JP6915530B2 - Method for producing ethylene-vinyl alcohol-based copolymer pellets and ethylene-vinyl alcohol-based copolymer pellets - Google Patents
Method for producing ethylene-vinyl alcohol-based copolymer pellets and ethylene-vinyl alcohol-based copolymer pellets Download PDFInfo
- Publication number
- JP6915530B2 JP6915530B2 JP2017252332A JP2017252332A JP6915530B2 JP 6915530 B2 JP6915530 B2 JP 6915530B2 JP 2017252332 A JP2017252332 A JP 2017252332A JP 2017252332 A JP2017252332 A JP 2017252332A JP 6915530 B2 JP6915530 B2 JP 6915530B2
- Authority
- JP
- Japan
- Prior art keywords
- evoh
- pellet
- boron compound
- lubricant
- boron
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Description
本発明は、フィルム成形したときに、フィッシュアイの発生が少ないフィルムを提供できるエチレン−ビニルアルコール系共重合体(以下、「EVOH」と称することがある)のペレットに関し、さらに詳しくは、ペレット表面に存在するホウ素化合物の含有量を調整し、かつ所定量の滑剤を含有したEVOHペレットおよびその製造方法に関する。 The present invention relates to pellets of an ethylene-vinyl alcohol-based copolymer (hereinafter, may be referred to as "EVOH") capable of providing a film in which fish eyes are less likely to occur when the film is molded. The present invention relates to EVOH pellets in which the content of the boron compound present in the film is adjusted and a predetermined amount of lubricant is contained, and a method for producing the same.
EVOHは、分子鎖に含まれる水酸基が強固に水素結合して結晶部を形成し、かかる結晶部が外部からの酸素等の気体の侵入を防止するため、酸素バリア性をはじめとして、優れたガスバリア性を示すことができる。このような特性を生かして、EVOHは、食品包装材料、医薬品包装材料、工業薬品包装材料、農薬包装材料等のフィルムやシート、あるいはボトル等の包装容器等に成形されて利用されている。 In EVOH, the hydroxyl groups contained in the molecular chain are strongly hydrogen-bonded to form a crystal portion, and the crystal portion prevents the invasion of gas such as oxygen from the outside. Therefore, EVOH has excellent gas barrier properties including oxygen barrier properties. Can show sex. Taking advantage of these characteristics, EVOH is used by being molded into films and sheets such as food packaging materials, pharmaceutical packaging materials, industrial chemical packaging materials, agricultural chemical packaging materials, and packaging containers such as bottles.
EVOHは、通常、溶融成形によって、フィルム状、シート状、ボトル状、カップ状、チューブ状、パイプ状等の形状に成形、加工されて、実用に供される。したがって、EVOHの成形性、加工性は重要である。 EVOH is usually formed and processed into a film shape, a sheet shape, a bottle shape, a cup shape, a tube shape, a pipe shape, or the like by melt molding, and is put into practical use. Therefore, the moldability and workability of EVOH are important.
そこで、溶融成形性の改善にあたり、特許文献1には、EVOH等の溶融成形可能なビニルアルコール系共重合体の膜成形性、特に成膜時のサージング防止の観点から、ホウ酸またはその塩を配合した組成物として、溶融粘度を高めたものを溶融成形することが有効であることが開示されている。 Therefore, in order to improve the melt moldability, Patent Document 1 describes boric acid or a salt thereof from the viewpoint of film moldability of a melt moldable vinyl alcohol copolymer such as EVOH, particularly from the viewpoint of preventing surging during film formation. It is disclosed that it is effective to melt-mold a composition having an increased melt viscosity as the blended composition.
また、特許文献2には、ホウ素化合物で処理したEVOHを、ポリオレフィンと共押出することにより、EVOH層とポリオレフィン層との接着性に優れた積層体が得られ、ガスバリア性能を要する分野において、好適な包装材を提供できることが開示されている。
特許文献2の、ホウ素化合物処理は、EVOH溶液または分散液にホウ素化合物を添加することにより行われ、ホウ素成分を含有したEVOHペレットを押出成形原料として用いている。
Further, in Patent Document 2, EVOH treated with a boron compound is co-extruded with polyolefin to obtain a laminate having excellent adhesiveness between the EVOH layer and the polyolefin layer, which is suitable in a field requiring gas barrier performance. It is disclosed that various packaging materials can be provided.
The boron compound treatment of Patent Document 2 is performed by adding a boron compound to an EVOH solution or a dispersion, and EVOH pellets containing a boron component are used as an extrusion molding raw material.
ところで、包装材料としてのEVOHフィルムまたは多層構造体の外観に対する昨今の要求の高まりから、0.1mm未満の小さなフィッシュアイについても、改善が求められるようになっている。
特許文献3では、EVOHにホウ素化合物を含有させる処理を行って得られるホウ素含有EVOHペレットについて、ペレットの含水率が0.1mm未満のフィッシュアイの発生と関係があることを見出し、含水率0.0001〜2重量%に乾燥させた後、水と接触させることにより、0.1mm未満のフィッシュアイの発生を抑制できることが開示されている。
By the way, due to the recent increase in demand for the appearance of EVOH film or multilayer structure as a packaging material, improvement is required even for small fish eyes of less than 0.1 mm.
In Patent Document 3, it has been found that the boron-containing EVOH pellets obtained by treating EVOH with a boron compound are related to the generation of fish eyes having a water content of less than 0.1 mm, and the water content is 0. It is disclosed that the generation of fish eyes of less than 0.1 mm can be suppressed by contacting with water after drying to 0001 to 2% by weight.
特許文献3の実施例では、ホウ素化合物の添加処理を施したEVOHペレットを水に浸漬した後、乾燥して、ホウ素化合物の含有量および含水率を調整したEVOHペレット〔含水率0.13〜0.4重量%、EVOH100重量部に対するホウ素含有量0.015〜0.039重量部(150〜390ppm)〕を製造し、このEVOHペレットを、多層押出装置に供給して、3種5層の多層積層体を製造している(実施例1,3,4)。そして、得られた多層構造体のフィッシュアイの評価は、目視観察により、直径0.01〜0.1mmのフィッシュアイの発生の個数をカウントすることにより行っている(段落〔0038〕−〔0041〕)。 In the examples of Patent Document 3, EVOH pellets to which a boron compound has been added are immersed in water and then dried to adjust the content and water content of the boron compound [moisture content 0.13 to 0]. .4% by weight, boron content per 100 parts by weight of EVOH 0.015 to 0.039 parts by weight (150 to 390 ppm)] was produced, and the EVOH pellets were supplied to a multi-layer extruder to supply 3 types and 5 layers of multi-layers. Laminates are manufactured (Examples 1, 3 and 4). Then, the fish eyes of the obtained multilayer structure are evaluated by visually observing and counting the number of fish eyes having a diameter of 0.01 to 0.1 mm (paragraphs [0038]-[0041]. ]).
近年、包装材料の外観に対する要求は益々厳しくなっており、成形時のサージング防止等の溶融成形性を確保しつつ、さらなるフィッシュアイの改善が望まれている。特に、EVOHを単層成膜した場合、多層構造体の場合よりも、大きなフィッシュアイが発生しやすく、また発生個数も多くなる傾向があるため、EVOHの単層膜でも、フィッシュアイの発生が抑制されたEVOHペレットが求められるようになっており、上記特許文献1〜3の開示技術では、まだまだ満足のいくものではなかった。 In recent years, the demand for the appearance of packaging materials has become more and more strict, and further improvement of fish eyes is desired while ensuring melt moldability such as prevention of surging during molding. In particular, when EVOH is formed into a single layer, large fish eyes are more likely to be generated and the number of EVOHs is likely to be larger than in the case of a multilayer structure. Therefore, even with a single layer film of EVOH, fish eyes are generated. Suppressed EVOH pellets have been required, and the techniques disclosed in Patent Documents 1 to 3 have not yet been satisfactory.
本発明は、以上のような事情に鑑みてなされたものであり、その目的とするところは、EVOH単層膜でも、フィッシュアイの発生を抑制できるホウ素化合物および滑剤を含有するEVOHペレットおよびその製造方法を提供することにある。 The present invention has been made in view of the above circumstances, and an object of the present invention is to produce an EVOH pellet containing a boron compound and a lubricant capable of suppressing the generation of fish eyes even in an EVOH monolayer film and its production. To provide a method.
本発明者らは、ホウ素化合物を含有させたEVOHペレットについて、フィッシュアイの発生との関係を調べた。種々検討した結果、フィッシュアイは、ホウ素化合物の凝集体がEVOHの局所的増粘を招くことにより発生すると考えられる。そして、単層成膜の場合、成形機の金属と接することになるペレット表層部に存在するホウ素化合物が凝集しやすくなり、結果として、フィッシュアイが発生しやすく、目立つのではないかと考えた。 The present inventors investigated the relationship between the generation of fish eyes and EVOH pellets containing a boron compound. As a result of various studies, it is considered that fish eyes are generated by agglomerates of boron compounds causing local thickening of EVOH. Then, in the case of single-layer film formation, it was thought that the boron compound existing in the surface layer portion of the pellet, which would come into contact with the metal of the molding machine, would easily aggregate, and as a result, fish eyes would easily occur and would be conspicuous.
一般に、EVOHペレットを押出機に供給すると、ペレット表面の摩擦力が高いためにスクリューへの噛み込みが悪くなり、押出機へ供給されにくくなる。本発明者らは、EVOHペレットは供給されない間は常に高温に曝され続けるため、熱劣化しやすくなり、結果としてフィッシュアイの増加を引き起こすと考えた。 Generally, when EVOH pellets are supplied to an extruder, the frictional force on the surface of the pellets is high, so that the EVOH pellets are poorly bitten into the screw and are difficult to be supplied to the extruder. The present inventors considered that EVOH pellets are constantly exposed to high temperatures while they are not supplied, so that they are susceptible to thermal deterioration, resulting in an increase in fish eyes.
上記2種類のフィッシュアイ発生のメカニズムを総合的に検討すると、EVOHペレットがスクリューへ噛み込まない間は、ホウ素化合物が存在する表面部が優先して加熱されるため、ホウ素化合物の凝集が起こりやすくなり、フィッシュアイの発生はより顕著になると推測される。 Comprehensively examining the above two types of fisheye generation mechanisms, the surface portion where the boron compound is present is preferentially heated while the EVOH pellet is not bitten into the screw, so that the boron compound is likely to aggregate. Therefore, it is presumed that the occurrence of fish eyes will become more prominent.
かかる認識の下、鋭意検討した結果、本発明者らは、ペレット表層部のホウ素化合物の含有量、さらに滑剤の含有量に着目し、ペレット表層部のホウ素化合物の含有量を、従来より少なくし、かつ、EVOH中の滑剤の含有量を所定範囲にすることにより、EVOHを押出機へ供給しやすくすることで、ペレット表面にホウ素化合物が多く存在する場合に発生するフィッシュアイが相乗的に低減できることを見出し、本発明を完成した。
なお、本発明のホウ素化合物および滑剤含有EVOHペレットを用いて得られる膜(層、フィルムを含む)は、単層膜であっても成形性に優れ、外観に優れているので、耐水性、強度等の観点から、他の樹脂層を積層した多層構造体においても、当然に適用できるものである。
Based on this recognition, as a result of diligent studies, the present inventors focused on the content of the boron compound in the surface layer of the pellet and the content of the lubricant, and reduced the content of the boron compound in the surface layer of the pellet to be lower than before. In addition, by setting the content of the lubricant in EVOH within a predetermined range, it becomes easier to supply EVOH to the extruder, and fish eyes generated when a large amount of boron compound is present on the pellet surface are synergistically reduced. We found what we could do and completed the present invention.
The film (including the layer and the film) obtained by using the boron compound and the lubricant-containing EVOH pellet of the present invention is excellent in moldability and appearance even if it is a single-layer film, and therefore has excellent water resistance and strength. From the above viewpoints, it can be naturally applied to a multilayer structure in which other resin layers are laminated.
すなわち、本発明は、ホウ素化合物および滑剤を含有するEVOHペレット(以下、「ホウ素化合物および滑剤含有EVOHペレット」と称する場合がある)であって、当該ペレット表層部のホウ素化合物含有量が、ホウ素換算で、当該ペレット重量あたり1.7ppm以下であり、かつ滑剤の含有量が当該ペレットの0.001〜0.15重量%であるEVOHペレットを第1の要旨とする。 That is, the present invention is an EVOH pellet containing a boron compound and a lubricant (hereinafter, may be referred to as "boron compound and a lubricant-containing EVOH pellet"), and the boron compound content in the surface layer of the pellet is converted to boron. The first gist is an EVOH pellet having an amount of 1.7 ppm or less per weight of the pellet and a lubricant content of 0.001 to 0.15% by weight of the pellet.
また、本発明は、EVOHペレットをホウ素化合物と接触させることによりホウ素化合物を含有させる工程、上記工程により得られたペレットを洗浄して、ペレット表層部のホウ素化合物含有量を、ホウ素換算でエチレン−ビニルアルコール系共重合体ペレット重量あたり1.7ppm以下にする工程、および滑剤を含有させる工程を備えたホウ素化合物および滑剤を含有するEVOHペレットの製造方法であって、上記洗浄する工程の洗浄が、乾燥後のペレットと、水のアルコールに対する重量比(水/アルコール)が80/20〜0/100の水/アルコール混合液またはアルコールとを接触させることであり、上記滑剤を含有させる工程が、滑剤を当該ペレットの0.001〜0.15重量%となるように含有させるEVOHペレットの製造方法を第2の要旨とする。 Further, the present invention is a step of adding a boron compound by contacting an EVOH pellet with a boron compound, washing the pellet obtained by the above step, and adjusting the boron compound content of the pellet surface layer to ethylene- in terms of boron. A method for producing an EVOH pellet containing a boron compound and a lubricant, which comprises a step of reducing the weight of the vinyl alcohol-based copolymer pellet to 1.7 ppm or less and a step of adding a lubricant. The step of adding the lubricant is to bring the dried pellets into contact with a water / alcohol mixture or alcohol having a weight ratio (water / alcohol) of 80/20 to 0/100 to alcohol. The second gist is a method for producing an EVOH pellet containing 0.001 to 0.15% by weight of the pellet.
本発明のホウ素化合物および滑剤含有EVOHペレットは、当該ペレット表層部のホウ素化合物含有量が、ホウ素換算で、当該ペレット重量あたり1.7ppm以下であり、かつ滑剤の含有量が当該ペレットの0.001〜0.15重量%である。そのため、本発明のホウ素化合物および滑剤含有EVOHペレットは、溶融成形性を確保しつつ、フィッシュアイの発生を抑制する効果に優れる。 In the boron compound and lubricant-containing EVOH pellet of the present invention, the boron compound content of the surface layer of the pellet is 1.7 ppm or less per the weight of the pellet in terms of boron, and the content of the lubricant is 0.001 of the pellet. ~ 0.15% by weight. Therefore, the boron compound and lubricant-containing EVOH pellets of the present invention are excellent in the effect of suppressing the generation of fish eyes while ensuring melt moldability.
また、本発明のなかでも、特に、ホウ素化合物および滑剤含有EVOHペレット全体のホウ素化合物全含有量が、ホウ素換算で上記ペレット重量あたり10〜1000ppmであると、成膜に適した粘度となり、成膜性能を向上させることができ、ひいてはフィッシュアイの発生を抑制する効果に優れたものとすることができる。 Further, among the present inventions, in particular, when the total content of the boron compound in the entire EVOH pellet containing a boron compound and a lubricant is 10 to 1000 ppm per the weight of the pellet in terms of boron, the viscosity becomes suitable for film formation, and the film is formed. The performance can be improved, and the effect of suppressing the occurrence of fish eyes can be excellent.
さらに、本発明のなかでも、特に、ホウ素化合物および滑剤含有EVOHペレット全体のホウ素化合物全含有量(ホウ素換算)に対する上記ペレット表層部のホウ素化合物含有量(ホウ素換算)の重量比(表層部ホウ素含有量/ホウ素全含有量)が、1.38×10-2以下であると、より一層フィッシュアイの発生を抑制する効果に優れたものとすることができ、また、フィルム外観を向上させることができる。 Further, among the present inventions, in particular, the weight ratio of the boron compound content (boron equivalent) of the pellet surface layer portion to the total boron compound content (boron equivalent) of the entire boron compound and lubricant-containing EVOH pellet (boron content in the surface layer portion). When the amount / total boron content) is 1.38 × 10-2 or less, the effect of further suppressing the generation of fish eyes can be further improved, and the appearance of the film can be improved. can.
そして、本発明のなかでも、特に、ホウ素化合物および滑剤含有EVOHペレットの含水率が0.01〜1重量%であると、より一層フィシュアイの発生を抑制する効果に優れたものとすることができ、また、フィルム外観を向上させることができる。 Further, among the present inventions, in particular, when the water content of the boron compound and the lubricant-containing EVOH pellet is 0.01 to 1% by weight, the effect of further suppressing the generation of fisheye can be made excellent. It can also improve the appearance of the film.
また、EVOHペレットをホウ素化合物と接触させることによりホウ素化合物を含有させる工程、上記工程により得られたペレットを洗浄して、ペレット表層部のホウ素化合物含有量を、ホウ素換算でエチレン−ビニルアルコール系共重合体ペレット重量あたり1.7ppm以下にする工程、および滑剤を含有させる工程を備えたホウ素化合物および滑剤を含有するEVOHペレットの製造方法であって、上記洗浄工程の洗浄が、乾燥後のペレットと、水のアルコールに対する重量比(水/アルコール)が80/20〜0/100の水/アルコール混合液またはアルコールとを接触させることであり、上記滑剤を含有させる工程が、滑剤を当該ペレットの0.001〜0.15重量%となるように含有させる、本発明のEVOHペレットの製造方法であると、表層部のホウ素含有量を減じ、更に滑剤を含有するEVOHペレットとすることができ、当該ペレットを用いた溶融成形品は、溶融成形性が良好で、フィッシュアイの発生が低減されたものとなる。 Further, a step of bringing the EVOH pellets into contact with a boron compound to contain the boron compound, and washing the pellets obtained by the above step to change the boron compound content of the pellet surface layer portion in terms of ethylene and vinyl alcohol. A method for producing EVOH pellets containing a boron compound and a lubricant, which comprises a step of reducing the weight of the polymer pellet to 1.7 ppm or less and a step of containing a lubricant. , The weight ratio (water / alcohol) of water to alcohol is 80/20 to 0/100 of contact with a water / alcohol mixture or alcohol, and the step of containing the lubricant is to bring the lubricant to 0 of the pellet. According to the method for producing EVOH pellets of the present invention, which is contained so as to be .001 to 0.15% by weight, the boron content of the surface layer portion can be reduced, and EVOH pellets containing a lubricant can be obtained. The melt-molded product using pellets has good melt-moldability and reduces the occurrence of fish eyes.
以下、本発明を詳細に説明するが、これらは望ましい実施態様の一例を示すものであり、これらの内容に特定されるものではない。 Hereinafter, the present invention will be described in detail, but these are examples of desirable embodiments and are not specified in their contents.
なお、本明細書において、上記ホウ素化合物および滑剤を含有するEVOHペレットにおけるホウ素量として測定された含有量については、「ホウ素化合物含有量(ホウ素換算)」または単に「ホウ素含有量」と称する。 In the present specification, the content measured as the boron content in the EVOH pellet containing the boron compound and the lubricant is referred to as "boron compound content (boron equivalent)" or simply "boron content".
本発明のホウ素化合物および滑剤含有EVOHペレットは、当該ペレットの表層部のホウ素含有量が、ホウ素換算で、当該ペレット重量あたり1.7ppm以下であり、かつ滑剤の含有量が当該ペレットの0.001〜0.15重量%である。 In the boron compound and lubricant-containing EVOH pellet of the present invention, the boron content of the surface layer of the pellet is 1.7 ppm or less per the weight of the pellet in terms of boron, and the content of the lubricant is 0.001 of the pellet. ~ 0.15% by weight.
ここで、「ペレット表層部のホウ素化合物含有量」とは、ホウ素化合物および滑剤含有EVOHペレットが含有するホウ素化合物のうち、表面近くに存在しているホウ素化合物の量を意味する。具体的には、ホウ素化合物および滑剤含有EVOHペレット4gを30℃メタノール20mLに6時間静置浸漬した後、得られたメタノール溶液中のホウ素含有量を誘導結合プラズマ質量分析計(ICP−MS)を用いて測定し、上記EVOHペレットの重量(4g)で除したものである。この「ペレット表層部のホウ素化合物」には、ペレット表面に付着しているだけのホウ素化合物、表面にブリードしてきたホウ素化合物等が含まれる。
そして、「ペレット表層部のホウ素化合物含有量」は、ホウ素化合物および滑剤含有EVOHペレット中に含有されているホウ素化合物含有量(「ペレットのホウ素化合物全含有量」)とは区別されるものである。
Here, the "boron compound content of the pellet surface layer portion" means the amount of the boron compound present near the surface among the boron compounds contained in the boron compound and the lubricant-containing EVOH pellet. Specifically, 4 g of EVOH pellets containing a boron compound and a lubricant was immersed in 20 mL of methanol at 30 ° C. for 6 hours, and then the inductively coupled plasma mass spectrometer (ICP-MS) was used to determine the boron content in the obtained methanol solution. It was measured using and divided by the weight (4 g) of the above EVOH pellets. The "boron compound on the surface layer of the pellet" includes a boron compound that is only attached to the surface of the pellet, a boron compound that has bleeded on the surface, and the like.
The "boron compound content in the surface layer of the pellet" is distinguished from the boron compound content in the boron compound and the lubricant-containing EVOH pellet ("total boron compound content in the pellet"). ..
以下、本発明のホウ素化合物および滑剤を含有するEVOHペレットの説明に先立って、各構成成分、および、ホウ素化合物と滑剤とを含有させる前のEVOHペレットの製造方法について説明する。 Hereinafter, prior to the description of the EVOH pellet containing the boron compound and the lubricant of the present invention, each component and a method for producing the EVOH pellet before containing the boron compound and the lubricant will be described.
<EVOH>
本発明のホウ素化合物および滑剤含有EVOHペレットを構成するEVOHは、通常、エチレンとビニルエステル系モノマーとの共重合体(エチレン−ビニルエステル系共重合体)をケン化させることにより得られる樹脂であり、一般的にエチレン−ビニルアルコール系共重合体やエチレン−ビニルエステル系共重合体ケン化物と称される非水溶性の熱可塑性樹脂である。重合法も公知の任意の重合法、例えば、溶液重合、懸濁重合、エマルジョン重合を用いて行うことができるが、一般的にはメタノール等の低級アルコール、特に好ましくはメタノールを溶媒とする溶液重合が用いられる。得られたエチレン−ビニルエステル系共重合体のケン化も公知の方法で行い得る。
このようにして製造されるEVOHは、エチレン由来の構造単位とビニルアルコール構造単位を主とし、必要に応じてケン化されずに残存した若干量のビニルエステル構造単位を通常含む。
<EVOH>
The EVOH constituting the boron compound and the lubricant-containing EVOH pellet of the present invention is usually a resin obtained by saponifying a copolymer (ethylene-vinyl ester-based copolymer) of ethylene and a vinyl ester-based monomer. , A water-insoluble thermoplastic resin generally called an ethylene-vinyl alcohol-based copolymer or an ethylene-vinyl ester-based copolymer saponified product. The polymerization method can also be carried out by using any known polymerization method, for example, solution polymerization, suspension polymerization or emulsion polymerization, but in general, solution polymerization using a lower alcohol such as methanol, particularly preferably methanol as a solvent. Is used. The obtained ethylene-vinyl ester copolymer can also be saponified by a known method.
The EVOH produced in this manner is mainly composed of ethylene-derived structural units and vinyl alcohol structural units, and usually contains a small amount of vinyl ester structural units remaining without saponification, if necessary.
上記ビニルエステル系モノマーとしては、市場からの入手のしやすさや製造時の不純物の処理効率がよい点から、代表的には酢酸ビニルが用いられる。他のビニルエステル系モノマーとしては、例えば、ギ酸ビニル、プロピオン酸ビニル、バレリン酸ビニル、酪酸ビニル、イソ酪酸ビニル、ピバリン酸ビニル、カプリン酸ビニル、ラウリン酸ビニル、ステアリン酸ビニル、バーサチック酸ビニル等の脂肪族ビニルエステル、安息香酸ビニル等の芳香族ビニルエステル等があげられ、通常炭素数3〜20、好ましくは炭素数4〜10、特に好ましくは炭素数4〜7の脂肪族ビニルエステルを用いることができる。これらは通常単独で用いるが、必要に応じて複数種を同時に用いてもよい。 As the vinyl ester-based monomer, vinyl acetate is typically used because it is easily available on the market and the processing efficiency of impurities during production is good. Examples of other vinyl ester-based monomers include vinyl formate, vinyl propionate, vinyl valerate, vinyl butyrate, vinyl isobutyrate, vinyl pivalate, vinyl caprate, vinyl laurate, vinyl stearate, vinyl versaticate and the like. Examples thereof include aliphatic vinyl esters and aromatic vinyl esters such as vinyl benzoate. Usually, an aliphatic vinyl ester having 3 to 20 carbon atoms, preferably 4 to 10 carbon atoms, and particularly preferably 4 to 7 carbon atoms is used. Can be done. These are usually used alone, but if necessary, a plurality of types may be used at the same time.
上記エチレンおよび上記ビニルエステル系モノマーは、通常、ナフサ等の石油由来の原料が用いられているが、シェールガス等天然ガス由来の原料や、さとうきび、テンサイ、トウモロコシ、ジャガイモ等に含まれる糖、デンプン等の成分、またはイネ、麦、キビ、草植物等に含まれるセルロース等の成分から精製した植物由来の原料からのモノマーを用いてもよい。 The ethylene and vinyl ester-based monomers usually use petroleum-derived raw materials such as naphtha, but natural gas-derived raw materials such as shale gas, sugars and starches contained in sugar cane, tensai, corn, potatoes and the like. Etc., or monomers from plant-derived raw materials purified from components such as cellulose contained in rice, wheat, millet, grass plants and the like may be used.
EVOHにおけるエチレン構造単位の含有量は、ISO14663に基づいて測定した値で、通常20〜60モル%、好ましくは25〜50モル%、特に好ましくは27〜48モル%である。かかる含有量が低すぎる場合は、高湿下のガスバリア性、溶融成形性が低下する傾向があり、逆に高すぎる場合は、ガスバリア性が低下する傾向がある。 The content of ethylene structural units in EVOH is a value measured based on ISO14663 and is usually 20 to 60 mol%, preferably 25 to 50 mol%, particularly preferably 27 to 48 mol%. If the content is too low, the gas barrier property and melt moldability under high humidity tend to decrease, and if the content is too high, the gas barrier property tends to decrease.
EVOHにおけるビニルエステル成分のケン化度は、JIS K6726(ただし、溶媒として水/メタノールを使用)に基づいて測定した値で、通常90〜100モル%、好ましくは95〜100モル%、特に好ましくは99〜100モル%である。かかるケン化度が低すぎる場合にはガスバリア性、熱安定性、耐湿性等が低下する傾向がある。 The saponification degree of the vinyl ester component in EVOH is a value measured based on JIS K6726 (however, water / methanol is used as a solvent), and is usually 90 to 100 mol%, preferably 95 to 100 mol%, particularly preferably. It is 99 to 100 mol%. If the saponification degree is too low, the gas barrier property, thermal stability, moisture resistance and the like tend to decrease.
また、該EVOHのメルトフローレート(MFR)(210℃、荷重2160g)は、通常0.5〜100g/10分であり、好ましくは1〜50g/10分、特に好ましくは2〜35g/10分である。かかるMFRが大きすぎる場合には、成膜性が不安定となる傾向があり、小さすぎる場合には粘度が高くなり過ぎて溶融押出しが困難となる傾向がある。 The melt flow rate (MFR) (210 ° C., load 2160 g) of the EVOH is usually 0.5 to 100 g / 10 minutes, preferably 1 to 50 g / 10 minutes, and particularly preferably 2 to 35 g / 10 minutes. Is. If the MFR is too large, the film forming property tends to be unstable, and if it is too small, the viscosity tends to be too high and melt extrusion tends to be difficult.
本発明で用いられるEVOHには、本発明の効果を阻害しない範囲(例えば10モル%以下)で、以下に示すコモノマーに由来する構造単位が、さらに含まれていてもよい。 The EVOH used in the present invention may further contain structural units derived from the commonomers shown below as long as the effects of the present invention are not impaired (for example, 10 mol% or less).
上記コモノマーとしては、プロピレン、1−ブテン、イソブテン等のオレフィン類、3−ブテン−1−オール、3−ブテン−1,2−ジオール、4−ペンテン−1−オール、5−ヘキセン−1,2−ジオール等の水酸基含有α−オレフィン類やそのエステル化物、アシル化物等の誘導体;2−メチレンプロパン−1,3−ジオール、3−メチレンペンタン−1,5−ジオール等のヒドロキシアルキルビニリデン類;1,3−ジアセトキシ−2−メチレンプロパン、1,3−ジプロピオニルオキシ−2−メチレンプロパン、1,3−ジブチロニルオキシ−2−メチレンプロパン等のヒドロキシアルキルビニリデンジアセテート類、アクリル酸、メタクリル酸、クロトン酸、(無水)フタル酸、(無水)マレイン酸、(無水)イタコン酸等の不飽和酸類あるいはその塩あるいは炭素数1〜18のモノまたはジアルキルエステル類;アクリルアミド、炭素数1〜18のN−アルキルアクリルアミド、N,N−ジメチルアクリルアミド、2−アクリルアミドプロパンスルホン酸あるいはその塩、アクリルアミドプロピルジメチルアミンあるいはその酸塩あるいはその4級塩等のアクリルアミド類;メタアクリルアミド、炭素数1〜18のN−アルキルメタクリルアミド、N,N−ジメチルメタクリルアミド、2−メタクリルアミドプロパンスルホン酸あるいはその塩、メタクリルアミドプロピルジメチルアミンあるいはその酸塩あるいはその4級塩等のメタクリルアミド類;N−ビニルピロリドン、N−ビニルホルムアミド、N−ビニルアセトアミド等のN−ビニルアミド類;アクリルニトリル、メタクリルニトリル等のシアン化ビニル類;炭素数1〜18のアルキルビニルエーテル、ヒドロキシアルキルビニルエーテル、アルコキシアルキルビニルエーテル等のビニルエーテル類;塩化ビニル、塩化ビニリデン、フッ化ビニル、フッ化ビニリデン、臭化ビニル等のハロゲン化ビニル化合物類;トリメトキシビニルシラン等のビニルシラン類;酢酸アリル、塩化アリル等のハロゲン化アリル化合物類;アリルアルコール、ジメトキシアリルアルコール等のアリルアルコール類;トリメチル−(3−アクリルアミド−3−ジメチルプロピル)−アンモニウムクロリド、アクリルアミド−2−メチルプロパンスルホン酸等のコモノマーがあげられる。これらは単独でもしくは2種以上併せて用いることができる。 Examples of the comonomer include olefins such as propylene, 1-butene and isobutene, 3-butene-1-ol, 3-butene-1,2-diol, 4-pentene-1-ol and 5-hexene-1,2. Hydroxyl-containing α-olefins such as −diol and derivatives such as esterified products and allyl groups thereof; hydroxyalkylvinylidenes such as 2-methylenepropane-1,3-diol and 3-methylenepentane-1,5-diol; 1 , 3-Diacetoxy-2-methylenepropane, 1,3-dipropionyloxy-2-methylenepropane, 1,3-dibutyronyloxy-2-methylenepropane and other hydroxyalkyl vinylidene diacetates, acryloacid, methacrylic acid , Crotonic acid, (anhydrous) phthalic acid, (anhydrous) maleic acid, (anhydrous) itaconic acid and other unsaturated acids or salts thereof or mono- or dialkyl esters having 1 to 18 carbon atoms; acrylamide, having 1 to 18 carbon atoms. Acrylamides such as N-alkylacrylamide, N, N-dimethylacrylamide, 2-acrylamide propanesulfonic acid or a salt thereof, acrylamidepropyldimethylamine or an ester thereof or a quaternary salt thereof; metaacrylamide, N having 1 to 18 carbon atoms. Methylamides such as -alkylmetharylamide, N, N-dimethylmethacrylate, 2-methallylamide propanesulfonic acid or a salt thereof, methallylamide propyldimethylamine or an ester thereof or a quaternary salt thereof; N-vinylpyrrolidone, N. -N-vinylamides such as vinylformamide and N-vinylacetamide; vinyl cyanide such as acrylonitrile and methacrylnitrile; vinyl ethers such as alkylvinyl ethers having 1 to 18 carbon atoms, hydroxyalkyl vinyl ethers and alkoxyalkyl vinyl ethers; vinyl chloride , Vinyl halide compounds such as vinylidene chloride, vinyl fluoride, vinylidene fluoride, vinyl bromide; vinylsilanes such as trimethoxyvinylsilane; allyl halides such as allyl acetate and allyl chloride; allyl alcohol, dimethoxyallyl alcohol Allyl alcohols such as trimethyl- (3-acrylamide-3-dimethylpropyl) -ammonium chloride, comonomers such as acrylamide-2-methylpropanesulfonic acid can be mentioned. These can be used alone or in combination of two or more.
特に、水酸基含有α−オレフィン類を共重合したEVOHは、二次成形性が良好になる点で好ましく、中でも側鎖に1級水酸基を有するEVOH、特には1,2−ジオール構造を側鎖に有するEVOHが好ましい。 In particular, EVOH obtained by copolymerizing a hydroxyl group-containing α-olefin is preferable in that the secondary moldability is improved. Among them, EVOH having a primary hydroxyl group in the side chain, particularly 1,2-diol structure in the side chain. EVOH having is preferable.
かかる1,2−ジオール構造を側鎖に有するEVOHは、側鎖に1,2−ジオール構造単位を含むものである。かかる1,2−ジオール構造単位とは、具体的には下記一般式(1)で示される構造単位である。 An EVOH having such a 1,2-diol structure in a side chain contains a 1,2-diol structural unit in the side chain. The 1,2-diol structural unit is specifically a structural unit represented by the following general formula (1).
上記一般式(1)式中、R1〜R6はそれぞれ独立して水素原子または有機基を示し、Xは単結合または結合鎖を示す。 In the above general formula (1), R 1 to R 6 independently represent a hydrogen atom or an organic group, and X represents a single bond or a bond chain.
上記一般式(1)で表される1,2−ジオール構造単位における有機基としては、例えばメチル基、エチル基、n−プロピル基、イソプロピル基、n−ブチル基、イソブチル基、tert−ブチル基等の飽和炭化水素基、フェニル基、ベンジル基等の芳香族炭化水素基、ハロゲン原子、水酸基、アシルオキシ基、アルコキシカルボニル基、カルボキシル基、スルホン酸基等があげられる。
R1〜R3は、通常炭素数1〜30、特には炭素数1〜15、さらには炭素数1〜4の飽和炭化水素基または水素原子が好ましく、水素原子が最も好ましい。R4〜R6は、通常炭素数1〜30、特には炭素数1〜15、さらには炭素数1〜4のアルキル基または水素原子が好ましく、水素原子が最も好ましい。特に、R1〜R6がすべて水素原子であるものが最も好ましい。
Examples of the organic group in the 1,2-diol structural unit represented by the general formula (1) include a methyl group, an ethyl group, an n-propyl group, an isopropyl group, an n-butyl group, an isobutyl group and a tert-butyl group. Examples thereof include saturated hydrocarbon groups such as, aromatic hydrocarbon groups such as phenyl group and benzyl group, halogen atoms, hydroxyl groups, acyloxy groups, alkoxycarbonyl groups, carboxyl groups and sulfonic acid groups.
R 1 to R 3 are usually preferably saturated hydrocarbon groups or hydrogen atoms having 1 to 30 carbon atoms, particularly 1 to 15 carbon atoms, and further preferably 1 to 4 carbon atoms, and hydrogen atoms are most preferable. R 4 to R 6 usually have 1 to 30 carbon atoms, particularly preferably 1 to 15 carbon atoms, more preferably an alkyl group or a hydrogen atom having 1 to 4 carbon atoms, and most preferably a hydrogen atom. In particular, it is most preferable that R 1 to R 6 are all hydrogen atoms.
また、上記一般式(1)で表される構造単位中のXは、代表的には単結合である。
なお、本発明の効果を阻害しない範囲であれば、Xは結合鎖であってもよい。かかる結合鎖としては特に限定されないが、例えば、アルキレン、アルケニレン、アルキニレン、フェニレン、ナフチレン等の炭化水素鎖(これらの炭化水素はフッ素、塩素、臭素等のハロゲン等で置換されていてもよい)の他、−O−、−(CH2O)m−、−(OCH2)m−、−(CH2O)mCH2−等のエーテル結合部位を含む構造;−CO−、−COCO−、−CO(CH2)mCO−、−CO(C6H4)CO−等のカルボニル基を含む構造;−S−、−CS−、−SO−、−SO2−等の硫黄原子を含む構造;−NR−、−CONR−、−NRCO−、−CSNR−、−NRCS−、−NRNR−等の窒素原子を含む構造;−HPO4−等のリン原子を含む構造等のヘテロ原子を含む構造;−Si(OR)2−、−OSi(OR)2−、−OSi(OR)2O−等の珪素原子を含む構造;−Ti(OR)2−、−OTi(OR)2−、−OTi(OR)2O−等のチタン原子を含む構造;−Al(OR)−、−OAl(OR)−、−OAl(OR)O−等のアルミニウム原子を含む構造等の金属原子を含む構造等があげられる。
また、mは自然数であり、通常1〜30、好ましくは1〜15、さらに好ましくは1〜10である。その中でも製造時あるいは使用時の安定性の点で−CH2OCH2−、および炭素数1〜10の炭化水素鎖が好ましく、さらには炭素数1〜6の炭化水素鎖、特には炭素数1であることが好ましい。
Further, X in the structural unit represented by the general formula (1) is typically a single bond.
In addition, X may be a binding chain as long as it does not hinder the effect of the present invention. The bonding chain is not particularly limited, but for example, a hydrocarbon chain such as alkylene, alkenylene, alkynylene, phenylene, naphthylene (these hydrocarbons may be substituted with halogens such as fluorine, chlorine and bromine). Other structures containing ether binding sites such as −O−, − (CH 2 O) m−, − (OCH 2 ) m−, − (CH 2 O) mCH 2 −; −CO−, −COCO−, − Structure containing carbonyl groups such as CO (CH 2 ) mCO-, -CO (C 6 H 4 ) CO-; Structure containing sulfur atoms such as -S-, -CS-, -SO-, -SO 2-; -NR -, - CONR -, - NRCO -, - CSNR -, - NRCS -, - structure containing a nitrogen atom such as NRNR-; -HPO 4 - structure containing a heteroatom structure such as that containing a phosphorus atom and the like; -Si (OR) 2 -, - OSi (OR) 2 -, - OSi (OR) structure containing 2 O- such as silicon atoms; -Ti (OR) 2 -, - OTi (OR) 2 -, - OTi (OR) 2 Structure containing titanium atom such as O−; Structure containing metal atom such as structure containing aluminum atom such as −Al (OR) −, −OAl (OR) −, −OAl (OR) O− Can be given.
Further, m is a natural number, and is usually 1 to 30, preferably 1 to 15, and more preferably 1 to 10. Among them, −CH 2 OCH 2 − and a hydrocarbon chain having 1 to 10 carbon atoms are preferable in terms of stability during production or use, and a hydrocarbon chain having 1 to 6 carbon atoms, particularly 1 carbon atom. Is preferable.
上記一般式(1)で表される1,2−ジオール構造単位における最も好ましい構造は、R1〜R6がすべて水素原子であり、Xが単結合であるものである。すなわち、下記一般式(1a)で示される構造単位が最も好ましい。 The most preferable structure in the 1,2-diol structural unit represented by the general formula (1) is that R 1 to R 6 are all hydrogen atoms and X is a single bond. That is, the structural unit represented by the following general formula (1a) is most preferable.
上記一般式(1a)で表される1,2−ジオール構造単位を含有する場合、その含有量は通常0.1〜20モル%、さらには0.1〜15モル%、特には0.1〜10モル%のものが好ましい。 When the 1,2-diol structural unit represented by the general formula (1a) is contained, the content thereof is usually 0.1 to 20 mol%, further 0.1 to 15 mol%, particularly 0.1. 10 mol% is preferable.
また、本発明で用いるEVOHは、さらにウレタン化、アセタール化、シアノエチル化、オキシアルキレン化等の「後変性」されたEVOHを用いることもできる。 Further, as the EVOH used in the present invention, "post-modified" EVOH such as urethanization, acetalization, cyanoethylation, and oxyalkyleneization can also be used.
<ホウ素化合物>
本発明で用いるホウ素化合物としては、ホウ酸またはその金属塩、例えば、ホウ酸ナトリウム(メタホウ酸ナトリウム、二ホウ酸ナトリウム、四ホウ酸ナトリウム、五ホウ酸ナトリウム、六ホウ酸ナトリウム、八ホウ酸ナトリウム等)、ホウ酸カリウム(メタホウ酸カリウム、四ホウ酸カリウム、五ホウ酸カリウム、六ホウ酸カリウム、八ホウ酸カリウム等)、ホウ酸リチウム(メタホウ酸リチウム、四ホウ酸リチウム、五ホウ酸リチウム等);ホウ酸カルシウム、ホウ酸バリウム(オルトホウ酸バリウム、メタホウ酸バリウム、二ホウ酸バリウム、四ホウ酸バリウム等)、ホウ酸マグネシウム(オルトホウ酸マグネシウム、二ホウ酸マグネシウム、メタホウ酸マグネシウム、四ホウ酸三マグネシウム、四ホウ酸五マグネシウム等);ホウ酸マンガン(ホウ酸第1マンガン、メタホウ酸マンガン、四ホウ酸マンガン等)、ホウ酸コバルト、ホウ酸亜鉛(四ホウ酸亜鉛、メタホウ酸亜鉛等)、ホウ酸カドミウム(オルトホウ酸カドミウム、四ホウ酸カドミウム等)、ホウ酸銀(メタホウ酸銀、四ホウ酸銀等)、ホウ酸銅(ホウ酸第2銅、メタホウ酸銅、四ホウ酸銅等)、ホウ酸ニッケル(オルトホウ酸ニッケル、二ホウ酸ニッケル、四ホウ酸ニッケル、八ホウ酸ニッケル等)、ホウ酸アルミニウム・カリウム、ホウ酸アンモニウム(メタホウ酸アンモニウム、四ホウ酸アンモニウム、五ホウ酸アンモニウム、八ホウ酸アンモニウム等)、ホウ酸鉛(メタホウ酸鉛、六ホウ酸鉛等)、ホウ酸ビスマス、等の他、ホウ砂、カーナイト、インヨーアイト、コトウ石、スイアン石、ザイベリ石等のホウ酸塩鉱物等があげられ、好適にはホウ砂、ホウ酸があげられる。これらは単独でもしくは2種以上併せて用いることができる。
<Boron compound>
The boron compound used in the present invention includes boric acid or a metal salt thereof, for example, sodium borate (sodium metaborate, sodium diborate, sodium tetraborate, sodium pentaborate, sodium hexaborate, sodium octaborate). Etc.), potassium borate (potassium metaborate, potassium tetraborate, potassium pentaborate, potassium hexaborate, potassium octaborate, etc.), lithium borate (lithium metaborate, lithium tetraborate, lithium pentaborate, etc.) Etc.); Calcium borate, barium borate (barium orthoborate, barium metaborate, barium diborate, barium tetraborate, etc.), magnesium borate (magnesium orthoborate, magnesium diborate, magnesium metaborate, tetraborate, etc.) Trimagnesium acid, pentamagnesium tetraborate, etc.); Manganese borate (primary borate, manganese metaborate, manganese tetraborate, etc.), cobalt borate, zinc borate (zinc tetraborate, zinc metaborate, etc.) ), Cadmium borate (cadmium orthoborate, cadmium tetraborate, etc.), silver borate (silver metaborate, silver tetraborate, etc.), copper borate (second copper borate, copper metaborate, copper tetraborate, etc.) Etc.), Nickel borate (nickel orthoborate, nickel diborate, nickel tetraborate, nickel octaborate, etc.), aluminum / potassium borate, ammonium borate (ammonium metaborate, ammonium tetraborate, pentaboric acid, etc.) Ammonium, ammonium octaborate, etc.), lead borate (lead metaborate, lead hexaborate, etc.), bismuth borate, etc. Examples thereof include borate minerals, and preferably boric acid and boric acid. These can be used alone or in combination of two or more.
<滑剤>
本発明で用いる滑剤としては、高級脂肪酸類があげられ、例えば、ラウリン酸、ミリスチン酸、パルミチン酸、ステアリン酸、ベヘニン酸、オレイン酸等の高級脂肪酸;これら高級脂肪酸のアルミニウム塩、カルシウム塩、亜鉛塩、マグネシウム塩、バリウム塩等の高級脂肪酸の金属塩;上記高級脂肪酸のメチルエステル、イソプロピルエステル、ブチルエステル、オクチルエステル等の高級脂肪酸のエステル;ステアリン酸アミド、ベヘニン酸アミド等の飽和高級脂肪酸アミド、オレイン酸アミド、エルカ酸アミド等の不飽和高級脂肪酸アミド、エチレンビスステアリン酸アミド、エチレンビスオレイン酸アミド、エチレンビスエルカ酸アミド、エチレンビスラウリン酸アミド等のビス高級脂肪酸アミド等の高級脂肪酸のアミドがあげられる。また、分子量500〜10000程度の低分子量ポリエチレン、低分子量ポリプロピレン、またはこれらの酸変性品等の低分子量ポリオレフィン;高級アルコール、エステルオリゴマー、フッ化エチレン樹脂等があげられる。これらは単独でもしくは2種以上併せて用いることができる。上記滑剤に用いる化合物において、押出安定性と市場入手性の観点で、高級脂肪酸類が好ましく、上記高級脂肪酸類の1分子における炭素数は通常、炭素数12〜25であり、好ましくは炭素数12〜23であり、特に好ましくは炭素数15〜20である。また、上記滑剤に用いる化合物において、上記高級脂肪酸類の価数は押出し安定性と市場入手性の観点から通常1〜5価であり、好ましくは1〜3価であり、特に好ましくは1〜2価である。このとき、かかる価数とは、上記滑剤に用いる化合物1分子に有する高級脂肪酸由来の構造の数を意味し、例えば滑剤としてビスステアリン酸アミドを用いる場合、炭素数18の高級脂肪酸分子に由来する構造を1分子内に2か所有するため、炭素数18の高級脂肪酸のアミドであり、高級脂肪酸の価数は2価であるとする。これらのなかでも、好ましくは高級脂肪酸、高級脂肪酸の金属塩、高級脂肪酸のエステル、高級脂肪酸のアミドであり、特に好ましくは高級脂肪酸の金属塩、高級脂肪酸のアミドであり、さらに好ましくは、押出安定性の観点から、高級脂肪酸のアミドである。
<Glidant>
Examples of the lubricant used in the present invention include higher fatty acids, for example, higher fatty acids such as lauric acid, myristic acid, palmitic acid, stearic acid, behenic acid, and oleic acid; aluminum salts, calcium salts, and zinc of these higher fatty acids. Metal salts of higher fatty acids such as salts, magnesium salts and barium salts; esters of higher fatty acids such as methyl ester, isopropyl ester, butyl ester and octyl ester of the higher fatty acids; saturated higher fatty acid amides such as stearate amide and behenic acid amide. Of higher fatty acids such as unsaturated higher fatty acid amides such as oleic acid amide and erucic acid amide, ethylene bisstearic acid amide, ethylene bisoleic acid amide, ethylene bis-erucic acid amide and bis higher fatty acid amide such as ethylene bislauric acid amide. Amid can be mentioned. Examples thereof include low molecular weight polyethylene having a molecular weight of about 500 to 10000, low molecular weight polypropylene, and low molecular weight polyolefins such as acid-modified products thereof; higher alcohols, ester oligomers, ethylene fluoride resins and the like. These can be used alone or in combination of two or more. In the compound used for the lubricant, higher fatty acids are preferable from the viewpoint of extrusion stability and market availability, and the number of carbon atoms in one molecule of the above higher fatty acids is usually 12 to 25, preferably 12 carbon atoms. It is ~ 23, and particularly preferably 15 to 20 carbon atoms. Further, in the compound used for the lubricant, the valence of the higher fatty acids is usually 1 to 5 valences, preferably 1 to 3 valences, and particularly preferably 1 to 2 valences from the viewpoint of extrusion stability and market availability. It is a value. At this time, such a valence means the number of structures derived from higher fatty acids contained in one molecule of the compound used for the lubricant. For example, when bisstearic acid amide is used as the lubricant, it is derived from a higher fatty acid molecule having 18 carbon atoms. Since it has two structures in one molecule, it is an amide of a higher fatty acid having 18 carbon atoms, and the valence of the higher fatty acid is divalent. Among these, a higher fatty acid, a metal salt of a higher fatty acid, an ester of a higher fatty acid, and an amide of a higher fatty acid are preferable, and a metal salt of a higher fatty acid and an amide of a higher fatty acid are particularly preferable, and extrusion stability is more preferable. From a sexual point of view, it is a higher fatty acid amide.
上記滑剤としては、固形状(粉末、微粉末、フレーク等)、半固体状、液体状、ペースト状、溶液状、エマルジョン状(水分散液)等の任意の性状のものが使用可能であるが、中でも粉末状が好ましい。粉末状の滑剤の粒径は、通常0.1〜100μm、好ましくは1〜75μm、特に好ましくは5〜50μmである。 As the lubricant, any property such as solid (powder, fine powder, flakes, etc.), semi-solid, liquid, paste, solution, emulsion (aqueous dispersion), etc. can be used. Of these, powder is preferable. The particle size of the powdered lubricant is usually 0.1 to 100 μm, preferably 1 to 75 μm, and particularly preferably 5 to 50 μm.
<EVOHペレットの製造>
EVOHからペレットを製造する方法としては、従来公知の方法を採用でき、例えば、
a)溶融状態のEVOHを押出機の吐出口から押し出し、溶融状態でカットした後、冷却固化してペレットを作製するホットカット方式、
b)溶融状態のEVOHを凝固浴中に押し出し、冷却固化により得られたEVOHストランドをカットするストランドカット方式、等があげらる。
<Manufacturing of EVOH pellets>
As a method for producing pellets from EVOH, a conventionally known method can be adopted, for example,
a) A hot-cut method in which EVOH in a molten state is extruded from the discharge port of an extruder, cut in a molten state, and then cooled and solidified to produce pellets.
b) A strand cut method in which the molten EVOH is extruded into a coagulation bath and the EVOH strands obtained by cooling and solidifying are cut.
上記a)ホットカット方式、b)ストランドカット方式のいずれにおいても、ペレット原料として使用するEVOHとしては、(α)EVOHの製造において、エチレン−ビニルエステル系共重合体の溶液をケン化することにより得られたEVOHの溶液またはスラリー、またはEVOH含水組成物(以下、「EVOH溶液・含水組成物」と称することがある);あるいは(β)EVOH(乾燥EVOH)のペレットを溶融し、かかる溶融状態のEVOHを用いることができる。 In both of the above a) hot-cut method and b) strand-cut method, the EVOH used as a pellet raw material is obtained by saponifying a solution of an ethylene-vinyl ester copolymer in the production of (α) EVOH. The obtained EVOH solution or slurry, or EVOH hydrous composition (hereinafter, may be referred to as "EVOH solution / hydrous composition"); or (β) EVOH (dry EVOH) pellets are melted, and such a molten state is obtained. EVOH can be used.
上記EVOH含水組成物とは、上記EVOHの溶液またはスラリーの含水率を、溶媒を用いて適宜調整したものであり、EVOH含水組成物中におけるEVOHの濃度は、通常20〜60重量%である。 The EVOH water-containing composition is obtained by appropriately adjusting the water content of the EVOH solution or slurry using a solvent, and the concentration of EVOH in the EVOH water-containing composition is usually 20 to 60% by weight.
上記の溶媒としては、アルコール、水/アルコール混合溶媒等を用いることができる。これらのうち、水/アルコール混合溶媒が好ましい。上記アルコールとしては、例えば、メタノール、エタノール、プロパノール、n−ブタノール、tert−ブタノール等の炭素数1〜10の脂肪族アルコールを用いることができ、特にメタノールが好ましい。また、水/アルコール混合重量比は、80/20〜5/95が好ましい。 As the above solvent, alcohol, water / alcohol mixed solvent and the like can be used. Of these, a water / alcohol mixed solvent is preferable. As the alcohol, for example, an aliphatic alcohol having 1 to 10 carbon atoms such as methanol, ethanol, propanol, n-butanol, and tert-butanol can be used, and methanol is particularly preferable. The water / alcohol mixed weight ratio is preferably 80/20 to 5/95.
また、上記EVOH含水組成物としては、通常EVOH100重量部に対し、アルコールを0〜10重量部、水を10〜500重量部含有することが好ましい。 The EVOH water-containing composition usually contains 0 to 10 parts by weight of alcohol and 10 to 500 parts by weight of water with respect to 100 parts by weight of EVOH.
上記EVOH含水組成物の含水率を調整する方法としては特に限定しないが、含水率を上げるためには、EVOHの溶液またはスラリーに上記の溶媒をスプレーする方法、EVOHの溶液またはスラリーと上記の溶媒とを混合する方法、EVOHの溶液またはスラリーを上記の溶媒の蒸気と接触させる方法等を採用できる。含水率を下げるためには、EVOHの溶液またはスラリーを適宜乾燥すればよく、例えば流動式熱風乾燥機あるいは静置式熱風乾燥機を用いて乾燥することができる。 The method for adjusting the water content of the EVOH water-containing composition is not particularly limited, but in order to increase the water content, a method of spraying the above solvent on the EVOH solution or slurry, the EVOH solution or slurry and the above solvent A method of mixing with, a method of bringing an EVOH solution or a slurry into contact with the vapor of the above solvent, or the like can be adopted. In order to reduce the water content, the EVOH solution or slurry may be appropriately dried, and can be dried using, for example, a fluid hot air dryer or a static hot air dryer.
つぎに、a)ホットカット方式および、b)ストランドカット方式について説明する。 Next, a) hot-cut method and b) strand-cut method will be described.
a)ホットカット方式
EVOH溶液・含水組成物をホットカット方式で製造するペレット原料として押出機に投入する場合、押出機内でのEVOH溶液・含水組成物の温度は、70〜170℃が好ましく、より好ましくは80〜170℃、さらに好ましくは90〜170℃である。EVOH溶液・含水組成物の温度が低すぎる場合は、EVOHが完全に溶融しない傾向があり、高すぎる場合は、EVOHが熱劣化を受けやすくなる傾向がある。
また、乾燥EVOHをペレット原料として使用する場合の押出機内でのEVOHの温度は150〜300℃が好ましく、より好ましくは160〜280℃、さらに好ましくは170〜250℃である。
なお、上記EVOH溶液・含水組成物および乾燥EVOHの温度とは、押出機シリンダーに設置した温度センサーにより押出機先端部吐出口付近で検出した温度をいう。
a) Hot-cut method When the EVOH solution / water-containing composition is put into an extruder as a pellet raw material to be produced by the hot-cut method, the temperature of the EVOH solution / water-containing composition in the extruder is preferably 70 to 170 ° C. It is preferably 80 to 170 ° C, more preferably 90 to 170 ° C. If the temperature of the EVOH solution / water-containing composition is too low, the EVOH tends not to melt completely, and if it is too high, the EVOH tends to be susceptible to thermal deterioration.
When dry EVOH is used as a pellet raw material, the temperature of EVOH in the extruder is preferably 150 to 300 ° C, more preferably 160 to 280 ° C, and even more preferably 170 to 250 ° C.
The temperature of the EVOH solution / water-containing composition and the dried EVOH refers to the temperature detected in the vicinity of the ejection port at the tip of the extruder by the temperature sensor installed in the extruder cylinder.
押出機のダイスから押し出されるEVOH溶液・含水組成物、すなわち溶融状態にあるEVOHは、冷却固化する前にカットされる。カット方式は、大気中でカットするホットカット方式(空中ホットカット方式)、冷却水で満たされたカッター設置容器内に押出され冷却水中でカットする水中カット方式のいずれでもよい。 The EVOH solution / water-containing composition extruded from the die of the extruder, that is, the EVOH in the molten state is cut before cooling and solidifying. The cutting method may be either a hot cutting method of cutting in the air (air hot cutting method) or an underwater cutting method of extruding into a cutter installation container filled with cooling water and cutting in cooling water.
上記水中カット方式における冷却水の温度は、溶融状態で押し出されたEVOHが瞬時に固化(凝固)しない程度の温度であり、EVOH溶液・含水組成物を原料として用いる場合の冷却水の温度は−20〜50℃とすることが好ましく、より好ましくは−5〜30℃である。
また、乾燥EVOHを原料とする場合、EVOH溶液・含水組成物を原料として用いる場合よりも凝固しやすいことから、水中カット方式における冷却水の温度は、EVOH含水組成物を原料とする場合よりも高く、通常0〜90℃であり、好ましくは20〜70℃である。
The temperature of the cooling water in the above-mentioned underwater cutting method is such that the EVOH extruded in the molten state does not instantly solidify (solidify), and the temperature of the cooling water when the EVOH solution / water-containing composition is used as a raw material is-. The temperature is preferably 20 to 50 ° C, more preferably −5 to 30 ° C.
Further, when dry EVOH is used as a raw material, it is easier to solidify than when an EVOH solution / water-containing composition is used as a raw material. Therefore, the temperature of the cooling water in the underwater cutting method is higher than that when the EVOH water-containing composition is used as a raw material. It is high, usually 0 to 90 ° C, preferably 20 to 70 ° C.
上記冷却水は、水に限定されず、水/アルコール混合溶液;ベンゼン等の芳香族炭化水素類;アセトン、メチルエチルケトン等のケトン類;ジプロピルエーテル等のエーテル類;酢酸メチル、酢酸エチル、プロピオン酸メチル等の有機エステル類等も用いることができる。これらのうち、取扱い性が容易という点から、水、または水/アルコール混合溶液が用いられる。水/アルコール混合溶液において、水/アルコール(重量比)は通常90/10〜99/1である。なお、上記アルコールとしては、メタノール、エタノール、プロパノール等の低級アルコールを用いることができ、工業上、メタノールが好ましく用いられる。 The cooling water is not limited to water, but is a water / alcohol mixed solution; aromatic hydrocarbons such as benzene; ketones such as acetone and methyl ethyl ketone; ethers such as dipropyl ether; methyl acetate, ethyl acetate and propionic acid. Organic esters such as methyl can also be used. Of these, water or a water / alcohol mixed solution is used because it is easy to handle. In the water / alcohol mixed solution, the water / alcohol (weight ratio) is usually 90/10 to 99/1. As the alcohol, lower alcohols such as methanol, ethanol and propanol can be used, and methanol is preferably used industrially.
b)ストランドカット方式
EVOH溶液・含水組成物をストランドカット方式で製造するペレット原料として押出機に投入する場合、凝固浴に押し出されるEVOHの温度は、通常、10〜100℃、凝固浴の温度は、押し出されたEVOHが冷却固化できる温度で、通常、−10〜40℃であり、滞留時間は、通常、10〜400秒間程度である。
また、乾燥EVOHをペレット原料として押出機に投入する場合、凝固浴にEVOHが押し出される温度は、通常、150〜300℃、凝固浴の温度は、通常、0〜90℃であり、滞留時間は2〜400秒間程度である。
b) Strand-cut method When the EVOH solution / water-containing composition is put into an extruder as a pellet raw material produced by the strand-cut method, the temperature of EVOH extruded into the coagulation bath is usually 10 to 100 ° C., and the temperature of the coagulation bath is , The temperature at which the extruded EVOH can be cooled and solidified, usually −10 to 40 ° C., and the residence time is usually about 10 to 400 seconds.
When dry EVOH is put into an extruder as a pellet raw material, the temperature at which EVOH is extruded into the coagulation bath is usually 150 to 300 ° C., the temperature of the coagulation bath is usually 0 to 90 ° C., and the residence time is It takes about 2 to 400 seconds.
凝固浴に用いる凝固液としては、上記a)ホットカット方式の冷却水と同様の溶液を採用することができる。 As the coagulation liquid used in the coagulation bath, a solution similar to the above-mentioned a) hot-cut type cooling water can be adopted.
このようにして、EVOHペレットが得られる。 In this way, EVOH pellets are obtained.
以上のようなEVOHペレットのうち、後述するホウ素化合物の含有処理の点から、ペレット内部に複数の孔を有する多孔質ペレットを用いることが好ましい。この孔内へホウ素化合物を浸透させることで、ホウ素化合物をペレット中に保持しやすくなり、効率的にホウ素化合物をペレット内部へ取り込ませることができる。上記、多孔質ペレットの孔の大きさは、その孔内へホウ素化合物が浸透できる範囲であればよく、特に限定されない。 Among the above EVOH pellets, it is preferable to use a porous pellet having a plurality of pores inside the pellet from the viewpoint of the treatment containing a boron compound described later. By infiltrating the boron compound into the pores, the boron compound can be easily retained in the pellet, and the boron compound can be efficiently taken into the pellet. The size of the pores of the porous pellets is not particularly limited as long as the boron compound can penetrate into the pores.
このような多孔質ペレットは、通常、ペレット原料として、上記EVOH樹脂含水組成物を使用し、当該EVOH含水組成物中のEVOH濃度、溶媒の種類、押し出し時の温度、凝固浴の温度、滞留時間等を調整することで、得ることができる。 Such a porous pellet usually uses the above-mentioned EVOH resin water-containing composition as a pellet raw material, and the EVOH concentration in the EVOH water-containing composition, the type of solvent, the temperature at the time of extrusion, the temperature of the coagulation bath, and the residence time. It can be obtained by adjusting the above.
また、多孔質ペレットの含水率は20〜80重量%が好ましい。当該含水率の多孔質ペレットは、後述のホウ素化合物の含有させる工程において、ホウ素化合物を均一かつ迅速に含有させることができる。 The water content of the porous pellets is preferably 20 to 80% by weight. The porous pellets having a water content can uniformly and rapidly contain the boron compound in the step of containing the boron compound, which will be described later.
EVOHペレットの形状は、通常、ペレットの製造方法に依存し、種々の形状のものを用いることができ、上記各方法によって得られるEVOHペレットおよび本発明のEVOH組成物ペレットの形状は任意である。ペレットの形状としては、例えば、球形、オーバル形、円柱形、立方体形、直方体形、不定形等があるが、通常、オーバル形、または円柱形であり、その大きさは、後に成形材料として用いる場合の利便性の観点から、オーバル形の場合は長径が通常1〜10mm、好ましくは2〜7mmであり、短径は通常1〜6mm、好ましくは2〜5mmであり、円柱形の場合は底面の直径が通常1〜10mm、好ましくは2〜7mmであり、長さは通常1〜10mm、好ましくは3〜8mmである。 The shape of the EVOH pellet usually depends on the method for producing the pellet, and various shapes can be used, and the shape of the EVOH pellet obtained by each of the above methods and the EVOH composition pellet of the present invention is arbitrary. The shape of the pellet includes, for example, spherical, oval, cylindrical, cubic, rectangular parallelepiped, amorphous, etc., but is usually oval or cylindrical, and the size thereof will be used later as a molding material. From the viewpoint of convenience in the case, the major axis is usually 1 to 10 mm, preferably 2 to 7 mm in the case of the oval type, the minor axis is usually 1 to 6 mm, preferably 2 to 5 mm in the case of the cylindrical type, and the bottom surface in the case of the cylindrical type. The diameter of the cylinder is usually 1 to 10 mm, preferably 2 to 7 mm, and the length is usually 1 to 10 mm, preferably 3 to 8 mm.
また、本発明で用いるEVOHペレットは、異なる他のEVOHペレットとの混合物であってもよく、上記他のEVOHペレットとしては、エチレン構造単位の含有量が異なるもの、ケン化度が異なるもの、メルトフローレート(MFR)が異なるもの、他の共重合成分が異なるもの、例えば、前記一般式(1)で表される1,2−ジオール構造単位の含有量が異なるもの、等をあげることができる。 Further, the EVOH pellet used in the present invention may be a mixture with other EVOH pellets different from each other, and the other EVOH pellets mentioned above include those having a different content of ethylene structural units, those having a different degree of saponification, and melts. Examples thereof include those having different flow rates (MFR) and those having different other copolymerization components, for example, those having different contents of 1,2-diol structural units represented by the general formula (1). ..
本発明のホウ素化合物および滑剤含有EVOHペレットは、上記EVOHペレットに特定量のホウ素化合物および滑剤を含有させることにより得られる。この本発明のホウ素化合物および滑剤含有EVOHペレットの製造方法は特に限定されるものではないが、以下に代表的な製造につき説明する。 The boron compound and lubricant-containing EVOH pellet of the present invention can be obtained by adding a specific amount of boron compound and lubricant to the EVOH pellet. The method for producing the boron compound and lubricant-containing EVOH pellets of the present invention is not particularly limited, but typical production will be described below.
<ホウ素化合物および滑剤含有EVOHペレットの製造>
本発明のホウ素化合物および滑剤含有EVOHペレットは、EVOHペレットとホウ素化合物とを接触させることによりホウ素化合物を含有させる工程、ホウ素化合物を含有するEVOHペレットを洗浄して、ペレット表層部のホウ素化合物含有量を、ホウ素換算で当該ペレット重量あたり1.7ppm以下にする工程、および滑剤を含有させる工程を経ることにより得ることができる。これらの工程は、どちらの工程を先に行ってもよく、また同時に行ってもよい。上記工程を同時に行う際は、例えば、ホウ素化合物と滑剤を含有する溶液を用いる等により行うことができる。
<Manufacture of EVOH pellets containing boron compounds and lubricants>
The boron compound and lubricant-containing EVOH pellet of the present invention is a step of adding a boron compound by contacting the EVOH pellet with the boron compound, and the EVOH pellet containing the boron compound is washed to contain the boron compound in the surface layer of the pellet. Can be obtained by going through a step of reducing the amount of boron to 1.7 ppm or less per the weight of the pellet and a step of adding a lubricant. Either of these steps may be performed first, or may be performed at the same time. When the above steps are performed at the same time, for example, a solution containing a boron compound and a lubricant can be used.
<ホウ素化合物を含有させる工程>
上記ホウ素化合物を含有させる工程は、前記EVOHペレットとホウ素化合物とを接触させることにより行う。
<Step of adding boron compound>
The step of containing the boron compound is performed by bringing the EVOH pellet into contact with the boron compound.
上記EVOHペレットとホウ素化合物とを接触させる方法としては、例えば、
i)EVOHペレット製造段階でEVOHとホウ素化合物とを接触させる方法、
ii)予め作製したEVOHペレットとホウ素化合物とを接触させる方法、
等により行うことができる。
As a method of bringing the EVOH pellet into contact with the boron compound, for example,
i) A method of contacting EVOH with a boron compound in the EVOH pellet manufacturing stage,
ii) A method of contacting a previously prepared EVOH pellet with a boron compound,
It can be done by such as.
上記i)のEVOHペレット製造段階でEVOHとホウ素化合物とを接触させる方法としては、例えば、ペレット原料(EVOH溶液・含水組成物、乾燥EVOH)にホウ素化合物を添加、あるいはホウ素化合物を含有する溶液を、ペレット製造する際の凝固液に使用する方法等があげられる。
ペレット原料としてEVOH溶液・含水組成物を用いる場合には、当該EVOH溶液・含水組成物にホウ素化合物を添加すればよい。また、乾燥EVOHペレットを溶融し、かかる溶融状態のEVOHを原料として用いる場合、乾燥EVOHに予めホウ素化合物を含有させればよい。
好ましくは、ホウ素化合物を添加したEVOH含水組成物を、凝固液中にストランド状に押し出し、得られたストランドを切断する方法である。
As a method of contacting EVOH with a boron compound in the EVOH pellet production step of i), for example, a boron compound is added to a pellet raw material (EVOH solution / water-containing composition, dried EVOH), or a solution containing the boron compound is added. , The method used for the coagulating liquid in the production of pellets and the like.
When an EVOH solution / water-containing composition is used as the pellet raw material, a boron compound may be added to the EVOH solution / water-containing composition. When the dried EVOH pellets are melted and the melted EVOH is used as a raw material, the dried EVOH may contain a boron compound in advance.
Preferably, the EVOH water-containing composition to which the boron compound is added is extruded into a coagulating liquid in the form of strands, and the obtained strands are cleaved.
上記ii)の予め作製したEVOHペレットとホウ素化合物とを接触させる方法としては、ホウ素化合物を含有する溶液をEVOHペレットに噴霧する方法;ホウ素化合物を含有する溶液にEVOHペレットを浸漬する方法;ホウ素化合物を含有する溶液を撹拌しながら、EVOHペレットを投入する方法等があげられる。これらのうち、ホウ素化合物をペレット内部にまで効率よく含有させることができる点で、ホウ素化合物を含有する溶液を撹拌しながら、EVOHペレットを投入する方法が好ましく用いられる。 As a method of contacting the EVOH pellet prepared in advance of ii) with the boron compound, a method of spraying a solution containing the boron compound onto the EVOH pellet; a method of immersing the EVOH pellet in the solution containing the boron compound; Examples thereof include a method of adding EVOH pellets while stirring the solution containing the above. Of these, a method in which the EVOH pellet is charged while stirring the solution containing the boron compound is preferably used because the boron compound can be efficiently contained inside the pellet.
上記ホウ素化合物を含有する溶液の溶媒としては、例えば、水;メタノール、エタノール、プロパノール等の低級アルコール;水/アルコール混合用液等を使用することができる。なお、水/アルコール混合溶液において、水/アルコール(重量比)は通常90/10〜99/1である。 As the solvent of the solution containing the boron compound, for example, water; lower alcohol such as methanol, ethanol, propanol; water / alcohol mixing solution and the like can be used. In the water / alcohol mixed solution, the water / alcohol (weight ratio) is usually 90/10 to 99/1.
また、EVOHペレットとホウ素化合物との接触処理に用いるホウ素化合物の溶液の濃度は、通常0.001〜1重量%、好ましくは0.003〜0.5重量%である。かかる濃度が低すぎると、所定量のホウ素化合物を含有させることが困難となる傾向があり、高すぎると最終的に得られる成形物の外観が低下する傾向にある。 The concentration of the solution of the boron compound used for the contact treatment between the EVOH pellet and the boron compound is usually 0.001 to 1% by weight, preferably 0.003 to 0.5% by weight. If the concentration is too low, it tends to be difficult to contain a predetermined amount of the boron compound, and if it is too high, the appearance of the finally obtained molded product tends to be deteriorated.
上記EVOHペレット中のホウ素化合物量(EVOHペレット中のホウ素化合物全含有量)は、ホウ素化合物を含有する溶液におけるホウ素化合物の濃度、接触処理時間、接触処理温度、接触処理時の撹拌速度や処理されるEVOHペレットの含水率等により、コントロールすることが可能である。 The amount of the boron compound in the EVOH pellet (total content of the boron compound in the EVOH pellet) is determined by the concentration of the boron compound in the solution containing the boron compound, the contact treatment time, the contact treatment temperature, the stirring speed at the time of the contact treatment, and the treatment. It can be controlled by the water content of the EVOH pellets.
以上のようなEVOHペレットとホウ素化合物とを接触させる方法のうち、種々のペレットに適用でき、汎用性に優れているという点で、ii)の予め作製したEVOHペレットとホウ素化合物とを接触させる方法が好ましい。より好ましくは、前記の多孔質EVOHペレットを、ホウ素化合物の溶液と接触させる方法である。 Among the methods for contacting the EVOH pellet with the boron compound as described above, the method for contacting the EVOH pellet prepared in advance in ii) with the boron compound in that it can be applied to various pellets and has excellent versatility. Is preferable. More preferably, it is a method of contacting the porous EVOH pellet with a solution of a boron compound.
このようなホウ素化合物接触処理により得られるホウ素化合物を含有するEVOHペレット〔ペレット表層部におけるホウ素化合物含有量については未調整であり、以下、このペレットを「表層部ホウ素調整前EVOHペレット」という〕に含有されるホウ素化合物量(EVOHペレット中のホウ素化合物全含有量)は、ホウ素換算で、通常10〜10000ppmであり、好ましくは20〜5000ppm、さらに好ましくは30〜3000ppmである。かかる含有量が少なすぎると、ホウ素化合物の添加効果が低下する傾向があり、多すぎると最終的に得られる成形物の外観が低下する傾向がある。 An EVOH pellet containing a boron compound obtained by such a boron compound contact treatment [the content of the boron compound in the surface layer of the pellet has not been adjusted, and the pellet is hereinafter referred to as "EVOH pellet before boron adjustment in the surface layer"]. The amount of the boron compound contained (total content of the boron compound in the EVOH pellet) is usually 10 to 10000 ppm, preferably 20 to 5000 ppm, and more preferably 30 to 3000 ppm in terms of boron. If the content is too small, the effect of adding the boron compound tends to decrease, and if it is too large, the appearance of the finally obtained molded product tends to deteriorate.
上記表層部ホウ素調整前EVOHペレット中に含有されるホウ素化合物の量〔ホウ素化合物全含有量(ホウ素換算)〕は、ペレットを濃硝酸とともにマイクロウェーブ分解法にて処理して得られた溶液に、純水を加えて定容したものを検液とし、誘導結合プラズマ発光分析計(ICP−AES)で測定される量である。 The amount of boron compound [total boron compound content (boron equivalent)] contained in the above-mentioned surface layer portion boron-adjusted EVOH pellet is determined by adding a solution obtained by treating the pellet with concentrated nitrate by a microwave decomposition method. The amount is measured by an inductively coupled plasma emission spectrometer (ICP-AES) using pure water as a test solution.
上記の工程によって得られる表層部ホウ素調整前EVOHペレットは、そのまま次の工程に供してもよいが、通常、ペレットを乾燥することが好ましい。かかる乾燥に際しては公知の方法を採用することができ、例えば、円筒・溝型撹拌乾燥器、円筒乾燥器、回転乾燥器、流動層乾燥器、振動流動層乾燥器、円錐回転型乾燥器等を用いた流動乾燥や回分式箱型乾燥器、バンド乾燥器、トンネル乾燥器、竪型サイロ乾燥器等を用いた静置乾燥等により乾燥すればよい。80〜150℃の窒素ガス等の気体を乾燥器内を通過させることで、表層部ホウ素調整前EVOHペレットに影響を及ぼさないで、効率よく乾燥させることができる。 The surface layer portion of the EVOH pellet before boron adjustment obtained by the above step may be used as it is in the next step, but it is usually preferable to dry the pellet. A known method can be adopted for such drying, for example, a cylindrical / groove type stirring dryer, a cylindrical dryer, a rotary dryer, a fluidized bed dryer, a vibrating fluidized bed dryer, a conical rotary dryer, or the like. It may be dried by the fluidized bed used or a static drying using a batch box type dryer, a band dryer, a tunnel dryer, a vertical silo dryer or the like. By passing a gas such as nitrogen gas at 80 to 150 ° C. through the dryer, the surface layer portion of the EVOH pellet before boron adjustment can be efficiently dried without affecting the EVOH pellets.
<EVOHペレットを洗浄する工程>
つぎにEVOHペレットを洗浄する工程について説明する。
上記表層部ホウ素調整前EVOHペレットは、当該ペレットに含まれるホウ素化合物の全含有量、およびペレット表層部のホウ素化合物の含有量にもよるが、洗浄処理によって、ペレット表層部におけるホウ素化合物の含有量を調整することができる。
<Process of cleaning EVOH pellets>
Next, the step of washing the EVOH pellets will be described.
The above-mentioned EVOH pellet before adjusting boron in the surface layer portion has a boron compound content in the pellet surface layer portion by a washing treatment, although it depends on the total content of the boron compound contained in the pellet and the content of the boron compound in the pellet surface layer portion. Can be adjusted.
上記洗浄処理は、洗浄用処理液と上記表層部ホウ素調整前EVOHペレットとを接触させることにより行われる。上記接触させる方法としては、例えば、洗浄用処理液に上記表層部ホウ素調整前EVOHペレットを浸漬し撹拌する方法、洗浄用処理液中で上記表層部ホウ素調整前EVOHペレットを循環させる方法、表層部ホウ素調整前EVOHペレットに洗浄用処理液を吹き付ける方法等により行うことができる。また、上記浸漬する方法においては、浸漬中に超音波等の振動を与えることも有効である。上記の方法のなかでも、工業上、好適には表層部ホウ素調整前EVOHペレットを洗浄用処理液に浸漬し撹拌する方法、洗浄用処理液中で表層部ホウ素調整前EVOHペレットを循環させる方法が用いられる。 The cleaning treatment is performed by bringing the cleaning treatment liquid into contact with the EVOH pellets before adjusting the surface layer boron. Examples of the contact method include a method of immersing the surface layer portion boron-adjusted EVOH pellets in a cleaning treatment liquid and stirring them, a method of circulating the surface layer portion boron-adjusted EVOH pellets in the cleaning treatment liquid, and a surface layer portion. This can be done by spraying a cleaning treatment liquid onto the EVOH pellets before boron adjustment. Further, in the above dipping method, it is also effective to apply vibration such as ultrasonic waves during dipping. Among the above methods, industrially, preferably, a method of immersing the EVOH pellets before boron adjustment in the surface layer in the cleaning treatment liquid and stirring the EVOH pellets, and a method of circulating the EVOH pellets in the surface layer before boron adjustment in the cleaning treatment liquid are preferable. Used.
上記洗浄用処理液としては、水/アルコール混合溶液またはアルコールが好ましく、より好ましくは水/アルコール混合溶液である。 The cleaning treatment solution is preferably a water / alcohol mixed solution or alcohol, and more preferably a water / alcohol mixed solution.
上記アルコールとしては、例えば、メタノール、エタノール、1−プロパノール、2−プロパノール、1−ブタノール、2−メチル−1−プロパノール、2−ブタノール、2−メチル−2−プロパノール等の炭素数1〜8、特には1〜5、さらには1〜3のアルコールを用いることが好ましく、これらのうち、入手容易かつ安価の点で、メタノールが特に好ましく用いられる。 Examples of the alcohol include methanol, ethanol, 1-propanol, 2-propanol, 1-butanol, 2-methyl-1-propanol, 2-butanol, 2-methyl-2-propanol and the like having 1 to 8 carbon atoms. In particular, it is preferable to use 1 to 5 alcohols and further 1 to 3 alcohols, and among these, methanol is particularly preferably used in terms of easy availability and low cost.
上記洗浄用処理液として水/アルコール混合液またはアルコールを用いる場合は、水/アルコール(重量比)が、80/20〜0/100、好ましくは65/35〜15/85、特に好ましくは50/50〜20/80である。水が多すぎても、アルコール濃度が高くなりすぎても、表層部のホウ素化合物含有量低減効果が低下する傾向があることから、上記範囲の水/アルコール混合溶液が好ましい。 When a water / alcohol mixed solution or alcohol is used as the cleaning treatment solution, the water / alcohol (weight ratio) is 80/20 to 0/100, preferably 65/35 to 15/85, and particularly preferably 50 /. It is 50 to 20/80. Even if the amount of water is too large or the alcohol concentration is too high, the effect of reducing the boron compound content in the surface layer tends to decrease. Therefore, a water / alcohol mixed solution in the above range is preferable.
一般にホウ素化合物の溶解度は、水よりもアルコールの方が高いため、ホウ素化合物の含有量を調整するための洗浄用処理液としては、アルコールを用いることが通常である。しかし、本発明においては、意外にも、洗浄用処理液としてアルコール単独よりも水/アルコール混合溶液を用いることにより、より効率的に表層部ホウ素調整前EVOHペレットからホウ素化合物を溶出させることができることを見出した。なお、ホウ素化合物の23℃の水10gに対する溶解度は、0.1〜10重量%程度であり、23℃のメタノール10gに対する溶解度は15〜30重量%程度である。 In general, the solubility of a boron compound is higher in alcohol than in water. Therefore, alcohol is usually used as a cleaning treatment liquid for adjusting the content of the boron compound. However, in the present invention, surprisingly, by using a water / alcohol mixed solution as the cleaning treatment solution rather than alcohol alone, the boron compound can be more efficiently eluted from the surface layer portion of the EVOH pellet before boron adjustment. I found. The solubility of the boron compound in 10 g of water at 23 ° C. is about 0.1 to 10% by weight, and the solubility of the boron compound in 10 g of methanol at 23 ° C. is about 15 to 30% by weight.
上記表層部ホウ素調整前EVOHペレットと洗浄用処理液との接触時間は、ホウ素化合物含有量が所定の濃度となる時間であれば特に限定されないが、通常5分間〜48時間、さらには10分間〜24時間が好ましく、洗浄用処理液の温度は、通常10〜80℃、さらには20〜60℃とすることが好ましい。 The contact time between the surface layer portion of the EVOH pellet before boron adjustment and the cleaning treatment liquid is not particularly limited as long as the boron compound content reaches a predetermined concentration, but is usually 5 minutes to 48 hours, and further 10 minutes to. 24 hours is preferable, and the temperature of the cleaning treatment liquid is usually 10 to 80 ° C., more preferably 20 to 60 ° C.
上記洗浄処理後のホウ素化合物含有EVOHペレットは、必要に応じて乾燥してもよい。具体的には、含水率0.01〜1重量%程度、好ましくは0.05〜0.5重量%程度まで乾燥することが好ましい。乾燥方法は、上記表層部ホウ素調整前EVOHペレットの乾燥方法と同様の方法を採用することができる。 The boron compound-containing EVOH pellets after the cleaning treatment may be dried if necessary. Specifically, it is preferable to dry to a moisture content of about 0.01 to 1% by weight, preferably about 0.05 to 0.5% by weight. As the drying method, the same method as the method for drying the EVOH pellets before adjusting the surface layer boron can be adopted.
上記洗浄処理により、ペレット表層部のホウ素化合物の含有量を減じることができ、本発明の第1の特徴であるペレット表層部のホウ素化合物含有量が、ホウ素換算で1.7ppm以下に低減されたホウ素化合物含有EVOHペレットが得られる。 By the above cleaning treatment, the content of the boron compound in the surface layer of the pellet can be reduced, and the content of the boron compound in the surface layer of the pellet, which is the first feature of the present invention, is reduced to 1.7 ppm or less in terms of boron. EVOH pellets containing a boron compound are obtained.
つぎに、本発明の第2の特徴である、滑剤をEVOHペレットに含有させる工程について説明する。 Next, a step of incorporating the lubricant into the EVOH pellet, which is the second feature of the present invention, will be described.
<滑剤を含有させる工程>
滑剤を含有するEVOHペレットは、前記EVOHペレットと滑剤とを接触させることにより製造することができる。
<Step of adding lubricant>
The EVOH pellet containing the lubricant can be produced by bringing the EVOH pellet into contact with the lubricant.
EVOHペレットに滑剤を含有させる方法としては、例えば、
iii)EVOHペレット製造段階で滑剤と接触させる方法、
iv)予め作製したEVOHペレットと滑剤とを接触させる方法、
等により行うことができる。
As a method of incorporating a lubricant in the EVOH pellet, for example,
iii) Method of contacting with lubricant at the EVOH pellet manufacturing stage,
iv) A method of contacting a prefabricated EVOH pellet with a lubricant,
It can be done by such as.
上記iii)EVOHペレット製造段階で滑剤と接触させる方法としては、例えば、ペレット原料(EVOH溶液・含水組成物、乾燥EVOH)に滑剤を添加する方法、滑剤を含有する溶液を凝固液に使用する方法等があげられる。
ペレット原料としてEVOH溶液・含水組成物を用いる場合には、例えば、EVOH溶液・含水組成物に滑剤を分散させればよい。また、乾燥EVOHを用いる場合には、乾燥EVOHペレットを溶融し、かかる溶融状態のEVOHと滑剤とを押出機で溶融混練すればよい。
As the method of contacting with the lubricant in the above-mentioned iii) EVOH pellet production stage, for example, a method of adding the lubricant to the pellet raw material (EVOH solution / water-containing composition, dried EVOH), a method of using the solution containing the lubricant in the coagulation liquid. And so on.
When an EVOH solution / water-containing composition is used as the pellet raw material, for example, the lubricant may be dispersed in the EVOH solution / water-containing composition. When dry EVOH is used, the dried EVOH pellets may be melted, and the melted EVOH and the lubricant may be melt-kneaded by an extruder.
上記iv)の予め作製したEVOHペレットと滑剤とを接触させる方法としては、滑剤を含有する溶液または分散液をEVOHペレットに噴霧する方法;滑剤を含有する溶液または分散液にEVOHペレットを浸漬する方法;滑剤を含有する溶液または分散液を撹拌しながら、EVOHペレットを投入する方法;滑剤の粉末をEVOHペレットに直接添加して混ぜ合わせる方法等があげられる。これらのうち、滑剤を効率よく含有させることができる点で、滑剤の粉末をEVOHペレットに直接添加して混ぜ合わせる方法が好ましく用いられる。 As a method of contacting the EVOH pellet prepared in advance of iv) with the lubricant, a method of spraying the solution or dispersion containing the lubricant on the EVOH pellet; a method of immersing the EVOH pellet in the solution or dispersion containing the lubricant. The EVOH pellets are added while stirring the solution or dispersion containing the lubricant; the lubricant powder is directly added to the EVOH pellets and mixed. Of these, a method in which the lubricant powder is directly added to the EVOH pellets and mixed is preferably used because the lubricant can be efficiently contained.
上記滑剤を含有する溶液または分散液における滑剤の濃度は、通常1〜80重量%、好ましくは20〜70重量%である。かかる濃度が低すぎると、所定量の滑剤を含有させることが困難となる傾向があり、高すぎると最終的に得られる成形物の外観が低下する傾向にある。なお、滑剤を含有する溶液または分散液を用いる場合の溶媒としては、前記ホウ素化合物を含有する溶液に用いたものと同様のものを用いることができる。 The concentration of the lubricant in the solution or dispersion containing the lubricant is usually 1 to 80% by weight, preferably 20 to 70% by weight. If the concentration is too low, it tends to be difficult to contain a predetermined amount of lubricant, and if it is too high, the appearance of the finally obtained molded product tends to be deteriorated. When a solution containing a lubricant or a dispersion is used, the same solvent as that used for the solution containing the boron compound can be used.
また、上記滑剤を含有する溶液または分散液を用いる方法においては、滑剤を含有する溶液または分散液との接触処理において、添加量、滑剤の濃度、接触処理時間、接触処理温度、接触処理時の撹拌速度や処理されるEVOHペレットの含水率等により、滑剤含有量をコントロールすることが可能である。 Further, in the method using the solution or dispersion containing the lubricant, in the contact treatment with the solution or dispersion containing the lubricant, the amount added, the concentration of the lubricant, the contact treatment time, the contact treatment temperature, and the contact treatment The lubricant content can be controlled by the stirring speed, the water content of the EVOH pellets to be treated, and the like.
上記、滑剤の粉末をEVOHペレットに直接添加する場合は、添加量を滑剤の含有量とすることができ、添加する滑剤量は、EVOHペレットに対して、通常、0.001〜0.15重量%であり、好ましくは0.003〜0.12重量%、さらに好ましくは0.005〜0.10重量%である。少なすぎると押出機のスクリュー表面とEVOHペレットとの摩擦が強くなるため、安定したペレット供給ができなくなることでフィッシュアイの増加を引き起こす傾向があり、多すぎると分散が不充分な滑剤が凝集することで逆にフィッシュアイの増加を引き起こしたり、EVOHペレットとスクリュー表面との摩擦が低下し、安定したペレット供給ができなくなることでフィッシュアイの増加を引き起こす傾向がある。 When the above-mentioned lubricant powder is directly added to the EVOH pellet, the addition amount can be the content of the lubricant, and the amount of the lubricant to be added is usually 0.001 to 0.15 weight with respect to the EVOH pellet. %, Preferably 0.003 to 0.12% by weight, more preferably 0.005 to 0.10% by weight. If the amount is too small, the friction between the screw surface of the extruder and the EVOH pellets becomes strong, which tends to cause an increase in fish eyes due to the inability to supply stable pellets. On the contrary, this tends to cause an increase in fish eyes, or a decrease in friction between the EVOH pellets and the screw surface, which makes it impossible to stably supply pellets, which tends to cause an increase in fish eyes.
以上のようなEVOHペレット滑剤とを接触させる方法のうち、種々のペレットに適用でき、汎用性に優れているという点で、上記iv)の予め作製したEVOHペレットと滑剤とを接触させる方法が好ましく、特に好ましくは、滑剤の粉末をEVOHペレットに直接添加して混ぜ合わせる方法である。 Among the methods of contacting the EVOH pellet lubricant as described above, the method of contacting the EVOH pellet prepared in advance in iv) with the lubricant is preferable in that it can be applied to various pellets and has excellent versatility. Particularly preferred is a method in which the lubricant powder is directly added to the EVOH pellet and mixed.
上記の滑剤含有EVOHペレットは、必要に応じて、乾燥してもよい。具体的には、通常、含水率0.01〜1重量%、好ましくは0.05〜0.5重量%である。乾燥方法は、表層部ホウ素調整前EVOHペレットの乾燥方法と同様の方法を採用することができる。 The lubricant-containing EVOH pellets may be dried, if necessary. Specifically, the water content is usually 0.01 to 1% by weight, preferably 0.05 to 0.5% by weight. As the drying method, the same method as the drying method of the EVOH pellets before adjusting the surface layer boron can be adopted.
上記工程により、滑剤含有EVOHペレットが得られる。 By the above steps, lubricant-containing EVOH pellets are obtained.
本発明のホウ素化合物および滑剤含有EVOHペレットは、上記ホウ素化合物を含有させる工程、EVOHペレットを洗浄する工程、および滑剤を含有させる工程を経ることにより得ることができる。 The boron compound and lubricant-containing EVOH pellets of the present invention can be obtained through the steps of adding the boron compound, washing the EVOH pellets, and adding the lubricant.
なかでも、作業効率の点からホウ素化合物を含有させる工程を行い、つぎにEVOHペレットを洗浄する工程、最後に滑剤を含有させる工程を行うことが好ましく、なかでもホウ素化合物を含有させる工程は工程ii)、滑剤を含有させる工程は工程iv)で行うことが特に好ましい。 Among them, from the viewpoint of work efficiency, it is preferable to carry out a step of containing a boron compound, then a step of washing the EVOH pellets, and finally a step of adding a lubricant, and among them, a step of containing a boron compound is step ii. ), The step of containing the lubricant is particularly preferably performed in step iv).
<ホウ素化合物および滑剤含有EVOHペレット>
ホウ素化合物および滑剤含有EVOHペレットにおける、ホウ素化合物の全含有量は、ホウ素化合物および滑剤含有EVOHペレット重量に対するホウ素換算で、10〜1000ppmであることが好ましく、より好ましくは20〜500ppm、さらに好ましくは30〜300ppmである。なお、上記ホウ素化合物および滑剤含有EVOHペレットにおけるホウ素化合物の全含有量は、前記表層部ホウ素調整前EVOHペレット中に含有されるホウ素化合物の量と同様の方法で測定することができる。
<EVOH pellets containing boron compounds and lubricants>
The total content of the boron compound in the boron compound and lubricant-containing EVOH pellets is preferably 10 to 1000 ppm, more preferably 20 to 500 ppm, still more preferably 30 in terms of boron relative to the weight of the boron compound and lubricant-containing EVOH pellets. ~ 300 ppm. The total content of the boron compound in the above-mentioned boron compound and the lubricant-containing EVOH pellet can be measured by the same method as the amount of the boron compound contained in the surface layer portion boron-adjusted EVOH pellet.
ホウ素化合物および滑剤含有EVOHペレットに含有されるホウ素化合物含有量が少なすぎると、溶融粘度が低くなり、成膜性能が低下する傾向があり、特にインフレーション成膜が困難になる傾向がある。したがって、少なくともホウ素化合物含有量が10ppm程度となるように、ホウ素化合物を含有させることが好ましい。 If the content of the boron compound contained in the boron compound and the lubricant-containing EVOH pellet is too small, the melt viscosity tends to be low, the film forming performance tends to be lowered, and inflationary filming tends to be particularly difficult. Therefore, it is preferable to contain the boron compound so that the content of the boron compound is at least about 10 ppm.
また、ホウ素化合物および滑剤含有EVOHペレットにおいて、ペレット表層部のホウ素化合物含有量は、ホウ素換算で、当該ペレット重量あたり1.7ppm以下であり、好ましくは1.6ppm以下、より好ましくは1.5ppm以下である。下限は、特に限定しないが、ホウ素化合物および滑剤含有EVOHペレット中のホウ素化合物全含有量が上記範囲内である場合、通常、1ppb以上、好ましくは50ppb以上、より好ましくは100ppb以上である。
上記ペレット表層部のホウ素化合物含有量が多くなりすぎると、フィッシュアイ等が発生しやすくなり、フィルム外観が低下することとなり、また、成膜性も低下することとなる。
Further, in the boron compound and lubricant-containing EVOH pellets, the boron compound content in the surface layer of the pellet is 1.7 ppm or less, preferably 1.6 ppm or less, and more preferably 1.5 ppm or less per weight of the pellet in terms of boron. Is. The lower limit is not particularly limited, but when the total content of the boron compound in the boron compound and the lubricant-containing EVOH pellet is within the above range, it is usually 1 ppb or more, preferably 50 ppb or more, and more preferably 100 ppb or more.
If the content of the boron compound in the surface layer of the pellet is too large, fish eyes and the like are likely to occur, the appearance of the film is deteriorated, and the film forming property is also deteriorated.
上記ペレット表層部のホウ素化合物含有量は、ホウ素化合物および滑剤含有EVOHペレット4gを30℃メタノール20mLに6時間静置浸漬した後、得られたメタノール溶液中のホウ素含有量を誘導結合プラズマ質量分析計(ICP−MS)を用いて測定し、上記EVOHペレットの重量(4g)で除したものである。 The boron compound content in the surface layer of the pellet was determined by inductively coupled plasma mass spectrometry of the boron compound content in the obtained methanol solution after 4 g of EVOH pellets containing a boron compound and a lubricant were immersed in 20 mL of methanol at 30 ° C. for 6 hours. It was measured using (ICP-MS) and divided by the weight (4 g) of the above EVOH pellets.
ホウ素化合物および滑剤含有EVOHペレットは、ホウ素化合物および滑剤含有EVOHペレット中のホウ素化合物全含有量(ホウ素換算)に対する前記ペレット表層部のホウ素化合物含有量(ホウ素換算)の重量比(表層部のホウ素含有量/ホウ素全含有量)を、1.38×10-2以下とすることが好ましく、より好ましくは1.35×10-2以下、さらに好ましくは1.30×10-2以下である。当該比率が高くなりすぎると、フィッシュアイが発生しやすくなり、フィルム外観が低下する傾向にある。なお、下限値は、通常1×10-7である。 The boron compound and lubricant-containing EVOH pellets are the weight ratio of the boron compound content (boron equivalent) of the pellet surface layer portion to the total boron compound content (boron equivalent) in the boron compound and lubricant-containing EVOH pellets (boron content of the surface layer portion). The amount / total boron content) is preferably 1.38 × 10 −2 or less, more preferably 1.35 × 10 −2 or less, and further preferably 1.30 × 10 −2 or less. If the ratio is too high, fish eyes are likely to occur and the appearance of the film tends to deteriorate. The lower limit is usually 1 × 10 -7 .
また、ホウ素化合物および滑剤含有EVOHペレットにおける滑剤含有量は、ホウ素化合物および滑剤含有EVOHペレットの0.001〜0.15重量%であり、好ましくは0.003〜0.12重量%、さらに好ましくは0.005〜0.10重量%である。かかる含有量が少なすぎると押出機のスクリュー表面とEVOHペレットの摩擦が強いために、安定したペレット供給ができなくなることでフィッシュアイの増加を引き起こす傾向があり、多すぎると分散が不充分な滑剤が凝集することで逆にフィッシュアイの増加を引き起こしたり、EVOHペレットとスクリュー表面との摩擦が低下し、安定したペレット供給ができなくなることでフィッシュアイの増加を引き起こす傾向がある。 The lubricant content of the boron compound and lubricant-containing EVOH pellets is 0.001 to 0.15% by weight, preferably 0.003 to 0.12% by weight, more preferably 0.003 to 0.12% by weight of the boron compound and lubricant-containing EVOH pellets. It is 0.005 to 0.10% by weight. If the content is too small, the friction between the screw surface of the extruder and the EVOH pellets is strong, which tends to cause an increase in fish eyes due to the inability to supply stable pellets. If the content is too large, the lubricant is poorly dispersed. On the contrary, the agglomeration of the sol tends to cause an increase in fish eyes, and the friction between the EVOH pellets and the screw surface is reduced, so that a stable pellet supply cannot be performed, which tends to cause an increase in fish eyes.
上記滑剤の含有量は、例えば、滑剤をEVOHペレット表面に添着させる場合は、滑剤の添加量を含有量とみなすことができる。滑剤をEVOHペレット内に含有させた場合、滑剤が例えば高級脂肪酸アミンであれば、微量全窒素分析装置を用いてホウ素化合物および滑剤含有EVOHペレット中の全窒素量を測定し、滑剤含有量に換算することでホウ素化合物および滑剤含有EVOHペレット中の滑剤の含有量を測定することができる。 As for the content of the lubricant, for example, when the lubricant is adhered to the surface of the EVOH pellet, the amount of the lubricant added can be regarded as the content. When the lubricant is contained in the EVOH pellet, if the lubricant is, for example, a higher fatty acid amine, the total nitrogen content in the boron compound and the lubricant-containing EVOH pellet is measured using a trace total nitrogen analyzer and converted to the lubricant content. By doing so, the content of the lubricant in the boron compound and the lubricant-containing EVOH pellet can be measured.
また、本発明のホウ素化合物および滑剤含有EVOHペレットの含水率は、通常0.01〜1重量%、好ましくは0.05〜0.5重量%である。含水率が少なすぎると水分子によるEVOHの可塑化が起こらず、押出成形時にEVOHペレットが溶融しづらくなって、未溶融物の欠点が生じやすくなる傾向があり、多すぎると押出成形時に発泡現象が起こり、成形物の外観が悪化しやすくなる傾向がある。 The water content of the boron compound and lubricant-containing EVOH pellets of the present invention is usually 0.01 to 1% by weight, preferably 0.05 to 0.5% by weight. If the water content is too low, the EVOH will not be plasticized by water molecules, and the EVOH pellets will be difficult to melt during extrusion molding, and defects of unmelted matter will tend to occur. If it is too high, a foaming phenomenon will occur during extrusion molding. Tends to occur and the appearance of the molded product tends to deteriorate.
〔その他の成分〕
本発明のホウ素化合物および滑剤含有EVOHペレットには、本発明の効果を阻害しない範囲(例えば20重量%以下、好ましくは10重量%以下)で、一般的にEVOH組成物に用いられるEVOH以外の樹脂を混合して得られる樹脂組成物も含むことができる。
[Other ingredients]
The boron compound and lubricant-containing EVOH pellets of the present invention include resins other than EVOH generally used in EVOH compositions within a range that does not impair the effects of the present invention (for example, 20% by weight or less, preferably 10% by weight or less). The resin composition obtained by mixing the above can also be included.
本発明のホウ素化合物および滑剤含有EVOHペレットには、本発明の効果を阻害しない範囲において、一般にEVOHに配合する配合剤、例えば、熱安定剤、酸化防止剤、帯電防止剤、着色剤、紫外線吸収剤、可塑剤、光安定剤、界面活性剤、抗菌剤、乾燥剤、アンチブロッキング剤、難燃剤、架橋剤、硬化剤、発泡剤、結晶核剤、防曇剤、生分解用添加剤、シランカップリング剤、酸素吸収剤等が含有されていてもよい。これらは単独でもしくは2種以上併せて用いることができる。 The boron compound and lubricant-containing EVOH pellets of the present invention are generally blended with EVOH as long as the effects of the present invention are not impaired, such as heat stabilizers, antioxidants, antistatic agents, colorants, and ultraviolet absorption. Agents, plasticizers, light stabilizers, surfactants, antibacterial agents, desiccants, antiblocking agents, flame retardants, cross-linking agents, hardeners, foaming agents, crystal nucleating agents, antifogging agents, biodegradation additives, silanes A coupling agent, an oxygen absorber, or the like may be contained. These can be used alone or in combination of two or more.
上記熱安定剤としては、溶融成形時の熱安定性等の各種物性を向上させる目的で、硫酸、亜硫酸、炭酸、リン酸等の無機酸類、またはこれらのアルカリ金属塩(ナトリウム、カリウム等)、アルカリ土類金属塩(カルシウム等)、亜鉛塩等の塩;等の添加剤を添加してもよい。これらは単独でもしくは2種以上併せて用いることができる。 The heat stabilizer includes inorganic acids such as sulfuric acid, sulfurous acid, carbonic acid, and phosphoric acid, or alkali metal salts (sodium, potassium, etc.) of these, for the purpose of improving various physical properties such as thermal stability during melt molding. Additives such as alkaline earth metal salts (calcium and the like), salts such as zinc salts; and the like may be added. These can be used alone or in combination of two or more.
これらの成分を配合する場合、その配合は、通常、ホウ素化合物または滑剤とEVOHペレットとの接触処理前、接触処理とともに、あるいは接触処理後のいずれの段階で行ってもよい。好ましくはホウ素または滑剤含有量への影響が少ないという点で、接触処理とともに行うことが好ましい。 When these components are blended, the blending may be usually carried out at any stage before the contact treatment of the boron compound or lubricant and the EVOH pellet, with the contact treatment, or after the contact treatment. It is preferably carried out together with the contact treatment in that it has little effect on the content of boron or lubricant.
その他の成分の配合方法は特に限定しないが、通常、これらの配合剤を含有する溶液にEVOHペレットを接触させることにより行うことができる。したがって、ホウ素化合物または滑剤との接触処理前であれば、EVOHペレットを上記配合剤を含有する溶液に浸漬することにより、あるいはホウ素化合物および滑剤の少なくとも一方を含有する溶液に、さらに上記配合剤も含有さることにより、配合することができる。 The method of blending the other components is not particularly limited, but it can usually be carried out by contacting the EVOH pellet with the solution containing these blending agents. Therefore, before the contact treatment with the boron compound or the lubricant, the EVOH pellet is immersed in the solution containing the above-mentioned compounding agent, or the solution containing at least one of the boron compound and the lubricant is further added to the above-mentioned compounding agent. By containing it, it can be blended.
本発明のホウ素化合物および滑剤含有EVOHペレットの溶融成形品は、単層膜であっても成形性に優れ、外観に優れているが、耐水性、強度等の観点から、必要に応じて、他の樹脂層を積層した多層構造体としてもよい。 The melt-molded product of the boron compound and the lubricant-containing EVOH pellet of the present invention is excellent in moldability and appearance even if it is a single-layer film. A multi-layer structure in which the resin layers of the above are laminated may be used.
以下、かかる多層構造体について説明する。
上記の多層構造体を製造するにあたっては、本発明のホウ素化合物および滑剤含有EVOHペレットを用いて成形された層の片面または両面に、他の基材(熱可塑性樹脂等)を積層するのであるが、積層方法としては、例えば、本発明のホウ素化合物および滑剤含有EVOHペレット等を用いて成形されたフィルム、シート等に他の基材を溶融押出ラミネートする方法、逆に他の基材に本発明のホウ素化合物および滑剤含有EVOHペレット等を溶融押出ラミネートする方法、本発明のホウ素化合物および滑剤含有EVOHペレット等と他の基材とを共押出する方法、本発明のホウ素化合物および滑剤含有EVOHペレット等を用いてなるフィルム、シート等(層)と他の基材(層)とを有機チタン化合物、イソシアネート化合物、ポリエステル系化合物、ポリウレタン化合物等の公知の接着剤を用いてドライラミネートする方法等があげられる。上記の溶融押出時の溶融成形温度は、150〜300℃の範囲から選ぶことが多い。
Hereinafter, such a multilayer structure will be described.
In producing the above-mentioned multilayer structure, another base material (thermoplastic resin or the like) is laminated on one side or both sides of a layer formed by using the boron compound and the lubricant-containing EVOH pellet of the present invention. As a laminating method, for example, a method of melt-extruding and laminating another base material on a film, a sheet or the like formed by using the boron compound of the present invention and an EVOH pellet containing a lubricant, or conversely, the present invention on another base material. A method of melt-extruding and laminating a boron compound and a lubricant-containing EVOH pellet, etc. A method of dry laminating a film, sheet, etc. (layer) made of Be done. The melt molding temperature at the time of melt extrusion is often selected from the range of 150 to 300 ° C.
かかる他の基材としては、熱可塑性樹脂が有用で、具体的には、直鎖状低密度ポリエチレン、低密度ポリエチレン、超低密度ポリエチレン、中密度ポリエチレン、高密度ポリエチレン等の各種ポリエチレン、エチレン−酢酸ビニル共重合体、アイオノマー、エチレン−プロピレン(ブロックまたはランダム)共重合体、エチレン−アクリル酸共重合体、エチレン−アクリル酸エステル共重合体、ポリプロピレン、プロピレン−α−オレフィン(炭素数4〜20のα−オレフィン)共重合体、ポリブテン、ポリペンテン等のオレフィンの単独または共重合体、あるいはこれらのオレフィンの単独または共重合体を不飽和カルボン酸またはそのエステルでグラフト変性したもの等の広義のポリオレフィン系樹脂、ポリエステル系樹脂、ポリアミド系樹脂(共重合ポリアミドも含む)、ポリ塩化ビニル、ポリ塩化ビニリデン、アクリル系樹脂、ポリスチレン系樹脂、ビニルエステル系樹脂、ポリエステルエラストマー、ポリウレタンエラストマー、塩素化ポリエチレン、塩素化ポリプロピレン、芳香族または脂肪族ポリケトン、さらにこれらを還元して得られるポリアルコール類、さらには本発明に用いられるEVOH以外の他のEVOH等があげられる。多層構造体の物性(特に強度)等の実用性の点から、ポリプロピレン、エチレン−プロピレン(ブロックまたはランダム)共重合体、ポリアミド系樹脂、ポリエチレン、エチレン−酢酸ビニル共重合体、ポリスチレン系樹脂、ポリエチレンテレフタレート(PET)、ポリエチレンナフタレート(PEN)が好ましく用いられる。 As such other base materials, thermoplastic resins are useful, and specifically, various polyethylenes such as linear low-density polyethylene, low-density polyethylene, ultra-low-density polyethylene, medium-density polyethylene, and high-density polyethylene, ethylene- Vinyl acetate copolymer, ionomer, ethylene-propylene (block or random) copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer, polypropylene, propylene-α-olefin (4 to 20 carbon atoms) Α-Olefin) Copolymers, olefins such as polybutene and polypentene alone or copolymers, or olefins alone or copolymers of these olefins graft-modified with unsaturated carboxylic acids or esters thereof. Based resin, polyester resin, polyamide resin (including copolymerized polyamide), polyvinyl chloride, polyvinylidene chloride, acrylic resin, polystyrene resin, vinyl ester resin, polyester elastomer, polyurethane elastomer, chlorinated polyethylene, chlorine Examples thereof include copolymerized polypropylene, aromatic or aliphatic polyketones, polyalcohols obtained by reducing them, and EVOH other than EVOH used in the present invention. From the viewpoint of practicality such as physical properties (particularly strength) of the multilayer structure, polypropylene, ethylene-propylene (block or random) copolymer, polyamide resin, polyethylene, ethylene-vinyl acetate copolymer, polystyrene resin, polyethylene Terephthalate (PET) and polyethylene naphthalate (PEN) are preferably used.
さらに、本発明のホウ素化合物および滑剤含有EVOHペレット等を用いて成形されたフィルムやシート等の成形物に、他の基材を押出コートしたり、他の基材のフィルム、シート等を、接着剤を用いてラミネートしたりする場合、かかる基材としては、上記の熱可塑性樹脂以外に、任意の基材(紙、金属箔、一軸または二軸延伸プラスチックフィルムまたはシートおよびその無機物蒸着物、織布、不織布、金属綿条、木質等)も使用可能である。 Further, another base material is extruded and coated on a molded product such as a film or a sheet formed by using the boron compound of the present invention and a lubricant-containing EVOH pellet or the like, or a film, a sheet or the like of another base material is adhered to the molded product. In the case of laminating with an agent, such a base material may be any base material (paper, metal foil, uniaxial or biaxially stretched plastic film or sheet and its inorganic vapor deposition, woven, etc., in addition to the above-mentioned thermoplastic resin. Cloth, non-woven fabric, metal cotton strip, wood, etc.) can also be used.
上記多層構造体の層構成は、本発明のホウ素化合物および滑剤含有EVOHペレットを用いて成形された層をa(a1、a2、・・・)、他の基材、例えば熱可塑性樹脂層をb(b1、b2、・・・)とするとき、かかるa層を最内層とする構成で、[内側]a/b[外側](以下同様)の二層構造のみならず、例えば、a/b/a、a1/a2/b、a/b1/b2、a1/b1/a2/b2、a1/b1/b2/a2/b2/b1等任意の組み合わせが可能であり、さらには、少なくとも本発明のホウ素化合物および滑剤含有EVOHペレット等と熱可塑性樹脂の混合物からなるリグラインド層をRとするとき、例えば、a/R/b、a/R/a/b、a/b/R/a/R/b、a/b/a/R/a/b、a/b/R/a/R/a/R/b等とすることも可能である。 In the layer structure of the multilayer structure, a layer formed by using the boron compound and the lubricant-containing EVOH pellet of the present invention is a (a1, a2, ...), And another base material, for example, a thermoplastic resin layer is b. In the case of (b1, b2, ...), In the configuration in which the a layer is the innermost layer, not only the two-layer structure of [inside] a / b [outside] (the same applies hereinafter), but also, for example, a / b. Any combination such as / a, a1 / a2 / b, a / b1 / b2, a1 / b1 / a2 / b2, a1 / b1 / b2 / a2 / b2 / b1 is possible, and at least of the present invention. When the regrind layer composed of a mixture of a boron compound, a lubricant-containing EVOH pellet, or the like and a thermoplastic resin is R, for example, a / R / b, a / R / a / b, a / b / R / a / R. It is also possible to use / b, a / b / a / R / a / b, a / b / R / a / R / a / R / b, and the like.
なお、上記の層構成において、それぞれの層間には、必要に応じて接着性樹脂層を設けることができる。かかる接着性樹脂としては、種々のものを使用することができるが、延伸性に優れた多層構造体が得られる点において、例えば不飽和カルボン酸またはその無水物をオレフィン系重合体(上述の広義のポリオレフィン系樹脂)に付加反応やグラフト反応等により化学的に結合させて得られる、カルボキシル基を含有する変性オレフィン系重合体をあげることができる。 In the above layer structure, an adhesive resin layer can be provided between the layers as needed. Various adhesive resins can be used, but in terms of obtaining a multilayer structure having excellent stretchability, for example, an unsaturated carboxylic acid or an anhydride thereof is used as an olefin polymer (in the broad sense described above). A modified olefin polymer containing a carboxyl group, which is obtained by chemically bonding to the polyolefin resin) by an addition reaction, a graft reaction, or the like.
具体的には、無水マレイン酸グラフト変性ポリエチレン、無水マレイン酸グラフト変性ポリプロピレン、無水マレイン酸グラフト変性エチレン−プロピレン(ブロックおよびランダム)共重合体、無水マレイン酸グラフト変性エチレン−エチルアクリレート共重合体、無水マレイン酸グラフト変性エチレン−酢酸ビニル共重合体等から選ばれた1種または2種以上の混合物が好適なものとしてあげられる。このときの、熱可塑性樹脂に含有される不飽和カルボン酸またはその無水物の量は、0.001〜3重量%が好ましく、さらに好ましくは0.01〜1重量%、特に好ましくは0.03〜0.5重量%である。該変性物中の変性量が少なすぎると接着性が低下する傾向があり、逆に多すぎると架橋反応を起こし、成形性が低下する傾向がある。 Specifically, maleic anhydride graft-modified polyethylene, maleic anhydride graft-modified polypropylene, maleic anhydride graft-modified ethylene-propylene (block and random) copolymer, maleic anhydride graft-modified ethylene-ethyl acrylate copolymer, anhydrous. One or a mixture of two or more selected from a maleic anhydride graft-modified ethylene-vinyl acetate copolymer and the like can be mentioned as suitable. At this time, the amount of the unsaturated carboxylic acid or its anhydride contained in the thermoplastic resin is preferably 0.001 to 3% by weight, more preferably 0.01 to 1% by weight, and particularly preferably 0.03. ~ 0.5% by weight. If the amount of modification in the modified product is too small, the adhesiveness tends to decrease, and conversely, if it is too large, a cross-linking reaction occurs and the moldability tends to decrease.
また、これらの接着性樹脂には、本発明のホウ素化合物および滑剤含有EVOHペレットに由来するEVOH、他のEVOH、ポリイソブチレン、エチレン−プロピレンゴム等のゴム・エラストマー成分、さらにはb層の樹脂等をブレンドすることも可能である。特に、接着性樹脂の母体のポリオレフィン系樹脂と異なるポリオレフィン系樹脂をブレンドすることにより、接着性が向上することがあり有用である。 In addition, these adhesive resins include EVOH derived from the boron compound and lubricant-containing EVOH pellets of the present invention, other rubber / elastomer components such as EVOH, polyisobutylene, ethylene-propylene rubber, and b-layer resin. It is also possible to blend. In particular, blending a polyolefin-based resin different from the polyolefin-based resin that is the base of the adhesive resin is useful because the adhesiveness may be improved.
多層構造体の各層の厚みは、層構成、b層の種類、用途や成形物の形態、要求される物性等により一概にいえないが、通常は、a層は5〜500μm、好ましくは10〜200μm、b層は10〜5000μm、好ましくは30〜1000μm、接着性樹脂層は5〜400μm、好ましくは10〜150μm程度の範囲から選択される。 The thickness of each layer of the multilayer structure cannot be unequivocally determined depending on the layer structure, the type of layer b, the application, the form of the molded product, the required physical properties, etc., but usually, the a layer is 5 to 500 μm, preferably 10 to 10 μm. The 200 μm, the b layer is selected from the range of 10 to 5000 μm, preferably 30 to 1000 μm, and the adhesive resin layer is selected from the range of 5 to 400 μm, preferably about 10 to 150 μm.
多層構造体は、そのまま各種形状のものに使用されるが、上記多層構造体の物性を改善するためには加熱延伸処理を施すことも好ましい。ここで、「加熱延伸処理」とは、熱的に均一に加熱されたフィルム、シート、パリソン状の積層体をチャック、プラグ、真空力、圧空力、ブロー等の成形手段により、カップ、トレイ、チューブ、フィルム状に均一に成形する操作を意味する。そして、かかる延伸については、一軸延伸、二軸延伸のいずれであってもよく、できるだけ高倍率の延伸を行ったほうが物性的に良好で、延伸時にピンホールやクラック、延伸ムラや偏肉、デラミ(delamination:層間剥離)等の生じない、ガスバリア性に優れた延伸成形物が得られる。 The multilayer structure is used as it is for various shapes, but it is also preferable to perform a heat stretching treatment in order to improve the physical properties of the multilayer structure. Here, the "heat-stretching treatment" refers to a film, a sheet, or a parison-shaped laminate that has been uniformly heated by a chuck, a plug, a vacuum force, a compressed air force, a blow, or the like, by means of a forming means such as a chuck, a plug, a vacuum force, a compressed air force, or a blow. It means the operation of uniformly molding into a tube or film. The stretching may be either uniaxial stretching or biaxial stretching, and it is better to perform stretching at the highest possible magnification in terms of physical properties. A stretched molded product having excellent gas barrier properties, which does not cause delamination (delamination) or the like, can be obtained.
上記多層構造体の延伸方法としては、ロール延伸法、テンター延伸法、チューブラー延伸法、延伸ブロー法、真空圧空成形等のうち延伸倍率の高いものも採用できる。二軸延伸の場合は同時二軸延伸方式、逐次二軸延伸方式のいずれの方式も採用できる。延伸温度は60〜170℃、好ましくは80〜160℃程度の範囲から選ばれる。延伸が終了した後、熱固定を行うことも好ましい。熱固定は周知の手段で実施可能であり、上記延伸フィルムを、緊張状態を保ちながら80〜170℃、好ましくは100〜160℃で2〜600秒間程度熱処理することによって、熱固定を行うことができる。 As the stretching method of the multilayer structure, a roll stretching method, a tenter stretching method, a tubular stretching method, a stretching blow method, vacuum compressed air forming, or the like, which has a high stretching ratio, can also be adopted. In the case of biaxial stretching, either the simultaneous biaxial stretching method or the sequential biaxial stretching method can be adopted. The stretching temperature is selected from the range of 60 to 170 ° C., preferably about 80 to 160 ° C. It is also preferable to perform heat fixation after the stretching is completed. The heat fixing can be carried out by a well-known means, and the heat fixing can be performed by heat-treating the stretched film at 80 to 170 ° C., preferably 100 to 160 ° C. for about 2 to 600 seconds while maintaining a tense state. can.
また、生肉、加工肉、チーズ等の熱収縮包装用途に用いる場合には、延伸後の熱固定は行わずに製品フィルムとし、上記の生肉、加工肉、チーズ等を該フィルムに収納した後、50〜130℃、好ましくは70〜120℃で、2〜300秒間程度の熱処理を行って、該フィルムを熱収縮させて密着包装をする。 When used for heat-shrink packaging of raw meat, processed meat, cheese, etc., it is used as a product film without heat fixing after stretching, and after storing the above-mentioned raw meat, processed meat, cheese, etc. in the film, The film is heat-shrinked at 50 to 130 ° C., preferably 70 to 120 ° C. for about 2 to 300 seconds, and then tightly packaged.
このようにして得られる多層構造体の形状としては、任意のものであってよく、フィルム、シート、テープ、異型断面押出物等が例示される。また、上記多層構造体は、必要に応じて、熱処理、冷却処理、圧延処理、印刷処理、ドライラミネート処理、溶液または溶融コート処理、製袋加工、深絞り加工、箱加工、チューブ加工、スプリット加工等を行うことができる。 The shape of the multilayer structure thus obtained may be any shape, and examples thereof include films, sheets, tapes, and extruded cross-sections. In addition, the above-mentioned multilayer structure may be heat-treated, cooled, rolled, printed, dry-laminated, solution or melt-coated, bag-made, deep-drawn, boxed, tube-processed, split-processed, if necessary. Etc. can be performed.
上記の如く得られたフィルム、シート、延伸フィルムからなる袋およびカップ、トレイ、チューブ、ボトル等からなる容器や蓋材は、一般的な食品の他、マヨネーズ、ドレッシング等の調味料、味噌等の発酵食品、サラダ油等の油脂食品、飲料、化粧品、医薬品等の各種の包装材料容器として有用である。 Bags and cups, trays, tubes, bottles, etc. made of films, sheets, stretched films, etc. obtained as described above can be used for general foods, seasonings such as mayonnaise, dressings, miso, etc. It is useful as a container for various packaging materials such as fermented foods, oil and fat foods such as salad oil, beverages, cosmetics, and pharmaceuticals.
以下、実施例をあげて本発明をさらに具体的に説明するが、本発明はその要旨を越えない限り、実施例の記載に限定されるものではない。
なお、例中「部」、「%」とあるのは、重量基準を意味する。
Hereinafter, the present invention will be described in more detail with reference to examples, but the present invention is not limited to the description of the examples as long as the gist of the present invention is not exceeded.
In the example, "part" and "%" mean the weight standard.
まず実施例および比較例で用いるペレットの測定評価方法について説明する。 First, a method for measuring and evaluating pellets used in Examples and Comparative Examples will be described.
〔測定評価方法〕
(1)ペレット中のホウ素化合物全含有量(ホウ素換算)
EVOHペレット0.1gを濃硝酸とともにマイクロウェーブ分解法にて処理して得られる溶液を純水にて定容(0.75mg/mL)したものを検液とし、誘導結合プラズマ発光分析計(ICP−AES)(アジレント・テクノロジー社製、720−ES型)で測定した。当該測定されるホウ素含有量は、ホウ素化合物に由来するホウ素量に該当する。なお、かかる測定評価方法は、表層部ホウ素調整前EVOHペレット、ホウ素化合物含有EVOHペレット、および、ホウ素化合物および滑剤含有EVOHペレットに適用する。
[Measurement evaluation method]
(1) Total content of boron compounds in pellets (boron equivalent)
A solution obtained by treating 0.1 g of EVOH pellets with concentrated nitric acid by the microwave decomposition method in pure water (0.75 mg / mL) was used as the test solution, and an inductively coupled plasma emission spectrometer (ICP) was used. -AES) (720-ES type manufactured by Agilent Technologies). The measured boron content corresponds to the amount of boron derived from the boron compound. The measurement and evaluation method is applied to the surface layer portion of the EVOH pellets before boron adjustment, the boron compound-containing EVOH pellets, and the boron compound and lubricant-containing EVOH pellets.
(2)ペレット表層部のホウ素化合物含有量(ホウ素換算)
ホウ素化合物(および滑剤)含有EVOHペレット4gを、メタノール(30℃)20mLに6時間静置浸漬し、得られたメタノール溶液を測定用試料として用いた。この測定用試料について、誘導結合プラズマ質量分析計(ICP−MS)(パーキンエルマー社製、ELAN DRCII)を用いてホウ素量を測定し、上記EVOHペレット重量(4g)で除してペレット表層部のホウ素含有量を求めた。当該測定されるホウ素含有量は、ホウ素化合物に由来するホウ素量に該当する。
(2) Boron compound content in the surface layer of the pellet (boron equivalent)
4 g of EVOH pellets containing a boron compound (and lubricant) was immersed in 20 mL of methanol (30 ° C.) for 6 hours, and the obtained methanol solution was used as a measurement sample. The amount of boron in this measurement sample was measured using an inductively coupled plasma mass spectrometer (ICP-MS) (ELAN DRCII, manufactured by PerkinElmer), and divided by the EVOH pellet weight (4 g) to divide the pellet surface layer. The boron content was determined. The measured boron content corresponds to the amount of boron derived from the boron compound.
(3)ペレットの含水率(%)
乾燥前のEVOHペレットの重量と、温度150℃、5時間乾燥後のEVOHペレットの重量から揮発分を求め、これをEVOHペレットの含水率とした。具体的には含水率は下記式で表わされる。なお、かかる測定評価方法は、EVOHペレット、表層部ホウ素調整前EVOHペレット、ホウ素化合物含有EVOHペレット、および、ホウ素化合物および滑剤含有EVOHペレットに適用する。
含水率(%)=(乾燥前のEVOHペレット重量−乾燥後のEVOHペレット重量)/乾燥前のEVOHペレット重量×100
(3) Moisture content of pellets (%)
The volatile content was determined from the weight of the EVOH pellet before drying and the weight of the EVOH pellet after drying at a temperature of 150 ° C. for 5 hours, and this was taken as the water content of the EVOH pellet. Specifically, the water content is expressed by the following formula. The measurement and evaluation method is applied to EVOH pellets, EVOH pellets having a surface layer before boron adjustment, EVOH pellets containing a boron compound, and EVOH pellets containing a boron compound and a lubricant.
Moisture content (%) = (EVOH pellet weight before drying-EVOH pellet weight after drying) / EVOH pellet weight before drying x 100
(4)フィッシュアイ
ホウ素化合物(および滑剤)含有EVOHペレットを用いて下記条件で、厚み30μmの単層フィルムを成膜した。
(成膜条件)
押出機:直径(D)40mm、L/D=28
スクリュー:フルフライトタイプ圧縮比=2.5
スクリーンパック:60/90/60メッシュ
ダイ:幅450mm、コートハンガータイプ
設定温度:C1/C2/C3/C4/A/D=190/200/210/210/210/210℃
スクリュー回転数:20rpm
ロール温度:80℃
(4) Using EVOH pellets containing a fisheye boron compound (and lubricant), a single-layer film having a thickness of 30 μm was formed under the following conditions.
(Film formation conditions)
Extruder: Diameter (D) 40 mm, L / D = 28
Screw: Full flight type compression ratio = 2.5
Screen pack: 60/90/60 mesh Die: Width 450 mm, coat hanger type Set temperature: C1 / C2 / C3 / C4 / A / D = 190/200/210/210/210/210 ° C
Screw rotation speed: 20 rpm
Roll temperature: 80 ° C
得られた厚み30μmの単層フィルムについて、デジタル欠陥検査装置(マミヤオーピー社製、GX−70LT)を用いて、フィッシュアイを計測した。
フィッシュアイの計測は、単層フィルムの下面から光を当て、光透過しなかった部分(直径0.1〜0.2mm)をフィッシュアイ1個として、100cm2(サイズ:10cm×10cm)のあたりのフィッシュアイ個数をカウントすることにより行った。なお、計測時の読み取り速度は3m/分である。
The fish eyes of the obtained single-layer film having a thickness of 30 μm were measured using a digital defect inspection device (GX-70LT manufactured by Mamiya-OP Co., Ltd.).
The fish eye is measured around 100 cm 2 (size: 10 cm x 10 cm) by shining light from the lower surface of the single-layer film and treating the part that did not transmit light (diameter 0.1 to 0.2 mm) as one fish eye. This was done by counting the number of fish eyes. The reading speed at the time of measurement is 3 m / min.
〔ホウ素化合物および滑剤含有EVOHペレットの製造〕
〈実施例1〉
EVOH〔エチレン含有量:44モル%、ケン化度:99.6モル%、MFR:3.8g/10分(210℃、荷重2160g)〕を水/メタノール混合溶媒〔水/メタノール=20/80(重量比)〕に溶解した溶液(60℃、EVOH濃度40%)を、5℃に維持した水を収容した水槽内にストランド状に押出して凝固させた後、カッターで切断して、円柱状(直径4mm、長さ4mm)のペレットを得た。次いで、このEVOHペレットを、30℃の温水に投入し、約4時間撹拌して、含水率50%の多孔質のEVOHペレットを得た。
[Manufacture of EVOH pellets containing boron compounds and lubricants]
<Example 1>
EVOH [ethylene content: 44 mol%, saponification degree: 99.6 mol%, MFR: 3.8 g / 10 minutes (210 ° C., load 2160 g)] with water / methanol mixed solvent [water / methanol = 20/80] (By weight ratio)], the solution (60 ° C., EVOH concentration 40%) was extruded into a strand shape in a water tank containing water maintained at 5 ° C. to solidify it, and then cut with a cutter to form a columnar shape. Pellets (diameter 4 mm, length 4 mm) were obtained. Next, the EVOH pellets were put into warm water at 30 ° C. and stirred for about 4 hours to obtain porous EVOH pellets having a water content of 50%.
多孔質のEVOHペレット100部を、0.0054%のホウ酸水溶液200部に投入し、30℃で5時間撹拌した。撹拌後、多孔質の表層部ホウ素調整前EVOHペレットを回収した。
この表層部ホウ素調整前EVOHペレットを、回分式塔型流動層乾燥器にて、75℃の窒素ガスを3時間通過させることにより、含水率20%まで乾燥させた。
次いで、回分式箱型通気式乾燥器を用いて、125℃の窒素ガスを18時間通過させて、含水率0.3%にまで乾燥させた。乾燥後の処理前ホウ素化合物含有EVOHペレットを、前記測定評価方法により測定したところ、130ppmであった。
100 parts of the porous EVOH pellet was put into 200 parts of a 0.0054% boric acid aqueous solution, and the mixture was stirred at 30 ° C. for 5 hours. After stirring, the porous EVOH pellets before boron adjustment in the surface layer were recovered.
The surface layer portion of the EVOH pellets before boron adjustment was dried to a moisture content of 20% by passing nitrogen gas at 75 ° C. for 3 hours in a batch type column-type fluidized bed dryer.
Then, using a batch box type ventilation dryer, nitrogen gas at 125 ° C. was passed for 18 hours to dry to a moisture content of 0.3%. The pre-treatment boron compound-containing EVOH pellet after drying was measured by the above-mentioned measurement and evaluation method and found to be 130 ppm.
上記のようにして得られた、乾燥後の表層部ホウ素調整前EVOHペレット(含水率0.3%、ホウ素全含有量130ppm)を、以下の洗浄処理に供した。 The dried EVOH pellets before boron adjustment (moisture content: 0.3%, total boron content: 130 ppm) were subjected to the following cleaning treatment.
乾燥後の表層部ホウ素調整前EVOHペレット5部と、洗浄用処理液として水/メタノール混合溶媒(水/メタノール=1/1(重量比))10部とを、ステンレス製容器に入れ、35℃で1時間撹拌した。その後、ペレットを取り出し、120℃、16時間、窒素気流下で乾燥した。以上のようにして、ホウ素化合物含有EVOHペレットを得た。 5 parts of EVOH pellets before boron adjustment on the surface layer after drying and 10 parts of water / methanol mixed solvent (water / methanol = 1/1 (weight ratio)) as a cleaning treatment liquid were placed in a stainless steel container at 35 ° C. Was stirred for 1 hour. Then, the pellet was taken out and dried at 120 ° C. for 16 hours under a nitrogen stream. As described above, an EVOH pellet containing a boron compound was obtained.
続いて、上記のホウ素化合物含有EVOHペレットに対して、滑剤(エチレンビスステアリン酸アミド:日油社製、アルフローH−50T)を0.0054%になるように添加して均一になるように振り混ぜた。 Subsequently, a lubricant (ethylene bisstearic acid amide: manufactured by NOF Corporation, Alflo H-50T) was added to the above-mentioned EVOH pellet containing a boron compound so as to be 0.0054%, and shaken so as to be uniform. mixed.
得られたホウ素化合物および滑剤含有EVOHペレットを、上記測定評価方法によりホウ素全含有量、表層部のホウ素含有量、を測定した。ホウ素全含有量は128.8ppm、表層部のホウ素含有量は1.1ppm(含水率0.10%)であった。 The obtained boron compound and lubricant-containing EVOH pellets were measured for the total boron content and the boron content of the surface layer by the above measurement and evaluation method. The total boron content was 128.8 ppm, and the boron content of the surface layer was 1.1 ppm (moisture content 0.10%).
得られたホウ素化合物および滑剤含有EVOHペレットを、単層Tダイ押出装置を用いて、最高温度210℃、スクリュー回転数20rpmで成膜し、厚み30μmの単層フィルムを製造した。この単層フィルムについて、上記測定評価方法によりフィッシュアイの発生個数を調べた。結果を後記の表1に示す。 The obtained boron compound and lubricant-containing EVOH pellets were formed into a film using a single-layer T-die extruder at a maximum temperature of 210 ° C. and a screw rotation speed of 20 rpm to produce a single-layer film having a thickness of 30 μm. For this single-layer film, the number of fish eyes generated was examined by the above measurement and evaluation method. The results are shown in Table 1 below.
〈実施例2,3〉
ホウ素化合物および滑剤含有EVOHペレット中の滑剤含有量を、後記の表1の含有量に調整した以外は、実施例1の場合と同様にして、ホウ素化合物および滑剤含有EVOHペレットを得た(含水率はいずれも0.10%)。
ついで、このペレットを用いて、実施例1と同様にして、単層フィルムを作製し、フィッシュアイの発生について評価した。その結果を後記の表1に示す。
<Examples 2 and 3>
A boron compound and lubricant-containing EVOH pellets were obtained in the same manner as in Example 1 except that the lubricant content in the boron compound and lubricant-containing EVOH pellets was adjusted to the content shown in Table 1 below (moisture content). Is 0.10%).
Then, using these pellets, a single-layer film was prepared in the same manner as in Example 1, and the occurrence of fish eyes was evaluated. The results are shown in Table 1 below.
〈実施例4〉
実施例1において滑剤としてステアリン酸カルシウムを用い、ホウ素化合物全含有量、表層部のホウ素化合物含有量および滑剤含有量を、後記の表1の含有量に調整し、ホウ素化合物および滑剤含有EVOHペレットを得た。また、得られたホウ素化合物および滑剤含有EVOHペレットのホウ素化合物全含有量、表層部のホウ素化合物含有量を測定した(含水率0.15%)。
ついで、このペレットを用いて、実施例1と同様にして単層フィルムを作製し、フィッシュアイの発生について評価した。結果を後記の表1に示す。
<Example 4>
In Example 1, calcium stearate was used as a lubricant, and the total content of the boron compound, the content of the boron compound on the surface layer and the content of the lubricant were adjusted to the contents shown in Table 1 below to obtain EVOH pellets containing the boron compound and the lubricant. rice field. Moreover, the total content of the boron compound and the content of the boron compound on the surface layer of the obtained boron compound and the lubricant-containing EVOH pellet were measured (moisture content 0.15%).
Then, using these pellets, a single-layer film was prepared in the same manner as in Example 1, and the occurrence of fish eyes was evaluated. The results are shown in Table 1 below.
〈実施例5〉
実施例1において滑剤としてステアリン酸マグネシウムを用い、ホウ素化合物全含有量、表層部のホウ素化合物含有量および滑剤含有量を、後記の表1の含有量に調整し、ホウ素化合物および滑剤含有EVOHペレットを得た。また、得られたホウ素化合物および滑剤含有EVOHペレットのホウ素化合物全含有量、表層部のホウ素化合物含有量を測定した(含水率0.15%)。
ついで、このペレットを用いて、実施例1と同様にして単層フィルムを作製し、フィッシュアイの発生について評価した。結果を後記の表1に示す。
<Example 5>
Magnesium stearate was used as a lubricant in Example 1, and the total content of the boron compound, the content of the boron compound on the surface layer and the content of the lubricant were adjusted to the contents shown in Table 1 below, and the boron compound and the lubricant-containing EVOH pellet were prepared. Obtained. Moreover, the total content of the boron compound and the content of the boron compound on the surface layer of the obtained boron compound and the lubricant-containing EVOH pellet were measured (moisture content 0.15%).
Then, using these pellets, a single-layer film was prepared in the same manner as in Example 1, and the occurrence of fish eyes was evaluated. The results are shown in Table 1 below.
〈比較例1〉
洗浄処理液を水に変更し、滑剤含有量を後記の表1の含有量に調整し、ホウ素化合物および滑剤含有EVOHペレットを得た。得られたホウ素化合物および滑剤含有EVOHペレットのホウ素全含有量、表層部のホウ素含有量を測定した(含水率0.13%)。
ついで、このペレットを用いて、実施例1と同様にして単層フィルムを作製し、フィッシュアイの発生について評価した。結果を後記の表1に示す。
<Comparative example 1>
The washing treatment liquid was changed to water, and the lubricant content was adjusted to the content shown in Table 1 below to obtain a boron compound and a lubricant-containing EVOH pellet. The total boron content of the obtained boron compound and the lubricant-containing EVOH pellet and the boron content of the surface layer were measured (moisture content 0.13%).
Then, using these pellets, a single-layer film was prepared in the same manner as in Example 1, and the occurrence of fish eyes was evaluated. The results are shown in Table 1 below.
〈比較例2〉
洗浄処理液による洗浄を行わず、滑剤を添加しなかった以外は、実施例1の場合と同様にして、ホウ素化合物含有EVOHペレットを得た。また、得られたホウ素化合物含有EVOHペレットのホウ素化合物全含有量、表層部のホウ素化合物含有量を測定した(含水率0.09%)。
ついで、このペレットを用いて、実施例1と同様にして単層フィルムを作製し、フィッシュアイの発生について評価した。結果を後記の表1に示す。
<Comparative example 2>
A boron compound-containing EVOH pellet was obtained in the same manner as in Example 1 except that the cleaning with the cleaning treatment solution was not performed and no lubricant was added. In addition, the total boron compound content of the obtained boron compound-containing EVOH pellet and the boron compound content of the surface layer were measured (moisture content 0.09%).
Then, using these pellets, a single-layer film was prepared in the same manner as in Example 1, and the occurrence of fish eyes was evaluated. The results are shown in Table 1 below.
〈比較例3,4〉
滑剤含有量を下記の表1の含有量に調整した以外は、実施例1の場合と同様にして、EVOHペレットを得た。得られたホウ素化合物および滑剤EVOHペレットのホウ素全含有量、表層部のホウ素含有量を測定した(含水率はいずれも0.10%)。
ついで、このペレットを用いて、実施例1と同様にして単層フィルムを作製し、フィッシュアイの発生について評価した。結果を下記の表1に示す。
<Comparative Examples 3 and 4>
EVOH pellets were obtained in the same manner as in Example 1 except that the lubricant content was adjusted to the content shown in Table 1 below. The total boron content of the obtained boron compound and the lubricant EVOH pellets and the boron content of the surface layer were measured (both water content was 0.10%).
Then, using these pellets, a single-layer film was prepared in the same manner as in Example 1, and the occurrence of fish eyes was evaluated. The results are shown in Table 1 below.
表層部のホウ素含有量が1.7ppm以下であり、かつ滑剤を当該ペレットの0.001〜0.15重量%含有する実施例1〜5のEVOHペレットは、比較例に比べてフィッシュアイの発生を大幅に抑制することができた。すなわち、実施例2と比較例1とを対比すると、ペレット全体のホウ素化合物含有量が同じレベルであり、かつ、滑剤含有量が同じであっても、ペレット表層部のホウ素化合物含有量を低減した実施例2のペレットの方がフィルム作製した際のフィルムのフィッシュアイ発生量が大幅に少ないことが分かる。 The EVOH pellets of Examples 1 to 5 having a surface layer having a boron content of 1.7 ppm or less and containing 0.001 to 0.15% by weight of a lubricant of the pellets generated fish eyes as compared with Comparative Examples. Was able to be significantly suppressed. That is, when Example 2 and Comparative Example 1 were compared, the boron compound content in the surface layer of the pellet was reduced even if the boron compound content of the entire pellet was the same level and the lubricant content was the same. It can be seen that the pellets of Example 2 generate significantly less fish eyes when the film is produced.
本発明のホウ素化合物および滑剤含有EVOHペレットは、ペレット表層部のホウ素化合物の含有量を減少させ、かつ滑剤の含有量を所定の範囲とすることで、成形性を損なうことなく、外観を向上させることができるため、従来のEVOHペレットよりも包装材料としての外観要求が厳しい分野に好適に利用することができる。 The boron compound and lubricant-containing EVOH pellets of the present invention improve the appearance without impairing moldability by reducing the content of the boron compound on the surface layer of the pellet and setting the content of the lubricant within a predetermined range. Therefore, it can be suitably used in a field where the appearance requirement as a packaging material is stricter than that of the conventional EVOH pellets.
Claims (5)
当該ペレット表層部のホウ素化合物含有量が、ホウ素換算で、当該ペレット重量あたり1.7ppm以下であり、かつ滑剤の含有量が当該ペレットの0.001〜0.15重量%であることを特徴とするエチレン−ビニルアルコール系共重合体ペレット。 Ethylene-vinyl alcohol-based copolymer pellets containing a boron compound and a lubricant.
The boron compound content of the surface layer of the pellet is 1.7 ppm or less per the weight of the pellet in terms of boron, and the content of the lubricant is 0.001 to 0.15% by weight of the pellet. Ethylene-vinyl alcohol-based copolymer pellets.
上記洗浄する工程の洗浄が、乾燥後のペレットと、水のアルコールに対する重量比(水/アルコール)が80/20〜0/100の水/アルコール混合溶液またはアルコールとを接触させることであり、
上記滑剤を含有させる工程が、滑剤を当該ペレットの0.001〜0.15重量%となるように含有させることを特徴とするエチレン−ビニルアルコール系共重合体ペレットの製造方法。 A step of bringing an ethylene-vinyl alcohol-based copolymer pellet into contact with a boron compound to contain a boron compound, and washing the pellet obtained by the above step to change the boron compound content of the surface layer of the pellet to ethylene in terms of boron. A method for producing an ethylene-vinyl alcohol-based copolymer pellet containing a boron compound and a lubricant, which comprises a step of reducing the weight to 1.7 ppm or less per vinyl alcohol-based copolymer pellet weight and a step of adding a lubricant.
The washing in the washing step is to bring the pellets after drying into contact with a water / alcohol mixed solution or alcohol having a weight ratio (water / alcohol) of water to alcohol of 80/20 to 0/100.
A method for producing an ethylene-vinyl alcohol-based copolymer pellet, wherein the step of containing the lubricant is such that the lubricant is contained in an amount of 0.001 to 0.15% by weight of the pellet.