nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
0nm
[Comparative Example 2] Example 1 except that a disk-shaped polycarbonate substrate was used in which the pre-pit depth was changed from 110 nm to 80 nm and the pre-groove depth was changed from 37 nm to 50 nm. An information recording medium having a recording layer having the thickness shown below was manufactured in the same manner as in Example 1. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 120 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
0nm

【0073】[実施例6]実施例1において、色
素塗布液の混合溶剤を2,2,3,3−テトラフロロ−
1−プロパノール68ml、エチルセルソルブ25ml
およびテトラクロロエタン7mlからなる混合溶剤に変
えた以外は実施例1と同様にして下記の膜厚の記録層を
有する情報記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  115nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  11
5nm
[Example 6] In Example 1, the mixed solvent of the dye coating solution was changed to 2,2,3,3-tetrafluoro-
1-propanol 68ml, ethyl cellosolve 25ml
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1, except that the mixed solvent was changed to 7 ml of tetrachloroethane and 7 ml of tetrachloroethane. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 115 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 11
5nm

【0074】[実施例7]実施例1において、色
素塗布液の混合溶剤を2,2,3,3−テトラフロロ−
1−プロパノール70ml、エチルセロソルブ20ml
およびテトラクロロエタン10mlからなる混合溶剤に
変えた以外は実施例1と同様にして下記の膜厚の記録層
を有する情報記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  110nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  11
0nm
[Example 7] In Example 1, the mixed solvent of the dye coating solution was changed to 2,2,3,3-tetrafluoro-
1-propanol 70ml, ethyl cellosolve 20ml
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1, except that the mixed solvent was changed to 10 ml of tetrachloroethane. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 110 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 11
0nm

【0075】[実施例8]実施例1において、円
盤状のポリカーボネート基板としてプリピットの深さを
110nmから170nmに変え、プリグルーブの深さ
を37nmから80nmに変えたものを使用し、且つ色
素塗布液の混合溶剤を2,2,3,3−テトラフロロ−
1−プロパノール100mlの単一溶剤に変えた以外は
実施例1と同様にして下記の膜厚の記録層を有する情報
記録媒体を製造した。 (1) プリピット底部:  135nm(2) プリ
ピット間部:    95nm(3) プリグルーブ底
部:  125nm(4) プリグルーブ間部:   
 95nm
[Example 8] A disc-shaped polycarbonate substrate in Example 1 with the pre-pit depth changed from 110 nm to 170 nm and the pre-groove depth changed from 37 nm to 80 nm was used, and dye coating was performed. The mixed solvent of the liquid is 2,2,3,3-tetrafluoro-
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1 except that 100 ml of 1-propanol was used as the single solvent. (1) Bottom of pre-pit: 135 nm (2) Area between pre-pits: 95 nm (3) Bottom of pre-groove: 125 nm (4) Area between pre-groove:
95nm

【0076】[比較例3]実施例1において
、色素塗布液の混合溶剤を2,2,3,3−テトラフロ
ロ−1−プロパノール45ml、エチルセルソルブ40
mlおよびテトラクロロエタン15mlからなる混合溶
剤に変えた以外は実施例1と同様にして下記の膜厚の記
録層を有する情報記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  105nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  10
5nm
[Comparative Example 3] In Example 1, the mixed solvent for the dye coating solution was 45 ml of 2,2,3,3-tetrafluoro-1-propanol and 40 ml of ethyl cellosolve.
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1, except that the mixed solvent was changed to 15 ml of tetrachloroethane and 15 ml of tetrachloroethane. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 105 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 10
5nm

【0077】[実施例9]実施例1において、円
盤状のポリカーボネート基板としてプリピットの深さを
110nmから140nmに変え、プリグルーブの深さ
を37nmから60nmに変えたものを使用し、且つ色
素塗布液の混合溶剤を2,2,3,3−テトラフロロ−
1−プロパノール45ml、エチルセルソルブ40ml
およびテトラクロロエタン15mlからなる混合溶剤に
変えた以外は実施例1と同様にして下記の膜厚の記録層
を有する情報記録媒体を製造した。 (1) プリピット底部:  130nm(2) プリ
ピット間部:  105nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  10
5nm
[Example 9] In Example 1, a disc-shaped polycarbonate substrate was used in which the pre-pit depth was changed from 110 nm to 140 nm, and the pre-groove depth was changed from 37 nm to 60 nm, and dye coating was performed. The mixed solvent of the liquid is 2,2,3,3-tetrafluoro-
1-propanol 45ml, ethyl cellosolve 40ml
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1 except that the mixed solvent was changed to 15 ml of tetrachloroethane. (1) Pre-pit bottom: 130 nm (2) Pre-pit space: 105 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 10
5nm

【0078】[実施例10]実施例1において、
円盤状のポリカーボネート基板としてプリピットの深さ
を110nmから180nmに変え、プリグルーブの深
さを37nmから95nmに変えたものを使用し、且つ
色素塗布液の色素を下記の色素C1.75gと上記色素
B0.175gに変え、そして混合溶剤を2,2,3,
3−テトラフロロ−1−プロパノール100mlの単一
溶剤に変えた以外は実施例1と同様にして下記の膜厚の
記録層を有する情報記録媒体を製造した。 (1) プリピット底部:  145nm(2) プリ
ピット間部:  100nm(3) プリグルーブ底部
:  140nm(4) プリグルーブ間部:  10
0nm色素C(屈折率:2.9):
[Example 10] In Example 1,
A disk-shaped polycarbonate substrate was used in which the pre-pit depth was changed from 110 nm to 180 nm and the pre-groove depth was changed from 37 nm to 95 nm, and the dye in the dye coating solution was 1.75 g of the following dye C and the above dye. Change to 0.175g of B, and change the mixed solvent to 2, 2, 3,
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1 except that 100 ml of 3-tetrafluoro-1-propanol was used as the single solvent. (1) Pre-pit bottom: 145 nm (2) Pre-pit space: 100 nm (3) Pre-groove bottom: 140 nm (4) Pre-groove space: 10
0nm dye C (refractive index: 2.9):

【0079】[0079]

【化3】[Chemical formula 3]

【0080】[実施例11]実施例1において、円盤状
のポリカーボネート基板としてプリピットの深さを11
0nmから250nmに変え、プリグルーブの深さを、
37nmから165nmに変えたものを使用し、色素塗
布液の色素を下記の色素D2.6gと上記色素B0.2
6gに変え、そして混合溶剤を2,2,3,3−テトラ
フロロ−1−プロパノール100mlの単一溶剤に変え
た以外は実施例1と同様にして下記の膜厚の記録層を有
する情報記録媒体を製造した。 色素D(屈折率:2.7):
[Example 11] In Example 1, the depth of the pre-pits was set to 11 for the disc-shaped polycarbonate substrate.
Change the pregroove depth from 0nm to 250nm,
Using a dye whose wavelength was changed from 37 nm to 165 nm, the dye in the dye coating solution was 2.6 g of the following dye D and 0.2 g of the above dye B.
An information recording medium having a recording layer with the following thickness was prepared in the same manner as in Example 1 except that the mixed solvent was changed to 100 ml of 2,2,3,3-tetrafluoro-1-propanol as a single solvent. was manufactured. Dye D (refractive index: 2.7):

【0081】[0081]

【化4】 (1) プリピット底部:  210nm(2) プリ
ピット間部:  120nm(3) プリグルーブ底部
:  200nm(4) プリグルーブ間部:  12
0nm
[Chemical formula 4] (1) Pre-pit bottom: 210 nm (2) Pre-pit space: 120 nm (3) Pre-groove bottom: 200 nm (4) Pre-groove space: 12
0nm

【0082】[実施例12]実施例1において、
円盤状のポリカーボネート基板としてプリピットの深さ
を110nmから105nmに変え、プリグルーブの深
さを37nmから30nmに変えたものを使用し、且つ
色素塗布液の混合溶剤を2,2,3,3−テトラフロロ
−1−プロパノール75ml、プロピレングリコールモ
ノメチルエーテル20mlおよびテトラクロロエタン5
mlからなる混合溶剤に変えた以外は実施例1と同様に
して下記の膜厚の記録層を有する情報記録媒体を製造し
た。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  125nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
5nm
[Example 12] In Example 1,
A disc-shaped polycarbonate substrate with pre-pit depth changed from 110 nm to 105 nm and pre-groove depth changed from 37 nm to 30 nm was used, and the mixed solvent of the dye coating solution was 2,2,3,3- 75 ml of tetrafluoro-1-propanol, 20 ml of propylene glycol monomethyl ether and 5 ml of tetrachloroethane
An information recording medium having a recording layer having the thickness shown below was manufactured in the same manner as in Example 1 except that the mixed solvent was changed to ml. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 125 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
5nm

【0083】[実施例13]実施例1において、
円盤状のポリカーボネート基板としてプリグルーブの深
さを37nmから35nmに変えたものを使用し、そし
て色素塗布液の混合溶剤を2,2,3,3−テトラフロ
ロ−1−プロパノール75ml、ジイソブチルケトン2
0mlおよびテトラクロロエタン5mlからなる混合溶
剤に変えた以外は実施例1と同様にして下記の膜厚の記
録層を有する情報記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  122nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
2nm
[Example 13] In Example 1,
A disk-shaped polycarbonate substrate with pregroove depth changed from 37 nm to 35 nm was used, and the mixed solvent of the dye coating solution was 75 ml of 2,2,3,3-tetrafluoro-1-propanol and 2 diisobutyl ketone.
An information recording medium having a recording layer with the following thickness was produced in the same manner as in Example 1 except that the mixed solvent was changed to 0 ml and 5 ml of tetrachloroethane. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 122 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
2nm

【0084】[実施例14]実施例1において、
色素塗布液の混合溶剤を2,2,3,3−テトラフロロ
−1−プロパノール75ml、エチルカプリレート20
mlおよびテトラクロロエタン5mlからなる混合溶剤
に変えた以外は実施例1と同様にして下記の膜厚の記録
層を有する情報記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  122nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
2nm
[Example 14] In Example 1,
The mixed solvent of the dye coating solution was 75 ml of 2,2,3,3-tetrafluoro-1-propanol and 20 ml of ethyl caprylate.
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1, except that the mixed solvent was changed to 5 ml of tetrachloroethane and 5 ml of tetrachloroethane. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 122 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
2nm

【0085】[実施例15]実施例1において、
色素塗布液の混合溶剤を2,2,3,3−テトラフロロ
−1−プロパノール75ml、1−ペンタノール20m
lおよびテトラクロロエタン5mlからなる混合溶剤に
変えた以外は実施例1と同様にして下記の膜厚の記録層
を有する情報記録媒体を製造した。 (1) プリピット底部:  125nm(2) プリ
ピット間部:  122nm(3) プリグルーブ底部
:  125nm(4) プリグルーブ間部:  12
2nm
[Example 15] In Example 1,
The mixed solvent of the dye coating solution was 75 ml of 2,2,3,3-tetrafluoro-1-propanol and 20 ml of 1-pentanol.
An information recording medium having a recording layer having the thickness shown below was produced in the same manner as in Example 1 except that the mixed solvent was changed to 5 ml of 1 and 5 ml of tetrachloroethane. (1) Pre-pit bottom: 125 nm (2) Pre-pit space: 122 nm (3) Pre-groove bottom: 125 nm (4) Pre-groove space: 12
2nm

【0086】[実施例16]実施例1において、
色素Aを色素Cに変え、色素塗布液の混合溶剤を2,2
,3,3−テトラフロロ−1−プロパノール82ml、
エチルセルソルブ13mlおよびテトラクロロエタン5
mlからなる混合溶剤に変えた以外は実施例1と同様に
して下記の膜厚の記録層を有する情報記録媒体を製造し
た。 (1) プリピット底部:  140nm(2) プリ
ピット間部:  135nm(3) プリグルーブ底部
:  140nm(4) プリグルーブ間部:  13
5nm
[Example 16] In Example 1,
Change dye A to dye C, and change the mixed solvent of the dye coating solution to 2,2
, 3,3-tetrafluoro-1-propanol 82ml,
13 ml of ethyl cellosolve and 5 ml of tetrachloroethane
An information recording medium having a recording layer having the thickness shown below was manufactured in the same manner as in Example 1 except that the mixed solvent was changed to ml. (1) Pre-pit bottom: 140 nm (2) Pre-pit space: 135 nm (3) Pre-groove bottom: 140 nm (4) Pre-groove space: 13
5nm

【0087】[実施例17]実施例1において、
色素記録層の代わりに下記のようにしてAl2 O3 
層、 相変化型金属記録層およびAl2 O3 層から
なる積層体を形成した以外は実施例1と同様にして下記
の層厚の積層体を有する情報記録媒体を製造した。上記
基板上に、Al2 O3 を真空蒸着することにより層
厚100nmのAl2O3 層を形成した。この層の上
に、(In3 SbTe2 )と(In22Sb37T
e41)とをターゲットにして共スパッタリング(Ar
圧力:2Pa、電力:200W)することにより(In
3 SbTe2 )50(In22Sb37Te41)
50の層厚20nmの記録層を形成した。記録層上にさ
らに真空蒸着で層厚100nmのAl2 O3 層を形
成した。 (1) プリピット底部:  20nm(2) プリピ
ット間部:  20nm(3) プリグルーブ底部: 
 20nm(4) プリグルーブ間部:  20nmな
お、上記基板のプリピットおよびプリグルーブの深さ、
記録層等の層厚は、その断面を超高解像度SEM(走査
型電子顕微鏡)で測定して得られたものである。
[Example 17] In Example 1,
Instead of the dye recording layer, Al2O3 is added as follows.
An information recording medium having a laminate having the following layer thickness was manufactured in the same manner as in Example 1 except that a laminate consisting of a phase change metal recording layer and an Al2O3 layer was formed. On the above substrate, an Al2O3 layer having a thickness of 100 nm was formed by vacuum evaporating Al2O3. On top of this layer, (In3SbTe2) and (In22Sb37T
Co-sputtering (Ar
Pressure: 2Pa, power: 200W) (In
3SbTe2)50(In22Sb37Te41)
A recording layer having a layer thickness of 20 nm was formed. An Al2O3 layer with a thickness of 100 nm was further formed on the recording layer by vacuum evaporation. (1) Pre-pit bottom: 20 nm (2) Pre-pit space: 20 nm (3) Pre-groove bottom:
20 nm (4) Area between pre-grooves: 20 nm The depth of the pre-pits and pre-grooves of the above substrate,
The layer thickness of the recording layer and the like was obtained by measuring its cross section using an ultra-high resolution SEM (scanning electron microscope).

【0088】[情報記録媒体の評価] 1)変調度 得られた情報記録媒体に下記の条件にて情報を記録、再
生した。記録再生評価装置として、光ディスク評価機D
DU1000(パルステック(株)製)を用いて記録を
行なった。すなわち、発振波長が780nmおよびNA
が0.5の光ヘッドを用いて、パワー7.4mW、線速
度1.4m/秒で、CDフォーマットのEFM信号を、
基板の直径72mmの位置から記録した。変調度の評価
は、プリピット部の再生を直径の66mmの位置にて、
上記記録情報の再生を直径72mmの位置にて行なった
。レーザーは記録に使用したのと同じものを用いて、再
生パワー0.5mWで、線速度1.4m/秒にて、再生
し、上記各位置での直流再生信号を測定し、最も反射光
量の多いレベルをItop 、低いレベルをIbot 
として下記式より変調度を求めた。 変調度={(Itop −Ibot )/Itop }
×100変調度の評価は、60を越える時が良好、70
を越える時が優秀といえる。
[Evaluation of Information Recording Medium] 1) Modulation degree Information was recorded and reproduced on the information recording medium obtained under the following conditions. Optical disc evaluation machine D as a recording/playback evaluation device
Recording was performed using DU1000 (manufactured by Pulstech Co., Ltd.). That is, the oscillation wavelength is 780 nm and the NA
Using an optical head with a power of 0.5, a power of 7.4 mW, a linear velocity of 1.4 m/s, a CD format EFM signal,
Recording was made from a position with a diameter of 72 mm on the substrate. To evaluate the modulation degree, reproduce the prepit part at a position of 66 mm in diameter.
The recorded information was reproduced at a position with a diameter of 72 mm. Using the same laser used for recording, playback was performed at a playback power of 0.5mW and a linear velocity of 1.4m/sec, and the DC playback signal at each of the above positions was measured. High level is Itop, low level is Ibot
The modulation degree was calculated from the following formula. Modulation degree = {(Itop − Ibot )/Itop }
Evaluation of ×100 modulation degree is good when it exceeds 60, 70
It can be said that it is excellent when it exceeds.

【0089】2)反射率 プリグルーブの未記録部の再生を71mmの位置にて上
記条件にて再生状態にし、直流再生信号の平均電圧(I
g )を測定する。市販CDの最内周のミラー部を反射
率計で反射率(Ro )を測定し、その位置を上記と同
様に再生状態で平均電圧(Io )を測定し、下記式よ
り反射率を求めた。 反射率==(Ig /Io )×Ro ×100反射率
の評価は、63を越える時が良好、70を越える時が優
秀といえる。
2) The unrecorded portion of the reflectance pregroove is reproduced at a position of 71 mm under the above conditions, and the average voltage of the DC reproduction signal (I
g). The reflectance (Ro) of the innermost mirror part of a commercially available CD was measured with a reflectance meter, and the average voltage (Io) was measured at that position in the same playback state as above, and the reflectance was determined from the following formula. . Reflectance==(Ig/Io)×Ro×100 When evaluating the reflectance, it can be said that when it exceeds 63, it is good, and when it exceeds 70, it is said that it is excellent.

【0090】3)プッシュプル信号の変動率得られた情
報記録媒体を上記評価機を用いて再生し、プリピット領
域およびプリグルーブ領域の夫々の領域において出力さ
れたトラッキングエラー信号を観測し、それぞれの領域
での最大振幅をA、最小振幅をBとして、2×(A−B
)/(A+B)の値を上記変動率として求めた。プッシ
ュプル信号の変動率の評価は、0.03〜0.12が良
好、0.04〜0.09が優秀といえる。 前記実施例及び比較例で得られた情報記録媒体の構成を
表1に、上記結果を表2に示す。
3) Fluctuation rate of push-pull signal The obtained information recording medium is reproduced using the above-mentioned evaluation machine, and the tracking error signals output in each of the pre-pit area and pre-groove area are observed, and each The maximum amplitude in the area is A, the minimum amplitude is B, 2×(A-B
)/(A+B) was determined as the above fluctuation rate. Regarding the evaluation of the fluctuation rate of the push-pull signal, it can be said that 0.03 to 0.12 is good and 0.04 to 0.09 is excellent. Table 1 shows the configurations of the information recording media obtained in the Examples and Comparative Examples, and Table 2 shows the results.

【0091】[0091]

【表1】[Table 1]

【0092】a:2,2,3,3−テトラフロロ−1−
プロパノール b:エチルセルソルブ c:テトラクロロエタン d:プロピレングリコールモノエチルエーテルe:ジイ
ソブチルケトン f:エチルカプリレート g:1−ペンタノール
a: 2,2,3,3-tetrafluoro-1-
Propanol b: Ethyl cellosolve c: Tetrachloroethane d: Propylene glycol monoethyl ether e: Diisobutyl ketone f: Ethyl caprylate g: 1-pentanol

【0093】[0093]

【表2】[Table 2]

【0094】上記結果より明らかなように、本発明の条
件を満足するプリピットの深さ、プリグルーブの深さ、
および記録層の膜厚を有する本発明の情報記録媒体は、
変調度、反射率が共に高く、さらにトラッキング性にも
優れたものである。
As is clear from the above results, the pre-pit depth, pre-groove depth, and
The information recording medium of the present invention has a recording layer thickness of
It has high modulation degree and reflectance, and also has excellent tracking performance.

【図面の簡単な説明】[Brief explanation of drawings]

【図1】本発明の情報記録媒体の一例を示す断面図であ
る。
FIG. 1 is a sectional view showing an example of an information recording medium of the present invention.

【図2】図1の部分拡大断面図である。FIG. 2 is a partially enlarged sectional view of FIG. 1;

【図3】本発明のプリピットの深さと記録層の膜厚との
関係を説明するためのプリピット部の断面図である。
FIG. 3 is a cross-sectional view of a prepit portion for explaining the relationship between the depth of the prepit and the thickness of the recording layer according to the present invention.

【図4】本発明のプリグルーブの深さと記録層の膜厚と
の関係を説明するためのプリピット部の断面図である。
FIG. 4 is a cross-sectional view of a pre-pit portion for explaining the relationship between the depth of a pre-groove and the thickness of a recording layer according to the present invention.

【符号の説明】[Explanation of symbols]

1  円盤状基板 2  記録層 3  反射層 4  保護層 5  再生専用領域 6  記録可能領域 8  プリピット 9  プリグルーブ 1 Disk-shaped substrate 2 Recording layer 3 Reflection layer 4 Protective layer 5 Play-only area 6 Recordable area 8 Prepit 9 Pregroove

Claims (2)

【特許請求の範囲】[Claims] 【請求項1】  表面に、プリピットからなる再生専用
領域とプリグルーブからなる記録可能領域とが設けられ
た円盤状基板の上に、レーザーによる情報の記録が可能
な記録層および反射層が、この順で設けられた情報記録
媒体において、該プリピットの深さと該記録層の膜厚と
の関係が下記式(I):       0.15λ≦ns dp −nd Δtp
 ≦0.24λ      (I)を満足し、且つ 該プリグルーブの深さと該記録層の膜厚との関係が下記
式(II):       0.02λ≦ns dg −nd Δtg
 ≦0.08λ      (II)[但し、ns は
基板の屈折率を表わし、nd は該記録層の屈折率を表
わし、dpはプリピットの深さ(nm)を表わし、Δt
p はプリピット底部の該記録層の膜厚とプリピット間
部の該記録層の膜厚との差(nm)を表わし、dg は
プリグルーブの深さ(nm)を表わし、Δtg はプリ
グルーブ底部の該記録層の膜厚とプリグルーブ間部の該
記録層の膜厚との差(nm)を表わし、そしてλは再生
時に使用するレーザーの波長を表わす。]を満足するこ
とを特徴とする情報記録媒体。
Claim 1: A recording layer capable of recording information using a laser and a reflective layer are provided on a disk-shaped substrate having a read-only area consisting of pre-pits and a recordable area consisting of pre-grooves on the surface thereof. In the information recording medium provided in this order, the relationship between the depth of the prepits and the thickness of the recording layer is expressed by the following formula (I): 0.15λ≦ns dp −nd Δtp
≦0.24λ (I), and the relationship between the depth of the pregroove and the thickness of the recording layer is expressed by the following formula (II): 0.02λ≦ns dg −nd Δtg
≦0.08λ (II) [However, ns represents the refractive index of the substrate, nd represents the refractive index of the recording layer, dp represents the depth of prepits (nm), and Δt
p represents the difference (nm) between the thickness of the recording layer at the bottom of the pre-pits and the thickness of the recording layer between the pre-pits, dg represents the depth (nm) of the pre-groove, and Δtg represents the difference (nm) between the thickness of the recording layer at the bottom of the pre-pits and the thickness of the recording layer between the pre-pits. It represents the difference (nm) between the thickness of the recording layer and the thickness of the recording layer between the pregrooves, and λ represents the wavelength of the laser used during reproduction. ] An information recording medium characterized by satisfying the following.
【請求項2】  該記録層が、色素からなる層である請
求項1に記載の情報記録媒体。
2. The information recording medium according to claim 1, wherein the recording layer is a layer made of a dye.
JP3135524A 1991-05-10 1991-05-10 Information recording medium Withdrawn JPH04335223A (en)