JP5360701B2 - Carrier core material for electrophotographic developer, carrier, production method thereof, and electrophotographic developer using the carrier - Google Patents

Carrier core material for electrophotographic developer, carrier, production method thereof, and electrophotographic developer using the carrier Download PDF

Info

Publication number
JP5360701B2
JP5360701B2 JP2008204427A JP2008204427A JP5360701B2 JP 5360701 B2 JP5360701 B2 JP 5360701B2 JP 2008204427 A JP2008204427 A JP 2008204427A JP 2008204427 A JP2008204427 A JP 2008204427A JP 5360701 B2 JP5360701 B2 JP 5360701B2
Authority
JP
Japan
Prior art keywords
carrier
core material
carrier core
electrophotographic developer
resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2008204427A
Other languages
Japanese (ja)
Other versions
JP2010039368A (en
Inventor
康二 安賀
隆志 小島
享 岩田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Powdertech Co Ltd
Original Assignee
Powdertech Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Powdertech Co Ltd filed Critical Powdertech Co Ltd
Priority to JP2008204427A priority Critical patent/JP5360701B2/en
Publication of JP2010039368A publication Critical patent/JP2010039368A/en
Application granted granted Critical
Publication of JP5360701B2 publication Critical patent/JP5360701B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

<P>PROBLEM TO BE SOLVED: To provide a carrier core material for an electrophotographic developer and a carrier capable of obtaining a desired resistance such as a medium resistance or a high resistance while having high magnetization not only without using heavy metals but also substantially without using Mn, having excellent charging characteristics, and having both of surface properties with appropriate ruggedness and uniform shapes, to provide a method for manufacturing them, and to provide an electrophotographic developer using the carrier, capable of extending service life, having a high charge amount and excellent in charging stability. <P>SOLUTION: The carrier core material for an electrophotographic developer contains Mg by 2 to 8.5 wt.%, Ti by 0.1 to 1.25 wt.% and Fe by 60 to 70 wt.%, and includes a BET specific surface area of 0.075 to 0.11 m<SP>2</SP>/g. The carrier for an electrophotographic developer includes the above carrier core material coated with a resin. The method for manufacturing the carrier core material or the carrier is disclosed. The electrophotographic developer uses the above carrier. <P>COPYRIGHT: (C)2010,JPO&amp;INPIT

Description

本発明は、複写機、プリンター等に用いられる二成分系電子写真現像剤に使用される電子写真現像剤用キャリア芯材、キャリア及びこれらの製造方法、並びに該キャリアを用いた電子写真現像剤に関する。   The present invention relates to a carrier core material for an electrophotographic developer used in a two-component electrophotographic developer used in a copying machine, a printer, and the like, a carrier, a production method thereof, and an electrophotographic developer using the carrier. .

電子写真現像方法は、現像剤中のトナー粒子を感光体上に形成された静電潜像に付着させて現像する方法であり、この方法で使用される現像剤は、トナー粒子とキャリア粒子からなる二成分系現像剤及びトナー粒子のみを用いる一成分系現像剤に分けられる。   The electrophotographic development method is a method in which toner particles in a developer are attached to an electrostatic latent image formed on a photoreceptor and developed, and the developer used in this method is composed of toner particles and carrier particles. The two-component developer and the one-component developer using only toner particles.

こうした現像剤のうち、トナー粒子とキャリア粒子からなる二成分系現像剤を用いた現像方法としては、古くはカスケード法等が採用されていたが、現在では、マグネットロールを用いる磁気ブラシ法が主流である。   Among these developers, as a developing method using a two-component developer composed of toner particles and carrier particles, the cascade method has been used in the past, but at present, the magnetic brush method using a magnet roll is the mainstream. It is.

二成分系現像剤において、キャリア粒子は、現像剤が充填されている現像ボックス内において、トナー粒子と共に攪拌されることによって、トナー粒子に所望の電荷を付与し、さらにこのように電荷を帯びたトナー粒子を感光体の表面に搬送して感光体上にトナー像を形成するための担体物質である。マグネットを保持する現像ロール上に残ったキャリア粒子は、この現像ロールから再び現像ボックス内に戻り、新たなトナー粒子と混合・攪拌され、一定期間繰り返して使用される。   In the two-component developer, the carrier particles are agitated together with the toner particles in the developing box filled with the developer, thereby imparting a desired charge to the toner particles, and thus being charged. A carrier material for transporting toner particles to the surface of the photoreceptor to form a toner image on the photoreceptor. The carrier particles remaining on the developing roll holding the magnet are returned to the developing box from the developing roll, mixed and stirred with new toner particles, and used repeatedly for a certain period.

二成分系現像剤は、一成分系現像剤とは異なり、キャリア粒子はトナー粒子と混合・攪拌され、トナー粒子を帯電させ、さらに搬送する機能を有しており、現像剤を設計する際の制御性が良い。従って、二成分系現像剤は高画質が要求されるフルカラー現像装置及び画像維持の信頼性、耐久性が要求される高速印刷を行う装置等に適している。   Unlike the one-component developer, the two-component developer has the function of mixing and stirring the carrier particles with the toner particles, charging the toner particles, and further transporting the toner particles. Good controllability. Therefore, the two-component developer is suitable for a full-color developing device that requires high image quality and a device that performs high-speed printing that requires image maintenance reliability and durability.

このようにして用いられる二成分系現像剤においては、画像濃度、カブリ、白斑、階調性、解像力等の画像特性が、初期の段階から所定の値を示し、しかもこれらの特性が耐刷期間中に変動せず、安定に維持されることが必要である。これらの特性を安定に維持するためには、二成分系現像剤中に含有されるキャリア粒子の特性が安定していることが必要になる。   In the two-component developer used in this manner, image characteristics such as image density, fog, vitiligo, gradation, and resolving power show predetermined values from the initial stage, and these characteristics are in the printing life period. It needs to be kept stable without fluctuating inside. In order to maintain these characteristics stably, it is necessary that the characteristics of the carrier particles contained in the two-component developer are stable.

二成分系現像剤を形成するキャリア粒子として、従来は、表面を酸化被膜で覆った鉄粉あるいは表面を樹脂で被覆した鉄粉等の鉄粉キャリアが使用されていた。このような鉄粉キャリアは、磁化が高く、導電性も高いことから、ベタ部の再現性のよい画像が得られやすいという利点がある。   Conventionally, iron powder carriers such as iron powder whose surface is covered with an oxide film or iron powder whose surface is coated with a resin have been used as carrier particles for forming a two-component developer. Since such an iron powder carrier has high magnetization and high conductivity, there is an advantage that an image with a good reproducibility of the solid portion can be easily obtained.

しかしながら、このような鉄粉キャリアは真比重が約7.8と重く、また磁化が高すぎることから、現像ボックス中におけるトナー粒子との攪拌・混合により、鉄粉キャリア表面へのトナー構成成分の融着、いわゆるトナースペントが発生しやすくなる。このようなトナースペントの発生により有効なキャリア表面積が減少し、トナー粒子との摩擦帯電能力が低下しやすくなる。   However, such an iron powder carrier has a heavy true specific gravity of about 7.8 and is too high in magnetization, so that the toner constituent components on the surface of the iron powder carrier are mixed by stirring and mixing with toner particles in the developing box. Fusing, so-called toner spent, is likely to occur. The generation of such toner spent reduces the effective carrier surface area and tends to reduce the triboelectric charging ability with the toner particles.

また、樹脂被覆鉄粉キャリアでは、耐久時のストレスにより表面の樹脂が剥離し、高導電性で絶縁破壊電圧が低い芯材(鉄粉)が露出することにより、電荷のリークが生ずることがある。このような電荷のリークにより、感光体上に形成された静電潜像が破壊され、ベタ部にハケスジ等が発生し、均一な画像が得られにくい。これらの理由から、酸化被膜鉄粉及び樹脂被覆鉄粉等の鉄粉キャリアは、現在では使用されなくなってきている。   Moreover, in the resin-coated iron powder carrier, the resin on the surface peels off due to stress during durability, and the core material (iron powder) with high conductivity and low dielectric breakdown voltage is exposed, which may cause charge leakage. . Due to such charge leakage, the electrostatic latent image formed on the photoconductor is destroyed, and a crack or the like is generated in the solid portion, so that it is difficult to obtain a uniform image. For these reasons, iron powder carriers such as oxide-coated iron powder and resin-coated iron powder are no longer used.

近年は、鉄粉キャリアに代わって真比重約5.0程度と軽く、また磁化も低いフェライトをキャリアとして用いたり、さらに表面に樹脂を被覆した樹脂コートフェライトキャリアが多く使用されており、現像剤寿命は飛躍的に伸びてきた。   In recent years, instead of iron powder carriers, ferrite with a true specific gravity of about 5.0, which is light and has a low magnetization, or a resin-coated ferrite carrier whose surface is coated with a resin has been widely used. Lifespan has increased dramatically.

このようなフェライトキャリアの製造方法としては、フェライトキャリア原料を所定量混合した後、仮焼、粉砕し、造粒後に焼成を行うのが一般的であり、条件によっては仮焼を省略できる場合もある。   As a method for producing such a ferrite carrier, a predetermined amount of ferrite carrier raw material is mixed, calcined, pulverized, and then fired after granulation. Depending on conditions, calcining may be omitted. is there.

ところで、最近、環境規制が厳しくなり、Ni、Cu、Zn等の金属の使用は避けられるようになってきており、環境規制に適応した金属の使用が求められており、キャリア芯材として用いられるフェライト組成はCu−Znフェライト、Ni−ZnフェライトからMnを用いたMnフェライト、Mn−Mg−Srフェライト等に移行している。   Recently, environmental regulations have become stricter, and the use of metals such as Ni, Cu, and Zn has been avoided, and the use of metals suitable for environmental regulations has been demanded, and it is used as a carrier core material. The ferrite composition has shifted from Cu—Zn ferrite, Ni—Zn ferrite to Mn ferrite using Mn, Mn—Mg—Sr ferrite and the like.

特許文献1(特開2006−337828号公報)には、表面が溝又は筋で10μm四方あたり2〜50の領域に分割されており、マンガンフェライトを主成分とする電子写真用フェライトキャリア芯材が記載されている。このフェライトキャリア芯材は、組成が均一で、一定の表面性、良好な流動性を有し、かつ高磁化、低抵抗であり、このフェライトキャリア芯材に樹脂を被覆したフェライトキャリアを用いた電子写真用現像剤は、帯電の立ち上がりが速く、経時における安定した帯電量を有するとされている。   Patent Document 1 (Japanese Patent Application Laid-Open No. 2006-337828) discloses a ferrite carrier core material for electrophotography in which the surface is divided into regions of 2 to 50 per 10 μm square by grooves or streaks, and the main component is manganese ferrite. Have been described. This ferrite carrier core material has a uniform composition, constant surface properties, good fluidity, high magnetization, low resistance, and an electron using a ferrite carrier in which this ferrite carrier core material is coated with a resin. Photographic developers are said to have a fast charge rise and a stable charge over time.

この特許文献1では、上記のようなフェライトキャリア芯材を製造するために、FeとMnのモル比(Fe/Mn)が4〜16のFeとMnを主成分とする複合酸化物を粉砕、混合後、造粒、焼成し、さらに解砕、分級する製造方法において、焼成を酸素濃度が5体積%以下の雰囲気で行うことが示されている。   In Patent Document 1, in order to produce the ferrite carrier core material as described above, a composite oxide mainly composed of Fe and Mn having a molar ratio of Fe to Mn (Fe / Mn) of 4 to 16 is crushed. It has been shown that in a production method in which granulation, firing, and further pulverization and classification are performed after mixing, firing is performed in an atmosphere having an oxygen concentration of 5% by volume or less.

しかし、Mnも各種法規制の対象になりつつあり、上記各種重金属はもとよりMnを使用しない新たなキャリア芯材が求められている。   However, Mn is also subject to various laws and regulations, and a new carrier core material that does not use Mn as well as the above various heavy metals is demanded.

Mnを用いたキャリア芯材に代わるものとして、Mgを用いたキャリア芯材が提案されている。例えば、特許文献2(特開2005−162597号公報)には、式XMgFeCa(XはLi、Na、Ti等又はその組み合わせ)で示されるMg系フェライト材料(キャリア芯材)が示され、飽和磁化が30〜80emu/g、絶縁破壊電圧が1.5〜5.0kVであるとされ、このMg系フェライト材料により、高画質化と環境規制への対応を図ることができるとされている。 As an alternative to a carrier core material using Mn, a carrier core material using Mg has been proposed. For example, Patent Document 2 (JP 2005-162597), wherein X a Mg b Fe c Ca d O e (X is Li, Na, Ti, etc., or a combination thereof) Mg-based ferrite material represented by (carrier Core material), saturation magnetization is 30 to 80 emu / g, and dielectric breakdown voltage is 1.5 to 5.0 kV. With this Mg-based ferrite material, high image quality and compliance with environmental regulations are achieved. It is supposed to be possible.

また、特許文献3(特表2006−524627号公報)には、式MgFeCaで示されるMg系フェライト材料(キャリア芯材)が示され、飽和磁化が30〜80emu/g、絶縁破壊電圧が1.5〜5.0kVであるとされ、環境規制に対応したクリーンな材料で構成され、鮮明で階調性に富みカブリのない高画質像が得られるとされている。 Patent Document 3 (Japanese Patent Publication No. 2006-524627) discloses an Mg-based ferrite material (carrier core material) represented by the formula Mg a Fe b Ca c O d and has a saturation magnetization of 30 to 80 emu / g. It is said that the dielectric breakdown voltage is 1.5 to 5.0 kV, and is composed of a clean material that complies with environmental regulations, and a high-quality image that is clear, rich in gradation, and free from fog is obtained.

このようにMgを用いたキャリア芯材は提案されているが、一般に磁化と抵抗はトレードオフの関係にあるため、高磁化と中抵抗〜高抵抗といった特性を両立することは難しい。そのため、Mnを添加することで磁化と抵抗のトレードオフの関係を緩和し高磁化かつ中抵抗〜高抵抗を実現し、現在は電子写真現像剤用キャリア芯材として利用されている。しかしながら、上述したように、各種重金属規制の強化に伴いMnを使用しにくい状況となりつつある。   Thus, although the carrier core material using Mg is proposed, since magnetization and resistance are generally in a trade-off relationship, it is difficult to achieve both high magnetization and characteristics such as medium resistance to high resistance. Therefore, by adding Mn, the trade-off relationship between magnetization and resistance is relaxed to realize high magnetization, medium resistance to high resistance, and it is currently used as a carrier core material for electrophotographic developer. However, as described above, it is becoming difficult to use Mn with the strengthening of various heavy metal regulations.

また、Mnを意図的に添加しないMg系キャリア芯材において、従来の焼成方法でも高磁化、かつ中抵抗〜高抵抗を実現する方法としては、本焼成後、表面酸化することで抵抗を所望のレベルに合わせ込む取り組みがなされてきたが、上記トレードオフの関係を十分解決できているとは言えない。   In addition, in a Mg-based carrier core material in which Mn is not intentionally added, as a method of realizing high magnetization and medium resistance to high resistance even with a conventional firing method, a desired resistance can be obtained by surface oxidation after firing. Efforts to match the level have been made, but it cannot be said that the above trade-off relationship has been sufficiently solved.

また、従来よりMg系フェライトはFe過剰で製造することで磁化を高くすることが出来ることが知られている。しかし、抵抗はFe過剰であるため極めて低いものとなってしまっている。また、Fe過剰のMg系フェライトは、本焼成時の酸素濃度が高い場合や表面酸化によって磁化が急激に低くなると言う特徴を持っており、この現象はマグネタイト中に含まれるFe2+の酸化によるものと考えられている。 Conventionally, it has been known that Mg-based ferrite can increase magnetization by being produced with an excess of Fe. However, the resistance is extremely low due to the excess of Fe. In addition, Fe-excess Mg-based ferrite is characterized by a sharp decrease in magnetization due to high oxygen concentration during surface firing or surface oxidation. This phenomenon is due to oxidation of Fe 2+ contained in magnetite. It is believed that.

一方、Fe以外の遷移金属を含有しないMg系フェライトの焼成温度は1250〜1350℃程度ときわめて高温であり、キャリア芯材に求められる表面性はほとんど凹凸のないものしか得られないだけでなく、焼成時にキャリア芯材粒子同士が凝集しやすく球形ではない粒子が多く含まれることとなる。そのため、意図的に重金属を含有せず、高磁化、中抵抗〜高抵抗で、かつ適度な凹凸を有する表面性と揃った形状を実現した電子写真現像剤用キャリア芯材は得られていないのが現状である。   On the other hand, the firing temperature of Mg-based ferrite that does not contain a transition metal other than Fe is as high as about 1250 to 1350 ° C., and not only the surface properties required for the carrier core material can be obtained with almost no unevenness, The carrier core particles are likely to aggregate during firing and contain many particles that are not spherical. Therefore, a carrier core material for an electrophotographic developer that does not intentionally contain a heavy metal, has a shape that has high magnetization, medium resistance to high resistance, and a surface property that has moderate unevenness has not been obtained. Is the current situation.

特開2006−337828号公報JP 2006-337828 A 特開2005−162597号公報Japanese Patent Laid-Open No. 2005-162597 特表2006−524627号公報JP 2006-524627 A

従って、本発明の目的は、各重金属のみならず、Mnを実質的に用いることなしに、高磁化でありながら中抵抗又は高抵抗といった所望の抵抗が得られ、かつ帯電特性に優れ、しかも適度な凹凸を有する表面性と揃った形状とを兼備する電子写真現像剤用キャリア芯材、キャリア及びこれらの製造方法、並びに該キャリアを用いた長寿命化が達成され、かつ高い帯電量を有し、帯電安定性にも優れた電子写真現像剤を提供することにある。   Therefore, the object of the present invention is to obtain a desired resistance such as medium resistance or high resistance while being highly magnetized without substantially using not only each heavy metal but also Mn, excellent charging characteristics, and moderate Carrier core material for electrophotographic developer having both surface properties with uniform irregularities, a carrier, a method for producing the same, and a long life using the carrier, and a high charge amount Another object of the present invention is to provide an electrophotographic developer having excellent charging stability.

本発明者らは、上記のような課題を解決すべく鋭意検討した結果、Mg、Ti、Sr及びFeを一定量含有し、かつ望ましくはMgフェライトを構成するスピネル構造以外に少なくともFe及びTiを含有する酸化物の結晶構造を含有し、一定範囲の比表面積を有するキャリア芯材及びこれに樹脂を被覆したキャリアが上記目的を達成し得ることを知見し、本発明に至った。 As a result of intensive studies to solve the above-mentioned problems, the inventors of the present invention contain a certain amount of Mg, Ti , Sr and Fe, and preferably at least Fe and Ti other than the spinel structure constituting Mg ferrite. The present inventors have found that a carrier core material having a crystal structure of an oxide to be contained and having a specific surface area within a certain range and a carrier coated with a resin can achieve the above object, and have reached the present invention.

すなわち、本発明は、Mgを2〜8.5重量%、Tiを0.1〜1.25重量%、Srを0.37〜2.5重量%及びFeを60〜70重量%含有し、BET比表面積が0.075〜0.11m/gであることを特徴とする電子写真現像剤用キャリア芯材を提供するものである。 That is, the present invention contains 2 to 8.5 wt% Mg, 0.1 to 1.25 wt% Ti, 0.37 to 2.5 wt% Sr and 60 to 70 wt% Fe, A carrier core material for an electrophotographic developer, which has a BET specific surface area of 0.075 to 0.11 m 2 / g.

本発明の上記電子写真現像剤用キャリア芯材は、Mgフェライトを構成するスピネル構造以外に少なくともFe及びTiを含有する酸化物の結晶構造を含有することが望ましい。   The carrier core material for an electrophotographic developer of the present invention preferably contains a crystal structure of an oxide containing at least Fe and Ti in addition to the spinel structure constituting Mg ferrite.

本発明の上記電子写真現像剤用キャリア芯材は、Mnの含有量が1重量%以下であることが望ましい。   The carrier core material for an electrophotographic developer of the present invention preferably has a Mn content of 1% by weight or less.

本発明の上記電子写真現像剤用キャリア芯材は、3K・1000/4π・A/mの磁場をかけたときの磁化が45〜75Am/kg、残留磁化が2〜10Am/kg及び保磁力が10〜80 3K・1000/4π・A/mであることが望ましい。 The carrier core material for an electrophotographic developer of the present invention, magnetization is 45~75Am 2 / kg when a magnetic field was applied in the 3K · 1000 / 4π · A / m, a residual magnetization of 2~10Am 2 / kg and a coercive The magnetic force is desirably 10 to 80 3K · 1000 / 4π · A / m.

本発明の上記電子写真現像剤用キャリア芯材は、レーザー回折式粒度分布測定装置により測定される平均粒径が15〜120μmであることが望ましい。   The carrier core material for an electrophotographic developer according to the present invention preferably has an average particle size of 15 to 120 μm as measured by a laser diffraction particle size distribution analyzer.

本発明の上記電子写真現像剤用キャリア芯材は、形状係数SF−2(真円度)が100〜120であることが望ましい。   The carrier core material for an electrophotographic developer according to the present invention preferably has a shape factor SF-2 (roundness) of 100 to 120.

本発明の上記電子写真現像剤用キャリア芯材は、印加電圧50Vにおける体積抵抗が1×10〜1×1010Ω・cmであることが好ましい。 The carrier core material for an electrophotographic developer according to the present invention preferably has a volume resistance of 1 × 10 6 to 1 × 10 10 Ω · cm at an applied voltage of 50V.

本発明の上記電子写真現像剤用キャリア芯材は、表面酸化処理され、酸化処理被膜が形成されていることが望ましく、その際の印加電圧50Vにおける体積抵抗が1×10〜1×1010Ω・cm、かつ印加電圧1000Vにおける体積抵抗が6×10〜1×1010Ω・cmであることが好ましい。 The carrier core material for an electrophotographic developer according to the present invention is desirably surface-oxidized to form an oxidized film, and the volume resistance at an applied voltage of 50 V is 1 × 10 6 to 1 × 10 10. It is preferable that the volume resistance at an applied voltage of 1000 V is 6 × 10 6 to 1 × 10 10 Ω · cm.

本発明は、上記キャリア芯材の表面が樹脂で被覆されている電子写真現像剤用キャリアを提供するものである。   The present invention provides a carrier for an electrophotographic developer in which the surface of the carrier core material is coated with a resin.

本発明の上記電子現像剤用キャリアにおいて、上記樹脂は、アクリル樹脂、シリコーン樹脂又は変性シリコーン樹脂であることが望ましい。   In the carrier for an electronic developer according to the present invention, the resin is preferably an acrylic resin, a silicone resin, or a modified silicone resin.

また、本発明は、Fe、TiMg及びSrの各化合物を粉砕、混合、仮焼した後、造粒し、得られた造粒物を1次焼成、本焼成し、さらに解砕、分級、表面酸化処理する電子写真現像剤用キャリア芯材の製造方法において、上記本焼成が、酸素濃度が5体積%以下で行われることを特徴とする上記電子写真現像剤用キャリア芯材の製造方法を提供するものである。 In the present invention, each compound of Fe, Ti 2 , Mg, and Sr is pulverized, mixed, calcined, granulated, and the resulting granulated product is subjected to primary firing, main firing, further pulverization, classification. in the manufacturing method of the carrier core material for electrophotographic developer to surface oxidation treatment, the main baking is, method of manufacturing the carrier core material for an electrophotographic developer, wherein the oxygen concentration is carried out at 5 vol% or less Is to provide.

本発明は、上記製造方法で得られたキャリア芯材の表面を樹脂で被覆することを特徴とする電子写真現像剤用キャリアの製造方法を提供するものである。   The present invention provides a method for producing a carrier for an electrophotographic developer, wherein the surface of the carrier core obtained by the above production method is coated with a resin.

本発明は、上記キャリア又は上記製造方法により得られたキャリアとトナーからなる電子写真現像剤を提供するものである。   The present invention provides an electrophotographic developer comprising the above carrier or the carrier obtained by the above production method and a toner.

本発明に係る電子写真現像剤用キャリア芯材は、各重金属のみならず、Mnを実質的に用いることなしに、高磁化でありながら中抵抗又は高抵抗といった所望の抵抗が得られ、かつ帯電特性に優れ、しかも適度な凹凸を有する表面性と揃った形状とを兼ね備える。そして、上記キャリア芯材に樹脂を被覆して得られるキャリアとトナーとからなる電子写真現像剤は、長寿命化が達成され、かつ高い帯電量を有し、帯電安定性にも優れる。また、本発明の製造方法によって、上記キャリア芯材及びキャリアが工業的規模をもって安定的に製造できる。   The carrier core material for an electrophotographic developer according to the present invention can obtain a desired resistance such as a medium resistance or a high resistance while being highly magnetized without using not only each heavy metal but also Mn. It has excellent characteristics and also has a surface shape with moderate irregularities and a uniform shape. An electrophotographic developer comprising a carrier and a toner obtained by coating the carrier core material with a resin has a long life, has a high charge amount, and is excellent in charging stability. Moreover, the carrier core material and the carrier can be stably produced on an industrial scale by the production method of the present invention.

以下、本発明を実施するための最良の形態について説明する。   Hereinafter, the best mode for carrying out the present invention will be described.

<本発明に係る電子写真現像剤用キャリア芯材及びキャリア>
本発明に係る電子写真現像剤用キャリア芯材は、Mgを2〜8.5重量%、好ましくは2.2〜8.3重量%、より好ましくは2.4〜8.3重量%、Tiを0.1〜1.25重量%、好ましくは0.15〜1.25重量%、より好ましくは0.18〜1.25重量%、Feを60〜70重量%、好ましくは60〜68.5重量%、より好ましくは60〜67重量%含有する。上記組成範囲において、高磁化でありながら中抵抗〜高抵抗が得られ、また電子写真現像剤用キャリアとして使用する際も帯電特性も安定しており良好である。
<Carrier Core Material and Carrier for Electrophotographic Developer According to the Present Invention>
In the carrier core material for an electrophotographic developer according to the present invention, Mg is 2 to 8.5% by weight, preferably 2.2 to 8.3% by weight, more preferably 2.4 to 8.3% by weight, Ti. 0.1 to 1.25 wt%, preferably 0.15 to 1.25 wt%, more preferably 0.18 to 1.25 wt%, Fe 60 to 70 wt%, preferably 60 to 68.%. 5% by weight, more preferably 60 to 67% by weight. Within the above composition range, medium resistance to high resistance can be obtained while being highly magnetized, and charging characteristics are stable and good when used as a carrier for an electrophotographic developer.

MgはMgOの電気陰性度がプラス側に偏っているためマイナストナーに対する相性はきわめて良く、MgOを含有するMgフェライトキャリアとフルカラー用のトナーで構成される帯電の立ち上がりが良い現像剤を得ることが出来る。   Since Mg is negatively negative in terms of MgO electronegativity, it has a very good compatibility with negative toners, and it is possible to obtain a developer having a good rise in charge composed of a Mg ferrite carrier containing MgO and a full color toner. I can do it.

TiOは電気陰性度がややマイナス側に偏っているため本来であればマイナストナーとの相性は良くないが、1.25重量%よりも少ない範囲でFeとTiの化合物(酸化物)としてマイナストナー用キャリア含有することで帯電性に関してはその影響を最小限にすることが出来る。 Since TiO 2 is slightly negative in electronegativity, it is not compatible with minus toners originally, but it is minus as a compound (oxide) of Fe and Ti within a range less than 1.25% by weight. By including the toner carrier, the influence on the charging property can be minimized.

Feの含有量が60重量%未満では、Mg及び/又はTiの添加量が相対的に増えることで非磁性成分及び/又は低磁化成分が増加し、所望の磁気特性が得られないことを意味しており、70重量%を超えるとMg及び/又はTiの添加効果は得られず実質的にマグネタイトと同等のキャリア芯材になってしまう。Mgの含有量はMg:Fe2+=1:2〜1:3付近が最も良い。Mgの含有量が2重量%未満では、キャリア芯材におけるマグネシウムフェライト相の生成量が少なく、マグネタイト相の生成量が相対的に増加することで保磁力が増大し所望の磁気特性が得られなくなる可能性があり、8.5重量%を超えるとキャリア芯材中にマグネシウムフェライト以外に酸化マグネシウムが生成し所望の磁気特性が得られなくなる可能性がある。Tiの含有量が0.15重量%未満では、FeとTiの複合酸化物の生成量が少ないため所望の磁気特性が得られない可能性があり、1.25重量%を超えると、FeとTiの複合酸化物による非磁性相が支配的になるため磁化が低くなりすぎ所望の磁気特性が得られなくなる可能性がある。 If the Fe content is less than 60% by weight, it means that the nonmagnetic component and / or low magnetization component increases due to the relative increase in the addition amount of Mg and / or Ti, and the desired magnetic properties cannot be obtained. However, if it exceeds 70% by weight, the effect of adding Mg and / or Ti cannot be obtained, and the carrier core material is substantially equivalent to magnetite. The Mg content is best around Mg: Fe 2+ = 1: 2 to 1: 3. If the Mg content is less than 2% by weight, the amount of magnesium ferrite phase produced in the carrier core material is small, and the amount of magnetite phase produced is relatively increased, so that the coercive force increases and the desired magnetic properties cannot be obtained. If it exceeds 8.5% by weight, magnesium oxide may be generated in addition to magnesium ferrite in the carrier core material, and desired magnetic properties may not be obtained. If the Ti content is less than 0.15% by weight, there is a possibility that desired magnetic properties may not be obtained due to a small amount of Fe and Ti composite oxides. If the Ti content exceeds 1.25% by weight, Fe and Ti Since the nonmagnetic phase due to the composite oxide of Ti becomes dominant, there is a possibility that the magnetization becomes too low to obtain desired magnetic characteristics.

本発明に係る電子写真現像剤用キャリア芯材は、BET比表面積が0.075〜0.11m/gである。BET比表面積が0.075m/g未満では、芯材表面の凹凸が少ないため樹脂被覆後の樹脂のアンカー効果が得られず、電子写真用キャリアとして寿命が短くなる可能性があり、BET比表面積が0.11m/gを超えると芯材表面の樹脂の凹凸が大きく樹脂がしみ込みやすくなるため電子写真用キャリアとして所望の特性が得られなくなる可能性がある。このBET比表面積は、下記により測定される。 The carrier core material for an electrophotographic developer according to the present invention has a BET specific surface area of 0.075 to 0.11 m 2 / g. When the BET specific surface area is less than 0.075 m 2 / g, since the core surface has few irregularities, the anchor effect of the resin after resin coating cannot be obtained, and the life as an electrophotographic carrier may be shortened. If the surface area exceeds 0.11 m 2 / g, the resin surface irregularities on the surface of the core material are so large that the resin can easily penetrate, so that there is a possibility that desired characteristics as an electrophotographic carrier cannot be obtained. This BET specific surface area is measured by the following.

(BET比表面積)
自動比表面積測定装置GEMINI2360」(島津製作所社製)を用いて、吸着ガスであるNを吸着させて測定したキャリア粒子のN吸着量から求めることができる。なお、ここでは、このN吸着量を測定する際に用いられる測定管は、測定前に、減圧状態にて50℃で2時間の空焼きを行った。さらに、この測定管にキャリア粒子5gを充填し、減圧状態で30℃の温度で2時間前処理を行った後に、25℃下でNガスをそれぞれ吸着させてその吸着量を測定した。それらの吸着量は、吸着等温線を描き、BET式から算出される値である。
(BET specific surface area)
Using an automatic specific surface area measuring apparatus GEMINI 2360 (manufactured by Shimadzu Corp.), it can be determined from the N 2 adsorption amount of carrier particles measured by adsorbing N 2 as an adsorption gas. Here, the measurement tube used for measuring the N 2 adsorption amount was baked for 2 hours at 50 ° C. in a reduced pressure state before the measurement. Further, 5 g of carrier particles were filled in this measuring tube, and after pretreatment at a temperature of 30 ° C. for 2 hours under reduced pressure, N 2 gas was adsorbed at 25 ° C., and the amount of adsorption was measured. These adsorption amounts are values calculated from the BET equation by drawing an adsorption isotherm.

本発明に係る電子写真現像剤用キャリア芯材は、Mgフェライトを構成するスピネル構造以外に少なくともFe及びTiを含有する酸化物の結晶構造を含有する。Fe過剰のMg系フェライトにTiを添加することで通常のフェライトを構成するスピネル結晶構造の化合物以外に比較的磁化の低いFe及びTiを含有する複合酸化物を必要とする磁化の範囲で生成させ、表面酸化処理時にスピネル相よりも優先的にFe及びTiを含有する複合酸化物を酸化させることで磁化を変化させることなく抵抗のみを制御することが可能となる。つまり、Fe及びTiを含有する複合酸化物中に含まれるFeの価数が変化することで抵抗を調整している。結晶構造については、下記によって測定される。   The carrier core material for an electrophotographic developer according to the present invention contains an oxide crystal structure containing at least Fe and Ti in addition to the spinel structure constituting Mg ferrite. By adding Ti to Fe-excess Mg-based ferrite, a composite oxide containing Fe and Ti with relatively low magnetization can be generated in the range of magnetization, in addition to the spinel crystal structure compound constituting ordinary ferrite. It is possible to control only the resistance without changing the magnetization by oxidizing the composite oxide containing Fe and Ti preferentially over the spinel phase during the surface oxidation treatment. That is, the resistance is adjusted by changing the valence of Fe contained in the composite oxide containing Fe and Ti. The crystal structure is measured by the following.

(結晶構造の測定:X線回折測定)
測定装置としてパナリティカル社製「X’PertPRO MPD」を用いた。X線源としてCo管球(CoKα線)を、光学系として集中光学系及び高速検出器「X‘Celarator」を用いて、測定は0.02°のステップスキャンで行った。測定結果は通常の粉末の結晶構造解析と同様に解析用ソフトウエア「X’Pert HighScore」を用いてデータ処理し、結晶構造の同定を行った。なお、結晶構造を同定を行う際にFe,Oを必須元素としMg、Ti、Srは含有する可能性のある元素とした。また、X線源についてはCu管球でも問題なく測定できるが、Feを多く含んだサンプルの場合には測定対象となるピークと比較してバックグラウンドが大きくなるので、Co管球を用いる方が好ましい。また、光学系は平行法でも同様の結果が得られる可能性があるが、X線強度が低く測定に時間がかかるため集中光学系での測定が好ましい。さらに、ステップスキャンの各点におけるカウント時間はスピネル構造の(311)面のピーク強度が約200000cpsとなるようにし、粒子の特定の優先方向への配向がないようにサンプルセルにキャリア芯材をセットし測定を行った。
(Measurement of crystal structure: X-ray diffraction measurement)
“X′PertPRO MPD” manufactured by Panalical Co., Ltd. was used as a measuring apparatus. Using a Co tube (CoKα ray) as an X-ray source and a concentrated optical system and a high-speed detector “X'Celarator” as an optical system, the measurement was performed by a step scan of 0.02 °. The measurement results were processed using data for analysis “X'Pert HighScore” in the same manner as in the crystal structure analysis of ordinary powders, and the crystal structure was identified. When identifying the crystal structure, Fe and O are essential elements, and Mg, Ti, and Sr are elements that may be contained. In addition, the X-ray source can be measured without problems even with a Cu tube, but in the case of a sample containing a large amount of Fe, the background becomes larger than the peak to be measured, so it is better to use a Co tube. preferable. In addition, the optical system may obtain the same result even when the parallel method is used, but measurement with a concentrated optical system is preferable because the X-ray intensity is low and measurement takes time. Furthermore, the count time at each point of the step scan is such that the peak intensity of the (311) plane of the spinel structure is about 200,000 cps, and the carrier core material is set in the sample cell so that the particles are not oriented in a specific preferred direction. And measured.

Mgフェライトを構成するスピネル構造としてMgFeが代表的なものであるが、元素の構成比からもわかるようにFe過剰であるためMgの一部がFeに置換され形式的にMgFey−x、(MgFe1−x)(Mgx‘Fe1−x’等で表現される結晶構造及びその一部がSrに置換されたものもすべて含まれるものとし、非酸化性雰囲気で焼成されることにより周期的にスピネル構造に格子欠陥が含まれるものも含むものとする。 MgFe 2 O 4 is a typical spinel structure constituting Mg ferrite. However, as can be seen from the composition ratio of the elements, since Fe is excessive, a part of Mg is replaced with Fe and formally Mg x Fe. The crystal structure represented by y-xO 4 , (Mg x Fe 1-x ) (Mg x ′ Fe 1-x ′ ) 2 O 4, etc., and all of which are partially substituted with Sr In addition, it also includes those in which lattice defects are periodically included in the spinel structure by firing in a non-oxidizing atmosphere.

Fe及びTiを含有する酸化物の結晶構造としてFeTiO、FeTiOが代表的なものであるがTiと比べてFeが圧倒的に存在量としては多く、FeTiO以外に(FeTiO(Fe、Fe(FeTi)O、(FeTi1−x)(Fex‘Ti1−x’)O等で表現される結晶構造及びその一部がSrに置換されたSrFeTi等で表わされる酸化物もすべて含まれるものとし、非酸化性雰囲気で焼成されることにより周期的に上記結晶構造に格子欠陥が含まれるものも含むものとする。 FeTiO 3 and Fe 2 TiO 5 are typical crystal structures of oxides containing Fe and Ti, but Fe is overwhelmingly abundant as compared to Ti, and other than Fe x TiO y (FeTiO 3). 3) x (Fe 2 O 3 ) y, Fe (Fe x Ti y) O 4, (Fe x Ti 1-x) (Fe x 'Ti 1-x') crystal structure and is represented by O 4 or the like that All oxides represented by Sr a Fe b Ti c O d partially substituted with Sr are also included, and the crystal structure contains lattice defects periodically by firing in a non-oxidizing atmosphere. It is also included.

本発明に係る電子写真現像剤用キャリア芯材は、Srを0.37〜2.5重量%含有する。Srを添加しない場合、酸素濃度が高い状態で本焼成を行うとFeが生成し磁化が下がることが多いが、Srを添加することでFeではなくSrフェライトが生成し、酸素濃度がふれても磁化が安定しやすくなる。さらに、1次焼成及び本焼成時にSrがグレイン表面に移動する効果によりさらに抵抗及び芯材の帯電量を上げる効果が期待できる。Srの含有量が2.5重量%を超えると、ハードフェライト化しはじめるため磁気ブラシ上で現像剤の流動性が急激に悪くなる恐れがある。 The carrier core material for an electrophotographic developer according to the present invention, that Yusuke 0.37 to 2.5 wt% including the Sr. When Sr is not added, Fe 2 O 3 is generated and magnetization is often reduced when firing is performed at a high oxygen concentration, but Sr ferrite is generated instead of Fe 2 O 3 by adding Sr, Even if the oxygen concentration is touched, the magnetization is easily stabilized. Furthermore, the effect of further increasing the resistance and the charge amount of the core material can be expected due to the effect of Sr moving to the grain surface during primary firing and main firing. When the content of Sr exceeds 2.5% by weight, the fluidity of the developer on the magnetic brush may be abruptly deteriorated because it begins to hard ferrite.

なお、Sr及びFeを含有する酸化物の結晶構造としては上記のようにSrO・6FeまたはSrFe1219として表現されるSrフェライトがあり、本発明に係る電子写真現像用キャリア芯材に含有されていても良い。 The crystal structure of the oxide containing Sr and Fe includes Sr ferrite expressed as SrO.6Fe 2 O 3 or SrFe 12 O 19 as described above, and the carrier core material for electrophotographic development according to the present invention. It may be contained in.

本発明に係る電子写真現像剤用キャリア芯材は、Mnの含有量が1重量%以下であることが望ましい。Mnは、意図的に含有させるものではないが、原料由来の不純物としてのMnの微量の含有は問題ない。これらFe、Mg、Ti、Sr及びMnの含有量は、下記によって測定される。   The carrier core material for an electrophotographic developer according to the present invention preferably has a Mn content of 1% by weight or less. Although Mn is not intentionally contained, the inclusion of a very small amount of Mn as an impurity derived from the raw material is not a problem. The contents of these Fe, Mg, Ti, Sr and Mn are measured by the following.

(Fe、Mg、Ti、Sr及びMnの含有量)
キャリア芯材0.2gを秤量し、純水60mlに1Nの塩酸20ml及び1Nの硝酸20mlを加えたものを加熱し、キャリア芯材を完全溶解させた水溶液を準備し、ICP分析装置(島津製作所製ICPS−1000IV)を用いてFe、Mg、Ti、Sr及びMnの含有量を測定した。
(Contents of Fe, Mg, Ti, Sr and Mn)
0.2 g of carrier core material is weighed, 60 ml of pure water plus 20 ml of 1N hydrochloric acid and 20 ml of 1N nitric acid is heated to prepare an aqueous solution in which the carrier core material is completely dissolved, and an ICP analyzer (Shimadzu Corporation) The contents of Fe, Mg, Ti, Sr, and Mn were measured using ICPS-1000IV).

本発明に係る電子写真現像剤用キャリア芯材は、3K・1000/4π・A/mの磁場をかけたときの磁化が45〜75Am/kgであることが望ましい。上記3K・1000/4π・A/mにおける磁化が45Am2/g未満であると、飛散物磁化が悪化しキャリア付着による画像欠陥の原因となる可能性があり、75Am2/gを超えると、磁気ブラシ上における現像剤の穂が硬くなりすぎ画質を劣化させる可能性がある。残留磁化は2〜10Am/kgであることが望ましい。上記3K・1000/4π・A/mにおける残留磁化は本発明に係る組成において2Am/kg未満にはならない。10Am/kgを超えると現像器中での現像剤の流動性が悪化し、十分に現像剤を攪拌しトナーに摩擦帯電を与えることが出来なくなる。保磁力は本発明に係る組成において10 3K・1000/4π・A/m未満にはならない。80 3K・1000/4π・A/m超えると現像器中での現像剤の流動性が悪化し、十分に現像剤を攪拌しトナーに摩擦帯電を与えることが出来なくなる。磁化、残留磁化及び保磁力は、下記によって測定される。 The carrier core material for an electrophotographic developer according to the present invention preferably has a magnetization of 45 to 75 Am 2 / kg when a magnetic field of 3K · 1000 / 4π · A / m is applied. If the magnetization at 3K · 1000 / 4π · A / m is less than 45 Am 2 / g, the scattered matter magnetization may deteriorate and cause image defects due to carrier adhesion. If the magnetization exceeds 75 Am 2 / g, the magnetic brush There is a possibility that the top of the developer becomes too hard and the image quality is deteriorated. The residual magnetization is desirably 2 to 10 Am 2 / kg. The remanent magnetization at 3K · 1000 / 4π · A / m is not less than 2 Am 2 / kg in the composition according to the present invention. If it exceeds 10 Am 2 / kg, the fluidity of the developer in the developing device deteriorates, and it becomes impossible to sufficiently stir the developer and give the toner triboelectric charge. The coercivity is not less than 10 3 K · 1000 / 4π · A / m in the composition according to the present invention. If it exceeds 80 3K · 1000 / 4π · A / m, the fluidity of the developer in the developing device deteriorates, and the developer cannot be sufficiently stirred to give the toner triboelectric charge. Magnetization, remanent magnetization and coercivity are measured by:

(磁気特性)
積分型B−HトレーサーBHU−60型(理研電子社製)を使用して測定した。電磁石間に磁場測定用Hコイル及び磁化測定用4πIコイルを入れる。この場合、試料は4πIコイルに入れる。電磁石の電流を変化させ磁場Hを変化させたHコイル及び4πIコイルの出力をそれぞれ積分し、H出力をX軸に、4πIコイルの出力をY軸に、ヒステリシスループを記録紙に描く。ここで測定条件としては、試料充填量:約1g、試料充填セル:内径7mmφ±0.02mm、高さ10mm±0.1mm、4πIコイル:巻数30回にて測定した。
(Magnetic properties)
It measured using the integral type BH tracer BHU-60 type (made by Riken Denshi Co., Ltd.). A magnetic field measuring H coil and a magnetization measuring 4πI coil are placed between the electromagnets. In this case, the sample is placed in a 4πI coil. The outputs of the H coil and the 4πI coil whose magnetic field H is changed by changing the current of the electromagnet are respectively integrated, and the H output is drawn on the X axis, the output of the 4πI coil is drawn on the Y axis, and a hysteresis loop is drawn on the recording paper. As measurement conditions, sample filling amount: about 1 g, sample filling cell: inner diameter 7 mmφ ± 0.02 mm, height 10 mm ± 0.1 mm, 4πI coil: measured with 30 turns.

本発明に係る電子写真現像剤用キャリア芯材は、レーザー回折式粒度分布測定装置により測定される平均粒径が好ましくは15〜120μm、より好ましくは15〜80μm、最も好ましくは15〜60μmである。体積平均粒径が15μm未満であると、キャリア付着が発生しやすくなるため好ましくない。体積平均粒径が120μmを超えると、画質が劣化しやすくなり、好ましくない。この体積平均粒径は、下記によって測定される。   The carrier core material for an electrophotographic developer according to the present invention preferably has an average particle size measured by a laser diffraction particle size distribution measuring device of 15 to 120 μm, more preferably 15 to 80 μm, and most preferably 15 to 60 μm. . If the volume average particle size is less than 15 μm, carrier adhesion tends to occur, which is not preferable. If the volume average particle diameter exceeds 120 μm, the image quality tends to deteriorate, which is not preferable. This volume average particle size is measured by:

(体積平均粒径)
装置として日機装株式会社製マイクロトラック粒度分析計(Model9320−X100)を用いた。分散媒には水を用いた。
(Volume average particle size)
As a device, a Nikkiso Co., Ltd. Microtrac particle size analyzer (Model 9320-X100) was used. Water was used as the dispersion medium.

本発明に係る電子写真現像剤用キャリア芯材は、形状係数SF−2(真円度)が100〜120であることが望ましい。形状係数SF−2は、キャリアの投影周囲長を2乗した値をキャリアの投影面積で割った値に4πで除し、さらに100倍して得られる数値であり、キャリアの形状が球に近いほど100に近い値になる。キャリア芯材の形状係数SF−2が120を超えると芯材表面の樹脂の凹凸が大きいことを意味し、樹脂がしみ込みやすくなるため電子写真用キャリアとして所望の特性が得られなくなる可能性がある。この形状係数SF−2(真円度)は、下記によって測定される。   The carrier core material for an electrophotographic developer according to the present invention preferably has a shape factor SF-2 (roundness) of 100 to 120. The shape factor SF-2 is a value obtained by dividing the value obtained by squaring the carrier projection perimeter length by the value obtained by dividing the value by the carrier projection area by 4π, and multiplying it by 100. The shape of the carrier is close to a sphere. The value becomes closer to 100. If the shape factor SF-2 of the carrier core material exceeds 120, it means that the unevenness of the resin on the surface of the core material is large, and the resin tends to penetrate, so that there is a possibility that desired characteristics cannot be obtained as an electrophotographic carrier. is there. This shape factor SF-2 (roundness) is measured by the following.

(形状係数SF−2(真円度))

Figure 0005360701
(Shape factor SF-2 (roundness))
Figure 0005360701

本発明に係る電子写真現像剤用キャリア芯材の印加電圧50Vにおける体積抵抗は、1×10〜1×1010Ω・cmであることが望ましい。体積抵抗が1×10Ω・cm未満では、抵抗が低すぎて帯電低下を引き起こす可能性がある。体積抵抗が1×1010Ω・cmを超えると、抵抗が高くなりすぎ、摩擦帯電に伴う電荷の移動が阻害される恐れがある。この体積抵抗の測定方法は後述する。 The volume resistance of the carrier core material for an electrophotographic developer according to the present invention at an applied voltage of 50 V is desirably 1 × 10 6 to 1 × 10 10 Ω · cm. If the volume resistance is less than 1 × 10 6 Ω · cm, the resistance is too low, which may cause a decrease in charge. When the volume resistance exceeds 1 × 10 10 Ω · cm, the resistance becomes too high, and there is a possibility that the movement of electric charge accompanying triboelectric charging is hindered. A method for measuring this volume resistance will be described later.

本発明に係る電子写真現像剤用キャリア芯材は、表面が酸化処理されていることが望ましい。この表面酸化処理によって形成される酸化処理被膜の厚さは、0.1nm〜5μmであることが好ましい。0.1nm未満であると、酸化被膜層の効果が小さく、5μmを超えると、磁化が低下したり、高抵抗になりすぎるため、現像能力が低下する等の不具合が発生し易くなる。また、必要に応じて、酸化処理の前に還元を行ってもよい。   The surface of the carrier core material for an electrophotographic developer according to the present invention is desirably oxidized. The thickness of the oxidized film formed by this surface oxidation treatment is preferably 0.1 nm to 5 μm. If the thickness is less than 0.1 nm, the effect of the oxide film layer is small, and if it exceeds 5 μm, the magnetization is lowered or the resistance becomes too high, so that problems such as a reduction in developing ability tend to occur. Moreover, you may reduce | restore before an oxidation process as needed.

この酸化処理されたキャリア芯材の印加電圧50Vにおける体積抵抗が、6×10〜1×1010Ω・cm、かつ印加電圧1000Vにおける体積抵抗が、6×10〜1×1010Ω・cmであることが望ましい。印加電圧50Vにおける体積抵抗が1×10Ω・cm未満では、抵抗が低すぎて帯電低下を引き起こす可能性がある。印加電圧50Vにおける体積抵抗が1×1010Ω・cmを超えると、抵抗が高くなりすぎ、摩擦帯電に伴う電荷の移動が阻害される恐れがある。印加電圧1000Vにおける体積抵抗が6×10Ω・cm未満では、抵抗が低すぎて帯電低下を引き起こす可能性がある。印加電圧1000Vにおける体積抵抗が1×1010Ω・cmを超えると、抵抗が高くなりすぎ、摩擦帯電に伴う電荷の移動が阻害される恐れがある。この体積抵抗は、下記によって測定される。 Volume resistivity in this oxidation process is applied voltage 50V of the carrier core material, 6 × 10 6 ~1 × 10 10 Ω · cm, and the volume resistivity of the applied voltage 1000V, 10 10 Ω · 6 × 10 6 ~1 × It is desirable to be cm. When the volume resistance at an applied voltage of 50 V is less than 1 × 10 6 Ω · cm, the resistance is too low, which may cause a decrease in charging. If the volume resistance at an applied voltage of 50 V exceeds 1 × 10 10 Ω · cm, the resistance becomes too high, and there is a possibility that the movement of electric charge accompanying frictional charging is hindered. If the volume resistance at an applied voltage of 1000 V is less than 6 × 10 6 Ω · cm, the resistance is too low, which may cause a decrease in charging. When the volume resistance at an applied voltage of 1000 V exceeds 1 × 10 10 Ω · cm, the resistance becomes too high, and there is a possibility that the movement of electric charges accompanying frictional charging is hindered. This volume resistance is measured by:

(体積抵抗)
断面積が4cmのフッ素樹脂製のシリンダーに高さ4mmとなるように試料を充填した後、両端に電極を取り付け、さらにその上から1kgの分銅を乗せて抵抗を測定した。抵抗の測定はケースレー社製6517A型絶縁抵抗測定器にて測定電圧50Vを印加し5秒後の抵抗を測定し、体積抵抗を算出した。
(Volume resistance)
A sample was filled in a fluororesin cylinder having a cross-sectional area of 4 cm 2 so that the height was 4 mm, electrodes were attached to both ends, and a weight of 1 kg was further placed thereon to measure resistance. The resistance was measured by applying a measurement voltage of 50 V with a Keithley 6517A type insulation resistance measuring instrument, measuring the resistance after 5 seconds, and calculating the volume resistance.

本発明に係る電子写真現像剤用キャリアは、上記キャリア芯材の表面が樹脂で被覆されている。   In the carrier for an electrophotographic developer according to the present invention, the surface of the carrier core material is coated with a resin.

本発明に係る電子写真現像剤用樹脂被覆キャリアは、樹脂被膜量が、キャリア芯材に対して0.1〜10重量%が望ましい。被膜量が0.01重量%未満ではキャリア表面に均一な被膜層を形成することが難しく、また10重量%を超えるとキャリア同士の凝集が発生してしまい、歩留まり低下等の生産性の低下と共に、実機内での流動性あるいは帯電量等の現像剤特性変動の原因となる。   The resin-coated carrier for an electrophotographic developer according to the present invention desirably has a resin coating amount of 0.1 to 10% by weight with respect to the carrier core material. If the coating amount is less than 0.01% by weight, it is difficult to form a uniform coating layer on the surface of the carrier. If the coating amount exceeds 10% by weight, the carriers are aggregated with a decrease in productivity such as a decrease in yield. This causes fluctuations in developer characteristics such as fluidity or charge amount in the actual machine.

ここに用いられる被膜形成樹脂は、組み合わせるトナー、使用される環境等によって適宜選択できる。その種類は特に限定されないが、例えば、フッ素樹脂、アクリル樹脂、エポキシ樹脂、ポリアミド樹脂、ポリアミドイミド樹脂、ポリエステル樹脂、不飽和ポリエステル樹脂、尿素樹脂、メラミン樹脂、アルキッド樹脂、フェノール樹脂、フッ素アクリル樹脂、アクリル−スチレン樹脂、シリコーン樹脂、あるいはアクリル樹脂、ポリエステル樹脂、エポキシ樹脂、ポリアミド樹脂、ポリアミドイミド樹脂、アルキッド樹脂、ウレタン樹脂、フッ素樹脂等の各樹脂で変性した変性シリコーン樹脂等が挙げられる。本発明では、アクリル樹脂、シリコーン樹脂又は変性シリコーン樹脂が最も好ましく用いられる。   The film forming resin used here can be appropriately selected depending on the toner to be combined, the environment in which it is used, and the like. The type is not particularly limited, for example, fluorine resin, acrylic resin, epoxy resin, polyamide resin, polyamideimide resin, polyester resin, unsaturated polyester resin, urea resin, melamine resin, alkyd resin, phenol resin, fluorine acrylic resin, Examples thereof include acrylic-styrene resins, silicone resins, or modified silicone resins modified with resins such as acrylic resins, polyester resins, epoxy resins, polyamide resins, polyamideimide resins, alkyd resins, urethane resins, and fluororesins. In the present invention, acrylic resin, silicone resin or modified silicone resin is most preferably used.

またキャリアの電気抵抗や帯電量、帯電速度をコントロールすることを目的に、被膜形成樹脂中に導電性剤を添加することができる。導電性剤はそれ自身の持つ電気抵抗が低いことから、添加量が多すぎると急激な電荷リークを引き起こしやすい。従って、添加量としては、被膜形成樹脂の固形分に対し0.25〜20.0重量%であり、好ましくは0.5〜15.0重量%、特に好ましくは1.0〜10.0重量%である。導電性剤としては、導電性カーボンや酸化チタン、酸化スズ等の酸化物、各種の有機系導電剤が挙げられる。   A conductive agent can be added to the film-forming resin for the purpose of controlling the electrical resistance, charge amount, and charging speed of the carrier. Since the conductive agent itself has a low electric resistance, an excessive amount of the conductive agent tends to cause an abrupt charge leak. Accordingly, the addition amount is 0.25 to 20.0% by weight, preferably 0.5 to 15.0% by weight, particularly preferably 1.0 to 10.0% by weight, based on the solid content of the film-forming resin. %. Examples of the conductive agent include conductive carbon, oxides such as titanium oxide and tin oxide, and various organic conductive agents.

また、上記被膜形成樹脂中には、帯電制御剤を含有させることができる。帯電制御剤の例としては、トナー用に一般的に用いられる各種の帯電制御剤や、各種シランカップリング剤が挙げられる。これは被膜形成によって芯材露出面積を比較的小さくなるように制御した場合、帯電付与能力が低下することがあるが、各種の帯電制御剤やシランカップリング剤を添加することにより、コントロールできるためである。使用できる帯電制御剤やカップリング剤の種類は特に限定されないが、ニグロシン系染料、4級アンモニウム塩、有機金属錯体、含金属モノアゾ染料等の帯電制御剤、アミノシランカップリング剤やフッ素系シランカップリング剤等が好ましい。   In addition, the film forming resin can contain a charge control agent. Examples of the charge control agent include various charge control agents generally used for toners and various silane coupling agents. This is because, when the core material exposed area is controlled to be relatively small by film formation, the charge imparting ability may decrease, but it can be controlled by adding various charge control agents and silane coupling agents. It is. The types of charge control agents and coupling agents that can be used are not particularly limited, but charge control agents such as nigrosine dyes, quaternary ammonium salts, organometallic complexes, and metal-containing monoazo dyes, aminosilane coupling agents, and fluorine-based silane couplings. An agent or the like is preferable.

(帯電量測定)
負帯電性市販トナー3gとキャリア47gを秤量し、50mlのガラスビンに入れて常温・常湿環境下(N/N環境:室温25℃、湿度55%)下に1時間暴露した。暴露後、常温・常湿環境下でボールミルでガラスビンが100回転になるように回転数を合わせて混合攪拌を行い、攪拌開始後1min、3min、10min、30min後にサンプリングし、帯電量をEpping社製吸引帯電量測定装置にて測定した。
(Charge amount measurement)
3 g of negatively chargeable commercially available toner and 47 g of a carrier were weighed and placed in a 50 ml glass bottle and exposed for 1 hour in a normal temperature and normal humidity environment (N / N environment: room temperature 25 ° C., humidity 55%). After exposure, mix and stir the mixture so that the glass bottle reaches 100 revolutions with a ball mill in a normal temperature and normal humidity environment, sample after 1 min, 3 min, 10 min, 30 min after the start of stirring, and charge amount made by Epping Measured with a suction charge measuring device.

<本発明に係る電子写真現像剤用キャリア芯材及びキャリアの製造方法>
次に、本発明に係る電子写真現像剤用キャリア芯材及びキャリアの製造方法について説明する。
<Carrier Core Material for Electrophotographic Developer According to the Present Invention and Carrier Manufacturing Method>
Next, the carrier core material for an electrophotographic developer and the method for producing the carrier according to the present invention will be described.

本発明に係る電子写真現像剤用キャリア芯材の製造方法は、Fe、TiMg及びSrの各化合物を粉砕、混合、仮焼を行った後、造粒し、得られた造粒物を1次焼成、本焼成し、さらに解砕、分級、表面酸化処理する。 The carrier core material for electrophotographic developer according to the present invention is produced by pulverizing, mixing and calcining each compound of Fe, Ti 2 , Mg and Sr , and granulating the resulting granulated product. Primary firing, main firing, crushing, classification, and surface oxidation treatment are performed.

Fe、TiMg及びSrの各化合物を粉砕、混合後、造粒して造粒物を調製する方法は、特に制限はなく、従来公知の方法が採用することができ、乾式による方法を用いても湿式による方法を用いてもよい。原料としてFeとTiOとMg(OH)及び/又はMgCOを混合し、さらにカーボンブラック及び/又はバインダーを添加し、非酸化性雰囲気又は弱還元性雰囲気で焼成し、少なくとも2価のFeを含有するスピネル相及びFeとTiを含有する複合酸化物相が存在するフェライト前駆体の状態を生成しておくことが良い。従来の製造方法では本焼成時にFeからスピネル相を生成させるため結晶構造の変化にかなりのエネルギーが必要となるが、あらかじめFeとTiOとMg(OH)及び/又はMgCOを混合し、さらにカーボンブラック及び/又はバインダーを添加し仮焼成を行った場合には、本焼成において必要最小限の結晶構造の変化だけでフェライト化が終了するので低温焼成が可能となる。なお、バインダーとしてはポリビニルアルコールやポリビニルピロリドンを使うことが好ましい。 The method of preparing each granulated product by pulverizing, mixing, and granulating each compound of Fe, Ti , Mg, and Sr is not particularly limited, and a conventionally known method can be adopted, and a dry method is used. Alternatively, a wet method may be used. Fe 2 O 3 , TiO 2 , Mg (OH) 2 and / or MgCO 3 are mixed as raw materials, carbon black and / or a binder are further added, and calcined in a non-oxidizing atmosphere or weakly reducing atmosphere, at least 2 It is preferable to generate a ferrite precursor state in which a spinel phase containing valent Fe and a composite oxide phase containing Fe and Ti are present. In the conventional manufacturing method, since a spinel phase is generated from Fe 2 O 3 at the time of main firing, considerable energy is required to change the crystal structure, but Fe 2 O 3 , TiO 2 , Mg (OH) 2 and / or When MgCO 3 is mixed and carbon black and / or binder is added and calcining is performed, low-temperature firing is possible because ferritization is completed with only a minimum change in the crystal structure in the main firing. . In addition, it is preferable to use polyvinyl alcohol or polyvinylpyrrolidone as a binder.

本発明の製造方法では、得られた造粒物を1次焼成、本焼成する。1次焼成は、非酸化性雰囲気下、500〜1100℃で行われる。   In the production method of the present invention, the obtained granulated product is subjected to primary firing and main firing. The primary firing is performed at 500 to 1100 ° C. in a non-oxidizing atmosphere.

次に、1280℃以下で本焼成が行われる。本焼成はより結晶構造をしっかりしたものとし、表面酸化による磁化の低下を防止する効果が期待できる。1次焼成を行うことで本焼成において1次焼成を行わない場合と比較して低温で焼成できるため、凹凸を持った芯材粒子としやすくなるだけでなく、高い球形度を確保することが可能となる。   Next, the main baking is performed at 1280 ° C. or lower. The main firing has a more solid crystal structure, and an effect of preventing a decrease in magnetization due to surface oxidation can be expected. By performing the primary firing, it can be fired at a lower temperature in comparison with the case where the primary firing is not performed in the main firing, so that not only the core particles with irregularities are easily formed but also high sphericity can be secured. It becomes.

本発明の製造方法では、上述したように、予め本焼成前の芯材粒子の造粒物の時点で原料由来の結晶構造だけでなく、少なくとも2価のFeを含有するスピネル相及びFeとTiを含有する複合酸化物相を含有し、さらに非酸化性雰囲気下、500〜1100℃で1次焼成を行うことでヘマタイトを経由せずにフェライト化を促進することが出来るので、本焼成においても従来と比較して1280℃以下の低温焼成が可能となる。   In the production method of the present invention, as described above, not only the crystal structure derived from the raw material but also the spinel phase containing at least divalent Fe and Fe and Ti in advance at the time of granulation of the core material particles before the main firing. In the main firing, ferritization can be promoted without passing through hematite by performing primary firing at 500 to 1100 ° C. in a non-oxidizing atmosphere. Compared to the conventional case, low temperature firing at 1280 ° C. or lower is possible.

本発明の製造方法では、本焼成を酸素濃度が5体積%以下の雰囲気で行う。酸素濃度が5体積%を超える場合は、焼成物の磁化が低くなりすぎ、キャリア飛散の原因となるので好ましくない。高磁化のキャリア芯材を得るために、酸素濃度3体積%以下が好ましく、1体積%以下がさらに好ましい。   In the production method of the present invention, the main baking is performed in an atmosphere having an oxygen concentration of 5% by volume or less. When the oxygen concentration exceeds 5% by volume, the magnetization of the fired product becomes too low, which causes carrier scattering, which is not preferable. In order to obtain a highly magnetized carrier core material, the oxygen concentration is preferably 3% by volume or less, more preferably 1% by volume or less.

その後、回収し、乾燥、分級を行いキャリア芯材を得る。分級方法としては、既存の風力分級、メッシュ濾過法、沈降法など用いて所望の粒径に粒度調整する。乾式回収を行う場合は、サイクロン等で回収することも可能である。   Thereafter, it is collected, dried and classified to obtain a carrier core material. As a classification method, the particle size is adjusted to a desired particle size using an existing air classification, mesh filtration method, sedimentation method, or the like. When dry collection is performed, it can also be collected with a cyclone or the like.

その後、必要に応じて、表面を低温加熱することで酸化被膜処理を施し、電気抵抗調整を行うことができる。酸化被膜処理は、一般的なロータリー式電気炉、バッチ式電気炉等を用い、例えば、300〜800℃で熱処理を行う。酸化皮膜を均一に芯材粒子に形成させるためにはロータリー式電気炉を用いることが好ましい。   Thereafter, if necessary, the surface can be heated at a low temperature to perform an oxide film treatment to adjust electric resistance. For the oxide film treatment, a general rotary electric furnace, batch electric furnace or the like is used, and for example, heat treatment is performed at 300 to 800 ° C. In order to uniformly form the oxide film on the core particles, it is preferable to use a rotary electric furnace.

本発明の電子写真現像剤用キャリアは、上記キャリア芯材の表面に、上記した樹脂を被覆し、樹脂被膜を形成する。被覆する方法としては、公知の方法、例えば刷毛塗り法、流動床によるスプレードライ方式、ロータリドライ方式、万能攪拌機による液浸乾燥法等により被覆することができる。被覆率を向上させるためには、流動床による方法が好ましい。   In the carrier for an electrophotographic developer of the present invention, the surface of the carrier core material is coated with the above resin to form a resin film. As a coating method, it can be coated by a known method such as a brush coating method, a spray drying method using a fluidized bed, a rotary drying method, an immersion drying method using a universal stirrer, or the like. In order to improve the coverage, a fluidized bed method is preferred.

樹脂をキャリア芯材に被覆後、焼き付けする場合には、外部加熱方式又は内部加熱方式のいずれでもよく、例えば固定式又は流動式電気炉、ロータリー式電気炉、バーナー炉でもよく、もしくはマイクロウェーブによる焼き付けでもよい。
UV硬化樹脂を用いる場合は、UV加熱器を用いる。焼き付けの温度は使用する樹脂により異なるが、融点又はガラス転移点以上の温度は必要であり、熱硬化性樹脂又は縮合架橋型樹脂等では、充分硬化が進む温度まで上げる必要がある。
When the resin is coated on the carrier core and then baked, either an external heating method or an internal heating method may be used, for example, a fixed or fluid electric furnace, a rotary electric furnace, a burner furnace, or by microwave It can be burned.
When a UV curable resin is used, a UV heater is used. Although the baking temperature varies depending on the resin to be used, a temperature equal to or higher than the melting point or the glass transition point is necessary. For a thermosetting resin or a condensation-crosslinking resin, it is necessary to raise the temperature to a point where the curing proceeds sufficiently.

<本発明に係る電子写真用現像剤>
次に、本発明に係る電子写真用現像剤について説明する。
本発明に係る電子写真現像剤は、上述した電子写真現像剤用キャリアとトナーとからなるものである。
<Electrophotographic developer according to the present invention>
Next, the electrophotographic developer according to the present invention will be described.
The electrophotographic developer according to the present invention comprises the above-described carrier for an electrophotographic developer and a toner.

本発明の電子写真現像剤を構成するトナー粒子には、粉砕法によって製造される粉砕トナー粒子と、重合法により製造される重合トナー粒子とがある。本発明ではいずれの方法により得られたトナー粒子も使用することができる。   The toner particles constituting the electrophotographic developer of the present invention include pulverized toner particles produced by a pulverization method and polymerized toner particles produced by a polymerization method. In the present invention, toner particles obtained by any method can be used.

粉砕トナー粒子は、例えば、結着樹脂、荷電制御剤、着色剤をヘンシェルミキサー等の混合機で充分に混合し、次いで、二軸押出機等で溶融混練し、冷却後、粉砕、分級し、外添剤を添加後、ミキサー等で混合することにより得ることができる。   The pulverized toner particles are, for example, a binder resin, a charge control agent, and a colorant are sufficiently mixed with a mixer such as a Henschel mixer, then melt-kneaded with a twin screw extruder or the like, cooled, pulverized, classified, After adding the external additive, it can be obtained by mixing with a mixer or the like.

粉砕トナー粒子を構成する結着樹脂としては特に限定されるものではないが、ポリスチレン、クロロポリスチレン、スチレン−クロロスチレン共重合体、スチレン−アクリル酸エステル共重合体、スチレン−メタクリル酸共重合体、更にはロジン変性マレイン酸樹脂、エポキシ樹脂、ポリエステル樹脂及びポリウレタン樹脂等を挙げることができる。これらは単独又は混合して用いられる。   The binder resin constituting the pulverized toner particles is not particularly limited, but polystyrene, chloropolystyrene, styrene-chlorostyrene copolymer, styrene-acrylic acid ester copolymer, styrene-methacrylic acid copolymer, Furthermore, rosin modified maleic acid resin, epoxy resin, polyester resin, polyurethane resin and the like can be mentioned. These may be used alone or in combination.

荷電制御剤としては、任意のものを用いることができる。例えば正荷電性トナー用としては、ニグロシン系染料及び4級アンモニウム塩等を挙げることができ、また、負荷電性トナー用としては、含金属モノアゾ染料等を挙げることができる。   Any charge control agent can be used. For example, nigrosine dyes and quaternary ammonium salts can be used for positively charged toners, and metal-containing monoazo dyes can be used for negatively charged toners.

着色剤(色剤)としては、従来より知られている染料、顔料が使用可能である。例えば、カーボンブラック、フタロシアニンブルー、パーマネントレッド、クロムイエロー、フタロシアニングリーン等を使用することができる。その他、トナーの流動性、耐凝集性向上のためのシリカ粉体、チタニア等のような外添剤をトナー粒子に応じて加えることができる。   As the colorant (colorant), conventionally known dyes and pigments can be used. For example, carbon black, phthalocyanine blue, permanent red, chrome yellow, phthalocyanine green, etc. can be used. In addition, external additives such as silica powder and titania for improving the fluidity and aggregation resistance of the toner can be added according to the toner particles.

重合トナー粒子は、懸濁重合法、乳化重合法、乳化凝集法、エステル伸長重合法、相転乳化法といった公知の方法で製造されるトナー粒子である。このような重合法トナー粒子は、例えば、界面活性剤を用いて着色剤を水中に分散させた着色分散液と、重合性単量体、界面活性剤及び重合開始剤を水性媒体中で混合攪拌し、重合性単量体を水性媒体中に乳化分散させて、攪拌、混合しながら重合させた後、塩析剤を加えて重合体粒子を塩析させる。塩析によって得られた粒子を、濾過、洗浄、乾燥させることにより、重合トナー粒子を得ることができる。その後、必要により乾燥されたトナー粒子に機能付与のため外添剤を添加することもできる。   The polymerized toner particles are toner particles produced by a known method such as a suspension polymerization method, an emulsion polymerization method, an emulsion aggregation method, an ester elongation polymerization method, or a phase inversion emulsification method. Such polymerized toner particles are prepared by, for example, mixing and stirring a colored dispersion in which a colorant is dispersed in water using a surfactant, a polymerizable monomer, a surfactant, and a polymerization initiator in an aqueous medium. Then, the polymerizable monomer is emulsified and dispersed in an aqueous medium, polymerized while stirring and mixing, and then a salting-out agent is added to salt out the polymer particles. Polymerized toner particles can be obtained by filtering, washing and drying the particles obtained by salting out. Thereafter, if necessary, an external additive may be added to the dried toner particles to provide a function.

更に、この重合トナー粒子を製造するに際しては、重合性単量体、界面活性剤、重合開始剤、着色剤以外に、定着性改良剤、帯電制御剤を配合することができ、これらにより得られた重合トナー粒子の諸特性を制御、改善することができる。また、水性媒体への重合性単量体の分散性を改善するとともに、得られる重合体の分子量を調整するために連鎖移動剤を用いることができる。   Further, in the production of the polymerized toner particles, in addition to the polymerizable monomer, the surfactant, the polymerization initiator, and the colorant, a fixability improving agent and a charge control agent can be blended and obtained. Various characteristics of the polymerized toner particles can be controlled and improved. A chain transfer agent can be used to improve the dispersibility of the polymerizable monomer in the aqueous medium and adjust the molecular weight of the resulting polymer.

上記重合トナー粒子の製造に使用される重合性単量体に特に限定はないが、例えば、スチレン及びその誘導体、エチレン、プロピレン等のエチレン不飽和モノオレフィン類、塩化ビニル等のハロゲン化ビニル類、酢酸ビニル等のビニルエステル類、アクリル酸メチル、アクリル酸エチル、メタクリル酸メチル、メタクリル酸エチル、メタクリル酸2−エチルヘキシル、アクリル酸ジメチルアミノエステル及びメタクリル酸ジエチルアミノエステル等のα−メチレン脂肪族モノカルボン酸エステル類等を挙げることができる。   The polymerizable monomer used for the production of the polymerized toner particles is not particularly limited. For example, styrene and its derivatives, ethylene unsaturated monoolefins such as ethylene and propylene, vinyl halides such as vinyl chloride, Α-methylene aliphatic monocarboxylic acids such as vinyl esters such as vinyl acetate, methyl acrylate, ethyl acrylate, methyl methacrylate, ethyl methacrylate, 2-ethylhexyl methacrylate, dimethylamino acrylate and diethylaminoester methacrylate Examples include esters.

上記重合トナー粒子の調製の際に使用される着色剤(色材)としては、従来から知られている染料、顔料が使用可能である。例えば、カーボンブラック、フタロシアニンブルー、パーマネントレッド、クロムイエロー及びフタロシアニングリーン等を使用することができる。また、これらの着色剤はシランカップリング剤やチタンカップリング剤等を用いてその表面が改質されていてもよい。   Conventionally known dyes and pigments can be used as the colorant (coloring material) used in the preparation of the polymerized toner particles. For example, carbon black, phthalocyanine blue, permanent red, chrome yellow, phthalocyanine green, and the like can be used. Moreover, the surface of these colorants may be modified using a silane coupling agent, a titanium coupling agent, or the like.

上記重合トナー粒子の製造に使用される界面活性剤としては、アニオン系界面活性剤、カチオン系界面活性剤、両イオン性界面活性剤及びノニオン系界面活性剤を使用することができる。   As the surfactant used in the production of the polymerized toner particles, an anionic surfactant, a cationic surfactant, an amphoteric surfactant and a nonionic surfactant can be used.

ここで、アニオン系界面活性剤としては、オレイン酸ナトリウム、ヒマシ油等の脂肪酸塩、ラウリル硫酸ナトリウム、ラウリル硫酸アンモニウム等のアルキル硫酸エステル、ドデシルベンゼンスルホン酸ナトリウム等のアルキルベンゼンスルホン酸塩、アルキルナフタレンスルホン酸塩、アルキルリン酸エステル塩、ナフタレンスルホン酸ホルマリン縮合物、ポリオキシエチレンアルキル硫酸エステル塩等を挙げることができる。また、ノニオン性界面活性剤としては、ポリオキシエチレンアルキルエーテル、ポリオキシエチレン脂肪酸エステル、ソルビタン脂肪酸エステル、ポリオキシエチレンアルキルアミン、グリセリン、脂肪酸エステル、オキシエチレン−オキシプロピレンブロックポリマー等を挙げることができる。更に、カチオン系界面活性剤としては、ラウリルアミンアセテート等のアルキルアミン塩、ラウリルトリメチルアンモニウムクロライド、ステアリルトリメチルアンモニウムクロライド等の第4級アンモニウム塩等を挙げることができる。また、両イオン性界面活性剤としては、アミノカルボン酸塩、アルキルアミノ酸等を挙げることができる。   Here, examples of the anionic surfactant include fatty acid salts such as sodium oleate and castor oil, alkyl sulfates such as sodium lauryl sulfate and ammonium lauryl sulfate, alkyl benzene sulfonates such as sodium dodecyl benzene sulfonate, and alkyl naphthalene sulfonic acids. Salt, alkyl phosphate ester salt, naphthalene sulfonic acid formalin condensate, polyoxyethylene alkyl sulfate ester salt and the like. Examples of the nonionic surfactant include polyoxyethylene alkyl ether, polyoxyethylene fatty acid ester, sorbitan fatty acid ester, polyoxyethylene alkylamine, glycerin, fatty acid ester, and oxyethylene-oxypropylene block polymer. . Furthermore, examples of the cationic surfactant include alkylamine salts such as laurylamine acetate, and quaternary ammonium salts such as lauryltrimethylammonium chloride and stearyltrimethylammonium chloride. Examples of amphoteric surfactants include aminocarboxylates and alkylamino acids.

上記のような界面活性剤は、重合性単量体に対して、通常は0.01〜10重量%の範囲内の量で使用することができる。このような界面活性剤は、単量体の分散安定性に影響を与えるとともに、得られた重合トナー粒子の環境依存性にも影響を及ぼす。上記範囲内の量で使用することは単量体の分散安定性の確保と重合トナー粒子の環境依存性を低減する観点から好ましい。   The surfactant as described above can be used usually in an amount in the range of 0.01 to 10% by weight with respect to the polymerizable monomer. Such a surfactant affects the dispersion stability of the monomer and also affects the environmental dependency of the obtained polymerized toner particles. Use in an amount within the above range is preferable from the viewpoint of ensuring the dispersion stability of the monomer and reducing the environmental dependency of the polymerized toner particles.

重合トナー粒子の製造には、通常は重合開始剤を使用する。重合開始剤には、水溶性重合開始剤と油溶性重合開始剤とがあり、本発明ではいずれをも使用することができる。本発明で使用することができる水溶性重合開始剤としては、例えば、過硫酸カリウム、過硫酸アンモニウム等の過硫酸塩、水溶性パーオキサイド化合物を挙げることができ、また、油溶性重合開始剤としては、例えば、アゾビスイソブチロニトリル等のアゾ系化合物、油溶性パーオキサイド化合物を挙げることができる。   For the production of polymerized toner particles, a polymerization initiator is usually used. The polymerization initiator includes a water-soluble polymerization initiator and an oil-soluble polymerization initiator, and any of them can be used in the present invention. Examples of the water-soluble polymerization initiator that can be used in the present invention include persulfates such as potassium persulfate and ammonium persulfate, water-soluble peroxide compounds, and oil-soluble polymerization initiators. Examples thereof include azo compounds such as azobisisobutyronitrile and oil-soluble peroxide compounds.

また、本発明において連鎖移動剤を使用する場合には、この連鎖移動剤としては、例えば、オクチルメルカプタン、ドデシルメルカプタン、tert−ドデシルメルカプタン等のメルカプタン類、四臭化炭素等を挙げることができる。   When a chain transfer agent is used in the present invention, examples of the chain transfer agent include mercaptans such as octyl mercaptan, dodecyl mercaptan, tert-dodecyl mercaptan, carbon tetrabromide, and the like.

更に、本発明で使用する重合トナー粒子が、定着性改善剤を含む場合、この定着性改良剤としては、カルナバワックス等の天然ワックス、ポリプロピレン、ポリエチレン等のオレフィン系ワックス等を使用することができる。   Further, when the polymerized toner particles used in the present invention contain a fixability improver, a natural wax such as carnauba wax, an olefin wax such as polypropylene or polyethylene can be used as the fixability improver. .

また、本発明で使用する重合トナー粒子が、帯電制御剤を含有する場合、使用する帯電制御剤に特に制限はなく、ニグロシン系染料、4級アンモニウム塩、有機金属錯体、含金属モノアゾ染料等を使用することができる。   Further, when the polymerized toner particles used in the present invention contain a charge control agent, the charge control agent to be used is not particularly limited, and nigrosine dyes, quaternary ammonium salts, organometallic complexes, metal-containing monoazo dyes, etc. Can be used.

また、重合トナー粒子の流動性向上等のために使用される外添剤としては、シリカ、酸化チタン、チタン酸バリウム、フッ素樹脂微粒子、アクリル樹脂微粒子等を挙げることができ、これらは単独であるいは組み合わせて使用することができる。   Examples of the external additive used for improving the fluidity of polymerized toner particles include silica, titanium oxide, barium titanate, fluororesin fine particles, and acrylic resin fine particles. Can be used in combination.

更に、水性媒体から重合粒子を分離するために使用される塩析剤としては、硫酸マグネシウム、硫酸アルミニウム、塩化バリウム、塩化マグネシウム、塩化カルシウム、塩化ナトリウム等の金属塩を挙げることができる。   Furthermore, examples of the salting-out agent used for separating the polymer particles from the aqueous medium include metal salts such as magnesium sulfate, aluminum sulfate, barium chloride, magnesium chloride, calcium chloride, and sodium chloride.

上記のようにして製造されたトナー粒子の体積平均粒径は、2〜15μm、好ましくは3〜10μmの範囲内にあり、重合トナー粒子の方が粉砕トナー粒子よりも、粒子の均一性が高い。トナー粒子が2μmよりも小さくなると、帯電能力が低下しかぶりやトナー飛散を引き起こしやすく、15μmを超えると、画質が劣化する原因となる。   The volume average particle size of the toner particles produced as described above is in the range of 2 to 15 μm, preferably 3 to 10 μm, and the polymerized toner particles have higher particle uniformity than the pulverized toner particles. . If the toner particles are smaller than 2 μm, the charging ability is lowered, and it is easy to cause fogging and toner scattering, and if it exceeds 15 μm, the image quality is deteriorated.

上記のように製造されたキャリアとトナーとを混合し、電子写真現像剤を得ることができる。キャリアとトナーの混合比、即ちトナー濃度は、3〜15重量%に設定することが好ましい。3重量%未満であると所望の画像濃度が得にくく、15重量%を超えると、トナー飛散やかぶりが発生しやすくなる。   An electrophotographic developer can be obtained by mixing the carrier and toner manufactured as described above. The mixing ratio of the carrier and the toner, that is, the toner concentration is preferably set to 3 to 15% by weight. If it is less than 3% by weight, it is difficult to obtain a desired image density. If it exceeds 15% by weight, toner scattering and fogging are likely to occur.

上記のように調製された本発明に係る電子写真現像剤は、有機光導電体層を有する潜像保持体に形成されている静電潜像を、バイアス電界を付与しながら、トナー及びキャリアを有する二成分現像剤の磁気ブラシによって反転現像する現像方式を用いたデジタル方式のコピー機、プリンター、FAX、印刷機等に使用することができる。また、磁気ブラシから静電潜像側に現像バイアスを印加する際に、DCバイアスにACバイアスを重畳する方法である交番電界を用いるフルカラー機等にも適用可能である。   The electrophotographic developer according to the present invention prepared as described above uses an electrostatic latent image formed on a latent image holding member having an organic photoconductor layer, while applying a bias electric field to the toner and the carrier. The present invention can be used in digital copiers, printers, fax machines, printers, and the like that use a developing method in which reversal development is performed using a two-component developer magnetic brush. Further, the present invention can also be applied to a full color machine using an alternating electric field, which is a method of superimposing an AC bias on a DC bias when a developing bias is applied from the magnetic brush to the electrostatic latent image side.

以下、実施例等に基づき本発明を具体的に説明する。   Hereinafter, the present invention will be specifically described based on examples and the like.

Feを8.12モル、Mgを1モル、Tiを0.135モル、Srを0.15モルとなるようにFe、Mg(OH)、TiO、SrCOを秤量し、固形分が50重量%となるように水を加えビーズミルで混合し、混合したスラリーをスプレードライヤーで造粒した。このとき、バインダー成分としてPVAを固形分の2重量%となるように、またポリカルボン酸系分散剤をスラリーの粘度が1〜2ポイズになるように添加し、得られた造粒物を1000℃にて非酸化性雰囲気でロータリー式の焼成炉で仮焼成し、有機物を除去しながらフェライト化を進めると同時に酸化鉄の一部を還元した。このとき仮焼成物の磁化は46Am/kgであった。 Fe 2 O 3 , Mg (OH) 2 , TiO 2 , and SrCO 3 were weighed so that the amount of Fe was 8.12 mol, Mg was 1 mol, Ti was 0.135 mol, and Sr was 0.15 mol. Water was added so that the content would be 50% by weight and mixed with a bead mill, and the mixed slurry was granulated with a spray dryer. At this time, PVA was added as a binder component so that the solid content would be 2% by weight, and a polycarboxylic acid-based dispersant was added so that the viscosity of the slurry would be 1 to 2 poises, and the resulting granulated product was 1000%. Temporary firing was performed in a non-oxidizing atmosphere at 0 ° C. in a rotary firing furnace, and ferrite was advanced while removing organic substances, and at the same time a part of iron oxide was reduced. At this time, the magnetization of the calcined product was 46 Am 2 / kg.

得られた仮焼成物をビーズミルにてスラリー粒径のD50が2μmとなるように粉砕した。このとき、バインダー成分としてPVAを固形分の0.15重量%となるように添加し、ポリカルボン酸系分散剤をスラリーの粘度が2〜3ポイズになるように添加し、得られた粉砕スラリーをスプレードライヤーにて再度造粒し、1000℃にて非酸化性雰囲気でロータリー式の焼成炉で1次焼成を行い、有機物を除去しながらフェライト化を進めると同時に酸化鉄の一部を還元した。1次焼成後の磁化は61emu/gであった。 The obtained calcined product was pulverized by a bead mill so that the slurry particle size D 50 was 2 μm. At this time, PVA is added as a binder component so that the solid content is 0.15% by weight, and a polycarboxylic acid-based dispersant is added so that the viscosity of the slurry is 2 to 3 poise, and the obtained pulverized slurry Was re-granulated with a spray dryer and subjected to primary firing in a rotary-type firing furnace at 1000 ° C. in a non-oxidizing atmosphere to promote ferritization while removing organic substances and at the same time reduce some of the iron oxide. . The magnetization after the primary firing was 61 emu / g.

1次焼成したものを80メッシュの篩を使って粗大粒子を除去した後1180℃、酸素濃度0容量%の条件で16時間焼成し焼成物を得た。得られた焼成物を解砕、分級、磁力選鉱を行い、体積平均粒径が37.1μmのキャリア芯材粒子を得た。このキャリア芯材粒子の磁化は65Am/kgであった。得られたキャリア芯材粒子の結晶構造をX線回折装置にて確認したところMgを含有するスピネル結晶構造のほかにFeとTiを含有する酸化物及びSrフェライトの結晶構造が確認された。 After the primary firing, coarse particles were removed using an 80-mesh sieve and then fired for 16 hours under the conditions of 1180 ° C. and oxygen concentration 0 volume% to obtain a fired product. The obtained fired product was crushed, classified, and subjected to magnetic separation, thereby obtaining carrier core particles having a volume average particle size of 37.1 μm. The magnetization of the carrier core particles was 65 Am 2 / kg. When the crystal structure of the obtained carrier core particles was confirmed by an X-ray diffractometer, in addition to the spinel crystal structure containing Mg, the crystal structure of oxides containing Fe and Ti and Sr ferrite was confirmed.

さらに得られたキャリア芯材粒子を表面酸化処理温度680℃、大気雰囲気の条件の元、ロータリー式の電気炉で表面酸化処理を行い表面酸化処理済みのキャリア芯材粒子を得た。この表面酸化処理を行ったキャリア芯材粒子の磁化は61Am/kgであった。 Further, the obtained carrier core particles were subjected to a surface oxidation treatment in a rotary electric furnace under the conditions of a surface oxidation treatment temperature of 680 ° C. and an atmospheric atmosphere to obtain surface oxidized carrier core particles. The magnetization of the carrier core particles subjected to this surface oxidation treatment was 61 Am 2 / kg.

Feを12.92モル、Mgを4モル、Tiを0.135モル、Srを0.05モルとした以外は実施例1と同様にして体積平均粒径が35.8μmのキャリア芯材粒子を得た。   Carrier core particles having a volume average particle diameter of 35.8 μm were obtained in the same manner as in Example 1 except that Fe was 12.92 mol, Mg was 4 mol, Ti was 0.135 mol, and Sr was 0.05 mol. Obtained.

Feを13.95モル、Mgを4モル、Tiを0.05モル、Srを0.15モルとした以外は実施例1と同様にして体積平均粒径が37.3μmのキャリア芯材粒子を得た。   Carrier core particles having a volume average particle diameter of 37.3 μm were obtained in the same manner as in Example 1 except that Fe was 13.95 mol, Mg was 4 mol, Ti was 0.05 mol, and Sr was 0.15 mol. Obtained.

Feを12.75モル、Mgを4モル、Tiを0.05モル、Srを0.05モルとした以外は実施例1と同様にして体積平均粒径が36.7μmのキャリア芯材粒子を得た。   Carrier core particles having a volume average particle diameter of 36.7 μm were obtained in the same manner as in Example 1 except that 12.75 mol of Fe, 4 mol of Mg, 0.05 mol of Ti, and 0.05 mol of Sr were used. Obtained.

Feを7.42モル、Mgを0.65モル、Tiを0.135モル、Srを0.15モルとした以外は実施例1と同様にして体積平均粒径が36.4μmのキャリア芯材粒子を得た。   Carrier core material having a volume average particle diameter of 36.4 μm as in Example 1 except that Fe is 7.42 mol, Mg is 0.65 mol, Ti is 0.135 mol, and Sr is 0.15 mol. Particles were obtained.

Feを6.22モル、Mgを0.65モル、Tiを0.135モル、Srを0.05モルとした以外は実施例1と同様にして体積平均粒径が37.0μmのキャリア芯材粒子を得た。   Carrier core material having a volume average particle diameter of 37.0 μm in the same manner as in Example 1 except that Fe is 6.22 mol, Mg is 0.65 mol, Ti is 0.135 mol, and Sr is 0.05 mol. Particles were obtained.

Feを7.25モル、Mgを0.65モル、Tiを0.05モル、Srを0.15モルとした以外は実施例1と同様にして体積平均粒径が36.9μmのキャリア芯材粒子を得た。   Carrier core material having a volume average particle diameter of 36.9 μm as in Example 1 except that Fe is 7.25 mol, Mg is 0.65 mol, Ti is 0.05 mol, and Sr is 0.15 mol. Particles were obtained.

Feを6.05モル、Mgを0.65モル、Tiを0.05モル、Srを0.05モルとした以外は実施例1と同様にして体積平均粒径が35.9μmのキャリア芯材粒子を得た。   Carrier core material having a volume average particle diameter of 35.9 μm as in Example 1 except that 6.05 mol of Fe, 0.65 mol of Mg, 0.05 mol of Ti, and 0.05 mol of Sr were used. Particles were obtained.

本焼成の温度を1250℃とした以外は実施例1と同様にして体積平均粒径が36.6μmのキャリア芯材粒子を得た。   Carrier core material particles having a volume average particle size of 36.6 μm were obtained in the same manner as in Example 1 except that the temperature of the main firing was 1250 ° C.

本焼成の温度を1150℃とした以外は実施例1と同様にして体積平均粒径が37.6μmのキャリア芯材粒子を得た。   Carrier core material particles having a volume average particle diameter of 37.6 μm were obtained in the same manner as in Example 1 except that the temperature for the main firing was 1150 ° C.

実施例1と同様の方法で平均粒径49.3μmのキャリア芯材粒子を得た後、信越シリコーン社製アクリル変性シリコーン樹脂KR−9706にライオン社製ケッチェンブラックEC600JDを添加したものを被覆樹脂として流動床コーティング装置により塗布した。このときアクリル変性シリコーン樹脂溶液はキャリア芯材に対する樹脂の固形分で2重量%となるように樹脂を秤量し、樹脂の固形分が10重量%となるようにトルエンを添加したものを使用した。さらに、ケッチェンブラックはアクリル変性シリコーン樹脂の固形分の10重量%となるように秤量した後、樹脂溶液に添加し、IKA社製ホモジナイザーULTRATURRAX T−50にて3分間分散させてからコーティングに使用した。樹脂を塗布した後、完全に揮発分をなくすために210℃設定の流動型乾燥機で3時間乾燥させて樹脂被覆キャリアを得た。   After obtaining carrier core particles having an average particle size of 49.3 μm in the same manner as in Example 1, a coating resin obtained by adding Ketjen Black EC600JD manufactured by Lion Corporation to acrylic modified silicone resin KR-9706 manufactured by Shin-Etsu Silicone Co., Ltd. As a fluid bed coater. At this time, the acryl-modified silicone resin solution was prepared by weighing the resin so that the solid content of the resin with respect to the carrier core was 2% by weight and adding toluene so that the solid content of the resin was 10% by weight. Furthermore, Ketjen Black is weighed so as to have a solid content of 10% by weight of the acrylic-modified silicone resin, then added to the resin solution, dispersed for 3 minutes with IKA homogenizer ULTRATURRAX T-50, and used for coating. did. After applying the resin, in order to completely eliminate the volatile matter, the resin-coated carrier was obtained by drying for 3 hours with a fluidized dryer set at 210 ° C.

実施例1と同様の方法で平均粒径48.5μmのキャリア芯材粒子を得た後、三菱レイヨン社製アクリル樹脂LR−269を被覆樹脂として混合攪拌機により塗布した。このとき樹脂溶液はキャリア芯材に対する樹脂の固形分で0.5重量%となるように樹脂を秤量し、樹脂の固形分が10重量%となるようにトルエンを添加したものを使用した。樹脂を塗布した後、完全に揮発分をなくすために145℃設定の熱風乾燥機で2時間乾燥させて樹脂被覆キャリアを得た。   After obtaining carrier core material particles having an average particle diameter of 48.5 μm by the same method as in Example 1, acrylic resin LR-269 manufactured by Mitsubishi Rayon Co., Ltd. was applied as a coating resin with a mixing stirrer. At this time, a resin solution was used in which the resin was weighed so that the solid content of the resin with respect to the carrier core was 0.5 wt%, and toluene was added so that the solid content of the resin would be 10 wt%. After applying the resin, in order to completely eliminate the volatile matter, the resin-coated carrier was obtained by drying with a hot air dryer set at 145 ° C. for 2 hours.

比較例Comparative example

(比較例1)
Feを16.75モル、Mgを5モル、Tiを0.15モル、Srを0.2モルとした以外は実施例1と同様にして体積平均粒径が37.0μmのキャリア芯材粒子を得た。
(Comparative Example 1)
Carrier core particles having a volume average particle size of 37.0 μm were obtained in the same manner as in Example 1 except that Fe was 16.75 mol, Mg was 5 mol, Ti was 0.15 mol, and Sr was 0.2 mol. Obtained.

(比較例2)
Feを14.35モル、Mgを5モル、Tiを0.15モル、Srを0モルとした以外は実施例1と同様にして体積平均粒径が35.1μmのキャリア芯材粒子を得た。
(Comparative Example 2)
Carrier core material particles having a volume average particle diameter of 35.1 μm were obtained in the same manner as in Example 1 except that 14.35 mol of Fe, 5 mol of Mg, 0.15 mol of Ti, and 0 mol of Sr were used. .

(比較例3)
Feを16.45モル、Mgを5モル、Tiを0モル、Srを0.2モルとした以外は実施例1と同様にして体積平均粒径が35.3μmのキャリア芯材粒子を得た。
(Comparative Example 3)
Carrier core material particles having a volume average particle diameter of 35.3 μm were obtained in the same manner as in Example 1 except that 16.45 mol of Fe, 5 mol of Mg, 0 mol of Ti, and 0.2 mol of Sr were used. .

(比較例4)
Feを14.05モル、Mgを5モル、Tiを0モル、Srを0モルとした以外は実施例1と同様にして体積平均粒径が35.9μmのキャリア芯材粒子を得た。
(Comparative Example 4)
Carrier core material particles having a volume average particle size of 35.9 μm were obtained in the same manner as in Example 1 except that Fe was 14.05 mol, Mg was 5 mol, Ti was 0 mol, and Sr was 0 mol.

(比較例5)
Feを7.15モル、Mgを0.2モル、Tiを0.15モル、Srを0.2モルとした以外は実施例1と同様にして体積平均粒径が37.4μmのキャリア芯材粒子を得た。
(Comparative Example 5)
Carrier core material having a volume average particle diameter of 37.4 μm as in Example 1 except that 7.15 mol of Fe, 0.2 mol of Mg, 0.15 mol of Ti, and 0.2 mol of Sr were used. Particles were obtained.

(比較例6)
Feを4.75モル、Mgを0.2モル、Tiを0.15モル、Srを0モルとした以外は実施例1と同様にして体積平均粒径が37.7μmのキャリア芯材粒子を得た。
(Comparative Example 6)
Carrier core particles having a volume average particle diameter of 37.7 μm were obtained in the same manner as in Example 1 except that 4.75 mol of Fe, 0.2 mol of Mg, 0.15 mol of Ti, and 0 mol of Sr were used. Obtained.

(比較例7)
Feを6.85モル、Mgを0.2モル、Tiを0モル、Srを0.2モルとした以外は実施例1と同様にして体積平均粒径が36.7μmのキャリア芯材粒子を得た。
(Comparative Example 7)
Carrier core particles having a volume average particle size of 36.7 μm were obtained in the same manner as in Example 1 except that Fe was 6.85 mol, Mg was 0.2 mol, Ti was 0 mol, and Sr was 0.2 mol. Obtained.

(比較例8)
Feを4.45モル、Mgを0.2モル、Tiを0モル、Srを0モルとした以外は実施例1と同様にして体積平均粒径が37.0μmのキャリア芯材粒子を得た。
(Comparative Example 8)
Carrier core particles having a volume average particle diameter of 37.0 μm were obtained in the same manner as in Example 1 except that 4.45 mol of Fe, 0.2 mol of Mg, 0 mol of Ti, and 0 mol of Sr were used. .

(比較例9)
本焼成の温度を1300℃とした以外は実施例1と同様にして体積平均粒径が36.5μmのキャリア芯材粒子を得た。
(Comparative Example 9)
Carrier core material particles having a volume average particle size of 36.5 μm were obtained in the same manner as in Example 1 except that the temperature for the main firing was 1300 ° C.

(比較例10)
本焼成の温度を1100℃とした以外は実施例1と同様にして体積平均粒径が36.8μmのキャリア芯材粒子を得た。
(Comparative Example 10)
Carrier core material particles having a volume average particle size of 36.8 μm were obtained in the same manner as in Example 1 except that the temperature for the main firing was 1100 ° C.

実施例1〜10及び比較例1〜10について、キャリア芯材の製造条件、体積平均粒径、BET比表面積、形状係数、電気抵抗、磁気特性、化学分析及び結晶構造を評価し、結果を表1〜表4に示した。また、実施例11及び12については電子写真用キャリアとして常温常湿下での帯電特性を評価し、結果を表5に示した。   About Examples 1-10 and Comparative Examples 1-10, the manufacturing conditions, volume average particle diameter, BET specific surface area, shape factor, electrical resistance, magnetic properties, chemical analysis and crystal structure of the carrier core material were evaluated, and the results are shown. 1 to Table 4. In Examples 11 and 12, the charging characteristics under normal temperature and humidity were evaluated as electrophotographic carriers, and the results are shown in Table 5.

Figure 0005360701
Figure 0005360701

Figure 0005360701
Figure 0005360701

Figure 0005360701
Figure 0005360701

Figure 0005360701
Figure 0005360701

Figure 0005360701
Figure 0005360701

表1〜表4の結果から明らかなように、実施例1〜10で得られた電子写真現像剤用キャリア芯材は使用に耐え得るものとなった。一方、比較例1〜4は、Feの含有量が少なく、比較例2及び比較例4は、Mgの含有量が多いため電子写真現像剤用キャリア芯材として使用できるものではなかった。特にTiを含有しない比較例3及び比較例4は本焼成後の磁化が低いだけでなくTiの添加効果が得られないため表面酸化処理後の磁化の低下が著しいものとなった。比較例5及び比較例7は、Mgの含有量が少なく、しかもSrの含有量が多いためBET比表面積が大きくなりすぎ樹脂被覆が十分できる表面性となっていないだけでなく、表面酸化処理後の残留磁化と保磁力が大きくなりすぎ電子写真現像剤用キャリア芯材として使用できるものではなかった。比較例6及び比較例8はMgの含有量が少なく、しかもSrを含有していないため本焼成後の抵抗が低くなった。さらに表面酸化処理後の印加電圧1000Vにおける抵抗も低いため電子写真現像剤用キャリア芯材として使用できるものではなかった。比較例9は磁化が高かったものの本焼成温度が高すぎるため、BET比表面積が小さくなり、キャリア芯材粒子の形状が悪く電子写真現像剤用キャリア芯材として使用できるものではなかった。比較例10は本焼成温度が低すぎるため、BET比表面積が大きくなり、キャリア芯材粒子の凹凸が大きく樹脂被覆が十分出来ない恐れがあり、電子写真現像剤用キャリア芯材として使用できるものではなかった。   As is clear from the results in Tables 1 to 4, the carrier core material for electrophotographic developers obtained in Examples 1 to 10 can withstand use. On the other hand, Comparative Examples 1 to 4 have a low Fe content, and Comparative Examples 2 and 4 have a high Mg content, and thus cannot be used as a carrier core material for an electrophotographic developer. In particular, Comparative Example 3 and Comparative Example 4 that do not contain Ti not only have a low magnetization after the main firing, but also cannot obtain the effect of addition of Ti, so the decrease in the magnetization after the surface oxidation treatment becomes significant. Comparative Example 5 and Comparative Example 7 have not only the surface property that the BET specific surface area becomes too large and the resin coating is sufficient because the content of Mg is small and the content of Sr is large. The remanent magnetization and coercive force of the film became too large to be used as a carrier core material for an electrophotographic developer. In Comparative Example 6 and Comparative Example 8, the Mg content was small and Sr was not contained, so the resistance after the main firing was low. Further, since the resistance at an applied voltage of 1000 V after the surface oxidation treatment was low, it could not be used as a carrier core material for an electrophotographic developer. In Comparative Example 9, although the magnetization was high but the main baking temperature was too high, the BET specific surface area was small, the shape of the carrier core particles was poor, and it could not be used as a carrier core for an electrophotographic developer. In Comparative Example 10, since the main baking temperature is too low, the BET specific surface area becomes large, the unevenness of the carrier core material particles is large, and there is a possibility that the resin coating cannot be sufficiently performed, so that it can be used as a carrier core material for an electrophotographic developer. There wasn't.

実施例11及び12は、キャリア芯材に樹脂を被覆したものであるが、表5に示されるように樹脂で被覆することでキャリアとして十分な帯電特性が得られることが確認された。   In Examples 11 and 12, the carrier core material was coated with a resin. As shown in Table 5, it was confirmed that sufficient charging characteristics as a carrier can be obtained by coating with a resin.

本発明に係る電子写真現像剤用キャリア芯材は、各重金属のみならず、Mnを実質的に用いることなしに、高磁化でありながら中抵抗又は高抵抗といった所望の抵抗が得られ、かつ高い帯電量と優れた帯電安定性を有し、しかも適度な凹凸を有する表面性と揃った形状とを兼ね備える。そして、上記キャリア芯材に樹脂を被覆して得られるキャリアとトナーとからなる電子写真現像剤は、長寿命化が達成され、かつ高い帯電量を有し、帯電安定性にも優れる。また、本発明の製造方法によって、上記キャリア芯材及びキャリアが工業的規模をもって安定的に製造できる。   The carrier core material for an electrophotographic developer according to the present invention can obtain a desired resistance such as medium resistance or high resistance while being highly magnetized without using not only each heavy metal but also Mn, and high. It has a charge amount and excellent charging stability, and also has a surface shape with appropriate irregularities and a uniform shape. An electrophotographic developer comprising a carrier and a toner obtained by coating the carrier core material with a resin has a long life, has a high charge amount, and is excellent in charging stability. Moreover, the carrier core material and the carrier can be stably produced on an industrial scale by the production method of the present invention.

従って、本発明は、特に高画質の要求されるフルカラー機並びに画像維持の信頼性及び耐久性の要求される高速機の分野に広く使用可能である。   Therefore, the present invention can be widely used in the field of full-color machines that particularly require high image quality and high-speed machines that require image maintenance reliability and durability.

Claims (15)

Mgを2〜8.5重量%、Tiを0.1〜1.25重量%、Srを0.37〜2.5重量%及びFeを60〜70重量%含有し、BET比表面積が0.075〜0.11m/gであることを特徴とする電子写真現像剤用キャリア芯材。 2 to 8.5% by weight of Mg, 0.1 to 1.25% by weight of Ti, 0.37 to 2.5% by weight of Sr and 60 to 70% by weight of Fe, and a BET specific surface area of 0. A carrier core material for an electrophotographic developer, wherein the carrier core material is 075 to 0.11 m 2 / g. Mgフェライトを構成するスピネル構造以外に少なくともFe及びTiを含有する酸化物の結晶構造を含有する請求項1に記載の電子写真現像剤用キャリア芯材。   The carrier core material for an electrophotographic developer according to claim 1, further comprising a crystal structure of an oxide containing at least Fe and Ti in addition to the spinel structure constituting the Mg ferrite. Mnの含有量が1重量%以下である請求項1又に記載の電子写真現像剤用キャリア芯材。 Claim 1 or electrophotographic developer carrier core material according to 2 Mn content is less than 1 wt%. 3K・1000/4π・A/mの磁場をかけたときの磁化が45〜75Am/kg、残留磁化が2〜10Am/kg及び保磁力が10〜80 3K・1000/4π・A/mである請求項1〜のいずれかに記載の電子写真現像剤用キャリア芯材。 When a magnetic field of 3K · 1000 / 4π · A / m is applied, the magnetization is 45 to 75 Am 2 / kg, the residual magnetization is 2 to 10 Am 2 / kg, and the coercive force is 10 to 80 3K · 1000 / 4π · A / m. The carrier core material for an electrophotographic developer according to any one of claims 1 to 3 . レーザー回折式粒度分布測定装置により測定される平均粒径が15〜120μmである請求項1〜のいずれかに記載の電子写真現像剤用キャリア芯材。 The carrier core material for an electrophotographic developer according to any one of claims 1 to 4 , wherein an average particle diameter measured by a laser diffraction particle size distribution analyzer is 15 to 120 µm. 形状係数SF−2(真円度)が100〜120である請求項1〜のいずれかに記載の電子写真現像剤用キャリア芯材。 The carrier core material for an electrophotographic developer according to any one of claims 1 to 5 , wherein the shape factor SF-2 (roundness) is 100 to 120. 印加電圧50Vにおける体積抵抗が1×10〜1×1010Ω・cmである請求項1〜のいずれかに記載の電子写真現像剤用キャリア芯材。 The carrier core material for an electrophotographic developer according to any one of claims 1 to 6 vol resistance of 1 × 10 6 ~1 × 10 10 Ω · cm at an applied voltage of 50 V. 表面酸化処理され、酸化処理被膜が形成されている請求項1〜のいずれかに記載の電子写真現像剤用キャリア芯材。 The carrier core material for an electrophotographic developer according to any one of claims 1 to 7 , wherein the surface is oxidized to form an oxidized film. 印加電圧50Vにおける体積抵抗が1×10〜1×1010Ω・cm、かつ印加電圧1000Vにおける体積抵抗が6×10〜1×1010Ω・cmである請求項に記載の電子写真現像剤用キャリア芯材。 Electrophotography according to claim 8 volume resistivity is 1 × 10 6 ~1 × 10 10 Ω · cm, and the volume resistivity at an applied voltage of 1000V 6 × 10 6 ~1 × 10 10 Ω · cm at an applied voltage of 50V Carrier core material for developer. 請求項1〜のいずれかに記載のキャリア芯材の表面が樹脂で被覆されている電子写真現像剤用キャリア。 The electrophotographic developer carrier surface of the carrier core material is coated with a resin according to any one of claims 1-9. 上記樹脂がアクリル樹脂、シリコーン樹脂又は変性シリコーン樹脂である請求項10に記載の電子写真現像剤用キャリア。 The carrier for an electrophotographic developer according to claim 10, wherein the resin is an acrylic resin, a silicone resin, or a modified silicone resin. Fe、TiMg及びSrの各化合物を粉砕、混合、仮焼した後、造粒し、得られた造粒物を1次焼成、本焼成し、さらに解砕、分級、表面酸化処理する電子写真現像剤用キャリア芯材の製造方法において、上記本焼成が、酸素濃度が5体積%以下で行われることを特徴とする請求項1〜9のいずれかに記載の電子写真現像剤用キャリア芯材の製造方法。 Electrons for pulverizing, mixing and calcining each compound of Fe, Ti 2 , Mg and Sr , granulating, and subjecting the resulting granulated product to primary firing, main firing, and further crushing, classification, and surface oxidation treatment 10. The carrier core for an electrophotographic developer according to any one of claims 1 to 9, wherein in the method for producing a carrier core material for a photographic developer, the main baking is performed at an oxygen concentration of 5% by volume or less. A method of manufacturing the material. 請求項12に記載の製造方法で得られたキャリア芯材の表面を樹脂で被覆することを特徴とする電子写真現像剤用キャリアの製造方法。 A method for producing a carrier for an electrophotographic developer, wherein the surface of the carrier core material obtained by the production method according to claim 12 is coated with a resin. 請求項10又は11に記載のキャリアとトナーからなる電子写真現像剤。 An electrophotographic developer comprising the carrier according to claim 10 and a toner. 請求項13に記載の製造方法により得られたキャリアとトナーからなる電子写真現像剤。 An electrophotographic developer comprising a carrier and a toner obtained by the production method according to claim 13 .
JP2008204427A 2008-08-07 2008-08-07 Carrier core material for electrophotographic developer, carrier, production method thereof, and electrophotographic developer using the carrier Active JP5360701B2 (en)