[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP7266036B2 - Temporary fixing substrate, temporary fixing method, and method for manufacturing electronic component - Google Patents

Temporary fixing substrate, temporary fixing method, and method for manufacturing electronic component Download PDF

Info

Publication number
JP7266036B2
JP7266036B2 JP2020532437A JP2020532437A JP7266036B2 JP 7266036 B2 JP7266036 B2 JP 7266036B2 JP 2020532437 A JP2020532437 A JP 2020532437A JP 2020532437 A JP2020532437 A JP 2020532437A JP 7266036 B2 JP7266036 B2 JP 7266036B2
Authority
JP
Japan
Prior art keywords
temporary fixing
substrate
fixing substrate
electronic component
bonding
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2020532437A
Other languages
Japanese (ja)
Other versions
JPWO2020022372A1 (en
Inventor
杉夫 宮澤
勝 野村
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
NGK Insulators Ltd
Original Assignee
NGK Insulators Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by NGK Insulators Ltd filed Critical NGK Insulators Ltd
Publication of JPWO2020022372A1 publication Critical patent/JPWO2020022372A1/en
Application granted granted Critical
Publication of JP7266036B2 publication Critical patent/JP7266036B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、シリコン基板の仮固定基板、仮固定方法および電子部品の製造方法に関するものである。 The present invention relates to a temporary fixing substrate for a silicon substrate, a temporary fixing method, and a method for manufacturing an electronic component.

近年、電子部品の小型化、低背化への要求が強まっており、その製造のためのシリコン基板についても、極端に薄くした状態で用いられるケースが多くなっている。この際、薄くしたシリコン基板は、剛性が不足し、搬送、研削・研磨といったプロセスに耐えられないため、ガラスやセラミックスからなる仮固定基板を用いてシリコン基板を支持する方法が知られている(特許文献1、2、3)。 In recent years, there has been an increasing demand for miniaturization and low-profile electronic components, and silicon substrates for manufacturing such components are often used in an extremely thin state. At this time, since the thinned silicon substrate lacks rigidity and cannot withstand processes such as transportation, grinding, and polishing, a method of supporting the silicon substrate using a temporary fixing substrate made of glass or ceramics is known ( Patent documents 1, 2, 3).

これらの従来技術では、熱硬化性樹脂によってシリコン基板を仮固定基板に対して接着し、冷却した後、シリコン基板を研削・研磨により薄板化する。次いで、さらに表面への多層配線形成等を行い、その後、仮固定基板からシリコン基板を剥がし、所望の寸法にダイシングする。接着層にあらかじめ剥離層を設けておき、仮固定基板側から剥離層に対してレーザー光をあてることで、シリコン基板を仮固定基板から剥離させる。 In these conventional techniques, a silicon substrate is bonded to a temporary fixing substrate with a thermosetting resin, cooled, and then thinned by grinding and polishing. Next, multilayer wiring is formed on the surface, and then the silicon substrate is peeled off from the temporary fixing substrate and diced into desired dimensions. A peeling layer is provided in advance on the adhesive layer, and a laser beam is applied to the peeling layer from the side of the temporary fixing substrate to separate the silicon substrate from the temporary fixing substrate.

シリコン基板を仮固定基板上に熱硬化性樹脂で接着する際、シリコン基板と仮固定基板との熱膨張差によって、接着体に反りが発生する。このため、特許文献2では、支持基板を予め接着体の反りとは逆方向に湾曲させておくことで、接着体の反りを少なくすることが試みられている。支持基板の反りは、加熱変形、研磨方法の変更、加工変質層の除去によって調節している。 When the silicon substrate is adhered to the temporary fixing substrate with a thermosetting resin, the bonded body warps due to the difference in thermal expansion between the silicon substrate and the temporary fixing substrate. Therefore, in Patent Document 2, an attempt is made to reduce the warpage of the adhesive body by previously curving the support substrate in the direction opposite to the warpage of the adhesive body. The warping of the supporting substrate is adjusted by heat deformation, changing the polishing method, and removing the work-affected layer.

特開2011-023438JP 2011-023438 特開2010-058989JP 2010-058989

しかし、熱硬化性樹脂の種類、接着温度、仮固定基板とシリコン基板の厚み、といった条件の制約から、接着後の接着体の湾曲量が大きくなることがある。この場合には、仮固定基板の反対側への初期の湾曲量を、接着体の湾曲量に応じて大きくしておく必要がある。しかし、そうした場合、接合の際に、接合設備での各基板のハンドリングが難しくなったり、接合時の圧力で割れることがあった。また、接着体を得た後、シリコン基板を研削・研磨により薄くすると、接着体の湾曲量はシリコン基板に接着する前の仮固定基板の初期の湾曲量に近づく。このため、接着直後の接着体の湾曲量にくらべて湾曲量が大きくなり、その後のプロセスを実施することが困難となる。 However, due to constraints such as the type of thermosetting resin, the bonding temperature, and the thickness of the temporary fixing substrate and the silicon substrate, the amount of bending of the bonded body after bonding may increase. In this case, it is necessary to increase the initial amount of bending of the temporary fixing substrate toward the opposite side in accordance with the amount of bending of the adhesive body. However, in such a case, handling of the substrates by the bonding equipment becomes difficult during bonding, and the substrates may crack due to the pressure during bonding. Further, when the silicon substrate is thinned by grinding and polishing after obtaining the bonded body, the amount of curvature of the bonded body approaches the initial amount of curvature of the temporary fixing substrate before bonding to the silicon substrate. For this reason, the amount of bending becomes greater than the amount of bending of the bonded body immediately after bonding, making it difficult to carry out subsequent processes.

本発明の課題は、シリコン基板や電子部品チップを接着し、仮固定するための固定面と、固定面の反対側にある底面とを備える仮固定基板において、仮固定基板をシリコン基板や電子部品チップに接着した後の接着体の湾曲量を一層低減できるようにすることである。 An object of the present invention is to provide a temporary fixing substrate having a fixing surface for bonding and temporarily fixing a silicon substrate or an electronic component chip and a bottom surface on the opposite side of the fixing surface, wherein the temporary fixing substrate is a silicon substrate or an electronic component chip. To further reduce the amount of bending of an adhesive body after bonding to a chip.

本発明は、シリコン基板と電子部品チップとの少なくとも一方を接着し、仮固定するための固定面と、前記固定面の反対側にある底面とを備え、セラミックスまたはガラスからなる仮固定基板であって、
外周平板部と、前記外周平板部によって包囲された凹状変形部とを有しており、前記固定面が前記外周平板部において平坦面であることを特徴とする。
The present invention is a temporary fixing substrate made of ceramics or glass, comprising a fixing surface for bonding and temporarily fixing at least one of a silicon substrate and an electronic component chip, and a bottom surface opposite to the fixing surface. hand,
It has an outer peripheral flat plate portion and a recessed deformed portion surrounded by the outer peripheral flat plate portion, and the fixing surface is a flat surface on the outer peripheral flat plate portion.

また、本発明は、前記仮固定基板の前記固定面に前記シリコン基板と電子部品チップとの少なくとも一方を接着して接着体を得る工程、および
前記シリコン層を前記仮固定基板から分離する工程
を有することを特徴とする。
Further, the present invention further comprises a step of bonding at least one of the silicon substrate and the electronic component chip to the fixing surface of the temporary fixing substrate to obtain an adhesive body, and a step of separating the silicon layer from the temporary fixing substrate. characterized by having

また、本発明は、前記仮固定基板の前記固定面に前記シリコン基板を接着して接着体を得る工程、
前記接着体の前記シリコン基板を加工してシリコン基板を薄くし、シリコン層を形成する工程、
前記シリコン層内または前記シリコン層上に電子部品チップを設ける工程、および
前記シリコン層および電子部品チップを前記仮固定基板から分離する工程
を有することを特徴とする、電子部品の製造方法に係るものである。
The present invention also provides a step of bonding the silicon substrate to the fixing surface of the temporary fixing substrate to obtain an adhesive body;
a step of processing the silicon substrate of the adhesive body to thin the silicon substrate and form a silicon layer;
A method for manufacturing an electronic component, comprising the steps of: providing an electronic component chip in or on the silicon layer; and separating the silicon layer and the electronic component chip from the temporary fixing substrate. is.

また、本発明は、前記仮固定基板の前記固定面に前記電子部品チップを接着して接着体を得る工程、および
前記電子部品チップを前記仮固定基板から分離する工程
を有することを特徴とする、電子部品の製造方法に係るものである。
Further, the present invention is characterized by comprising a step of bonding the electronic component chip to the fixing surface of the temporary fixing substrate to obtain an adhesive body, and a step of separating the electronic component chip from the temporary fixing substrate. , and a method for manufacturing an electronic component.

本発明によれば、シリコン基板と電子部品チップとの少なくとも一方を接着し、仮固定するための固定面と、固定面の反対側にある底面とを備え、セラミックスからなる仮固定基板において、仮固定基板の初期の湾曲が同じであっても、仮固定基板をシリコン基板や電子部品チップに接着した後の接着体の湾曲量を一層低減できる。この結果、仮固定基板の初期の湾曲量を過度に大きくしておく必要がなく、接合設備での各基板のハンドリングが容易であり、接合時の圧力で割れることも抑制できる。また、接着体を得た後、例えばシリコン基板を研削・研磨により薄くした後、接着体の湾曲量を小さくでき、この後の接着体のハンドリングも容易となる。 According to the present invention, the temporary fixing substrate comprising a fixing surface for bonding and temporarily fixing at least one of a silicon substrate and an electronic component chip, and a bottom surface on the opposite side of the fixing surface, is made of ceramics. Even if the initial curvature of the fixing substrate is the same, the amount of bending of the adhesive body after bonding the temporary fixing substrate to the silicon substrate or the electronic component chip can be further reduced. As a result, there is no need to excessively increase the amount of initial curvature of the temporarily fixed substrate, each substrate can be easily handled in the bonding equipment, and cracking due to pressure during bonding can be suppressed. Further, after obtaining the bonded body, for example, after thinning the silicon substrate by grinding and polishing, the amount of bending of the bonded body can be reduced, and the subsequent handling of the bonded body is facilitated.

(a)は、接合前のシリコン基板2および仮固定基板1を示し、(b)は、シリコン基板2と仮固定基板1とを接合した接着体を示し、(c)は、接着体のシリコン層2Aを薄くした状態を示す。(a) shows the silicon substrate 2 and the temporary fixing substrate 1 before bonding, (b) shows the bonding body obtained by bonding the silicon substrate 2 and the temporary fixing substrate 1, and (c) shows the silicon substrate of the bonding body. The thinned state of layer 2A is shown. (a)は、シリコン層2A上に配線6を設けた状態を示し、(b)は、仮固定基板1をシリコン基板から分離した状態を示す。(a) shows a state in which the wiring 6 is provided on the silicon layer 2A, and (b) shows a state in which the temporary fixing substrate 1 is separated from the silicon substrate. (a)は、シリコン基板12と、湾曲した仮固定基板11とを示す模式図であり(接合前)、(b)は、シリコン基板12と仮固定基板11とを接合している状態を示し、(c)は、接着体14を示す。(a) is a schematic diagram showing a silicon substrate 12 and a curved temporary fixing substrate 11 (before bonding), and (b) shows a state in which the silicon substrate 12 and the temporary fixing substrate 11 are bonded. , (c) shows the adhesive body 14 . (a)は、接着体のシリコン層14Aを薄くした状態を示し、(b)は、シリコン層14Aと仮固定基板11Aとの接着体を示し、(c)は、シリコン層12Bを仮固定基板11Aから分離した状態を示す。(a) shows the state in which the silicon layer 14A of the adhesive is thinned, (b) shows the adhesive between the silicon layer 14A and the temporary fixing substrate 11A, and (c) shows the silicon layer 12B as the temporary fixing substrate. 11A separated. (a)は、加工前の材料20を示し、(b)は、本発明の実施例に係る仮固定基板21を示し,(c)は仮固定基板21の平面図である。(a) shows a material 20 before processing, (b) shows a temporary fixing substrate 21 according to an embodiment of the present invention, and (c) is a plan view of the temporary fixing substrate 21. FIG. (a)は、シリコン基板22と仮固定基板21とを示す模式図であり(接合前)、(b)は、シリコン基板22と仮固定基板21とを接合している状態を示し、(c)は、接着体23を示す。(a) is a schematic diagram showing the silicon substrate 22 and the temporary fixing substrate 21 (before bonding), (b) shows the state in which the silicon substrate 22 and the temporary fixing substrate 21 are bonded, and (c) ) indicates the adhesive 23 . (a)は、接着体のシリコン基板22Bを薄くした状態を示し、(b)は、シリコン基板22Bと仮固定基板21Aとの接着体を示し、(c)は、シリコン基板22Bを仮固定基板21から分離した状態を示す。(a) shows the state in which the silicon substrate 22B of the bonded body is thinned, (b) shows the bonded body between the silicon substrate 22B and the temporary fixing substrate 21A, and (c) shows the silicon substrate 22B as the temporary fixing substrate. 21 is shown separated. 図8は、平面的に見て長方形状の仮固定基板31を示す模式図である。FIG. 8 is a schematic diagram showing a rectangular temporary fixing substrate 31 when viewed in plan. (a)は、電子部品チップ36を樹脂モールド35によって仮固定した状態を示し、(b)は、光照射によって電子部品36および樹脂モールド35を仮固定基板1から分離した状態を示す。(a) shows a state in which the electronic component chip 36 is temporarily fixed by the resin mold 35, and (b) shows a state in which the electronic component 36 and the resin mold 35 are separated from the temporary fixing substrate 1 by light irradiation.

最初に、図1、図2を参照しつつ、仮固定基板を用いたシリコン基板の仮固定および分離方法について述べる。
まず、図1(a)に示す例では、シリコン基板2の接合面2a側に所定の導体3を設けておく。そして、シリコン基板2の表面2a上に接着層4、剥離層5を設ける。仮固定基板1の接合面1aを剥離層5の表面5aに対向させる。
First, referring to FIGS. 1 and 2, a method for temporarily fixing and separating a silicon substrate using a temporary fixing substrate will be described.
First, in the example shown in FIG. 1A, a predetermined conductor 3 is provided on the bonding surface 2a side of the silicon substrate 2. As shown in FIG. Then, an adhesive layer 4 and a peeling layer 5 are provided on the surface 2a of the silicon substrate 2. As shown in FIG. The bonding surface 1a of the temporary fixing substrate 1 is made to face the surface 5a of the release layer 5. As shown in FIG.

次いで、図1(b)に示すように、シリコン基板2と仮固定基板1とを接合し、接着体を得る。次いで、シリコン基板2の非接合面2bを加工し、図1(c)に示すようにシリコン層2Aを薄くする。2cは加工面である。本例では、シリコン層2Aを薄くした時点で、導体3Aはシリコン層2Aを貫通している。 Next, as shown in FIG. 1(b), the silicon substrate 2 and the temporary fixing substrate 1 are bonded to obtain an adhesive body. Next, the non-bonding surface 2b of the silicon substrate 2 is processed to thin the silicon layer 2A as shown in FIG. 1(c). 2c is a processing surface. In this example, the conductor 3A penetrates the silicon layer 2A when the silicon layer 2A is thinned.

次いで、図2(a)に示すように、シリコン基板2A上に所定の配線層6を形成する。7は、配線層の上に設置するデバイスチップ(電子部品チップ)に給電するための再配線層であり、フォトプロセスやめっき法により形成される。この配線層の上に必要に応じ、複数のデバイスチップを設置(図示せず)し、次いで、仮固定基板側から所定波長およびエネルギーのレーザ光を照射し、剥離層5で仮固定基板1の剥離を生じさせる。これによって、図2(b)に示すように、シリコン層2Aは、接着層4、配線層6とともに仮固定基板から分離され、次の処理工程に供される。 Next, as shown in FIG. 2A, a predetermined wiring layer 6 is formed on the silicon substrate 2A. Reference numeral 7 denotes a rewiring layer for supplying power to a device chip (electronic component chip) placed on the wiring layer, and is formed by photoprocessing or plating. If necessary, a plurality of device chips are placed on the wiring layer (not shown), then a laser beam having a predetermined wavelength and energy is irradiated from the temporary fixing substrate side, and the temporary fixing substrate 1 is separated from the peeling layer 5. Cause delamination. As a result, as shown in FIG. 2(b), the silicon layer 2A is separated from the temporary fixing substrate together with the adhesive layer 4 and the wiring layer 6, and is subjected to the next processing step.

ここで、シリコン基板を仮固定基板上に熱硬化性樹脂で接着する際、シリコン基板と仮固定基板との熱膨張差によって、接着体に湾曲が発生する。このため、図3(a)に示すように、仮固定基板11を、予め接着体の湾曲とは逆方向に湾曲させておく方法が知られている。すなわち、仮固定基板11の接合面11aが凹み、11bが膨らむように、仮固定基板11を湾曲させる。12aは接合面であり、12bは非接合面である。ここで、Lは、仮固定基板11が湾曲していない場合の仮想面であり、Wは湾曲量であるが、接合面が凹んでいる場合にはマイナス符号とし,接合面が突出している場合にはプラス符号とする。 Here, when the silicon substrate is adhered to the temporary fixing substrate with a thermosetting resin, the bonding body is curved due to the difference in thermal expansion between the silicon substrate and the temporary fixing substrate. Therefore, as shown in FIG. 3A, a method is known in which the temporary fixing substrate 11 is preliminarily curved in a direction opposite to that of the bonding body. That is, the temporary fixing substrate 11 is curved so that the bonding surface 11a of the temporary fixing substrate 11 is recessed and the joint surface 11b is bulging. 12a is a bonding surface and 12b is a non-bonding surface. Here, L is a virtual surface when the temporary fixing substrate 11 is not curved, and W is the amount of curvature. is a plus sign.

次いで、図3(b)に示すように、治具13の間に仮固定基板11、シリコン基板12をはさみ、矢印Aのように加圧しながら加熱する。好ましくは仮固定基板11とシリコン基板12との間に、図示しない熱硬化性接着剤を介在させ、効果させることで、仮固定基板11とシリコン基板とを接着する。この時点では、加熱および加圧によって仮固定基板11、シリコン基板12はともに平坦な状態になる。 Next, as shown in FIG. 3(b), the temporary fixing substrate 11 and the silicon substrate 12 are sandwiched between jigs 13, and heated while being pressurized as indicated by arrow A. Next, as shown in FIG. Preferably, a thermosetting adhesive (not shown) is interposed between the temporary fixing substrate 11 and the silicon substrate 12, and is effective to bond the temporary fixing substrate 11 and the silicon substrate. At this point, both the temporary fixing substrate 11 and the silicon substrate 12 are flattened by heating and pressing.

接合が終了すると、図3(c)に示すように、仮固定基板11Aとシリコン基板12Aとの接着体14が得られる。ただし、接着体においては、仮固定基板11Aは、初期とは反対側に反っている。これは、仮固定基板11Aのほうが熱膨張係数がシリコンよりも大きいので、冷却時に矢印Bのように収縮し、この結果、接着体14の全体が反対側に向かって湾曲するからである。湾曲量Wはプラス符号となる。 When the bonding is completed, as shown in FIG. 3(c), an adhesive body 14 of the temporary fixing substrate 11A and the silicon substrate 12A is obtained. However, in the adhesive body, the temporary fixing substrate 11A warps in the opposite direction from the initial state. This is because the temporary fixing substrate 11A has a larger coefficient of thermal expansion than silicon, so it shrinks in the direction of arrow B when cooled, and as a result, the entire bonding body 14 curves toward the opposite side. The amount of curvature W becomes a plus sign.

次いで、図4(a)に示すように、治具15の平坦面15a上に接着体14Aを乗せ、矢印Cのように圧力を加えて接着体を平坦にしつつ加工する。これによって、シリコン基板が薄くなって、薄いシリコン層12Bが形成されるとともに、シリコン層および仮固定基板11Aは平坦化する。次いで,接着体14Aを治具15から取り外すと、図4(b)に示すように接着体14Aは再び湾曲する。ただし、接着体14Aの湾曲量Wは、図3(c)に示すような薄板加工前の湾曲量Wよりも小さくなっており、接合前の仮固定基板の湾曲に近づいている(図3(a))。 Next, as shown in FIG. 4(a), the bonded body 14A is placed on the flat surface 15a of the jig 15, and pressure is applied in the direction of arrow C to flatten the bonded body. As a result, the silicon substrate is thinned to form a thin silicon layer 12B, and the silicon layer and the temporary fixing substrate 11A are flattened. Next, when the bonded body 14A is removed from the jig 15, the bonded body 14A is curved again as shown in FIG. 4(b). However, the amount of curvature W of the adhesive body 14A is smaller than the amount of curvature W before thin plate processing as shown in FIG. a)).

次いで、図4(c)に示すように、仮固定基板からシリコン層を分離する。このとき、仮固定基板11Aの形状は初期形状に戻る傾向がある。一方、シリコン層は薄板化しているので、ほぼ平坦となっている。 Next, as shown in FIG. 4(c), the silicon layer is separated from the temporary fixing substrate. At this time, the shape of the temporary fixing substrate 11A tends to return to the initial shape. On the other hand, since the silicon layer is thinned, it is almost flat.

ここで、図3(a)における仮固定基板11の初期の湾曲量Wをマイナス符号方向に大きく設定しておくことによって、図3(c)に示す接合後の接着体14の湾曲量W(初期と反対のプラス符号)を小さくすることができる。しかし、熱硬化性樹脂の種類、接着温度、仮固定基板とシリコン基板の厚み、といった条件の制約から、接着後の接着体の湾曲量が大きくなることがある(図3(c))。この場合には、仮固定基板の反対側への初期の湾曲量を、接着体の湾曲量に応じて大きくしておく必要がある(図3(a))。しかし、そうした場合、図3(b)に示す接合の際に、接合設備での各基板のハンドリングが難しくなったり、接合時の圧力で割れることがあった。また、接着体を得た後、シリコン基板を研削・研磨により薄くすると、接着体の湾曲量はシリコン基板に接着する前の仮固定基板の初期の湾曲量に近づく(図4(b))。このため、接着直後の接着体の湾曲量にくらべて湾曲量が大きくなり、その後のプロセスを実施することが困難となる。 Here, by setting the initial amount of curvature W of the temporary fixing substrate 11 in FIG. plus sign opposite to the initial) can be decreased. However, due to constraints such as the type of thermosetting resin, the bonding temperature, and the thickness of the temporary fixing substrate and the silicon substrate, the amount of bending of the bonded body after bonding may increase (FIG. 3(c)). In this case, it is necessary to increase the initial amount of bending of the temporary fixing substrate toward the opposite side according to the amount of bending of the adhesive (FIG. 3A). However, in such a case, handling of the substrates in the bonding equipment becomes difficult during the bonding shown in FIG. Further, when the silicon substrate is thinned by grinding and polishing after obtaining the bonded body, the amount of curvature of the bonded body approaches the initial amount of curvature of the temporary fixing substrate before bonding to the silicon substrate (FIG. 4(b)). For this reason, the amount of bending becomes greater than the amount of bending of the bonded body immediately after bonding, making it difficult to carry out subsequent processes.

図5~図8は、本発明の実施例に係るものである。
図5(a)は、仮固定基板の材料20を示す。仮固定基板材料20の厚さ(一対の主面20aと20bとの間隔)は一定である。
5 to 8 relate to an embodiment of the invention.
FIG. 5(a) shows the material 20 of the temporary fixing substrate. The thickness of the temporary fixing substrate material 20 (the distance between the pair of main surfaces 20a and 20b) is constant.

次いで、図5(b)、(c)に示すように、材料20の主面20a側が凹むように変形させ、仮固定基板21を得る。ここで、仮固定基板21の厚さ(一対の主面21aと21bとの間隔)は一定である。仮固定基板21の周縁部には外周平板部21cが設けられており、仮固定基板21の内側に凹状変形部21dが設けられている。外周平板部21cはリング状の平板形状をなしており、図5(a)に示す加工前の形態を維持している。Lは外周平板部21cの主面21a(平坦面21e)に沿った仮想面である。一方、凹状変形部21dは、仮想面Lから下側(主面21b側)へと向かって変形し、凹んでいる。本例では、凹状変形部21dの平面形状は円形である。凹状変形部21bの仮想面Lからの凹みの最大値を湾曲量Wとする。 Next, as shown in FIGS. 5(b) and 5(c), the material 20 is deformed so that the principal surface 20a side is recessed to obtain the temporary fixing substrate 21. Next, as shown in FIG. Here, the thickness of the temporary fixing substrate 21 (the distance between the pair of main surfaces 21a and 21b) is constant. A peripheral flat plate portion 21 c is provided on the peripheral edge portion of the temporary fixing substrate 21 , and a concave deformation portion 21 d is provided inside the temporary fixing substrate 21 . The outer peripheral flat plate portion 21c has a ring-shaped flat plate shape and maintains the shape before processing shown in FIG. 5(a). L is a virtual surface along the main surface 21a (flat surface 21e) of the outer peripheral flat plate portion 21c. On the other hand, the concave deformation portion 21d is deformed downward (toward the main surface 21b) from the imaginary plane L and is concave. In this example, the planar shape of the concave deformation portion 21d is circular. Let the amount of curvature W be the maximum value of the recess from the imaginary plane L of the concave deformation portion 21b.

図6(a)に示す例では、シリコン基板22の接合面22aと仮固定基板21の接合面21aとを対向させる。なお、シリコン基板22の接合面22a側には所定の接着剤層や剥離層を更に形成できる。次いで、図6(b)に示すように、治具13の間に仮固定基板21、シリコン基板22をはさみ、矢印Aのように加圧しながら加熱する。仮固定基板21とシリコン基板22との間には、図示しない熱硬化性接着剤を介在させ、効果させることで、仮固定基板21とシリコン基板22とを接着する。この時点では、加熱および加圧によって仮固定基板21、シリコン基板22はともに平坦な状態になる。 In the example shown in FIG. 6A, the bonding surface 22a of the silicon substrate 22 and the bonding surface 21a of the temporary fixing substrate 21 are opposed to each other. A predetermined adhesive layer or peeling layer can be further formed on the bonding surface 22a side of the silicon substrate 22. FIG. Next, as shown in FIG. 6(b), the temporarily fixed substrate 21 and the silicon substrate 22 are sandwiched between jigs 13, and heated while being pressurized as indicated by arrow A. Next, as shown in FIG. A thermosetting adhesive (not shown) is interposed between the temporary fixing substrate 21 and the silicon substrate 22, and is effective to bond the temporary fixing substrate 21 and the silicon substrate 22 together. At this point, both the temporary fixing substrate 21 and the silicon substrate 22 are flattened by heating and pressing.

接合が終了すると、図6(c)に示すように、仮固定基板21Aとシリコン基板22Aとの接着体23が得られる。ただし、接着体においては、仮固定基板21Aは、初期とは反対側に沿っている。これは、仮固定基板21Aのほうが熱膨張係数がシリコンよりも大きいので、冷却時に矢印Bのように収縮し、この結果、接着体23の全体が反対側に向かって湾曲するからである。 When the bonding is completed, as shown in FIG. 6(c), an adhesive body 23 of the temporary fixing substrate 21A and the silicon substrate 22A is obtained. However, in the bonded body, the temporary fixing substrate 21A is along the side opposite to the initial one. This is because the temporary fixing substrate 21A has a larger coefficient of thermal expansion than silicon, so it shrinks in the direction of arrow B when cooled, and as a result, the entire bonding body 23 curves toward the opposite side.

次いで、図7(a)に示すように、治具15の平坦面15a上に接着体23を乗せ、矢印Cのように圧力を加えて接着体を平坦にしつつ加工する。これによって、シリコン基板22Aが薄くなって、薄いシリコン層22Bが形成されるとともに、シリコン層および仮固定基板は平坦化する。22cは加工面である。次いで,接着体23Aを治具15から取り外すと、図7(b)に示すように接着体23Aは再び湾曲する。ただし、仮固定基板は、初期の形状に近づいている。すなわち、接着体23Aの湾曲量Wは、図6(c)に示すような薄板加工前の湾曲量Wよりも小さくなっており、接合前の仮固定基板の形状に近づいている。 Next, as shown in FIG. 7(a), the bonded body 23 is placed on the flat surface 15a of the jig 15, and pressure is applied in the direction of arrow C to flatten the bonded body. As a result, the silicon substrate 22A is thinned to form a thin silicon layer 22B, and the silicon layer and the temporary fixing substrate are flattened. 22c is a processing surface. Next, when the bonded body 23A is removed from the jig 15, the bonded body 23A is curved again as shown in FIG. 7(b). However, the temporary fixing substrate is close to the initial shape. That is, the amount of curvature W of the adhesive body 23A is smaller than the amount of curvature W before thin plate processing as shown in FIG. 6C, and approaches the shape of the temporary fixing substrate before bonding.

次いで、図7(c)に示すように、仮固定基板からシリコン層22Bを分離する。このとき、仮固定基板21の形状は初期形状に戻る傾向がある。一方、シリコン基板は薄板化しているので、ほぼ平坦となっている。 Next, as shown in FIG. 7C, the silicon layer 22B is separated from the temporary fixing substrate. At this time, the shape of the temporary fixing substrate 21 tends to return to the initial shape. On the other hand, since the silicon substrate is thinned, it is almost flat.

ここで、本発明においては、図6(a)に示すように、仮固定基板の初期の湾曲量が同じであっても、仮固定基板をシリコン基板に接着したときに(図6(b)参照)、外周平板部21cは変形せず、凹状変形部21dのみが治具13によって平坦に変形する。そして、外周平板部はリング状をなしており、凹状変形部を包囲していることから、仮固定基板の形状が大きく変形しないようなアンカーとして作用する。この結果、接着体23を治具13から取り外した後の湾曲量を低減できる(図6(c)参照)。 Here, in the present invention, as shown in FIG. 6(a), even if the amount of initial curvature of the temporary fixing substrate is the same, when the temporary fixing substrate is bonded to the silicon substrate (FIG. 6(b)) ), the outer peripheral flat plate portion 21 c is not deformed, and only the concave deformation portion 21 d is flattened by the jig 13 . Since the outer peripheral flat plate portion is ring-shaped and surrounds the concave deformation portion, it acts as an anchor to prevent the shape of the temporarily fixed substrate from being greatly deformed. As a result, it is possible to reduce the amount of bending after the bonded body 23 is removed from the jig 13 (see FIG. 6(c)).

この結果、仮固定基板の初期の湾曲量が同等であっても、接着体23を治具13から取り外した後の湾曲量を低減できる。また、接着体23を治具13から取り外した後の湾曲量が同等である場合には、仮固定基板の初期の湾曲量を低減できる。ゆえに、接合設備での各基板のハンドリングが容易であり、接合時の圧力で割れることも抑制できる。また、接着体を得た後、シリコン基板を研削・研磨により薄くした後(図7(b)参照))、接着体23Aの湾曲量を小さくでき、この後の接着体のハンドリングも容易となる。 As a result, even if the initial amount of bending of the temporarily fixed substrate is the same, the amount of bending after removing the bonding body 23 from the jig 13 can be reduced. In addition, when the amount of bending after removing the adhesive body 23 from the jig 13 is the same, the amount of initial bending of the temporarily fixed substrate can be reduced. Therefore, each substrate can be easily handled in bonding equipment, and cracking due to pressure during bonding can be suppressed. In addition, after obtaining the bonded body and thinning the silicon substrate by grinding and polishing (see FIG. 7(b)), the amount of bending of the bonded body 23A can be reduced, and the subsequent handling of the bonded body is facilitated. .

以下、本発明の仮固定基板を電子部品チップの接着に利用した実施形態について述べる。
まず、仮固定基板の前記固定面に電子部品を接着し、樹脂モールドによって仮固定する。例えば、図9(a)に示すように、仮固定基板1の固定面1a上に接着剤層を設ける。こうした接着剤としては、両面テープやホットメルト系の接着剤などを例示できる。また、接着剤層を仮固定基板上に設ける方法としては、ロール塗布、スプレー塗布、スクリーン印刷、スピンコートなど種々の方法を採用できる。
Embodiments in which the temporary fixing substrate of the present invention is used for bonding electronic component chips will be described below.
First, an electronic component is adhered to the fixing surface of the temporary fixing substrate and temporarily fixed by resin molding. For example, as shown in FIG. 9A, an adhesive layer is provided on the fixing surface 1a of the temporary fixing substrate 1. As shown in FIG. Examples of such adhesives include double-sided tapes and hot-melt adhesives. Various methods such as roll coating, spray coating, screen printing, and spin coating can be employed as methods for providing the adhesive layer on the temporary fixing substrate.

次いで、仮固定基板1上に多数の電子部品36を設置し、接着剤層を硬化させて接着層34を形成する。この硬化工程は、接着剤の性質に合わせて行うが、加熱、紫外線照射を例示できる。 Next, a large number of electronic components 36 are placed on the temporary fixing substrate 1 and the adhesive layer is cured to form the adhesive layer 34 . This curing step is carried out according to the properties of the adhesive, and heating and ultraviolet irradiation can be exemplified.

次いで、液状の樹脂モールド剤を流し込み、樹脂モールド剤を硬化させる。これによって、図9(a)に示すように、樹脂モールド35内に電子部品36を固定する。ただし、35bは、電子部品の隙間37を充填する樹脂であり、35aは、電子部品を被覆する樹脂である。
モールド樹脂としては、エポキシ系樹脂、ポリイミド系樹脂、ポリウレタン系樹脂、ウレタン系樹脂などが挙げられる。
Next, a liquid resin molding agent is poured and cured. As a result, the electronic component 36 is fixed inside the resin mold 35, as shown in FIG. 9(a). However, 35b is a resin that fills the gap 37 of the electronic component, and 35a is a resin that covers the electronic component.
Examples of molding resins include epoxy resins, polyimide resins, polyurethane resins, and urethane resins.

次いで、矢印Aに示すように、仮固定基板1の底面1b側から光を照射することによって、仮固定基板1から電子部品36および樹脂モールド35を分離する(図9(b)参照)。
仮固定基板の底面側から照射する光の波長は電子部品や樹脂モールドの種類によって適宜変更するが、例えば200nm~400nmとすることができる。
Next, as indicated by arrow A, the electronic component 36 and the resin mold 35 are separated from the temporary fixing substrate 1 by irradiating light from the bottom surface 1b side of the temporary fixing substrate 1 (see FIG. 9B).
The wavelength of the light irradiated from the bottom side of the temporary fixing substrate can be appropriately changed depending on the type of electronic component or resin mold, and can be, for example, 200 nm to 400 nm.

以下、本発明の各構成要素について更に述べる。
仮固定基板の材質は、機械的強度および薬品に対する耐久性の点からセラミックスが好ましく、アルミナ、窒化アルミニウム、YAG、サイアロン、スピネルが特に好ましい。
Each component of the present invention will be further described below.
The material of the temporary fixing substrate is preferably ceramics in terms of mechanical strength and durability against chemicals, and particularly preferably alumina, aluminum nitride, YAG, sialon, and spinel.

好適な実施形態においては、仮固定基板を構成する材料が透光性アルミナである。この場合、好ましくは純度99.9%以上(好ましくは99.95%以上)の高純度アルミナ粉末に対して、100ppm以上、300ppm以下の酸化マグネシウム粉末を添加する。このような高純度アルミナ粉末としては、大明化学工業株式会社製の高純度アルミナ粉体を例示できる。また、この酸化マグネシウム粉末の純度は99.9%以上が好ましく、平均粒径は50μm以下が好ましい。 In a preferred embodiment, the material constituting the temporary fixing substrate is translucent alumina. In this case, 100 ppm or more and 300 ppm or less of magnesium oxide powder is added to high-purity alumina powder of preferably 99.9% or more (preferably 99.95% or more) purity. As such a high-purity alumina powder, a high-purity alumina powder manufactured by Taimei Chemical Industry Co., Ltd. can be exemplified. The magnesium oxide powder preferably has a purity of 99.9% or more and an average particle size of 50 μm or less.

また、好適な実施形態においては、焼結助剤として、アルミナ粉末に対して、ジルコニア(ZrO)を200~800ppm、イットリア(Y)を10~30ppm添加することが好ましい。In a preferred embodiment, 200 to 800 ppm of zirconia (ZrO 2 ) and 10 to 30 ppm of yttria (Y 2 O 3 ) are preferably added to the alumina powder as sintering aids.

仮固定基板の成形方法は特に限定されず、ドクターブレード法、押し出し法、モールドキャスト法など任意の方法であってよい。特に好ましくは、ベース基板をドクタープレード法を用いて製造する。 A method for molding the temporary fixing substrate is not particularly limited, and may be any method such as a doctor blade method, an extrusion method, or a mold casting method. Particularly preferably, the base substrate is manufactured using a doctor blade method.

好適な実施形態においては、セラミック粉末、分散媒および結合剤を含むスラリーを製造し、このスラリーをドクターブレード法によりテープ状に成型し、これを所望の厚さ形状になるように積層、打ち抜きすることで成形体を得る。 In a preferred embodiment, a slurry containing ceramic powder, a dispersion medium and a binder is prepared, the slurry is formed into a tape shape by a doctor blade method, and the tape is laminated to a desired thickness and punched out. A compact is obtained in this way.

次いで、成形体を乾燥し、好ましくは大気中で仮焼し、次いで、水素中で本焼成する。本焼成時の焼結温度は、焼結体の緻密化という観点から、1700~1900℃が好ましく、1750~1850℃が更に好ましい。この焼結体をダイヤラップ等により表面研磨を行い、厚さムラを一定以下となるように調整するとともに、両面を鏡面化する。 The compact is then dried, preferably calcined in air, and then calcined in hydrogen. The sintering temperature during main firing is preferably 1700 to 1900° C., more preferably 1750 to 1850° C., from the viewpoint of densification of the sintered body. The surface of this sintered body is polished with a dial wrap or the like to adjust the thickness unevenness to a certain level or less, and both surfaces are mirror-finished.

このように焼成時に十分に緻密な焼結体を生成させた後に、厚さムラの調整、表面を鏡面化した上でアニール処理を実施することで精度よく湾曲量の調整を行うことができる。このアニール温度は、変形や異常粒成長発生を防止するといった観点から1700℃以下であることが好ましく、最高温度が1600℃以下であることが更に好ましい。一方で焼結体のクリープ変形を十分に行い、湾曲量を精度よく調整するためには1200℃以上が好ましく、1400℃以上であることが更に好ましい。また、アニール時間は、1~6時間であることが好ましい。 After generating a sufficiently dense sintered body at the time of firing in this way, the amount of curvature can be adjusted with high accuracy by adjusting the thickness unevenness, mirror-finishing the surface, and performing annealing treatment. From the viewpoint of preventing deformation and abnormal grain growth, the annealing temperature is preferably 1700° C. or lower, and more preferably the maximum temperature is 1600° C. or lower. On the other hand, the temperature is preferably 1200° C. or higher, more preferably 1400° C. or higher, in order to sufficiently perform creep deformation of the sintered body and adjust the amount of curvature with high precision. Also, the annealing time is preferably 1 to 6 hours.

また、仮固定基板を構成するガラスは、珪酸塩系ガラスや硼珪酸塩系ガラスであってよい。 Further, the glass constituting the temporary fixing substrate may be silicate-based glass or borosilicate-based glass.

本発明の仮固定基板は、外周平板部と、外周平板部によって包囲された凹状変形部とを有しており、前記固定面が前記外周平板部において平坦面である。ここで、外周平板部の幅F(図5(b)、(c)参照)は、仮固定基板21の幅Rの4%以上であることが好ましく、これによって接着体の湾曲量を抑制する効果が高くなる。この観点からは、外周平板部の幅Fは、仮固定基板21の幅Rの8%以上であることが更に好ましく、10%以上であることが特に好ましい。 The temporary fixing substrate of the present invention has an outer peripheral flat plate portion and a concave deformed portion surrounded by the outer peripheral flat plate portion, and the fixing surface is a flat surface in the outer peripheral flat plate portion. Here, the width F of the outer peripheral flat plate portion (see FIGS. 5B and 5C) is preferably 4% or more of the width R of the temporary fixing substrate 21, thereby suppressing the amount of bending of the adhesive body. more effective. From this point of view, the width F of the outer peripheral plate portion is more preferably 8% or more of the width R of the temporary fixing substrate 21, and particularly preferably 10% or more.

また、外周平板部の幅Fは、仮固定基板21の幅Rの60%以下であることが好ましく、これによって接着体の湾曲量を抑制する効果が高くなる。この観点からは、外周平板部の幅Fは、仮固定基板21の幅Rの40%以下であることが更に好ましく、30%以下であることが特に好ましい。 Further, the width F of the outer peripheral flat plate portion is preferably 60% or less of the width R of the temporary fixing substrate 21, thereby enhancing the effect of suppressing the amount of bending of the adhesive body. From this point of view, the width F of the outer peripheral plate portion is more preferably 40% or less of the width R of the temporary fixing substrate 21, and particularly preferably 30% or less.

なお、仮固定基板の幅Rは、仮固定基板を平面的に横断する線分の長さである。また、外周平板部の幅Fは、仮固定基板を平面的に横断する前記線分のうち、前記外周平板部を横断する線分の長さの合計値である。例えば、図5(c)に示すような平面図においては、仮固定基板の幅方向の2箇所の外周平板部の幅はそれぞれF/2であるが、この場合には外周平板部の幅は、(F/2+F/2)=Fとなる。 Note that the width R of the temporary fixing substrate is the length of a line segment crossing the temporary fixing substrate in plan view. The width F of the outer peripheral flat plate portion is the sum of the lengths of the line segments crossing the outer peripheral flat plate portion among the line segments crossing the temporary fixing substrate in plan view. For example, in the plan view shown in FIG. 5(c), the widths of the two outer peripheral flat plate portions in the width direction of the temporary fixing substrate are each F/2. , (F/2+F/2)=F.

また、仮固定基板を横断する線分の方向によっては仮固定基板の幅R、外周平板部の幅Fが変化する場合がある。例えば図8に示す例では、仮固定基板31の平面形状が長方形であり、仮固定基板31の厚さ(主面31aと反対側の主面との間隔)は一定である。仮固定基板31の周縁部には外周平板部31cが設けられており、外周平板部31cの内側に凹状変形部31dが設けられている。外周平板部31cは平板形状をなしており、外周平板部31の主面31aは平坦面31eを構成している。凹状変形部31dは、仮想面から下側へと向かって変形し、凹んでいる。本例では、凹状変形部31dの平面形状は長方形である。例えば、仮固定基板の平面形状が長方形である場合には、縦方向の幅R2と横方向の幅R1とは異なっている上、縦方向の外周平板部の幅F2(F2/2+F2/2)と横方向の外周平板部の幅F1(F1/2+F1/2)とが異なる場合がある。この場合には、縦方向と横方向とで(外周平板部の幅/仮固定基板の幅(F1/R1、F2/R2)がそれぞれ4~60%であることが好ましい。 Further, the width R of the temporary fixing substrate and the width F of the peripheral flat plate portion may change depending on the direction of the line segment crossing the temporary fixing substrate. For example, in the example shown in FIG. 8, the planar shape of the temporary fixing substrate 31 is rectangular, and the thickness of the temporary fixing substrate 31 (the distance between the main surface 31a and the opposite main surface) is constant. An outer peripheral flat plate portion 31c is provided on the peripheral edge portion of the temporary fixing substrate 31, and a concave deformation portion 31d is provided inside the outer peripheral flat plate portion 31c. The outer peripheral flat plate portion 31c has a flat plate shape, and the main surface 31a of the outer peripheral flat plate portion 31 forms a flat surface 31e. The concave deformation portion 31d is deformed downward from the imaginary plane and is concave. In this example, the planar shape of the concave deformation portion 31d is a rectangle. For example, when the planar shape of the temporary fixing substrate is rectangular, the width R2 in the vertical direction is different from the width R1 in the horizontal direction, and the width F2 (F2/2+F2/2) of the peripheral flat plate portion in the vertical direction is and the lateral width F1 (F1/2+F1/2) of the outer peripheral plate portion may differ. In this case, it is preferable that (the width of the peripheral flat plate portion/the width of the temporary fixing substrate (F1/R1, F2/R2)) be 4 to 60% in the vertical direction and the horizontal direction.

接合前の仮固定基板においては、凹状変形部の湾曲量Wが0.1mm以上であることが好ましく、これによって接着体の湾曲量を抑制できる。この観点からは、凹状変形部の湾曲量Wは0.3mm以上であることが更に好ましく、0.6mm以上であることが特に好ましい。 In the temporarily fixed substrate before bonding, the amount of curvature W of the concave deformation portion is preferably 0.1 mm or more, thereby suppressing the amount of curvature of the adhesive body. From this point of view, the curvature amount W of the concave deformation portion is more preferably 0.3 mm or more, and particularly preferably 0.6 mm or more.

また、凹状変形部の形状については、断面における輪郭を、円弧状、放物線状、円錐状、皿状とすることができる。ただし、湾曲量の抑制を効果的に行うためには、凹状変形部の断面における輪郭が放物線状であることが好ましい。また、外周平坦部と湾曲部の境界部分を緩やかにする(曲率半径Rを大きくする)ことで、シリコン基板と接着する際、クラックの発生を抑制することができる。 As for the shape of the concave deformed portion, the cross-sectional contour can be arc-shaped, parabolic, conical, or dish-shaped. However, in order to effectively suppress the amount of curvature, it is preferable that the cross-sectional contour of the concave deformation portion is parabolic. Further, by making the boundary portion between the outer peripheral flat portion and the curved portion gentle (increasing the radius of curvature R), it is possible to suppress the occurrence of cracks when bonding to the silicon substrate.

また、接合前の仮固定基板においては、凹状変形部の湾曲量が2.5mm以下であることが好ましく、これによって接合装置内へのハンドリングの問題が抑えられ、また接合時の破損を防止し易い。この観点からは、凹状変形部の湾曲量は2.0mm以下であることが好ましく、1.0mm以下であることが更に好ましい。 In addition, in the temporarily fixed substrate before bonding, it is preferable that the amount of curvature of the concave deformation portion is 2.5 mm or less. easy. From this point of view, the amount of curvature of the concave deformation portion is preferably 2.0 mm or less, more preferably 1.0 mm or less.

このとき、仮固定基板全体における厚みムラ(いわゆるTTV)が大きいと、シリコン基板や電子部品チップとの貼り合わせの際、接着層の厚みムラが発生し、接着後の変形の原因となるため、厚みムラは10um以下が好ましい。また、接着されたシリコン基板や電子部品チップに高精度の配線形成を行う場合、厚みムラは5um以下が好ましく、3um以下であることが更に好ましい。 At this time, if the thickness unevenness (so-called TTV) in the entire temporary fixing substrate is large, the thickness unevenness of the adhesive layer occurs when the silicon substrate and the electronic component chip are bonded together, causing deformation after bonding. Thickness unevenness is preferably 10 μm or less. Further, when highly accurate wiring is formed on a bonded silicon substrate or electronic component chip, the thickness unevenness is preferably 5 μm or less, more preferably 3 μm or less.

なお、凹状変形部の湾曲量は以下のようにして測定する。すなわち、外周平板部の固定面(平坦面)を凹状変形部上に延長することで仮想面Lを得る。そして、仮想面Lから見て凹状変形部のうちら最も深い部分の深さを湾曲量Wと定義する。また、具体的な測定装置としては、平坦なテーブル上に設置した基板の形状をレーザー測長機で計測することで可能となる。 The amount of curvature of the concave deformed portion is measured as follows. That is, the imaginary surface L is obtained by extending the fixing surface (flat surface) of the outer peripheral plate portion onto the concave deformation portion. Then, the depth of the deepest portion of the concave deformed portion as viewed from the imaginary plane L is defined as the amount of curvature W. As shown in FIG. As a specific measuring device, it is possible to measure the shape of a substrate placed on a flat table with a laser length measuring machine.

仮固定基板とシリコン基板等のそれぞれの平面形状、平面寸法は特に限定されない。仮固定基板とシリコン基板等とは、互いに同じ平面形状、平面寸法を有していてもよいし、異なる平面形状、平面寸法を有していてもよい。具体的には、例えば、仮固定基板、シリコン基板等のそれぞれは、円板状であってもよいし、矩形状、長円状、楕円状、三角形状、多角形状などであってもよい。なかでも、仮固定基板とシリコン基板のそれぞれが、円板状、正多角形状である場合のように、点対称であることが好ましく、円板状であることがさらに好ましい。この場合は、点対称軸を中心として各方位で均等に熱収縮が生じる。 The planar shapes and planar dimensions of the temporary fixing substrate and the silicon substrate are not particularly limited. The temporary fixing substrate and the silicon substrate or the like may have the same planar shape and planar dimensions, or may have different planar shapes and planar dimensions. Specifically, for example, each of the temporary fixing substrate, the silicon substrate, and the like may be disk-shaped, rectangular, oval, elliptical, triangular, polygonal, or the like. In particular, it is preferable that the temporary fixing substrate and the silicon substrate are point-symmetrical, such as a disk shape or a regular polygonal shape, and more preferably a disk shape. In this case, thermal contraction occurs evenly in each azimuth around the axis of point symmetry.

なお、仮固定基板、シリコン基板等が円板状である場合は、その直径(幅)は、100~300mmとすることが好ましい。シリコン基板にオリフラやノッチが形成されている場合、仮固定基板にも同様のオリフラやノッチを形成すると、接着の際の位置決めがしやすく、接着ズレ不良を低減することができる。また、仮固定基板、シリコン基板が正方形または長方形である場合は、その一辺の長さは、100~1000mmとすることが好ましい。この場合、角部はRまたはC形状とすることが、接着後の湾曲量を抑制するとの観点から好ましい。 When the temporary fixing substrate, the silicon substrate, or the like is disc-shaped, the diameter (width) is preferably 100 to 300 mm. When orientation flats and notches are formed on the silicon substrate, forming similar orientation flats and notches on the temporary fixing substrate facilitates positioning during adhesion and reduces adhesion misalignment. Further, when the temporary fixing substrate and the silicon substrate are square or rectangular, the length of one side is preferably 100 to 1000 mm. In this case, it is preferable to form the corners in an R or C shape from the viewpoint of suppressing the amount of bending after bonding.

仮固定基板の厚さは、例えば、0.2~5.0mmであることが好ましく、0,5~2.0mmであることが更に好ましい。これを0.2mm以上とすることによって、接着後の反り抑制がし易くなるとともに、仮固定基板の破損を防止し易くなる。また、これを5.0mm以下とすることによって、基板重量が抑えられ、搬送がしやすくなる。 The thickness of the temporary fixing substrate is, for example, preferably 0.2 to 5.0 mm, more preferably 0.5 to 2.0 mm. By setting this to 0.2 mm or more, it becomes easy to suppress warpage after bonding, and it becomes easy to prevent breakage of the temporarily fixed substrate. Further, by setting this to 5.0 mm or less, the weight of the substrate can be suppressed and the transportation becomes easier.

仮固定基板とシリコン基板等とを熱硬化性樹脂を用いて接合する場合は、仮固定基板とシリコン基板等とを重ね合わせて加圧固定した状態で加熱して熱硬化性接着剤を硬化させることにより、接着体を得る。 When the temporary fixing substrate and the silicon substrate or the like are bonded using a thermosetting resin, the temporary fixing substrate and the silicon substrate or the like are superimposed and pressurized and fixed, and heated to cure the thermosetting adhesive. Thus, an adherent is obtained.

仮固定基板とシリコン基板等とを接着する接着剤としては、熱硬化性樹脂の他、UV(紫外線硬化型)接着剤、両面テープやホットメルト系の接着剤などを例示できる。また、接着剤を仮固定基板上に設ける方法としては、ロール塗布、スプレー塗布、スクリーン印刷、スピンコートなど種々の方法を採用できる。 Examples of adhesives for bonding the temporary fixing substrate and the silicon substrate include thermosetting resins, UV (ultraviolet curable) adhesives, double-sided tapes, hot-melt adhesives, and the like. Moreover, various methods such as roll coating, spray coating, screen printing, and spin coating can be employed as the method of providing the adhesive on the temporary fixing substrate.

また、接着層と仮固定基板との間に剥離層を形成することが好ましい。こうした剥離層としては、レーザー光の照射により剥離層が炭化して剥離するレーザー剥離型のものに加え、UV光の照射により失活し、粘着性が失われ剥離するUV剥離型のもの、加熱により層内の成分が発泡し剥離する加熱剥離型のものも採用できる。 Moreover, it is preferable to form a release layer between the adhesive layer and the temporary fixing substrate. As such a release layer, in addition to the laser release type in which the release layer is carbonized and peeled off by laser light irradiation, the UV release type in which the release layer is deactivated by UV light irradiation, loses its adhesiveness and peels off, and is heated. It is also possible to employ a heat-peeling type in which the components in the layer are foamed and peeled off.

本発明のシリコン基板には、各種電子部品構造を作製できる。例えばCCDやCMOSを作製する場合は、仮固定基板にシリコン基板を接合した後に、シリコン基板を薄くし、次いで薄膜形成工程及びパターニング工程を行うことによって配線層を形成する。この際、仮固定基板とシリコン基板との接着体の湾曲が大きいと、パターニング工程において、微細な配線構造を高精度にパターニングすることが難しいため、本発明は特に有用である。 Various electronic component structures can be fabricated on the silicon substrate of the present invention. For example, when manufacturing a CCD or a CMOS, a wiring layer is formed by bonding a silicon substrate to a temporary fixing substrate, thinning the silicon substrate, and then performing a thin film forming process and a patterning process. At this time, if the bonding body between the temporary fixing substrate and the silicon substrate has a large curvature, it is difficult to pattern a fine wiring structure with high precision in the patterning process, so the present invention is particularly useful.

また、シリコン基板上に電子部品チップを設置し、各電子部品チップと配線層とを電気的に接続することができる。そして、シリコン基板を仮固定基板から分離した後に、シリコン基板を割断することによって、各電子部品チップを分離することができる。 Also, electronic component chips can be placed on a silicon substrate, and each electronic component chip can be electrically connected to the wiring layer. After the silicon substrate is separated from the temporary fixing substrate, the electronic component chips can be separated by cutting the silicon substrate.

また、本発明は、いわゆるFOWLP技術に対して好適に適用できる。FOWLP技術においては、電子部品チップを一旦サポートウェハー(仮固定基板)上に再配置し、樹脂モールドで封止した後、樹脂モールドの表面に配線を形成し、次いで電子部品チップおよびモールド樹脂をサポートウェハー(仮固定基板)から剥離することで、薄型構造の実現が可能となる。そして、樹脂モールドおよびこれに封止された電子部品チップを仮固定基板から分離した後に、樹脂モールドを割断し、各電子部品チップをそれぞれ分離することができる。この場合においても、仮固定基板上で電子部品チップの樹脂封止、配線形成を行った際に各部材のとの熱膨張差によって生じる接着体の湾曲が問題となるが、本発明を用いることでこれを改善することができる。 Also, the present invention can be suitably applied to so-called FOWLP technology. In FOWLP technology, electronic component chips are once relocated on a support wafer (temporary fixed substrate), sealed with a resin mold, wiring is formed on the surface of the resin mold, and then the electronic component chips and mold resin are supported. A thin structure can be realized by peeling from the wafer (temporary fixing substrate). Then, after the resin mold and the electronic component chips sealed therewith are separated from the temporary fixing substrate, the resin mold can be cut to separate the respective electronic component chips. Even in this case, when the electronic component chip is resin-sealed and the wiring is formed on the temporary fixing substrate, there is a problem of the bending of the adhesive due to the difference in thermal expansion between the members. can improve this.

また、仮固定基板に接着する電子部品を大面積化した場合には、仮固定基板と電子部品チップとの熱膨張差によって生じる接着体の湾曲が問題となるが、本発明を用いることでこれを改善することができる。特に仮固定基板の面積に対する電子部品チップが占める面積が60%を超えるとこの傾向が顕著となるため、本発明が有用である。 Further, when the electronic component to be adhered to the temporary fixing substrate has a large area, there is a problem of bending of the adhesive due to the difference in thermal expansion between the temporary fixing substrate and the electronic component chip. can be improved. In particular, when the area occupied by the electronic component chip exceeds 60% of the area of the temporary fixing substrate, this tendency becomes remarkable, so the present invention is useful.

仮固定基板に外周平板部と凹状変形部とを形成する際には、外周平板部に適合する平坦部と凹状変形部に適合する突起とを有する治具を準備し、仮固定基板を加熱しながら治具を押しつけることによって塑性変形させる。あるいは、同様の平坦部と突起とを有する金型中に平板を収容し、加熱しながら金型を押圧することで、外周平板部と凹状変形部とを形成できる。 When forming the peripheral flat plate portion and the concave deformation portion on the temporary fixing substrate, a jig having a flat portion that fits the peripheral flat plate portion and a protrusion that fits the concave deformation portion is prepared, and the temporary fixing substrate is heated. It is plastically deformed by pressing the jig while pressing. Alternatively, by placing a flat plate in a mold having similar flat portions and protrusions and pressing the mold while heating, the outer peripheral flat plate portion and the recessed deformation portion can be formed.

シリコン基板を加工によって薄くする際には、グラインダーを用いることができる。すなわち、仮固定基板とシリコン基板の接着体の、仮固定基板側をバキュームチャック等で固定し、シリコン基板側を研削砥石で加工することで、所望の厚さとすることができる。 A grinder can be used when thinning the silicon substrate by processing. That is, a desired thickness can be obtained by fixing the temporarily fixed substrate side of the bonded body of the temporarily fixed substrate and the silicon substrate with a vacuum chuck or the like and processing the silicon substrate side with a grinding wheel.

(実施例1~7)
以下の成分を混合したスラリーを調製した。
(原料粉末)
・純度99.99%のα-アルミナ粉末 100質量部
・MgO(マグネシア) 250ppm
・ZrO2(ジルコニア) 400ppm
・Y2O3(イットリア) 15ppm
(分散媒)
・2-エチルヘキサノール 45質量部
(結合剤)
・PVB樹脂 4質量部
(分散剤)
・高分子界面活性剤 3質量部
(可塑剤)
・DOP 0.1質量部
(Examples 1 to 7)
A slurry was prepared by mixing the following ingredients.
(Raw material powder)
・ 100 parts by mass of α-alumina powder with a purity of 99.99% ・ MgO (magnesia) 250 ppm
・ZrO2 (zirconia) 400 ppm
・Y2O3 (yttria) 15 ppm
(dispersion medium)
・ 45 parts by mass of 2-ethylhexanol (binder)
PVB resin 4 parts by mass (dispersant)
Polymeric surfactant 3 parts by mass (plasticizer)
・DOP 0.1 part by mass

このスラリーを、ドクターブレード法を用いて焼成後の厚さに換算して0.7mmとなるようテープ状に成形し、焼成後の大きさに換算してφ300mmとなるよう切断した。得られた粉末成形体を、大気中1240℃で仮焼(予備焼成)の後、基板をモリブデン製の板に載せ、水素3:窒素1の雰囲気中で、1800℃で2.5時間保持し、焼成を行った。その後、グラインダーによる研削、ダイヤモンド砥粒によるラップ、CMPリキッドによる研磨を順に行い、厚さ0.6mmの仮固定基板材料20を得た(図5(a))。 This slurry was formed into a tape shape using a doctor blade method so that the thickness after firing was 0.7 mm, and the tape was cut to have a size of φ300 mm after firing. After calcining (pre-firing) the obtained powder compact at 1240° C. in the atmosphere, the substrate was placed on a molybdenum plate and held at 1800° C. for 2.5 hours in an atmosphere of hydrogen 3:nitrogen 1. , was fired. Thereafter, grinding with a grinder, lapping with diamond abrasive grains, and polishing with CMP liquid were performed in order to obtain a temporary fixing substrate material 20 having a thickness of 0.6 mm (FIG. 5(a)).

次いで、材料20を所定の形状の冶具に挟み、1600℃の温度で熱処理し、変形させることで、仮固定基板21を得た(図5(b)(c)参照)。 Next, the material 20 was sandwiched between jigs of a predetermined shape, heat-treated at a temperature of 1600° C., and deformed to obtain a temporary fixing substrate 21 (see FIGS. 5B and 5C).

得られた仮固定基板と同じ径のシリコン基板とを熱硬化性樹脂で接着し、その際のクラック発生有無、接着後の湾曲量を測定した。ただし、剥離層は加熱剥離型接着剤を用いた。次いで、シリコン基板を0.1mm厚まで研削加工し、研削後の接着体の湾曲量を測定した。 The resulting temporarily fixed substrate and a silicon substrate having the same diameter were bonded with a thermosetting resin, and the presence or absence of crack generation at that time and the amount of bending after bonding were measured. However, a heat peeling adhesive was used for the peeling layer. Next, the silicon substrate was ground to a thickness of 0.1 mm, and the amount of curvature of the bonded body after grinding was measured.

ただし、成形条件や治具の形状を変更することによって、仮固定基板の直径(幅)、外周平板部の幅、湾曲量Wを、表1に示すように種々変更した。 However, the diameter (width) of the temporarily fixed substrate, the width of the peripheral flat plate portion, and the amount of curvature W were variously changed as shown in Table 1 by changing the molding conditions and the shape of the jig.

そして、各例について、接着時のクラックの有無(目視)、接着後の接着体の湾曲量、シリコン基板を研削加工した後の接着体の湾曲量をそれぞれ測定した。測定結果を表1に示す。 For each example, the presence or absence of cracks during bonding (visual observation), the amount of bending of the bonded body after bonding, and the amount of bending of the bonded body after grinding the silicon substrate were measured. Table 1 shows the measurement results.

Figure 0007266036000001
Figure 0007266036000001

(比較例1~3)
実施例1と同様の実験を行った。ただし、本例では、熱処理の際の冶具形状を調整し、仮固定基板に外周平板部を設けなかった。また、成形条件や治具の形状を変更することによって、仮固定基板の直径φ、湾曲量Wを、表2に示すように種々変更した。外周平板部の幅は0mmとなる。
(Comparative Examples 1 to 3)
An experiment similar to that of Example 1 was performed. However, in this example, the shape of the jig during the heat treatment was adjusted, and the temporary fixing substrate was not provided with the peripheral flat plate portion. Further, by changing the molding conditions and the shape of the jig, the diameter φ and the amount of curvature W of the temporarily fixed substrate were variously changed as shown in Table 2. The width of the outer peripheral plate portion is 0 mm.

そして、各例について、接着時のクラックの有無(目視)、接着後の接着体の湾曲量、シリコン基板を研削加工した後の接着体の湾曲量をそれぞれ測定した。測定結果を表2に示す。 For each example, the presence or absence of cracks during bonding (visual observation), the amount of bending of the bonded body after bonding, and the amount of bending of the bonded body after grinding the silicon substrate were measured. Table 2 shows the measurement results.

Figure 0007266036000002
Figure 0007266036000002

外周平板部のない比較例の仮固定基板を使用した場合には、接着体の湾曲量が相対的に大きくなっており、シリコン基板の研磨後の湾曲量も大きくなっている。 In the case of using the temporary fixing substrate of the comparative example having no peripheral flat plate portion, the amount of bending of the adhesive body is relatively large, and the amount of bending of the silicon substrate after polishing is also large.

本発明の仮固定基板を使用した場合には、仮固定基板の湾曲量が比較例と同じであっても、接着体の湾曲量が小さくなっている。また、外周平板部の幅の比率を4~60%とすることで、本発明の効果が一層顕著になっていた。 When the temporary fixing substrate of the present invention is used, even if the amount of bending of the temporary fixing substrate is the same as that of the comparative example, the amount of bending of the adhesive body is small. Further, by setting the ratio of the width of the outer peripheral plate portion to 4 to 60%, the effect of the present invention became even more remarkable.

また、実施例1~7の各仮固定基板を製造し、電子部品チップを接着し、樹脂モールドで封止した。他は実施例1~7と同様にして電子部品チップおよび樹脂モールドを仮固定基板から分離した。そして樹脂モールドを割断して各電子部品チップを得た。接着時のクラックの有無(目視)、接着後の接着体の湾曲量をそれぞれ測定したが、実施例1~7と同様の結果を得た。 Further, each of the temporary fixing substrates of Examples 1 to 7 was produced, an electronic component chip was adhered thereto, and the substrate was sealed with a resin mold. Otherwise, the electronic component chip and the resin mold were separated from the temporary fixing substrate in the same manner as in Examples 1-7. Then, the resin mold was cut to obtain each electronic component chip. The presence or absence of cracks during bonding (visual observation) and the amount of bending of the bonded body after bonding were measured, and the same results as in Examples 1 to 7 were obtained.

Claims (13)

シリコン基板と電子部品チップとの少なくとも一方を接着し、仮固定するための固定面と、前記固定面の反対側にある底面とを備え、セラミックスまたはガラスからなる仮固定基板であって、
外周平板部と、前記外周平板部によって包囲された凹状変形部とを有しており、前記固定面が前記外周平板部において平坦面であることを特徴とする、仮固定基板。
A temporary fixing substrate made of ceramics or glass, comprising a fixing surface for bonding and temporarily fixing at least one of a silicon substrate and an electronic component chip, and a bottom surface opposite to the fixing surface,
A temporary fixing substrate comprising an outer peripheral flat plate portion and a recessed deformation portion surrounded by the outer peripheral flat plate portion, wherein the fixing surface is a flat surface in the outer peripheral flat plate portion.
前記セラミックスが透光性アルミナであることを特徴とする、請求項1記載の仮固定基板。 2. The temporary fixing substrate according to claim 1, wherein said ceramics is translucent alumina. 前記外周平板部の幅が前記仮固定基板の幅の4~60%であることを特徴とする、請求項1または2記載の仮固定基板。 3. The temporary fixing substrate according to claim 1, wherein the width of said peripheral flat plate portion is 4 to 60% of the width of said temporary fixing substrate. 前記凹状変形部の湾曲量が0.1~2.5mmであることを特徴とする、請求項1~3のいずれか一つの請求項に記載の仮固定基板。 The temporary fixing substrate according to any one of claims 1 to 3, characterized in that the amount of curvature of the concave deformation portion is 0.1 to 2.5 mm. 請求項1~4のいずれか一つの請求項に記載の仮固定基板の前記固定面に前記シリコン基板と前記電子部品チップとの少なくとも一方を接着して接着体を得る工程
を有することを特徴とする、仮固定方法。
A method comprising a step of bonding at least one of the silicon substrate and the electronic component chip to the fixing surface of the temporary fixing substrate according to any one of claims 1 to 4 to obtain an adhesive body. Temporary fixation method.
前記接着体の前記シリコン基板を加工してシリコン基板を薄くし、シリコン層を形成する工程、および
前記シリコン層を前記仮固定基板から分離する工程
を有することを特徴とする、請求項5記載の方法。
6. The method according to claim 5, further comprising a step of processing the silicon substrate of the adhesive body to thin the silicon substrate to form a silicon layer, and a step of separating the silicon layer from the temporary fixing substrate. Method.
前記シリコン層に電子部品構造を設ける工程を有することを特徴とする、請求項6記載の方法。 7. The method of claim 6, comprising the step of providing an electronic component structure in said silicon layer. 前記仮固定基板の前記固定面に前記電子部品チップを接着した後、前記電子部品チップを樹脂モールドで覆う工程を有していることを特徴とする、請求項5記載の方法。 6. The method according to claim 5, further comprising a step of covering the electronic component chip with a resin mold after bonding the electronic component chip to the fixing surface of the temporary fixing substrate. 請求項1~4のいずれか一つの請求項に記載の仮固定基板の前記固定面に前記シリコン基板を接着して接着体を得る工程、
前記接着体の前記シリコン基板を加工してシリコン基板を薄くし、シリコン層を形成する工程、
前記シリコン層内または前記シリコン層上に電子部品チップを設ける工程、および
前記シリコン層および前記電子部品チップを前記仮固定基板から分離する工程
を有することを特徴とする、電子部品の製造方法。
A step of bonding the silicon substrate to the fixing surface of the temporary fixing substrate according to any one of claims 1 to 4 to obtain an adhesive body;
a step of processing the silicon substrate of the adhesive body to thin the silicon substrate and form a silicon layer;
A method of manufacturing an electronic component, comprising: providing an electronic component chip in or on the silicon layer; and separating the silicon layer and the electronic component chip from the temporary fixing substrate.
前記シリコン層を前記仮固定基板から分離した後、前記シリコン層を分割する工程を有することを特徴とする、請求項9記載の方法。 10. The method of claim 9, further comprising dividing the silicon layer after separating the silicon layer from the temporary fixing substrate. 前記シリコン層内に配線を設け、この配線を前記電子部品チップと接続する工程を有することを特徴とする、請求項9または10記載の方法。 11. A method according to claim 9 or 10, characterized by the step of providing wiring in said silicon layer and connecting said wiring with said electronic component chip. 請求項1~4のいずれか一つの請求項に記載の仮固定基板の前記固定面に前記電子部品チップを接着して接着体を得る工程、および
前記電子部品チップを前記仮固定基板から分離する工程
を有することを特徴とする、電子部品の製造方法。
A step of bonding the electronic component chip to the fixing surface of the temporary fixing substrate according to any one of claims 1 to 4 to obtain an adherent, and separating the electronic component chip from the temporary fixing substrate. A method for manufacturing an electronic component, comprising:
前記仮固定基板の前記固定面に前記電子部品チップを接着した後、前記電子部品チップを樹脂モールドで覆う工程を有していることを特徴とする、請求項12記載の方法。
13. The method according to claim 12, further comprising a step of covering the electronic component chip with a resin mold after bonding the electronic component chip to the fixing surface of the temporary fixing substrate.
JP2020532437A 2018-07-26 2019-07-24 Temporary fixing substrate, temporary fixing method, and method for manufacturing electronic component Active JP7266036B2 (en)