[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP5168762B2 - Method for manufacturing organic electroluminescence element - Google Patents

Method for manufacturing organic electroluminescence element Download PDF

Info

Publication number
JP5168762B2
JP5168762B2 JP2005222683A JP2005222683A JP5168762B2 JP 5168762 B2 JP5168762 B2 JP 5168762B2 JP 2005222683 A JP2005222683 A JP 2005222683A JP 2005222683 A JP2005222683 A JP 2005222683A JP 5168762 B2 JP5168762 B2 JP 5168762B2
Authority
JP
Japan
Prior art keywords
cleaning
substrate
organic
layer
electrode
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP2005222683A
Other languages
Japanese (ja)
Other versions
JP2007042315A (en
Inventor
真昭 村山
洋祐 ▲高▼島
伸彦 高嶋
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Konica Minolta Inc
Original Assignee
Konica Minolta Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Konica Minolta Inc filed Critical Konica Minolta Inc
Priority to JP2005222683A priority Critical patent/JP5168762B2/en
Publication of JP2007042315A publication Critical patent/JP2007042315A/en
Application granted granted Critical
Publication of JP5168762B2 publication Critical patent/JP5168762B2/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Description

有機エレクトロルミネッセンス素子(以下、有機EL素子とも言う)の製造方法に関する。詳しくは、有機EL素子を形成する基板の洗浄方法に関する。   The present invention relates to a method for manufacturing an organic electroluminescence element (hereinafter also referred to as an organic EL element). In detail, it is related with the washing | cleaning method of the board | substrate which forms an organic EL element.

近年、フラットディスプレイなどの表示装置や、電子写真複写機、プリンタ−などの光源に有機EL素子の使用が検討されている。   In recent years, the use of organic EL elements for light sources such as display devices such as flat displays, electrophotographic copying machines, and printers has been studied.

この有機EL素子は蛍光性有機物の非常に薄い薄膜を第一電極(以下、陽極とも言う)と第二電極(以下、陰極とも言う)ではさみ電流を流すことで発光する電流駆動型発光素子である。通常、有機物は絶縁体であるが有機層の膜厚を非常に薄くすることにより電流注入が可能となり有機EL素子として駆動する事が可能となる。そして10V以下の低電圧で駆動することが可能であり、これにより高効率な発光を得ることも可能なため将来のディスプレイとして注目を浴びている。   This organic EL element is a current-driven light-emitting element that emits light by flowing a very thin thin film of a fluorescent organic substance between a first electrode (hereinafter also referred to as an anode) and a second electrode (hereinafter also referred to as a cathode). is there. Usually, the organic substance is an insulator, but by making the film thickness of the organic layer very thin, current can be injected and it can be driven as an organic EL element. It can be driven at a low voltage of 10 V or less, and it is possible to obtain highly efficient light emission.

特に最近においては従来の励起一重項を用いる有機EL素子の効率を遙かにしのぐ励起三重項を用いるリン光発光有機EL素子がS.R.Forrest等により見い出されている(Appl.Phys.Lett.(1999),75(1),4−6)。さらにC.Adachi等が報告(J.Appl.Phys.,90,5048(2001))しているように60lm/Wにも及ぶ視感度効率を出すまでに及び、このような素子はディスプレイのみならず、照明への応用が期待される。   In particular, phosphorescent organic EL devices using excited triplets that far exceed the efficiency of conventional organic EL devices using excited singlets have been disclosed by S.C. R. Forrest et al. (Appl. Phys. Lett. (1999), 75 (1), 4-6). Furthermore, C.I. As reported by Adachi et al. (J. Appl. Phys., 90, 5048 (2001)), such an element is used not only for a display but also for illumination. Application to is expected.

有機EL素子においては、有機層は非常に薄いため基板(以下、支持体、基体、基材、支持基板とも言う)の平滑性の影響を受けやすく、電極表面に付着したゴミ(微細な塵)等の異物による電極表面の粗さに影響される。   In organic EL elements, the organic layer is very thin, so it is easily affected by the smoothness of the substrate (hereinafter also referred to as support, substrate, substrate, and support substrate), and dust (fine dust) adhering to the electrode surface It is affected by the roughness of the electrode surface due to foreign matters such as.

前記異物による電極表面の粗さは、第一電極と第二電極間の電流のリーク発生の原因となり、逆方向への電流即ちリーク電流があるとクロストークや輝度ムラ等の有機EL素子の表示品質の低下を招き、更には不良な素子の発熱等発光に寄与しないエネルギー消費が発生し、発光効率が低下する。   The roughness of the electrode surface due to the foreign matter causes the leakage of current between the first electrode and the second electrode. If there is a current in the reverse direction, that is, a leakage current, display of organic EL elements such as crosstalk and luminance unevenness. This leads to a decrease in quality, and further energy consumption that does not contribute to light emission such as heat generation of defective elements occurs, resulting in a decrease in light emission efficiency.

更に、有機層の成膜において、前記異物による電極表面の粗さに起因する突起により陰となる未蒸着部分や薄膜部が原因となり、電極ショートあるいは薄膜化部分の電流集中による絶縁破壊により電極ショートが生ずるという問題がある。   Furthermore, in the formation of the organic layer, the electrode short-circuit is caused by the non-deposited portion or the thin film portion which is shadowed by the protrusion due to the roughness of the electrode surface due to the foreign matter, and the dielectric breakdown due to the current short circuit of the electrode short or thinned portion. There is a problem that occurs.

上記問題に関し、下記のような技術が開示されている。   The following techniques are disclosed regarding the above problems.

正孔注入電極の有機化合物層に接する側の表面粗さを5.0nm以下、最大粗さを55nm以下に、また表面に付着した異物の直径を3μm以下に規定する(例えば、特許文献1参照)。   The surface roughness of the hole injection electrode on the side in contact with the organic compound layer is defined as 5.0 nm or less, the maximum roughness is defined as 55 nm or less, and the diameter of the foreign matter adhering to the surface is defined as 3 μm or less (for example, see Patent Document 1). ).

有機EL素子用支持基板において、フィルム内、フィルムと電極との界面および電極表面における1μm以上の異物、突起物、穴、空孔などの欠陥の合計数を1m2当たりの換算値で100個以下に規定する(例えば、特許文献2参照)。 In the support substrate for an organic EL element, the total number of defects such as foreign matters, projections, holes, holes and the like of 1 μm or more in the film, the interface between the film and the electrode, and the electrode surface is 100 or less in terms of conversion value per 1 m 2. (See, for example, Patent Document 2).

有機EL層と対応する第一電極上の異物が存在しない部分における該第一電極の表面から保護膜の外面までの膜厚が、前記第一電極上に存在する異物の大きさより大きく形成する(例えば、特許文献3参照)。   The film thickness from the surface of the first electrode to the outer surface of the protective film in the portion where the foreign matter on the first electrode corresponding to the organic EL layer does not exist is larger than the size of the foreign matter present on the first electrode ( For example, see Patent Document 3).

有機層の一層に温度上昇に伴い高抵抗化するリーク防止層を設けることにより、有機層中のある一カ所への電流の集中を防ぎ有機EL素子の破壊を防止する(例えば、特許文献4参照)。   By providing a leak prevention layer that increases in resistance as the temperature rises in one layer of the organic layer, current concentration to a certain place in the organic layer is prevented and destruction of the organic EL element is prevented (see, for example, Patent Document 4). ).

水の接触角が25°未満となるように洗浄処理された、透明導電性基材の透明導電膜の表面に、素子を構成する単層または複層の有機層を形成する(例えば、特許文献5参照)。   A single-layer or multi-layer organic layer constituting the element is formed on the surface of the transparent conductive film of the transparent conductive substrate that has been cleaned so that the contact angle of water is less than 25 ° (for example, Patent Documents) 5).

基板上に配線電極を形成した後、有機層成膜までのいずれかの工程でドライアイス粒子を高速流体と共に基板上に吹き付けて洗浄を行い、ドライアイス粒子をEL基板上に吹き付けることにより、基板上に付着した微細な粒子を除去する(例えば、特許文献6参照)。
特開2002−75660号公報 特開平6−124785号公報 特開2004−362912号公報 特開2004−95388号公報 特開平7−220873号公報 特開2003−31362号公報
After forming the wiring electrode on the substrate, the substrate is cleaned by spraying dry ice particles on the substrate together with the high-speed fluid in any process until the organic layer is formed, and spraying the dry ice particles on the EL substrate. Fine particles adhering to the top are removed (for example, see Patent Document 6).
JP 2002-75660 A JP-A-6-124785 JP 2004-362912 A JP 2004-95388 A JP 7-220873 A JP 2003-31362 A

有機EL素子は前述のように電極表面の粗さに影響され、前記電極表面の粗さに起因するリーク電流が発生すると有機EL素子の表示品質の低下を招く。従って、異物を除去し、前記電極表面の粗さを抑制することが必要となる。前記電極表面の異物除去の方法としては乾式洗浄及び湿式洗浄等が知られている。   As described above, the organic EL element is affected by the roughness of the electrode surface, and if a leakage current due to the roughness of the electrode surface is generated, the display quality of the organic EL element is degraded. Therefore, it is necessary to remove foreign matter and suppress the roughness of the electrode surface. Known methods for removing foreign matter on the electrode surface include dry cleaning and wet cleaning.

これに対し、特許文献1及び2では、電極の表面粗さ、表面付着異物について定義しているが、達成するための手段については言及していない。条件を満たす基板を抜き取り検査により良否を選別するが、多くの基板が不良品になる可能性もある。また、不良品の基板を再度洗浄する、あるいは排除する等生産効率を低下させる要因になる。   On the other hand, Patent Documents 1 and 2 define the surface roughness of the electrode and the surface-attached foreign matter, but do not mention means for achieving it. A board that satisfies the conditions is sampled to determine whether it is good or bad, but many boards may be defective. Moreover, it becomes a factor which reduces production efficiency, such as wash | cleaning or removing a defective board | substrate again.

特許文献3では、第一電極の表面から保護膜の外面までの膜厚を、前記第一電極上に存在する異物の大きさより大きく形成することにより、保護層のピンホールをなくすことは可能で、水分及び酸素が有機層へ侵入することを防止することは可能であるが、電極間のショートによるリークを抑制することは困難である。また、異物除去の対策に至っていない。   In Patent Document 3, it is possible to eliminate pinholes in the protective layer by forming the film thickness from the surface of the first electrode to the outer surface of the protective film larger than the size of the foreign matter existing on the first electrode. Although it is possible to prevent moisture and oxygen from entering the organic layer, it is difficult to suppress leakage due to a short circuit between the electrodes. In addition, no measures have been taken to remove foreign matter.

特許文献4では、リーク電流は抑制されるが、高抵抗化した部分は未発光となり、発光面積が小さくなる。また、リーク防止層を付設するため生産工程が増加し複雑となり生産性低下の要因となる。   In Patent Document 4, the leakage current is suppressed, but the high resistance portion does not emit light, and the light emitting area is reduced. In addition, since the leak prevention layer is provided, the production process increases and becomes complicated, resulting in a decrease in productivity.

特許文献5では、水の接触角で基板表面の汚染状態を検出する方法では、異物付着の有無を検出することは困難である。   In Patent Document 5, it is difficult to detect the presence or absence of foreign matter by the method of detecting the contamination state of the substrate surface with the contact angle of water.

特許文献6では、ドライアイス粒子を高速流体と共に基板上に吹き付けて洗浄を行うため、ドライアイス粒子の衝突による電極剥離等基板電極へのダメージが大きく、また洗浄設備が複雑、高価となり洗浄コストの増加を招く。   In Patent Document 6, since cleaning is performed by spraying dry ice particles on a substrate together with a high-speed fluid, damage to the substrate electrode such as electrode peeling due to collision of dry ice particles is large, and cleaning equipment is complicated and expensive, resulting in a low cleaning cost. Incurs an increase.

本発明は、上記状況に鑑みなされたもので、有機EL素子における電極形成後の基板洗浄工程において、乾式洗浄と湿式洗浄を組み合わせ、乾式洗浄後に湿式洗浄を実施することで異物除去を効果的に行い基板電極表面の洗浄性能の向上を図ることにより、電極間のショートによるリーク電流を抑制することができる有機EL素子の製造方法を提供することを目的とする。   The present invention has been made in view of the above situation, and in the substrate cleaning step after electrode formation in the organic EL element, the dry cleaning and the wet cleaning are combined, and the foreign cleaning is effectively performed by performing the wet cleaning after the dry cleaning. An object of the present invention is to provide a method of manufacturing an organic EL element capable of suppressing leakage current due to a short circuit between electrodes by improving the cleaning performance of the substrate electrode surface.

また、ロールツーロール方式での有機EL素子製造に適した洗浄工程を有する有機EL素子の製造方法を提供することを目的とする。   Moreover, it aims at providing the manufacturing method of the organic EL element which has the washing | cleaning process suitable for organic EL element manufacture by a roll-to-roll system.

上記目的は、下記の構成により達成される。
(請求項1)
基板上に少なくとも第一電極と有機物質からなる一層以上の発光層と第二電極を成膜してなる有機エレクトロルミネッセンス素子の製造方法において、
前記基板上に第一電極が成膜してなる基板の前記第一電極を洗浄する乾式洗浄と湿式洗浄からなる洗浄工程を具備するとともに、前記洗浄工程は前記乾式洗浄工程、前記湿式洗浄工程及び前記乾式洗浄工程をこの順に連続して行い、前記湿式洗浄に使用する溶媒が超純水であることを特徴とする有機エレクトロルミネッセンス素子の製造方法。
(請求項2)
前記乾式洗浄で基板電極表面における水の接触角を45°以下とし、前記湿式洗浄を行うことを特徴とする請求項1に記載の有機エレクトロルミネッセンス素子の製造方法。
(請求項3)
前記乾式洗浄の方法は、紫外線オゾン洗浄、プラズマ洗浄の少なくとも何れか1つであることを特徴とする請求項1または2に記載の有機エレクトロルミネッセンス素子の製造方法。
(請求項4)
前記湿式洗浄の方法は、洗浄浴槽浸漬、超音波洗浄浴槽浸漬、流水式洗浄浴槽浸漬、流水式超音波洗浄浴槽浸漬、流水式シャワー及び流水式超音波シャワー方式の少なくとも何れか1つであることを特徴とする請求項1乃至3の何れか1項に記載の有機エレクトロルミネッセンス素子の製造方法
請求項
前記洗浄工程は、連続シート状基板をロールツーロール方式でウェブ搬送しながら前記連続シート状基板を洗浄することを特徴とする請求項1乃至の何れか1項に記載の有機エレクトロルミネッセンス素子の製造方法。
(請求項
前記洗浄工程と同一のウェブ搬送ライン上に有機層成膜工程とを具備するとともに、前記洗浄工程で洗浄した後、同一のウェブ搬送ラインで連続シート状基板電極上に少なくとも1層以上の有機層を成膜することを特徴とする請求項に記載の有機エレクトロルミネッセンス素子の製造方法。
The above object is achieved by the following configuration.
(Claim 1)
In the method for producing an organic electroluminescent element, wherein at least a first electrode and a light emitting layer composed of an organic substance and a second electrode are formed on a substrate.
A cleaning process comprising a dry cleaning process and a wet cleaning process for cleaning the first electrode of a substrate formed by forming a first electrode on the substrate; and the cleaning process includes the dry cleaning process, the wet cleaning process, and the dry cleaning process the have rows successively in this order, the method of manufacturing the organic electroluminescent device solvent used for the wet cleaning, characterized in that ultrapure water.
(Claim 2)
The method for producing an organic electroluminescent element according to claim 1, wherein the wet cleaning is performed by setting the contact angle of water on the surface of the substrate electrode to 45 ° or less in the dry cleaning.
(Claim 3)
3. The method of manufacturing an organic electroluminescence element according to claim 1, wherein the dry cleaning method is at least one of ultraviolet ozone cleaning and plasma cleaning.
(Claim 4)
The wet cleaning method is at least one of cleaning bath immersion, ultrasonic cleaning bath immersion, flowing water cleaning bath immersion, flowing water ultrasonic cleaning bath immersion, flowing water shower, and flowing water ultrasonic shower method. The manufacturing method of the organic electroluminescent element of any one of Claims 1 thru | or 3 characterized by these .
( Claim 5 )
The washing step, the organic electroluminescent device according to any one of claims 1 to 4, characterized in that washing the continuous sheet-like substrate while web transport the continuous sheet-like substrate in a roll-to-roll method Production method.
(Claim 6 )
An organic layer film forming step on the same web conveyance line as the washing step, and after washing in the washing step, at least one organic layer on the continuous sheet-like substrate electrode in the same web conveyance line The method of manufacturing an organic electroluminescence element according to claim 5 , wherein the film is formed.

上記構成により、有機EL素子の製造における基板電極表面の洗浄において、湿式洗浄前に乾式洗浄を行うことで、基板電極表面の有機汚染を除去し、水の接触角を45°以下とすることにより、次の湿式洗浄で有機汚染に埋没していた異物の粒子の除去を効率よく行うことができる。また、安定した異物除去性能が確保でき洗浄工程の短縮化を図ることが可能となる。   With the above configuration, in the cleaning of the substrate electrode surface in the manufacture of the organic EL element, by performing dry cleaning before wet cleaning, organic contamination of the substrate electrode surface is removed, and the contact angle of water is set to 45 ° or less. The foreign particles embedded in the organic contamination can be efficiently removed by the next wet cleaning. In addition, stable foreign substance removal performance can be ensured and the cleaning process can be shortened.

また、前述のように乾式洗浄で有機汚染を除去し、水の接触角を45°以下とすることにより、湿式洗浄に使用する溶媒が水系溶媒のみで効率よく異物除去が可能になり、かつ連続シート状基板をウェブ搬送させ有機EL素子を製造するロールツーロール方式における連続洗浄工程ラインの短縮化が可能になる。   In addition, as described above, organic contamination is removed by dry cleaning, and the contact angle of water is set to 45 ° or less, so that the solvent used for wet cleaning can be efficiently removed only with an aqueous solvent, and continuously. It is possible to shorten the continuous cleaning process line in the roll-to-roll method in which the sheet-like substrate is conveyed on the web to manufacture the organic EL element.

上記により、駆動時にリーク電流の発生が無い安定した品質で、かつ生産効率の良い有機EL素子の製造が可能となり、有機EL素子の発光効率及び寿命の向上を図ることができる。   According to the above, it becomes possible to manufacture an organic EL element having a stable quality with no leakage current during driving and high production efficiency, and it is possible to improve the light emission efficiency and life of the organic EL element.

以下に本発明に係る有機ELパネルの構成層と一般構成及び有機ELパネルの製造方法の形態について順次説明する。   The constituent layers and general configuration of the organic EL panel according to the present invention and the mode of the method for manufacturing the organic EL panel will be sequentially described below.

なお、図5に、本発明に係る有機ELパネルの一例として、パッシブマトリックス方式のフルカラー有機EL素子の層構成(図5(a))、及び図5(a)の矢示A方向から見た正面図(図5(b))を示したが、本発明に係る有機ELパネルはこれに限定されるものではない。   In addition, in FIG. 5, as an example of the organic EL panel according to the present invention, the layer configuration of the passive matrix type full-color organic EL element (FIG. 5A) and the direction of arrow A in FIG. Although the front view (FIG. 5B) is shown, the organic EL panel according to the present invention is not limited to this.

フルカラー有機ELパネル900は、支持体1上に、陽極902、正孔輸送層903、発光層904、電子輸送層905、陰極906をそれぞれパターン様に形成し、支持体1、バリアフィルム907及び接着層908でこれらの各層を封入した構成となっている。   In the full color organic EL panel 900, an anode 902, a hole transport layer 903, a light emitting layer 904, an electron transport layer 905, and a cathode 906 are formed in a pattern on the support 1, respectively, and the support 1, the barrier film 907, and the adhesion are formed. A layer 908 encloses each of these layers.

<有機EL素子の構成層と一般構成>
本発明に係る有機ELパネルの層構成の好ましい具体例を下記に示すが、以下の形態に限定されるものではない。
(1)陽極/発光層ユニット/電子輸送層/陰極
(2)陽極/正孔輸送層/発光層ユニット/電子輸送層/陰極
(3)陽極/正孔輸送層/発光層ユニット/正孔阻止層/電子輸送層/陰極
(4)陽極/正孔輸送層/発光層ユニット/正孔阻止層/電子輸送層/陰極バッファ−層(以下、電子注入層とも言う)/陰極
(5)陽極/陽極バッファ−層(以下、正孔注入層とも言う)/正孔輸送層/発光層ユニット/正孔阻止層/電子輸送層/陰極バッファ−層/陰極
ここで、発光層ユニットには、発光極大波長が各々430nm〜480nm、510nm〜550nm、600nm〜640nmの範囲にある少なくとも何れか1層の発光層を有する。
<Structure layers and general structure of organic EL elements>
Although the preferable specific example of the laminated constitution of the organic electroluminescent panel which concerns on this invention is shown below, it is not limited to the following forms.
(1) Anode / light emitting layer unit / electron transport layer / cathode (2) Anode / hole transport layer / light emitting layer unit / electron transport layer / cathode (3) Anode / hole transport layer / light emitting layer unit / hole blocking Layer / electron transport layer / cathode (4) anode / hole transport layer / light emitting layer unit / hole blocking layer / electron transport layer / cathode buffer layer (hereinafter also referred to as electron injection layer) / cathode (5) anode / Anode buffer layer (hereinafter also referred to as hole injection layer) / hole transport layer / light emitting layer unit / hole blocking layer / electron transport layer / cathode buffer layer / cathode Here, the light emitting layer unit has a light emission maximum. At least one of the light emitting layers having wavelengths of 430 nm to 480 nm, 510 nm to 550 nm, and 600 nm to 640 nm, respectively.

発光層ユニットは、白色バックライト(以下、白色BLとも言う)用途の場合では各色発光層の積層、もしくは各色発光材料の混合材料を使用することで、フルカラ−の場合は各色をパタ−ニングすることで達成される。   In the case of a white backlight (hereinafter also referred to as white BL), the light emitting layer unit patterns each color in the case of a full color by using a laminate of each color light emitting layer or a mixed material of each color light emitting material. Is achieved.

《陽極》
有機EL素子における陽極としては、仕事関数の大きい(4eV以上)金属、合金、電気伝導性化合物及びこれらの混合物を電極物質とするものが好ましく用いられる。このような電極物質の具体例としてはAu等の金属、CuI、インジウムチンオキシド(ITO)、SnO2、ZnO等の導電性透明材料が挙げられる。また、IDIXO(In23−ZnO)等非晶質で透明導電膜を作製可能な材料を用いてもよい。陽極はこれらの電極物質を蒸着やスパッタリング等の方法により、薄膜を形成させ、フォトリソグラフィ−法で所望の形状のパタ−ンを形成してもよく、あるいはパタ−ン精度をあまり必要としない場合は(100μm以上程度)、上記電極物質の蒸着やスパッタリング時に所望の形状のマスクを介してパタ−ンを形成してもよい。あるいは、有機導電性化合物のように塗布可能な物質を用いる場合には、印刷方式、コ−ティング方式など湿式製膜法を用いることもできる。この陽極より発光を取り出す場合には、透過率を10%より大きくすることが望ましく、また陽極としてのシ−ト抵抗は数百Ω/□以下が好ましい。更に膜厚は材料にもよるが、通常10nm〜1000nm、好ましくは10nm〜200nmの範囲で選ばれる。
"anode"
As the anode in the organic EL element, an electrode material made of a metal, an alloy, an electrically conductive compound, or a mixture thereof having a high work function (4 eV or more) is preferably used. Specific examples of such electrode materials include metals such as Au, and conductive transparent materials such as CuI, indium tin oxide (ITO), SnO 2 and ZnO. Alternatively, an amorphous material such as IDIXO (In 2 O 3 —ZnO) capable of forming a transparent conductive film may be used. For the anode, these electrode materials may be formed into a thin film by a method such as vapor deposition or sputtering, and a pattern having a desired shape may be formed by photolithography, or the pattern accuracy is not so required. (About 100 μm or more), the pattern may be formed through a mask having a desired shape when the electrode material is deposited or sputtered. Or when using the substance which can be apply | coated like an organic electroconductivity compound, wet film forming methods, such as a printing system and a coating system, can also be used. When light emission is extracted from the anode, it is desirable that the transmittance is greater than 10%, and the sheet resistance as the anode is preferably several hundred Ω / □ or less. Further, although the film thickness depends on the material, it is usually selected in the range of 10 nm to 1000 nm, preferably 10 nm to 200 nm.

《陰極》
一方、陰極としては、仕事関数の小さい(4eV以下)金属(電子注入性金属と称する)、合金、電気伝導性化合物及びこれらの混合物を電極物質とするものが用いられる。このような電極物質の具体例としては、ナトリウム、ナトリウム−カリウム合金、マグネシウム、リチウム、マグネシウム/銅混合物、マグネシウム/銀混合物、マグネシウム/アルミニウム混合物、マグネシウム/インジウム混合物、アルミニウム/酸化アルミニウム(Al23)混合物、インジウム、リチウム/アルミニウム混合物、希土類金属等が挙げられる。これらの中で、電子注入性及び酸化等に対する耐久性の点から、電子注入性金属とこれより仕事関数の値が大きく安定な金属である第二金属との混合物、例えば、マグネシウム/銀混合物、マグネシウム/アルミニウム混合物、マグネシウム/インジウム混合物、アルミニウム/酸化アルミニウム(Al23)混合物、リチウム/アルミニウム混合物、アルミニウム等が好適である。陰極はこれらの電極物質を蒸着やスパッタリング等の方法により薄膜を形成させることにより、作製することができる。また、陰極としてのシ−ト抵抗は数百Ω/□以下が好ましく、膜厚は通常10nm〜5μm、好ましくは50nm〜200nmの範囲で選ばれる。なお、発光した光を透過させるため、有機EL素子の陽極または陰極のいずれか一方が、透明または半透明であれば発光輝度が向上し好都合である。
"cathode"
On the other hand, as the cathode, a material having a low work function (4 eV or less) metal (referred to as an electron injecting metal), an alloy, an electrically conductive compound, and a mixture thereof as an electrode material is used. Specific examples of such electrode materials include sodium, sodium-potassium alloy, magnesium, lithium, magnesium / copper mixture, magnesium / silver mixture, magnesium / aluminum mixture, magnesium / indium mixture, aluminum / aluminum oxide (Al 2 O 3 ) Mixtures, indium, lithium / aluminum mixtures, rare earth metals and the like. Among these, from the point of durability against electron injection and oxidation, etc., a mixture of an electron injecting metal and a second metal which is a stable metal having a larger work function than this, for example, a magnesium / silver mixture, Suitable are a magnesium / aluminum mixture, a magnesium / indium mixture, an aluminum / aluminum oxide (Al 2 O 3 ) mixture, a lithium / aluminum mixture, aluminum and the like. The cathode can be produced by forming a thin film of these electrode materials by a method such as vapor deposition or sputtering. The sheet resistance as the cathode is preferably several hundred Ω / □ or less, and the film thickness is usually selected in the range of 10 nm to 5 μm, preferably 50 nm to 200 nm. In order to transmit the emitted light, if either one of the anode or the cathode of the organic EL element is transparent or translucent, the emission luminance is advantageously improved.

また、陰極に上記金属を1nm〜20nmの膜厚で作製した後に、陽極の説明で挙げた導電性透明材料をその上に作製することで、透明または半透明の陰極を作製することができ、これを応用することで陽極と陰極の両方が透過性を有する素子を作製することができる。   Moreover, after producing the said metal by the film thickness of 1 nm-20 nm to a cathode, the transparent or semi-transparent cathode can be produced by producing the electroconductive transparent material quoted by description of the anode on it, By applying this, an element in which both the anode and the cathode are transmissive can be manufactured.

次に、本発明の有機EL素子の構成層として用いられる、注入層、阻止層、電子輸送層等について説明する。   Next, an injection layer, a blocking layer, an electron transport layer, and the like used as a constituent layer of the organic EL element of the present invention will be described.

《注入層:電子注入層、正孔注入層》
注入層は必要に応じて設け、電子注入層と正孔注入層があり、上記の如く陽極と発光層または正孔輸送層の間、及び陰極と発光層または電子輸送層との間に存在させてもよい。
<< Injection layer: electron injection layer, hole injection layer >>
The injection layer is provided as necessary, and there are an electron injection layer and a hole injection layer, and as described above, it exists between the anode and the light emitting layer or the hole transport layer and between the cathode and the light emitting layer or the electron transport layer. May be.

注入層とは、駆動電圧低下や発光輝度向上のために電極と有機層間に設けられる層のことで、「有機EL素子とその工業化最前線(1998年11月30日エヌ・ティ−・エス社発行)」の第2編第2章「電極材料」(123〜166頁)に詳細に記載されており、正孔注入層(陽極バッファ−層)と電子注入層(陰極バッファ−層)とがある。   An injection layer is a layer provided between an electrode and an organic layer in order to lower drive voltage and improve light emission luminance. “Organic EL element and its forefront of industrialization (November 30, 1998, NTS Corporation) Issue) ”, Chapter 2,“ Electrode Materials ”(pages 123 to 166) in detail, and a hole injection layer (anode buffer layer) and an electron injection layer (cathode buffer layer) are is there.

陽極バッファ−層(正孔注入層)は、特開平9−45479号公報、同9−260062号公報、同8−288069号公報等にもその詳細が記載されており、具体例として、銅フタロシアニンに代表されるフタロシアニンバッファ−層、酸化バナジウムに代表される酸化物バッファ−層、アモルファスカ−ボンバッファ−層、ポリアニリン(エメラルディン)やポリチオフェン等の導電性高分子を用いた高分子バッファ−層等が挙げられる。   The details of the anode buffer layer (hole injection layer) are described in JP-A-9-45479, JP-A-9-260062, JP-A-8-288069, and the like. Specific examples thereof include copper phthalocyanine. Phthalocyanine buffer layer typified by, oxide buffer layer typified by vanadium oxide, amorphous carbon buffer layer, polymer buffer layer using a conductive polymer such as polyaniline (emeraldine) or polythiophene Etc.

陰極バッファ−層(電子注入層)は、特開平6−325871号公報、同9−17574号公報、同10−74586号公報等にもその詳細が記載されており、具体的にはストロンチウムやアルミニウム等に代表される金属バッファ−層、フッ化リチウムに代表されるアルカリ金属化合物バッファ−層、フッ化マグネシウムに代表されるアルカリ土類金属化合物バッファ−層、酸化アルミニウムに代表される酸化物バッファ−層等が挙げられる。上記バッファ−層(注入層)はごく薄い膜であることが望ましく、素材にもよるがその膜厚は0.1nm〜5μmの範囲が好ましい。   The details of the cathode buffer layer (electron injection layer) are described in JP-A-6-325871, JP-A-9-17574, JP-A-10-74586, and the like. Specifically, strontium or aluminum Metal buffer layer represented by lithium fluoride, alkali metal compound buffer layer represented by lithium fluoride, alkaline earth metal compound buffer layer represented by magnesium fluoride, oxide buffer represented by aluminum oxide Layer and the like. The buffer layer (injection layer) is preferably a very thin film, and the film thickness is preferably in the range of 0.1 nm to 5 μm, although it depends on the material.

《阻止層:正孔阻止層、電子阻止層》
阻止層は、上記の如く、有機化合物薄膜の基本構成層の他に必要に応じて設けられるものである。例えば、特開平11−204258号公報、同11−204359号公報、及び「有機EL素子とその工業化最前線(1998年11月30日エヌ・ティ−・エス社発行)」の237頁等に記載されている正孔阻止(ホ−ルブロック)層がある。
<Blocking layer: hole blocking layer, electron blocking layer>
As described above, the blocking layer is provided as necessary in addition to the basic constituent layer of the organic compound thin film. For example, as described in JP-A Nos. 11-204258 and 11-204359, and “Organic EL elements and their forefront of industrialization” (issued by NTT Corporation on November 30, 1998). There is a hole blocking layer that is applied.

正孔阻止層とは広い意味では電子輸送層の機能を有し、電子を輸送する機能を有しつつ正孔を輸送する能力が著しく小さい正孔阻止材料からなり、電子を輸送しつつ正孔を阻止することで電子と正孔の再結合確率を向上させることができる。また、後述する電子輸送層の構成を必要に応じて、正孔阻止層として用いることができる。   The hole blocking layer has a function of an electron transport layer in a broad sense, and is made of a hole blocking material that has a function of transporting electrons and has a remarkably small ability to transport holes. The probability of recombination of electrons and holes can be improved by blocking. Moreover, the structure of the electron carrying layer mentioned later can be used as a hole-blocking layer as needed.

一般に有機EL素子の正孔阻止層は、発光層に隣接して設けられていることが好ましい。   In general, the hole blocking layer of the organic EL device is preferably provided adjacent to the light emitting layer.

また、複数の発光色の異なる発光層を有する場合にはその発光極大波長が最も短波にある発光層が、全発光層中、最も陽極に近いことが好ましいが、このような場合、前記最短波発光層と、該最短波発光層の次に陽極に近い発光層との間に正孔阻止層を追加して設けることが好ましい。更に、該位置に設けられる正孔阻止層に含有される化合物の50質量%以上が、前記最短波発光層のホスト化合物に対し、そのイオン化ポテンシャルが0.3eV以上大きいことが好ましい。   In the case of having a plurality of light emitting layers having different emission colors, it is preferable that the light emitting layer whose emission maximum wavelength is the shortest wave is closest to the anode among all the light emitting layers. It is preferable to additionally provide a hole blocking layer between the light emitting layer and the light emitting layer next to the anode next to the shortest wave light emitting layer. Furthermore, it is preferable that 50% by mass or more of the compound contained in the hole blocking layer provided at the position has an ionization potential of 0.3 eV or more higher than the host compound of the shortest wave emitting layer.

イオン化ポテンシャルは、化合物のHOMO(最高被占分子軌道)レベルにある電子を真空準位に放出するのに必要なエネルギ−で定義され、例えば下記に示すような方法により求めることができる。
(1)米国Gaussian社製の分子軌道計算用ソフトウェアであるGaussian98(Gaussian98、Revision A.11.4,M.J.Frisch,et al,Gaussian,Inc.,Pittsburgh PA,2002.)を用い、キ−ワ−ドとしてB3LYP/6−31G*を用いて構造最適化を行うことにより算出した値(eV単位換算値)の小数点第2位を四捨五入した値としてイオン化ポテンシャルを求めることができる。この計算値が有効な背景には、この手法で求めた計算値と実験値の相関が高いためである。
(2)イオン化ポテンシャルは光電子分光法で直接測定する方法により求めることもできる。光電子分光法による測定方法としては、例えば、低エネルギ−電子分光装置「Model AC−1」(理研計器社製)を用いる方法が挙げられる。また、紫外光電子分光法による測定方法を用いることも可能である。
The ionization potential is defined by the energy required to emit an electron at the HOMO (highest occupied molecular orbital) level of the compound to the vacuum level, and can be obtained by the following method, for example.
(1) Gaussian 98 (Gaussian 98, Revision A.11.4, MJ Frisch, et al, Gaussian, Inc., Pittsburgh PA, 2002.), which is molecular orbital calculation software manufactured by Gaussian, USA -The ionization potential can be obtained as a value obtained by rounding off the second decimal place of a value (eV unit converted value) calculated by performing structural optimization using B3LYP / 6-31G * as a word. This calculation value is effective because the correlation between the calculation value obtained by this method and the experimental value is high.
(2) The ionization potential can also be obtained by a method of directly measuring by photoelectron spectroscopy. Examples of the measurement method using photoelectron spectroscopy include a method using a low energy electron spectrometer “Model AC-1” (manufactured by Riken Keiki Co., Ltd.). It is also possible to use a measurement method by ultraviolet photoelectron spectroscopy.

一方、電子阻止層とは広い意味では正孔輸送層の機能を有し、正孔を輸送する機能を有しつつ電子を輸送する能力が著しく小さい材料からなり、正孔を輸送しつつ電子を阻止することで電子と正孔の再結合確率を向上させることができる。また、後述する正孔輸送層の構成を必要に応じて電子阻止層として用いることができる。本発明に係る正孔阻止層、電子輸送層の膜厚としては好ましくは3nm〜100nmで有り、更に好ましくは5nm〜30nmである。   On the other hand, the electron blocking layer has a function of a hole transport layer in a broad sense, and is made of a material having a function of transporting holes while having a very small ability to transport electrons, and transporting electrons while transporting holes. By blocking, the recombination probability of electrons and holes can be improved. Moreover, the structure of the positive hole transport layer mentioned later can be used as an electron blocking layer as needed. The film thickness of the hole blocking layer and the electron transport layer according to the present invention is preferably 3 nm to 100 nm, and more preferably 5 nm to 30 nm.

《発光層》
本発明に係る発光層は、電極または電子輸送層、正孔輸送層から注入されてくる電子及び正孔が再結合して発光する層であり、発光する部分は発光層の層内であっても発光層と隣接層との界面であってもよい。
<Light emitting layer>
The light emitting layer according to the present invention is a layer that emits light by recombination of electrons and holes injected from the electrode, the electron transport layer, or the hole transport layer, and the light emitting portion is in the layer of the light emitting layer. May be the interface between the light emitting layer and the adjacent layer.

(ホスト化合物)
本発明の有機EL素子の発光層には、以下に示すホスト化合物とリン光性化合物(リン光発光性化合物ともいう)が含有されることが好ましい。
(Host compound)
The light emitting layer of the organic EL device of the present invention preferably contains the following host compound and phosphorescent compound (also referred to as phosphorescent compound).

ここで、本発明においてホスト化合物とは、発光層に含有される化合物の内で、その層中での質量比が20%以上であり、かつ室温(25℃)においてリン光発光のリン光量子収率が、0.1未満の化合物と定義される。好ましくはリン光量子収率が0.01未満である。   Here, in the present invention, the host compound is a compound contained in the light emitting layer, the mass ratio in the layer is 20% or more, and phosphorescence quantum yield of phosphorescence emission at room temperature (25 ° C.). A rate is defined as a compound of less than 0.1. The phosphorescence quantum yield is preferably less than 0.01.

ホスト化合物としては、公知のホスト化合物を単独で用いてもよく、または複数種併用して用いてもよい。ホスト化合物を複数種用いることで、電荷の移動を調整することが可能であり、有機EL素子を高効率化することができる。また、リン光性化合物を複数種用いることで、異なる発光を混ぜることが可能となり、これにより任意の発光色を得ることができる。リン光性化合物の種類、ド−プ量を調整することで白色発光が可能であり、照明、バックライトへの応用もできる。   As the host compound, known host compounds may be used alone or in combination of two or more. By using a plurality of types of host compounds, it is possible to adjust the movement of charges, and the organic EL element can be made highly efficient. In addition, by using a plurality of phosphorescent compounds, it is possible to mix different light emission, thereby obtaining an arbitrary emission color. White light emission is possible by adjusting the kind of phosphorescent compound and the amount of doping, and can also be applied to illumination and backlight.

これらの公知のホスト化合物としては、正孔輸送能、電子輸送能を有しつつ、且つ発光の長波長化を防ぎ、なお且つ高Tg(ガラス転移温度)である化合物が好ましい。   As these known host compounds, compounds having a hole transporting ability and an electron transporting ability, preventing the emission of longer wavelengths, and having a high Tg (glass transition temperature) are preferable.

公知のホスト化合物の具体例としては、以下の文献に記載されている化合物が挙げられる。   Specific examples of known host compounds include compounds described in the following documents.

特開2001−257076号公報、同2002−308855号公報、同2001−313179号公報、同2002−319491号公報、同2001−357977号公報、同2002−334786号公報、同2002−8860号公報、同2002−334787号公報、同2002−15871号公報、同2002−334788号公報、同2002−43056号公報、同2002−334789号公報、同2002−75645号公報、同2002−338579号公報、同2002−105445号公報、同2002−343568号公報、同2002−141173号公報、同2002−352957号公報、同2002−203683号公報、同2002−363227号公報、同2002−231453号公報、同2003−3165号公報、同2002−234888号公報、同2003−27048号公報、同2002−255934号公報、同2002−260861号公報、同2002−280183号公報、同2002−299060号公報、同2002−302516号公報、同2002−305083号公報、同2002−305084号公報、同2002−308837号公報等。   JP-A-2001-257076, 2002-308855, 2001-313179, 2002-319491, 2001-357777, 2002-334786, 2002-8860, 2002-334787, 2002-15871, 2002-334788, 2002-43056, 2002-334789, 2002-75645, 2002-338579, 2002-105445 gazette, 2002-343568 gazette, 2002-141173 gazette, 2002-352957 gazette, 2002-203683 gazette, 2002-363227 gazette, 2002-231453 gazette, No. 003-3165, No. 2002-234888, No. 2003-27048, No. 2002-255934, No. 2002-286061, No. 2002-280183, No. 2002-299060, No. 2002. -302516, 2002-305083, 2002-305084, 2002-308837, and the like.

本発明においては、複数の発光層を有するが、これら各層のホスト化合物の50質量%以上が同一の化合物であることが、有機層全体に渡って均質な膜性状を得やすいことから好ましく、更には該化合物の燐光発光エネルギ−が2.9eV以上であることが、ド−パントからのエネルギ−移動を効率的に抑制し、高輝度を得る上で有利となることから好ましい。   In the present invention, it has a plurality of light emitting layers, but it is preferable that 50% by mass or more of the host compound in each layer is the same compound because it is easy to obtain a uniform film property over the entire organic layer. It is preferable that the phosphorescence emission energy of the compound is 2.9 eV or more because it is advantageous for efficiently suppressing energy transfer from the dopant and obtaining high luminance.

(リン光性化合物(リン光発光性化合物))
発光層に使用される材料(以下、発光材料という)としては、上記のホスト化合物を含有すると同時に、リン光性化合物を含有することが好ましい。これにより、より発光効率の高い有機EL素子とすることができる。
(Phosphorescent compound (phosphorescent compound))
The material used for the light emitting layer (hereinafter referred to as the light emitting material) preferably contains a phosphorescent compound at the same time as the host compound. Thereby, it can be set as an organic EL element with higher luminous efficiency.

本発明に係るリン光性化合物は、励起三重項からの発光が観測される化合物であり、室温(25℃)にてリン光発光する化合物であり、リン光量子収率が、25℃において0.01以上の化合物である。リン光量子収率は好ましくは0.1以上である。上記リン光量子収率は、第4版実験化学講座7の分光IIの398頁(1992年版、丸善)に記載の方法により測定できる。溶液中でのリン光量子収率は種々の溶媒を用いて測定できるが、本発明に用いられるリン光性化合物は、任意の溶媒のいずれかにおいて上記リン光量子収率が達成されればよい。   The phosphorescent compound according to the present invention is a compound in which light emission from an excited triplet is observed, is a compound that emits phosphorescence at room temperature (25 ° C.), and has a phosphorescence quantum yield of 0.2 at 25 ° C. 01 or more compounds. The phosphorescence quantum yield is preferably 0.1 or more. The phosphorescence quantum yield can be measured by the method described in Spectroscopic II, page 398 (1992 edition, Maruzen) of Experimental Chemistry Course 4 of the 4th edition. Although the phosphorescence quantum yield in a solution can be measured using various solvents, the phosphorescence quantum yield used in the present invention only needs to achieve the above phosphorescence quantum yield in any solvent.

リン光性化合物の発光は原理としては2種挙げられ、一つはキャリアが輸送されるホスト化合物上でキャリアの再結合が起こってホスト化合物の励起状態が生成し、このエネルギ−をリン光性化合物に移動させることでリン光性化合物からの発光を得るというエネルギ−移動型、もう一つはリン光性化合物がキャリアトラップとなり、リン光性化合物上でキャリアの再結合が起こりリン光性化合物からの発光が得られるというキャリアトラップ型であるが、いずれの場合においても、リン光性化合物の励起状態のエネルギ−はホスト化合物の励起状態のエネルギ−よりも低いことが条件である。   There are two types of light emission of the phosphorescent compound in principle. One is the recombination of the carrier on the host compound to which the carrier is transported and the excited state of the host compound is generated, and this energy is phosphorescent. An energy transfer type in which light emission from the phosphorescent compound is obtained by transferring to the compound, and another is that the phosphorescent compound becomes a carrier trap, and carrier recombination occurs on the phosphorescent compound and the phosphorescent compound In any case, the excited state energy of the phosphorescent compound is lower than the excited state energy of the host compound.

リン光性化合物は、有機EL素子の発光層に使用される公知のものの中から適宜選択して用いることができる。   The phosphorescent compound can be appropriately selected from known compounds used for the light emitting layer of the organic EL device.

本発明で用いられるリン光性化合物としては、好ましくは元素の周期表で8族〜10族の金属を含有する錯体系化合物であり、更に好ましくはイリジウム化合物、オスミウム化合物、または白金化合物(白金錯体系化合物)、希土類錯体であり、中でも最も好ましいのはイリジウム化合物である。   The phosphorescent compound used in the present invention is preferably a complex compound containing a group 8-10 metal in the periodic table of elements, more preferably an iridium compound, an osmium compound, or a platinum compound (platinum complex). System compounds), rare earth complexes, and most preferred are iridium compounds.

以下に、リン光性化合物の具体例を示すが、本発明はこれらに限定されない。これらの化合物は、例えば、Inorg.Chem.40巻、1704〜1711に記載の方法等により合成できる。   Although the specific example of a phosphorescent compound is shown below, this invention is not limited to these. These compounds are described, for example, in Inorg. Chem. 40, 1704-1711, and the like.

Figure 0005168762
Figure 0005168762

Figure 0005168762
Figure 0005168762

Figure 0005168762
Figure 0005168762

Figure 0005168762
Figure 0005168762

Figure 0005168762
Figure 0005168762

Figure 0005168762
Figure 0005168762

Figure 0005168762
Figure 0005168762

本発明においては、リン光性化合物のリン光発光極大波長としては特に制限されるものではなく、原理的には中心金属、配位子、配位子の置換基等を選択することで得られる発光波長を変化させることができる。   In the present invention, the phosphorescence emission maximum wavelength of the phosphorescent compound is not particularly limited, and can be obtained in principle by selecting a central metal, a ligand, a ligand substituent, and the like. The emission wavelength can be changed.

本発明の有機EL素子や本発明に係る化合物の発光する色は、「新編色彩科学ハンドブック」(日本色彩学会編、東京大学出版会、1985)の108頁の図4.16において、分光放射輝度計CS−1000(コニカミノルタセンシング社製)で測定した結果をCIE色度座標に当てはめたときの色で決定される。   The light emission color of the organic EL device of the present invention and the compound according to the present invention is shown in FIG. 4.16 on page 108 of “New Color Science Handbook” (edited by the Japan Color Society, University of Tokyo Press, 1985). It is determined by the color when the result measured with the total CS-1000 (manufactured by Konica Minolta Sensing) is applied to the CIE chromaticity coordinates.

本発明で言うところの白色素子とは、2度視野角正面輝度を前記方法により測定した際に、1000Cd/m2でのCIE1931表色系における色度がX=0.33±0.77、Y=0.33±0.77の領域内にあることをいう。 The white element referred to in the present invention means that the chromaticity in the CIE 1931 color system at 1000 Cd / m 2 is X = 0.33 ± 0.77 when the front luminance at 2 ° viewing angle is measured by the above method. It is in the region of Y = 0.33 ± 0.77.

発光層は上記化合物を、例えば、真空蒸着法、スピンコ−ト法、キャスト法、LB法、インクジェット法等の公知の薄膜化法により製膜して形成することができる。   The light emitting layer can be formed by forming the above compound by a known thinning method such as a vacuum deposition method, a spin coating method, a casting method, an LB method, and an ink jet method.

白色パネルにおいては、発光層は発光極大波長が各々430nm〜480nm、510nm〜550nm、600nm〜640nmの範囲にある発光スペクトルの異なる少なくとも3層以上の層を含むことが好ましい。3層以上であれば、特に制限はない。4層より多い場合には、同一の発光スペクトルを有する層が複数層あってもよい。発光極大波長が430nm〜480nmにある層を青発光層、510nm〜550nmにある層を緑発光層、600nm〜640nmの範囲にある層を赤発光層と、以下称する。   In the white panel, it is preferable that the light emitting layer includes at least three layers having different emission spectra having emission maximum wavelengths in the range of 430 nm to 480 nm, 510 nm to 550 nm, and 600 nm to 640 nm, respectively. If it is three or more layers, there will be no restriction | limiting in particular. When there are more than four layers, there may be a plurality of layers having the same emission spectrum. A layer having an emission maximum wavelength in the range of 430 nm to 480 nm is referred to as a blue light emitting layer, a layer in the range of 510 nm to 550 nm is referred to as a green light emitting layer, and a layer in the range of 600 nm to 640 nm is referred to as a red light emitting layer.

発光層の膜厚の総和は特に制限はないが、通常2nm〜5μm、好ましくは2nm〜200nmの範囲で選ばれる。本発明においては、更に10nm〜20nmの範囲にあるのが好ましい。薄すぎると膜の均質性が得られにくい。またこれより厚いと発光を得るのに高電圧を要するため好ましくない。膜厚を20nm以下にすると電圧面のみならず、駆動電流に対する発光色の安定性が向上する効果があり好ましい。   The total thickness of the light emitting layer is not particularly limited, but is usually 2 nm to 5 μm, preferably 2 nm to 200 nm. In the present invention, it is preferably in the range of 10 nm to 20 nm. If it is too thin, it is difficult to obtain film uniformity. If it is thicker than this, a high voltage is required to obtain light emission, which is not preferable. A film thickness of 20 nm or less is preferable because it has the effect of improving the stability of the emission color with respect to the driving current as well as the voltage surface.

個々の発光層の膜厚は、好ましくは2nm〜100nmの範囲で選ばれ、2nm〜20nmの範囲にあるのが更に好ましい。青、緑、赤の各発光層の膜厚の関係については、特に制限はないが、3発光層中、青発光層(複数層ある場合はその総和)が最も厚いことが好ましい。   The film thickness of each light emitting layer is preferably selected in the range of 2 nm to 100 nm, and more preferably in the range of 2 nm to 20 nm. Although there is no restriction | limiting in particular about the film thickness relationship of each light emitting layer of blue, green, and red, It is preferable that the blue light emitting layer (the sum total when there are multiple layers) is the thickest among three light emitting layers.

また、前記の極大波長を維持する範囲において、各発光層には複数の発光性化合物を混合してもよい。例えば、青発光層に、極大波長430nm〜480nmの青発光性化合物と、同510nm〜550nmの緑発光性化合物を混合して用いてもよい。   Moreover, in the range which maintains the said maximum wavelength, you may mix a several luminescent compound in each light emitting layer. For example, the blue light emitting layer may be used by mixing a blue light emitting compound having a maximum wavelength of 430 nm to 480 nm and a green light emitting compound having the same wavelength of 510 nm to 550 nm.

《正孔輸送層》
正孔輸送層とは正孔を輸送する機能を有する正孔輸送材料からなり、広い意味で正孔注入層、電子阻止層も正孔輸送層に含まれる。正孔輸送層は単層または複数層設けることができる。
《Hole transport layer》
The hole transport layer is made of a hole transport material having a function of transporting holes, and in a broad sense, a hole injection layer and an electron blocking layer are also included in the hole transport layer. The hole transport layer can be provided as a single layer or a plurality of layers.

正孔輸送材料としては、正孔の注入または輸送、電子の障壁性のいずれかを有するものであり、有機物、無機物のいずれであってもよい。例えば、トリアゾ−ル誘導体、オキサジアゾ−ル誘導体、イミダゾ−ル誘導体、ポリアリ−ルアルカン誘導体、ピラゾリン誘導体及びピラゾロン誘導体、フェニレンジアミン誘導体、アリ−ルアミン誘導体、アミノ置換カルコン誘導体、オキサゾ−ル誘導体、スチリルアントラセン誘導体、フルオレノン誘導体、ヒドラゾン誘導体、スチルベン誘導体、シラザン誘導体、アニリン系共重合体、また導電性高分子オリゴマ−、特にチオフェンオリゴマ−等が挙げられる。   The hole transport material has any one of hole injection or transport and electron barrier properties, and may be either organic or inorganic. For example, triazole derivatives, oxadiazol derivatives, imidazole derivatives, polyarylalkane derivatives, pyrazoline derivatives and pyrazolone derivatives, phenylenediamine derivatives, arylamine derivatives, amino-substituted chalcone derivatives, oxazole derivatives, styrylanthracene derivatives Fluorenone derivatives, hydrazone derivatives, stilbene derivatives, silazane derivatives, aniline copolymers, and conductive polymer oligomers, particularly thiophene oligomers.

正孔輸送材料としては上記のものを使用することができるが、ポルフィリン化合物、芳香族第3級アミン化合物及びスチリルアミン化合物、特に芳香族第3級アミン化合物を用いることが好ましい。   The above-mentioned materials can be used as the hole transport material, but it is preferable to use a porphyrin compound, an aromatic tertiary amine compound and a styrylamine compound, particularly an aromatic tertiary amine compound.

芳香族第3級アミン化合物及びスチリルアミン化合物の代表例としては、N,N,N′,N′−テトラフェニル−4,4′−ジアミノフェニル;N,N′−ジフェニル−N,N′−ビス(3−メチルフェニル)−〔1,1′−ビフェニル〕−4,4′−ジアミン(TPD);2,2−ビス(4−ジ−p−トリルアミノフェニル)プロパン;1,1−ビス(4−ジ−p−トリルアミノフェニル)シクロヘキサン;N,N,N′,N′−テトラ−p−トリル−4,4′−ジアミノビフェニル;1,1−ビス(4−ジ−p−トリルアミノフェニル)−4−フェニルシクロヘキサン;ビス(4−ジメチルアミノ−2−メチルフェニル)フェニルメタン;ビス(4−ジ−p−トリルアミノフェニル)フェニルメタン;N,N′−ジフェニル−N,N′−ジ(4−メトキシフェニル)−4,4′−ジアミノビフェニル;N,N,N′,N′−テトラフェニル−4,4′−ジアミノジフェニルエ−テル;4,4′−ビス(ジフェニルアミノ)クオ−ドリフェニル;N,N,N−トリ(p−トリル)アミン;4−(ジ−p−トリルアミノ)−4′−〔4−(ジ−p−トリルアミノ)スチリル〕スチルベン;4−N,N−ジフェニルアミノ−(2−ジフェニルビニル)ベンゼン;3−メトキシ−4′−N,N−ジフェニルアミノスチルベンゼン;N−フェニルカルバゾ−ル、更には米国特許第5,061,569号明細書に記載されている2個の縮合芳香族環を分子内に有するもの、例えば、4,4′−ビス〔N−(1−ナフチル)−N−フェニルアミノ〕ビフェニル(NPD)、特開平4−308688号公報に記載されているトリフェニルアミンユニットが3つスタ−バ−スト型に連結された4,4′,4″−トリス〔N−(3−メチルフェニル)−N−フェニルアミノ〕トリフェニルアミン(MTDATA)等が挙げられる。   Representative examples of aromatic tertiary amine compounds and styrylamine compounds include N, N, N ', N'-tetraphenyl-4,4'-diaminophenyl; N, N'-diphenyl-N, N'- Bis (3-methylphenyl)-[1,1′-biphenyl] -4,4′-diamine (TPD); 2,2-bis (4-di-p-tolylaminophenyl) propane; 1,1-bis (4-di-p-tolylaminophenyl) cyclohexane; N, N, N ′, N′-tetra-p-tolyl-4,4′-diaminobiphenyl; 1,1-bis (4-di-p-tolyl) Aminophenyl) -4-phenylcyclohexane; bis (4-dimethylamino-2-methylphenyl) phenylmethane; bis (4-di-p-tolylaminophenyl) phenylmethane; N, N'-diphenyl-N, N ' − (4-methoxyphenyl) -4,4'-diaminobiphenyl; N, N, N ', N'-tetraphenyl-4,4'-diaminodiphenyl ether; 4,4'-bis (diphenylamino) qua -Dryphenyl; N, N, N-tri (p-tolyl) amine; 4- (di-p-tolylamino) -4 '-[4- (di-p-tolylamino) styryl] stilbene; 4-N, N- Diphenylamino- (2-diphenylvinyl) benzene; 3-methoxy-4'-N, N-diphenylaminostilbenzene; N-phenylcarbazole, and further described in US Pat. No. 5,061,569 Having two condensed aromatic rings in the molecule, for example, 4,4'-bis [N- (1-naphthyl) -N-phenylamino] biphenyl (NPD), JP-A-4-3086 4,4 ', 4 "-tris [N- (3-methylphenyl) -N-phenylamino] trimethyl triphenylamine unit described in Japanese Patent No. 8 is linked in three starburst types. Phenylamine (MTDATA) etc. are mentioned.

更にこれらの材料を高分子鎖に導入した、またはこれらの材料を高分子の主鎖とした高分子材料を用いることもできる。また、p型−Si、p型−SiC等の無機化合物も正孔注入材料、正孔輸送材料として使用することができる。   Furthermore, a polymer material in which these materials are introduced into a polymer chain or these materials are used as a polymer main chain can also be used. In addition, inorganic compounds such as p-type-Si and p-type-SiC can also be used as the hole injection material and the hole transport material.

また、特開平11−251067号公報、J.Huang et.al.著文献(Applied Physics Letters 80(2002), p.139)に記載されているような所謂p型正孔輸送材料を用いることもできる。本発明においては、より高効率の発光素子が得られることから、これらの材料を用いることが好ましい。   JP-A-11-251067, J. Org. Huang et. al. A so-called p-type hole transport material described in a book (Applied Physics Letters 80 (2002), p. 139) can also be used. In the present invention, it is preferable to use these materials because a light-emitting element with higher efficiency can be obtained.

正孔輸送層は上記正孔輸送材料を、例えば、真空蒸着法、スピンコ−ト法、キャスト法、インクジェット法を含む印刷法、LB法等の公知の方法により、薄膜化することにより形成することができる。正孔輸送層の膜厚については特に制限はないが、通常は5nm〜5μm程度、好ましくは5nm〜200nmである。この正孔輸送層は上記材料の1種または2種以上からなる一層構造であってもよい。   The hole transport layer is formed by thinning the hole transport material by a known method such as a vacuum deposition method, a spin coating method, a casting method, a printing method including an ink jet method, or an LB method. Can do. Although there is no restriction | limiting in particular about the film thickness of a positive hole transport layer, Usually, 5 nm-about 5 micrometers, Preferably it is 5 nm-200 nm. The hole transport layer may have a single layer structure composed of one or more of the above materials.

また、不純物をド−プしたp性の高い正孔輸送層を用いることもできる。その例としては、特開平4−297076号公報、特開2000−196140号公報、特開2001−102175号公報、J.Appl.Phys.,95,5773(2004)などに記載されたものが挙げられる。   Alternatively, a hole transport layer having high p property doped with impurities can be used. Examples thereof include JP-A-4-297076, JP-A-2000-196140, JP-A-2001-102175, J.A. Appl. Phys. 95, 5773 (2004), and the like.

《電子輸送層》
電子輸送層とは電子を輸送する機能を有する材料からなり、広い意味で電子注入層、正孔阻止層も電子輸送層に含まれる。電子輸送層は単層または複数層設けることができる。
《Electron transport layer》
The electron transport layer is made of a material having a function of transporting electrons, and in a broad sense, an electron injection layer and a hole blocking layer are also included in the electron transport layer. The electron transport layer can be provided as a single layer or a plurality of layers.

従来、単層の電子輸送層、及び複数層とする場合は発光層に対して陰極側に隣接する電子輸送層に用いられる電子輸送材料(正孔阻止材料を兼ねる)としては、陰極より注入された電子を発光層に伝達する機能を有していればよく、その材料としては従来公知の化合物の中から任意のものを選択して用いることができ、例えば、ニトロ置換フルオレン誘導体、ジフェニルキノン誘導体、チオピランジオキシド誘導体、カルボジイミド、フレオレニリデンメタン誘導体、アントラキノジメタン及びアントロン誘導体、オキサジアゾ−ル誘導体等が挙げられる。更に、上記オキサジアゾ−ル誘導体において、オキサジアゾ−ル環の酸素原子を硫黄原子に置換したチアジアゾ−ル誘導体、電子吸引基として知られているキノキサリン環を有するキノキサリン誘導体も、電子輸送材料として用いることができる。更にこれらの材料を高分子鎖に導入した、またはこれらの材料を高分子の主鎖とした高分子材料を用いることもできる。   Conventionally, in the case of a single electron transport layer and a plurality of layers, an electron transport material (also serving as a hole blocking material) used for an electron transport layer adjacent to the light emitting layer on the cathode side is injected from the cathode. As long as it has a function of transferring electrons to the light-emitting layer, any material can be selected and used from among conventionally known compounds. For example, nitro-substituted fluorene derivatives, diphenylquinone derivatives Thiopyran dioxide derivatives, carbodiimides, fluorenylidenemethane derivatives, anthraquinodimethane and anthrone derivatives, oxadiazol derivatives, and the like. Further, in the above oxadiazol derivative, a thiadiazol derivative in which the oxygen atom of the oxadiazol ring is substituted with a sulfur atom, or a quinoxaline derivative having a quinoxaline ring known as an electron withdrawing group can also be used as an electron transport material. it can. Furthermore, a polymer material in which these materials are introduced into a polymer chain or these materials are used as a polymer main chain can also be used.

また、8−キノリノ−ル誘導体の金属錯体、例えば、トリス(8−キノリノ−ル)アルミニウム(Alq)、トリス(5,7−ジクロロ−8−キノリノ−ル)アルミニウム、トリス(5,7−ジブロモ−8−キノリノ−ル)アルミニウム、トリス(2−メチル−8−キノリノ−ル)アルミニウム、トリス(5−メチル−8−キノリノ−ル)アルミニウム、ビス(8−キノリノ−ル)亜鉛(Znq)等、及びこれらの金属錯体の中心金属がIn、Mg、Cu、Ca、Sn、GaまたはPbに置き替わった金属錯体も、電子輸送材料として用いることができる。その他、メタルフリ−もしくはメタルフタロシアニン、またはそれらの末端がアルキル基やスルホン酸基等で置換されているものも、電子輸送材料として好ましく用いることができる。また、発光層の材料として例示したジスチリルピラジン誘導体も、電子輸送材料として用いることができるし、正孔注入層、正孔輸送層と同様に、n型−Si、n型−SiC等の無機半導体も電子輸送材料として用いることができる。   Also, metal complexes of 8-quinolinol derivatives such as tris (8-quinolinol) aluminum (Alq), tris (5,7-dichloro-8-quinolinol) aluminum, tris (5,7-dibromo). -8-quinolinol) aluminum, tris (2-methyl-8-quinolinol) aluminum, tris (5-methyl-8-quinolinol) aluminum, bis (8-quinolinol) zinc (Znq), etc. , And metal complexes in which the central metal of these metal complexes is replaced with In, Mg, Cu, Ca, Sn, Ga, or Pb can also be used as the electron transport material. In addition, metal-free or metal phthalocyanine, or those having terminal ends substituted with an alkyl group or a sulfonic acid group can be preferably used as the electron transport material. In addition, the distyrylpyrazine derivative exemplified as the material of the light emitting layer can also be used as an electron transport material, and similarly to the hole injection layer and the hole transport layer, inorganic such as n-type-Si and n-type-SiC can be used. A semiconductor can also be used as an electron transport material.

電子輸送層は上記電子輸送材料を、例えば、真空蒸着法、スピンコ−ト法、キャスト法、インクジェット法を含む印刷法、LB法等の公知の方法により、薄膜化することにより形成することができる。電子輸送層の膜厚については特に制限はないが、通常は5nm〜5μm程度、好ましくは5nm〜200nmである。電子輸送層は上記材料の1種または2種以上からなる一層構造であってもよい。   The electron transport layer can be formed by thinning the electron transport material by a known method such as a vacuum deposition method, a spin coating method, a casting method, a printing method including an ink jet method, or an LB method. . Although there is no restriction | limiting in particular about the film thickness of an electron carrying layer, Usually, 5 nm-about 5 micrometers, Preferably it is 5 nm-200 nm. The electron transport layer may have a single layer structure composed of one or more of the above materials.

また、不純物をド−プしたn性の高い電子輸送層を用いることもできる。その例としては、特開平4−297076号公報、特開平10−270172号公報、特開2000−196140号公報、特開2001−102175号公報、J.Appl.Phys.,95,5773(2004)などに記載されたものが挙げられる。   Alternatively, an electron transport layer having high n property doped with impurities can be used. Examples thereof include JP-A-4-297076, JP-A-10-270172, JP-A-2000-196140, JP-A-2001-102175, J. Pat. Appl. Phys. 95, 5773 (2004), and the like.

《支持体》
一般に、有機EL素子に用いることのできる支持体としては、ガラス、プラスチック等の種類には特に限定はなく、また、透明であっても不透明であってもよい。前記支持体としては、ガラス板、ポリマー板・フィルム等が挙げられる。前記支持体の形状は、枚葉シートあるいは連続帯状シートでもよい。
<Support>
In general, the support that can be used in the organic EL element is not particularly limited in the type of glass, plastic, and the like, and may be transparent or opaque. Examples of the support include glass plates, polymer plates and films. The shape of the support may be a single sheet or a continuous strip.

支持体側から光を取り出す場合には、支持体は透明であることが好ましい。好ましく用いられる透明な支持体としては、ガラス、石英、透明樹脂フィルムを挙げることができる。   In the case where light is extracted from the support side, the support is preferably transparent. Examples of the transparent support preferably used include glass, quartz, and a transparent resin film.

ガラス板としては、ソーダ石灰ガラス、バリウムストロンチウム含有ガラス、鉛ガラス、アルミノケイ酸ガラス、ホウケイ酸ガラス、バリウムホウケイ酸ガラス及び石英ガラス等を挙げることができる。   Examples of the glass plate include soda lime glass, barium strontium-containing glass, lead glass, aluminosilicate glass, borosilicate glass, barium borosilicate glass, and quartz glass.

ポリマー板としてはポリカーボネート、アクリル、ポリエチレンテレフタレート、ポリエーテルサルファイド及びポリサルフォン等を挙げることができる。   Examples of the polymer plate include polycarbonate, acrylic, polyethylene terephthalate, polyether sulfide, and polysulfone.

樹脂フィルムとしては、例えば、ポリエチレンテレフタレ−ト(PET)、ポリエチレンナフタレ−ト(PEN)等のポリエステル、ポリエチレン、ポリプロピレン、セロファン、セルロ−スジアセテ−ト、セルロ−ストリアセテ−ト、セルロ−スアセテ−トブチレ−ト、セルロ−スアセテ−トプロピオネ−ト(CAP)、セルロ−スアセテ−トフタレ−ト(TAC)、セルロ−スナイトレ−ト等のセルロ−スエステル類又はそれらの誘導体、ポリ塩化ビニリデン、ポリビニルアルコ−ル、ポリエチレンビニルアルコ−ル、シンジオタクティックポリスチレン、ポリカ−ボネ−ト、ノルボルネン樹脂、ポリメチルペンテン、ポリエ−テルケトン、ポリイミド、ポリエ−テルスルホン(PES)、ポリフェニレンスルフィド、ポリスルホン類、ポリエ−テルイミド、ポリエ−テルケトンイミド、ポリアミド、フッ素樹脂、ナイロン、ポリメチルメタクリレ−ト、アクリル或いはポリアリレ−ト類、ア−トン(商品名JSR社製)或いはアペル(商品名三井化学社製)といったシクロオレフィン系樹脂等を挙げられる。樹脂フィルムの表面には、無機物、有機物の被膜またはその両者のハイブリッド被膜が形成されていてもよく、水蒸気透過度が0.01g/m2/day/atm以下のバリア性フィルムであることが好ましく、更には、酸素透過度10-3ml/m2/day以下、水蒸気透過度10-5g/m2/day以下の高バリア性フィルムであることが好ましい。 Examples of the resin film include polyesters such as polyethylene terephthalate (PET) and polyethylene naphthalate (PEN), polyethylene, polypropylene, cellophane, cellulose diacetate, cellulosic triacetate, and cellulose acetate. Cellulose esters such as tobutyrate, cellulose acetate propionate (CAP), cellulose acetate phthalate (TAC), and cellulose nitrate or derivatives thereof, polyvinylidene chloride, polyvinyl alcohol Polyethylene vinyl alcohol, syndiotactic polystyrene, polycarbonate, norbornene resin, polymethylpentene, polyether ketone, polyimide, polyethersulfone (PES), polyphenylene sulfide, polysulfones, Lier Terimide, Polyether Ketoneimide, Polyamide, Fluororesin, Nylon, Polymethylmethacrylate, Acrylic or Polyarylate, Aton (trade name, manufactured by JSR) or Apel (trade name, manufactured by Mitsui Chemicals) ) And the like. An inorganic or organic film or a hybrid film of both may be formed on the surface of the resin film, and it is preferably a barrier film having a water vapor permeability of 0.01 g / m 2 / day / atm or less. Furthermore, a high barrier film having an oxygen permeability of 10 −3 ml / m 2 / day or less and a water vapor permeability of 10 −5 g / m 2 / day or less is preferable.

該バリア膜を形成する材料としては、水分や酸素など素子の劣化をもたらすものの浸入を抑制する機能を有する材料であればよく、例えば、酸化珪素、二酸化珪素、窒化珪素などを用いることができる。更に該膜の脆弱性を改良するためにこれら無機層と有機材料からなる層の積層構造を持たせることがより好ましい。無機層と有機層の積層順については特に制限はないが、両者を交互に複数回積層させることが好ましい。   As a material for forming the barrier film, any material may be used as long as it has a function of suppressing intrusion of an element such as moisture or oxygen that causes deterioration of the element. For example, silicon oxide, silicon dioxide, silicon nitride, or the like can be used. Further, in order to improve the brittleness of the film, it is more preferable to have a laminated structure of these inorganic layers and layers made of organic materials. Although there is no restriction | limiting in particular about the lamination | stacking order of an inorganic layer and an organic layer, It is preferable to laminate | stack both alternately several times.

該バリア膜の形成方法については、特に限定はなく、例えば真空蒸着法、スパッタリング法、反応性スパッタリング法、分子線エピタキシ−法、クラスタ−イオンビ−ム法、イオンプレ−ティング法、プラズマ重合法、大気圧プラズマ重合法、プラズマCVD法、レ−ザ−CVD法、熱CVD法、コ−ティング法などを用いることができるが、特開2004−68143号公報に記載されているような大気圧プラズマ重合法によるものが特に好ましい。   The method for forming the barrier film is not particularly limited. For example, a vacuum deposition method, a sputtering method, a reactive sputtering method, a molecular beam epitaxy method, a cluster ion beam method, an ion plating method, a plasma polymerization method, a large size, and the like. An atmospheric pressure plasma polymerization method, a plasma CVD method, a laser CVD method, a thermal CVD method, a coating method, or the like can be used, but an atmospheric pressure plasma weight as described in JP-A-2004-68143 is used. A legal method is particularly preferred.

不透明な支持体の例としては、例えばアルミ、ステンレス等の金属板・フィルムや不透明樹脂基板等が挙げられる。   Examples of the opaque support include metal plates / films such as aluminum and stainless steel, opaque resin substrates, and the like.

《封止》
本発明に用いられる封止手段としては、例えば封止部材と、電極、支持体とを接着剤で接着する方法を挙げることができる。
<Sealing>
As a sealing means used for this invention, the method of adhere | attaching a sealing member, an electrode, and a support body with an adhesive agent can be mentioned, for example.

一般に、封止部材としては、有機EL素子の表示領域を覆うように配置されておればよく、凹板状でも、平板状でもよい。また、透明性、電気絶縁性は特に問わない。   Generally, the sealing member may be disposed so as to cover the display area of the organic EL element, and may be a concave plate shape or a flat plate shape. Further, transparency and electrical insulation are not particularly limited.

具体的には、ガラス板、ポリマ−板・フィルム、金属板・フィルム等が挙げられる。ガラス板としては、特にソ−ダ石灰ガラス、バリウム・ストロンチウム含有ガラス、鉛ガラス、アルミノケイ酸ガラス、ホウケイ酸ガラス、バリウムホウケイ酸ガラス、石英等を挙げることができる。また、ポリマ−板としては、ポリカ−ボネ−ト、アクリル、ポリエチレンテレフタレ−ト、ポリエ−テルサルファイド、ポリサルフォン等を挙げることができる。金属板としては、ステンレス、鉄、銅、アルミニウム、マグネシウム、ニッケル、亜鉛、クロム、チタン、モリブテン、シリコン、ゲルマニウムおよびタンタルからなる群から選ばれる一種以上の金属または合金からなるものが挙げられる。本発明においては、支持体が可とう性を有する事と素子を薄膜化できるということからポリマ−フィルム、金属フィルムを好ましく使用することができる。更には、ポリマ−フィルムは、酸素透過度10-3ml/m2/day以下、水蒸気透過度10-5g/m2/day以下のであることが好ましい。 Specific examples include a glass plate, a polymer plate / film, and a metal plate / film. Examples of the glass plate include soda lime glass, barium / strontium-containing glass, lead glass, aluminosilicate glass, borosilicate glass, barium borosilicate glass, and quartz. Examples of the polymer plate include polycarbonate, acrylic, polyethylene terephthalate, polyether sulfide, polysulfone and the like. Examples of the metal plate include those made of one or more metals or alloys selected from the group consisting of stainless steel, iron, copper, aluminum, magnesium, nickel, zinc, chromium, titanium, molybdenum, silicon, germanium, and tantalum. In the present invention, a polymer film and a metal film can be preferably used because the support has flexibility and the device can be thinned. Furthermore, the polymer film preferably has an oxygen permeability of 10 −3 ml / m 2 / day or less and a water vapor permeability of 10 −5 g / m 2 / day or less.

接着剤として具体的には、アクリル酸系オリゴマ−、メタクリル酸系オリゴマ−の反応性ビニル基を有する光硬化および熱硬化型接着剤、2−シアノアクリル酸エステルなどの湿気硬化型等の接着剤を挙げることができる。また、エポキシ系などの熱および化学硬化型(二液混合)を挙げることができる。また、ホットメルト型のポリアミド、ポリエステル、ポリオレフィンを挙げることができる。また、カチオン硬化タイプの紫外線硬化型エポキシ樹脂接着剤を挙げることができる。   Specific examples of adhesives include photocuring and thermosetting adhesives having reactive vinyl groups of acrylic acid oligomers and methacrylic acid oligomers, and moisture curing adhesives such as 2-cyanoacrylates. Can be mentioned. Moreover, the heat | fever and chemical curing types (two-component mixing), such as an epoxy type, can be mentioned. Moreover, hot-melt type polyamide, polyester, and polyolefin can be mentioned. Moreover, a cationic curing type ultraviolet curing epoxy resin adhesive can be mentioned.

なお、有機EL素子が熱処理により劣化する場合があるので、室温から80℃までに接着硬化できるものが好ましい。また、前記接着剤中に乾燥剤を分散させておいてもよい。封止部分への接着剤の塗布は、市販のディスペンサ−を使ってもよいし、スクリ−ン印刷のように印刷してもよい。   In addition, since an organic EL element may deteriorate by heat processing, what can be adhesive-hardened from room temperature to 80 degreeC is preferable. A desiccant may be dispersed in the adhesive. Application | coating of the adhesive agent to a sealing part may use a commercially available dispenser, and may print it like screen printing.

また、有機層を挟み支持体と対向する側の電極の外側に、該電極と有機層を被覆し、支持体と接する形で無機物、有機物の層を形成し封止膜とすることも好適にできる。この場合、該膜を形成する材料としては、水分や酸素など素子の劣化をもたらすものの浸入を抑制する機能を有する材料であればよく、例えば、酸化珪素、二酸化珪素、窒化珪素などを用いることができる。更に該膜の脆弱性を改良するためにこれら無機層と有機材料からなる層の積層構造を持たせることが好ましい。これらの膜の形成方法については、特に限定はなく、例えば真空蒸着法、スパッタリング法、反応性スパッタリング法、分子線エピタキシ−法、クラスタ−イオンビ−ム法、イオンプレ−ティング法、プラズマ重合法、大気圧プラズマ重合法、プラズマCVD法、レ−ザ−CVD法、熱CVD法、コ−ティング法などを用いることができる。   In addition, it is also preferable to coat the electrode and the organic layer on the outside of the electrode facing the support with the organic layer interposed therebetween, and form an inorganic or organic layer in contact with the support to form a sealing film. it can. In this case, the material for forming the film may be any material that has a function of suppressing intrusion of elements that cause deterioration of the element such as moisture and oxygen. For example, silicon oxide, silicon dioxide, silicon nitride, or the like is used. it can. Furthermore, in order to improve the brittleness of the film, it is preferable to have a laminated structure of these inorganic layers and layers made of organic materials. The method for forming these films is not particularly limited. For example, vacuum deposition, sputtering, reactive sputtering, molecular beam epitaxy, cluster ion beam, ion plating, plasma polymerization, An atmospheric pressure plasma polymerization method, a plasma CVD method, a laser CVD method, a thermal CVD method, a coating method, or the like can be used.

封止部材と有機EL素子の表示領域との間隙には、気相および液相では、窒素、アルゴン等の不活性気体や、フッ化炭化水素、シリコンオイルのような不活性液体を注入することも可能である。また、真空とすることも可能である。また、内部に吸湿性化合物を封入することもできる。   In the gap between the sealing member and the display area of the organic EL element, an inert gas such as nitrogen or argon, or an inert liquid such as fluorinated hydrocarbon or silicon oil is injected in the gas phase and the liquid phase. Is also possible. A vacuum can also be used. Moreover, a hygroscopic compound can also be enclosed inside.

吸湿性化合物としては例えば金属酸化物(例えば、酸化ナトリウム、酸化カリウム、酸化カルシウム、酸化バリウム、酸化マグネシウム、酸化アルミニウム等)、硫酸塩(例えば、硫酸ナトリウム、硫酸カルシウム、硫酸マグネシウム、硫酸コバルト等)、金属ハロゲン化物(例えば、塩化カルシウム、塩化マグネシウム、フッ化セシウム、フッ化タンタル、臭化セリウム、臭化マグネシウム、沃化バリウム、沃化マグネシウム等)、過塩素酸類(例えば過塩素酸バリウム、過塩素酸マグネシウム等)等があげられ、硫酸塩、金属ハロゲン化物および過塩素酸類においては無水塩が好適に用いられる。   Examples of the hygroscopic compound include metal oxides (eg, sodium oxide, potassium oxide, calcium oxide, barium oxide, magnesium oxide, aluminum oxide), sulfates (eg, sodium sulfate, calcium sulfate, magnesium sulfate, cobalt sulfate, etc.). Metal halides (eg, calcium chloride, magnesium chloride, cesium fluoride, tantalum fluoride, cerium bromide, magnesium bromide, barium iodide, magnesium iodide, etc.), perchloric acids (eg, barium perchlorate, In particular, anhydrous salts are preferably used in sulfates, metal halides and perchloric acids.

《光取出し加工》
有機エレクトロルミネッセンス素子は、空気よりも屈折率の高い(屈折率が1.7〜2.1程度)層の内部で発光し、発光層で発生した光のうち15%から20%程度の光しか取り出せないことが一般的に言われている。これは、臨界角以上の角度θで界面(透明基板と空気との界面)に入射する光は、全反射を起こし素子外部に取り出すことができないことや、透明電極ないし発光層と透明基板との間で光が全反射を起こし、光が透明電極ないし発光層を導波し、結果として、光が素子側面方向に逃げるためである。
《Light extraction processing》
An organic electroluminescence element emits light inside a layer having a refractive index higher than that of air (refractive index is about 1.7 to 2.1), and only 15% to 20% of the light generated in the light emitting layer. It is generally said that it cannot be taken out. This is because light incident on the interface (interface between the transparent substrate and air) at an angle θ greater than the critical angle causes total reflection and cannot be taken out of the device, or between the transparent electrode or light emitting layer and the transparent substrate. This is because light is totally reflected between the light and the light is guided through the transparent electrode or the light emitting layer, and as a result, the light escapes in the direction of the side surface of the device.

この光の取り出しの効率を向上させる手法としては、例えば、透明基板表面に凹凸を形成し、透明基板と空気界面での全反射を防ぐ方法(例えば、米国特許第4774435明細書)。基板に集光性を持たせることにより効率を向上させる方法(例えば、特開昭63−314795号公報)。素子の側面等に反射面を形成する方法(例えば、特開平1−220394号公報)。基板と発光体の間に中間の屈折率を持つ平坦層を導入し、反射防止膜を形成する方法(例えば、特開昭62−172691号公報)。基板と発光体の間に基板よりも低屈折率を持つ平坦層を導入する方法(例えば、特開2001−202827号公報)。基板、透明電極層や発光層のいずれかの層間(含む、基板と外界間)に回折格子を形成する方法(例えば、特開平11−283751号公報)などがある。   As a technique for improving the light extraction efficiency, for example, a method of forming irregularities on the surface of the transparent substrate to prevent total reflection at the interface between the transparent substrate and the air (for example, US Pat. No. 4,774,435). A method for improving efficiency by providing a substrate with a light condensing property (for example, JP-A-63-314795). A method of forming a reflective surface on the side surface of the element (for example, Japanese Patent Laid-Open No. 1-220394). A method of forming an antireflection film by introducing a flat layer having an intermediate refractive index between a substrate and a light emitter (for example, Japanese Patent Application Laid-Open No. 62-172691). A method of introducing a flat layer having a lower refractive index than the substrate between the substrate and the light emitter (for example, JP-A-2001-202827). There is a method of forming a diffraction grating between any one of the substrate, the transparent electrode layer and the light emitting layer (including between the substrate and the outside) (for example, JP-A-11-283951).

これらの方法を本発明の有機エレクトロルミネッセンス素子と組み合わせて用いることができるが、基板と発光体の間に基板よりも低屈折率を持つ平坦層を導入する方法、あるいは基板、透明電極層や発光層のいずれかの層間(含む、基板と外界間)に回折格子を形成する方法を好適に用いることができる。   These methods can be used in combination with the organic electroluminescence device of the present invention. However, a method of introducing a flat layer having a lower refractive index than the substrate between the substrate and the light emitter, or a substrate, a transparent electrode layer, and light emission A method of forming a diffraction grating between any of the layers (including between the substrate and the outside) can be suitably used.

これらの手段を組み合わせることにより、更に高輝度あるいは耐久性に優れた素子を得ることができる。   By combining these means, it is possible to obtain an element having higher luminance or durability.

透明電極と透明基板の間に低屈折率の媒質を光の波長よりも長い厚みで形成すると、透明電極から出てきた光は、媒質の屈折率が低いほど、外部への取り出し効率が高くなる。   When a low refractive index medium is formed between the transparent electrode and the transparent substrate with a thickness longer than the wavelength of light, the light extracted from the transparent electrode has a higher extraction efficiency to the outside as the refractive index of the medium is lower. .

低屈折率層としては、例えば、エアロゲル、多孔質シリカ、フッ化マグネシウム、フッ素系ポリマ−などが挙げられる。透明基板の屈折率は一般に1.5〜1.7程度であるので、低屈折率層は、屈折率がおよそ1.5以下であることが好ましい。またさらに1.35以下であることが好ましい。   Examples of the low refractive index layer include aerogel, porous silica, magnesium fluoride, fluorine polymer, and the like. Since the refractive index of the transparent substrate is generally about 1.5 to 1.7, the low refractive index layer preferably has a refractive index of about 1.5 or less. Furthermore, it is preferable that it is 1.35 or less.

また、低屈折率媒質の厚みは、媒質中の波長の2倍以上となるのが望ましい。これは、低屈折率媒質の厚みが、光の波長程度になってエバネッセントで染み出した電磁波が基板内に入り込む膜厚になると、低屈折率層の効果が薄れるからである。   The thickness of the low refractive index medium is preferably at least twice the wavelength in the medium. This is because the effect of the low refractive index layer is diminished when the thickness of the low refractive index medium is about the wavelength of light and the electromagnetic wave that has exuded by evanescent enters the substrate.

全反射を起こす界面もしくはいずれかの媒質中に回折格子を導入する方法は、光取り出し効率の向上効果が高いという特徴がある。この方法は、回折格子が1次の回折や、2次の回折といったいわゆるブラッグ回折により、光の向きを屈折とは異なる特定の向きに変えることができる性質を利用して、発光層から発生した光のうち、層間での全反射等により外に出ることができない光を、いずれかの層間もしくは、媒質中(透明基板内や透明電極内)に回折格子を導入することで光を回折させ、光を外に取り出そうとするものである。   The method of introducing a diffraction grating into an interface or any medium that causes total reflection is characterized by a high effect of improving light extraction efficiency. This method is generated from the light emitting layer by utilizing the property that the diffraction grating can change the direction of light to a specific direction different from refraction by so-called Bragg diffraction such as first-order diffraction or second-order diffraction. Of the light, light that cannot go out due to total reflection between layers, etc., is diffracted by introducing a diffraction grating in any layer or medium (in the transparent substrate or transparent electrode) It tries to take out light.

導入する回折格子は、二次元的な周期屈折率を持っていることが望ましい。これは、発光層で発光する光はあらゆる方向にランダムに発生するので、ある方向にのみ周期的な屈折率分布を持っている一般的な1次元回折格子では、特定の方向に進む光しか回折されず、光の取り出し効率がさほど上がらない。しかしながら、屈折率分布を二次元的な分布にすることにより、あらゆる方向に進む光が回折され、光の取り出し効率が上がる。   The introduced diffraction grating desirably has a two-dimensional periodic refractive index. This is because light emitted from the light-emitting layer is randomly generated in all directions, so in a general one-dimensional diffraction grating having a periodic refractive index distribution only in a certain direction, only light traveling in a specific direction is diffracted. The light extraction efficiency does not increase so much. However, by making the refractive index distribution a two-dimensional distribution, light traveling in all directions is diffracted, and light extraction efficiency is increased.

回折格子を導入する位置としては前述のとおり、いずれかの層間もしくは、媒質中(透明基板内や透明電極内)でも良いが、光が発生する場所である有機発光層の近傍が望ましい。   As described above, the position where the diffraction grating is introduced may be in any of the layers or in the medium (in the transparent substrate or the transparent electrode), but is preferably in the vicinity of the organic light emitting layer where light is generated.

このとき、回折格子の周期は、媒質中の光の波長の約1/2〜3倍程度が好ましい。   At this time, the period of the diffraction grating is preferably about 1/2 to 3 times the wavelength of light in the medium.

回折格子の配列は、正方形のラチス状、三角形のラチス状、ハニカムラチス状など、2次元的に配列が繰り返されることが好ましい。   The arrangement of the diffraction gratings is preferably two-dimensionally repeated, such as a square lattice, a triangular lattice, or a honeycomb lattice.

《集光シ−ト》
本発明の有機エレクトロルミネッセンス素子を面光源用に使用する場合は、基板の光取出し側に、例えばマイクロレンズアレイ上の構造を設けるように加工したり、あるいは、所謂集光シ−トと組み合わせることにより、特定方向、例えば素子発光面に対し正面方向に集光することにより、特定方向上の輝度を高めることができる。
<Condensation sheet>
When the organic electroluminescence device of the present invention is used for a surface light source, it is processed so as to provide, for example, a structure on a microlens array on the light extraction side of the substrate, or combined with a so-called condensing sheet. Thus, by focusing light in a specific direction, for example, in the front direction with respect to the element light emitting surface, the luminance in the specific direction can be increased.

マイクロレンズアレイの例としては、基板の光取り出し側に一辺が30μmでその頂角が90度となるような四角錐を2次元に配列する。一辺は10μm〜100μmが好ましい。これより小さくなると回折の効果が発生して色付く、大きすぎると厚みが厚くなり好ましくない。   As an example of the microlens array, quadrangular pyramids having a side of 30 μm and an apex angle of 90 degrees are two-dimensionally arranged on the light extraction side of the substrate. One side is preferably 10 μm to 100 μm. If it becomes smaller than this, the effect of diffraction will generate | occur | produce and color, and if too large, thickness will become thick and is not preferable.

集光シ−トとしては、例えば液晶表示装置のLEDバックライトで実用化されているものを用いることが可能である。このようなシ−トとして例えば、住友スリ−エム社製輝度上昇フィルム(BEF)などを用いることができる。プリズムシ−トの形状としては、例えば基材に頂角90度、ピッチ50μmの△状のストライプが形成されたものであってもよいし、頂角が丸みを帯びた形状、ピッチをランダムに変化させた形状、その他の形状であっても良い。   As the condensing sheet, for example, an LED backlight of a liquid crystal display device that is put into practical use can be used. As such a sheet, for example, a brightness enhancement film (BEF) manufactured by Sumitomo 3M Ltd. can be used. As the shape of the prism sheet, for example, the base material may be formed with a Δ-shaped stripe having an apex angle of 90 degrees and a pitch of 50 μm, or the apex angle is rounded and the pitch is changed randomly. Other shapes may be used.

また、発光素子からの光放射角を制御するために光拡散板・フィルムを、集光シ−トと併用してもよい。例えば、拡散フィルム「ライトアップ」((株)きもと製)などを用いることができる。   Moreover, in order to control the light emission angle from a light emitting element, you may use a light diffusing plate and a film together with a condensing sheet. For example, a diffusion film “light up” (manufactured by Kimoto Co., Ltd.) can be used.

<本発明に係る有機EL素子の製造方法の実施の形態>
次に本発明に係る有機ELパネルの製造方法の実施の形態について説明する。本発明は、以下の実施の形態に限定されるものではない。
<Embodiment of the manufacturing method of the organic EL element which concerns on this invention>
Next, an embodiment of a method for producing an organic EL panel according to the present invention will be described. The present invention is not limited to the following embodiments.

有機ELパネルの層構成の例は、前述の有機ELパネルの層構成の好ましい具体例に記述したが、本実施の形態では、本発明に係る基板上に電極物質、例えばITO(インジウムチンオキシド)等を成膜しフォトエッチングでパターニングを行うことにより第一電極(陽極)を形成した電極表面の洗浄工程及び洗浄工程から有機層成膜工程について説明する。   Although the example of the layer structure of the organic EL panel is described in the preferred specific example of the layer structure of the organic EL panel described above, in this embodiment, an electrode material such as ITO (indium tin oxide) is formed on the substrate according to the present invention. The electrode layer cleaning step and the organic layer forming step from the cleaning step where the first electrode (anode) is formed by patterning by photoetching and the like will be described.

(実施の形態1)
図1は、乾式洗浄と湿式洗浄を組み合わせた洗浄工程の実施形態1の模式図である。
(Embodiment 1)
FIG. 1 is a schematic diagram of Embodiment 1 of a cleaning process in which dry cleaning and wet cleaning are combined.

図1に示すように、第一電極が形成された基板1は乾式洗浄装置21で乾式洗浄を行い、有機物汚染を除去することにより基板電極上の水の接触角を45°以下とする。乾式洗浄が十分でなく、有機汚染残が発生した場合には、基板電極上の水の接触角が45°を超え、次の湿式洗浄の効率を低下させる。   As shown in FIG. 1, the substrate 1 on which the first electrode is formed is dry-cleaned by a dry-cleaning device 21 to remove organic contaminants so that the contact angle of water on the substrate electrode is 45 ° or less. When dry cleaning is not sufficient and organic contamination residue is generated, the contact angle of water on the substrate electrode exceeds 45 °, which reduces the efficiency of the next wet cleaning.

乾式洗浄は、紫外線オゾン洗浄及びプラズマ洗浄の少なくとも何れか1つで行われる。紫外線オゾン洗浄は、紫外線を用いて活性酸素を発生させ、同時に基板表面に付着した有機物を分解、酸化し揮発除去する方式で、エキシマランプを用いる方法、低圧水銀ランプを用いる方法等がある。プラズマ洗浄は、酸素ガスやアルゴンガスに高周波を印可しプラズマを発生させ、基板表面に照射し化学反応により洗浄する方式である。   The dry cleaning is performed by at least one of ultraviolet ozone cleaning and plasma cleaning. Ultraviolet ozone cleaning is a method of generating active oxygen using ultraviolet rays and simultaneously decomposing, oxidizing and volatilizing and removing organic substances adhering to the substrate surface. There are a method using an excimer lamp, a method using a low-pressure mercury lamp, and the like. Plasma cleaning is a method in which a high frequency is applied to oxygen gas or argon gas to generate plasma, and the substrate surface is irradiated and cleaned by a chemical reaction.

図2は、紫外線オゾン洗浄を用いた、枚葉シート状基板1の乾式洗浄装置の例である。コンベア等の搬送手段C1に基板1を載置して紫外線オゾン洗浄装置21に搬送し、搬送しながら乾式洗浄を行う。基板を固定テーブル等に載置し、基板を搬送させずに洗浄しても良い。本実施の形態においては、200W低圧水銀ランプ(セン特殊光源(株)製)を用い、照射距離10mm、照射時間1分で洗浄処理を行い、基板電極表面における水の接触角を45°以下としている。   FIG. 2 is an example of a dry cleaning apparatus for the single wafer sheet substrate 1 using ultraviolet ozone cleaning. The substrate 1 is placed on the transport means C1 such as a conveyor, transported to the ultraviolet ozone cleaning device 21, and dry cleaning is performed while transporting. The substrate may be placed on a fixed table or the like and cleaned without transporting the substrate. In this embodiment, a 200 W low-pressure mercury lamp (manufactured by Sen Special Light Source Co., Ltd.) is used to perform a cleaning process with an irradiation distance of 10 mm and an irradiation time of 1 minute, and the contact angle of water on the substrate electrode surface is set to 45 ° or less. Yes.

前記基板電極表面における水の接触角は、洗浄しながらの測定は困難なため、別途サンプル基板で洗浄及び測定を行い水の接触角が45°以下となる洗浄条件を定め、その条件で洗浄を行う。   Since the contact angle of water on the surface of the substrate electrode is difficult to measure while washing, cleaning and measurement are separately performed on the sample substrate, and the cleaning condition is set such that the contact angle of water is 45 ° or less. Do.

また、水の接触角の測定は、JIS R 3257規格の試験法に基づき、接触角計(協和界面科学(株)製DropMaster700)で行っている。   The contact angle of water is measured with a contact angle meter (DropMaster 700 manufactured by Kyowa Interface Science Co., Ltd.) based on the test method of JIS R 3257 standard.

乾式洗浄装置21で乾式洗浄が終了した基板1は、湿式洗浄装置22で湿式洗浄される。有機汚染に埋没されていた異物の粒子は、前述のように乾式洗浄で有機汚染が除去され、基板電極上の水の接触角が45°以下とされるため、湿式洗浄で効率よく除去することができる。また、洗浄に用いられる溶媒は、水系溶媒のみで行うことができる。   The substrate 1 that has been dry-cleaned by the dry-cleaning device 21 is wet-cleaned by the wet-cleaning device 22. Foreign particles embedded in organic contamination should be removed efficiently by wet cleaning because organic contamination is removed by dry cleaning as described above and the contact angle of water on the substrate electrode is 45 ° or less. Can do. Moreover, the solvent used for washing | cleaning can be performed only with an aqueous solvent.

湿式洗浄は、超音波洗浄浴槽浸漬、流水式洗浄浴槽浸漬、流水式超音波洗浄浴槽浸漬、流水式シャワー及び流水式超音波シャワー方式の少なくとも何れか1つで行われる。   The wet cleaning is performed by at least one of an ultrasonic cleaning bath immersion, a flowing water cleaning bath immersion, a flowing ultrasonic cleaning bath immersion, a flowing shower, and a flowing ultrasonic shower method.

超音波洗浄浴槽浸漬方式とは、溶媒を貯水した超音波洗浄浴槽に基板1を浸漬して洗浄をする方法である。流水式洗浄浴槽浸漬方式とは、流水している洗浄浴槽に基板1を浸漬して洗浄する方法である。流水式超音波洗浄浴槽浸漬方式とは、前記流水式洗浄浴槽浸漬方式において洗浄浴槽内の溶媒に超音波発生手段により超音波振動を付加して洗浄する方法である。流水式シャワー方式とは、シャワーノズルより溶媒を基板1に吹きつけ洗浄する方法である。流水式超音波シャワー方式とは、前記流水式シャワー方式において吹きつける溶媒に超音波発生手段により超音波振動を付加して洗浄する方法である。   The ultrasonic cleaning bath immersion method is a method of cleaning by immersing the substrate 1 in an ultrasonic cleaning bath in which a solvent is stored. The flowing water type washing bath immersion method is a method in which the substrate 1 is immersed and washed in a flowing washing bath. The flowing water type ultrasonic cleaning bath immersion method is a method in which ultrasonic vibration is applied to the solvent in the cleaning bath by the ultrasonic wave generating means to perform cleaning in the flowing water type cleaning bath immersion method. The flowing water shower method is a method in which a solvent is sprayed onto the substrate 1 from a shower nozzle for cleaning. The flowing water type ultrasonic shower method is a method of cleaning by adding ultrasonic vibration to the solvent sprayed in the flowing water type shower method by ultrasonic generating means.

前記溶媒中の異物粒子サイズ及び粒子数は、異物粒子サイズ0.5μm以上の粒子数が1500個/ml以下が好ましい。異物粒子サイズ0.5μm未満は管理が困難であり、かつ異物粒子サイズ0.5μm以上の粒子数を管理することで省くことができる。異物粒子サイズ0.5μm以上の粒子数が1500個/mlを超えると有機EL素子駆動時にリーク電流が発生しやすくなる。   The foreign particle size and the number of particles in the solvent are preferably 1500 particles / ml or less with a foreign particle size of 0.5 μm or more. The foreign particle size of less than 0.5 μm is difficult to manage and can be omitted by managing the number of particles having a foreign particle size of 0.5 μm or more. When the number of particles having a foreign particle size of 0.5 μm or more exceeds 1500 / ml, a leak current is likely to occur when the organic EL element is driven.

図3は、流水式超音波シャワーを用いた湿式洗浄の例である。   FIG. 3 shows an example of wet cleaning using a flowing water type ultrasonic shower.

基板1を洗浄槽221の図示しない基板保持手段で保持し、水系溶媒B1を溶媒貯水容器224より供給ポンプP1でシャワーノズル222を介して、基板1の洗浄面に流水シャワー方式で供給し、基板1を洗浄する。溶媒B1のシャワーに超音波発生装置223により超音波振動が付加される。基板1は、洗浄槽221に溜められた溶媒B1と接しないよう、洗浄槽221の最上液面より常に上部に保持される。   The substrate 1 is held by a substrate holding means (not shown) of the cleaning tank 221, and the aqueous solvent B 1 is supplied from the solvent storage container 224 to the cleaning surface of the substrate 1 through the shower nozzle 222 by the supply pump P 1 by the flowing water shower method. Wash 1 Ultrasonic vibration is applied to the shower of the solvent B1 by the ultrasonic generator 223. The substrate 1 is always held above the uppermost liquid surface of the cleaning tank 221 so as not to contact the solvent B1 stored in the cleaning tank 221.

前記流水シャワー方式で基板洗浄した溶媒B1は、洗浄槽221に落下し溜められる。溜められた溶媒B1は、ポンプP2で移送しフィルター225を介して溶媒貯水容器224に戻され循環される。循環する溶媒B1は、図3の破線に示すように直接供給経路に戻しても良い。   The solvent B1 that has been subjected to substrate cleaning by the flowing water shower method is dropped and stored in the cleaning tank 221. The accumulated solvent B1 is transferred by the pump P2, returned to the solvent storage container 224 through the filter 225, and circulated. The circulating solvent B1 may be returned directly to the supply path as shown by the broken line in FIG.

洗浄槽221中の溶媒B1の異物粒子数は、LPC(粒子数計測手段)51により所定時間毎に計測される。前記所定時間の間隔は、洗浄工程の仕様により適宜設定が可能である。本実施形態では、10秒ごととしている。計測されたデータを基に粒子数分析手段である分析部52で単位容量当たりの粒子数に分析し、分析データは、演算部53に送られ予め定めた判定方法、例えば前記分析データを予め定めた清浄度の可否を判定する判定基準値と比較する、あるいは分析データの経時変化の有無等で基板清浄度の可否の判定が行われる。   The number of foreign particles of the solvent B1 in the cleaning tank 221 is measured every predetermined time by an LPC (particle number measuring means) 51. The interval of the predetermined time can be appropriately set according to the specifications of the cleaning process. In this embodiment, it is every 10 seconds. Based on the measured data, the analysis unit 52, which is a particle number analysis means, analyzes the number of particles per unit volume. The analysis data is sent to the calculation unit 53, and a predetermined determination method, for example, the analysis data is determined in advance. The substrate cleanliness is determined based on whether the analysis data is changed over time or the like.

湿式洗浄装置22で湿式洗浄が終了した基板1は、乾燥装置23で乾燥される。乾燥方法は、公知のスピン乾燥法、熱風乾燥法、エアナイフ乾燥法を用いることができる。   The substrate 1 that has been wet-cleaned by the wet-cleaning device 22 is dried by the drying device 23. As a drying method, a known spin drying method, hot air drying method, or air knife drying method can be used.

乾乾燥装置23で燥が終了した基板1は乾式洗浄装置24で乾式洗浄される。乾式洗浄装置24の態様は、前記乾式洗浄装置21に準ずる。   The substrate 1 that has been dried by the dry-drying device 23 is dry-cleaned by the dry-cleaning device 24. The mode of the dry cleaning device 24 is in accordance with the dry cleaning device 21.

乾式洗浄装置24で乾式洗浄が終了した基板1は、図示しない有機層を成膜する有機層成膜装置で有機層が形成される。有機層成膜は、例えば真空蒸着法、スピンコート法、キャスト法、LB法、インクジェット法等公知の方法を用いることができる。   On the substrate 1 that has been dry-cleaned by the dry-cleaning device 24, an organic layer is formed by an organic layer film-forming device that forms an organic layer (not shown). The organic layer can be formed by a known method such as a vacuum deposition method, a spin coating method, a casting method, an LB method, or an ink jet method.

(実施の形態2)
図4は、連続シート状基板をロールツーロール方式でウェブ搬送しながら前記連続シート状基板を乾式洗浄と湿式洗浄を組み合わせた洗浄工程で洗浄を行い、同一のウェブ搬送ラインで有機層の成膜を行う実施の形態2の模式図である。
(Embodiment 2)
FIG. 4 shows a process of cleaning the continuous sheet substrate in a roll-to-roll manner while transporting the web by a roll-to-roll method in a cleaning process combining dry cleaning and wet cleaning, and forming an organic layer on the same web transport line. It is a schematic diagram of Embodiment 2 which performs.

図4に示すように、第一電極が形成された連続シート状基板1Aのウェブ搬送ライン上に、乾式洗浄装置21、第一湿式洗浄装置22A、第二湿式洗浄装置22B、乾燥装置23、乾式洗浄装置24及び有機層成膜装置3が配設される。本実施の形態では、湿式洗浄工程は第一湿式洗浄装置22A及び第二湿式洗浄装置22Bの二段としたが、これに限定されるものではない。同様に、連続シート状基板1Aのウェブ搬送ライン上に配設される他の装置の装置段数も本実施の形態に限定されるものではない。   As shown in FIG. 4, a dry cleaning device 21, a first wet cleaning device 22 </ b> A, a second wet cleaning device 22 </ b> B, a drying device 23, a dry process are provided on the web conveyance line of the continuous sheet-like substrate 1 </ b> A on which the first electrode is formed. A cleaning device 24 and an organic layer film forming device 3 are provided. In the present embodiment, the wet cleaning process has two stages of the first wet cleaning apparatus 22A and the second wet cleaning apparatus 22B, but is not limited thereto. Similarly, the number of apparatus stages of other apparatuses disposed on the web conveyance line of the continuous sheet substrate 1A is not limited to this embodiment.

送り出しロール1A1から送り出された連続シート状基板1Aは、乾式洗浄装置21で乾式洗浄を行い、有機物汚染を除去することにより基板電極上の水の接触角を45°以下とする。乾式洗浄が十分でなく、有機汚染残が発生した場合には、基板電極上の水の接触角が45°を超え、次の湿式洗浄の効率を低下させる。   The continuous sheet-like substrate 1A fed from the feed roll 1A1 is dry-cleaned by the dry-cleaning device 21 to remove organic contaminants so that the contact angle of water on the substrate electrode is 45 ° or less. When dry cleaning is not sufficient and organic contamination residue is generated, the contact angle of water on the substrate electrode exceeds 45 °, which reduces the efficiency of the next wet cleaning.

乾式洗浄は、紫外線オゾン洗浄及びプラズマ洗浄の少なくとも何れか1つで行われる。紫外線オゾン洗浄は、紫外線を用いて活性酸素を発生させ、同時に基板表面に付着した有機物を分解、酸化し揮発除去する方式で、エキシマランプを用いる方法、低圧水銀ランプを用いる方法等がある。プラズマ洗浄は、酸素ガスやアルゴンガスに高周波を印可しプラズマを発生させ、基板表面に照射し化学反応により洗浄する方式である。   The dry cleaning is performed by at least one of ultraviolet ozone cleaning and plasma cleaning. Ultraviolet ozone cleaning is a method of generating active oxygen using ultraviolet rays and simultaneously decomposing, oxidizing and volatilizing and removing organic substances adhering to the substrate surface. There are a method using an excimer lamp, a method using a low-pressure mercury lamp, and the like. Plasma cleaning is a method in which a high frequency is applied to oxygen gas or argon gas to generate plasma, and the substrate surface is irradiated and cleaned by a chemical reaction.

本実施の形態では、乾式洗浄装置21に紫外線オゾン洗浄を用いている。送り出しロール1A1から送り出された連続シート状基板1Aは、ウェブ搬送しながら紫外線オゾン洗浄装置21で洗浄される。   In the present embodiment, ultraviolet ozone cleaning is used for the dry cleaning device 21. The continuous sheet-like substrate 1A fed from the feed roll 1A1 is cleaned by the ultraviolet ozone cleaning device 21 while carrying the web.

本実施の形態においては、200W低圧水銀ランプ(セン特殊光源(株)製)を用い、照射距離10mm、照射時間1分で洗浄処理を行い、基板電極表面における水の接触角を45°以下としている。   In this embodiment, a 200 W low-pressure mercury lamp (manufactured by Sen Special Light Source Co., Ltd.) is used to perform a cleaning process with an irradiation distance of 10 mm and an irradiation time of 1 minute, and the contact angle of water on the substrate electrode surface is set to 45 ° or less. Yes.

前記基板電極表面における水の接触角は、洗浄しながらの測定は困難なため、別途サンプル基板で洗浄及び測定を行い水の接触角が45°以下となる洗浄条件を定め、その条件で洗浄を行う。   Since the contact angle of water on the surface of the substrate electrode is difficult to measure while washing, cleaning and measurement are separately performed on the sample substrate, and the cleaning condition is set such that the contact angle of water is 45 ° or less. Do.

また、水の接触角の測定は、JIS R 3257規格の試験法に基づき、接触角計(協和界面科学(株)製DropMaster700)で行っている。   The contact angle of water is measured with a contact angle meter (DropMaster 700 manufactured by Kyowa Interface Science Co., Ltd.) based on the test method of JIS R 3257 standard.

乾式洗浄装置21で乾式洗浄が終了した連続シート状基板1Aは、湿式洗浄装置22A及び22Bで湿式洗浄される。有機汚染に埋没されていた異物の粒子は、前述のように乾式洗浄で有機汚染が除去され、基板電極上の水の接触角が45°以下とされるため、湿式洗浄で効率よく除去することができる。また、洗浄に用いられる溶媒は、水系溶媒のみとすることができる。   The continuous sheet substrate 1A that has been dry-cleaned by the dry-cleaning device 21 is wet-cleaned by the wet-cleaning devices 22A and 22B. Foreign particles embedded in organic contamination should be removed efficiently by wet cleaning because organic contamination is removed by dry cleaning as described above and the contact angle of water on the substrate electrode is 45 ° or less. Can do. Moreover, the solvent used for washing | cleaning can be only an aqueous solvent.

湿式洗浄は、超音波洗浄浴槽浸漬、流水式洗浄浴槽浸漬、流水式超音波洗浄浴槽浸漬、流水式シャワー及び流水式超音波シャワー方式の少なくとも何れか1つで行われる。連続シート状基板1Aに連続して均一な洗浄を行うため、流水式洗浄浴槽浸漬、流水式超音波洗浄浴槽浸漬、流水式シャワー及び流水式超音波シャワー方式の何れかが好ましい。前記各洗浄方法及び溶媒の態様については、実施形態1に記載の内容に準ずる。   The wet cleaning is performed by at least one of an ultrasonic cleaning bath immersion, a flowing water cleaning bath immersion, a flowing ultrasonic cleaning bath immersion, a flowing shower, and a flowing ultrasonic shower method. In order to perform continuous and uniform cleaning on the continuous sheet-like substrate 1A, any of a flowing water type cleaning bath immersion, a flowing water type ultrasonic cleaning bath immersion, a flowing water type shower and a flowing water type ultrasonic shower method is preferable. About the aspect of each said washing | cleaning method and a solvent, it applies to the content of Embodiment 1.

乾式洗浄装置21での洗浄が終了した連続シート状基板1Aは、ウェブ搬送されながら湿式洗浄装置22A及び22Bで洗浄される。本実施の形態では、湿式洗浄に流水式超音波シャワー方式を用いている。流水式超音波シャワー方式を用いた湿式洗浄装置の態様については、実施形態1に記載の内容に準ずる。   The continuous sheet-like substrate 1A that has been cleaned by the dry cleaning device 21 is cleaned by the wet cleaning devices 22A and 22B while being conveyed on the web. In this embodiment, a flowing water type ultrasonic shower system is used for wet cleaning. About the aspect of the wet-cleaning apparatus using a flowing water type ultrasonic shower system, it applies to the content of Embodiment 1.

湿式洗浄装置22A及び22Bで湿式洗浄が終了した連続シート状基板1Aは、乾燥装置2Cで乾燥される。乾燥方法は、公知の熱風乾燥法、エアナイフ乾燥法を用いることができる。   The continuous sheet substrate 1A that has been wet-cleaned by the wet-cleaning devices 22A and 22B is dried by the drying device 2C. As the drying method, a known hot air drying method or air knife drying method can be used.

乾乾燥装置23で燥が終了した基板1は乾式洗浄装置24で乾式洗浄される。乾式洗浄装置24の態様は、前記乾式洗浄装置21に準ずる。   The substrate 1 that has been dried by the dry-drying device 23 is dry-cleaned by the dry-cleaning device 24. The mode of the dry cleaning device 24 is in accordance with the dry cleaning device 21.

乾式洗浄装置24で乾式洗浄が終了した基板1は、有機層を成膜する有機層成膜装置3で有機層が形成される。有機層成膜は、例えば真空蒸着法、キャスト法、LB法、インクジェット法等公知の方法を用いることができる。   On the substrate 1 that has been dry-cleaned by the dry-cleaning device 24, an organic layer is formed by the organic layer film-forming device 3 that forms an organic layer. The organic layer can be formed by a known method such as a vacuum deposition method, a casting method, an LB method, or an ink jet method.

有機層が形成された連続シート状基板1Aは、巻き取りロールに巻き取られる。   The continuous sheet-like substrate 1A on which the organic layer is formed is wound around a winding roll.

前記洗浄後、連続シート状基板1Aの同一のウェブ搬送ラインでの搬送において、連続シート状基板電極面を非接触状態で搬送することが、基板洗浄後の清浄度を維持するために好ましい。   In order to maintain the cleanliness after cleaning the substrate, it is preferable to transfer the continuous sheet-like substrate electrode surface in a non-contact state in the transfer of the continuous sheet-like substrate 1A on the same web transfer line after the cleaning.

以下、実施例を挙げて本発明の具体的な効果を示すが、本発明の態様はこれに限定されるものではない。   Hereinafter, although an example is given and the concrete effect of the present invention is shown, the mode of the present invention is not limited to this.

一つのドットの大きさが2.0mm×2.0mmで、3ドット×3ドットの合計9ドット(発光領域)で構成される有機EL素子を以下に示す方法で製造した。   An organic EL element having a size of one dot of 2.0 mm × 2.0 mm and a total of 9 dots (light emitting region) of 3 dots × 3 dots was manufactured by the method described below.

<基板の準備>
基板としては、厚さ1.1mm、30mm×30mmのソーダ石灰ガラス板を準備した。尚、ソーダ石灰ガラス板の全面には、酸やアルカリから保護するためのシリカコートしたものを使用した。
<Preparation of substrate>
As a substrate, a soda-lime glass plate having a thickness of 1.1 mm and 30 mm × 30 mm was prepared. The entire surface of the soda-lime glass plate was silica-coated to protect from acid and alkali.

<第一電極の形成>
準備した基板に、ITOをスパッタリング蒸着法で、ガラス板全面に厚さ150nmで製膜した後、パターニングを行い縦縞状のITOからなる第一電極を形成した。
<Formation of the first electrode>
On the prepared substrate, ITO was deposited on the entire surface of the glass plate with a thickness of 150 nm by a sputtering vapor deposition method, and then patterned to form a first electrode made of vertically striped ITO.

パターニング処理
ITO膜の上にレジストを全面に塗り、プリベーク後、所定のパターンに露光現象を行い、現象後、ポストベークを行った後、塩化第2鉄溶液に浸漬して、エッチングを行ってITO膜をパターニングし、ガラス板上に縦縞状のITOからなる第一電極を形成した。エッチング終了後、レジスト剥離を行う。形成した第一電極は、幅2.0mm、間隔1.0mm、3本とした。
A resist is applied on the entire surface of the patterned ITO film. After pre-baking, a predetermined pattern is exposed to light, and after the phenomenon, post-baking is performed, followed by immersion in a ferric chloride solution and etching. The film was patterned to form a first electrode made of vertically striped ITO on a glass plate. After the etching is completed, the resist is removed. The formed first electrodes had a width of 2.0 mm, an interval of 1.0 mm, and three.

<第一電極形成基板の洗浄>
第一電極を形成した基板を乾式洗浄し、基板電極表面における水の接触角を変えた基板を作製しNo.1−1〜1−12とした。
<Cleaning the first electrode forming substrate>
The substrate on which the first electrode was formed was dry-cleaned to produce a substrate in which the contact angle of water on the surface of the substrate electrode was changed. 1-1 to 1-12.

乾式洗浄
200W低圧水銀ランプ(セン特殊光源(株)製)を用い、紫外線オゾン洗浄を行った。表1に示す様に照射距離と照射時間を調整することで、基板電極表面における水の接触角を変えた第一電極形成基板を準備しNo.1−1〜1−12とした。尚、前記基板電極表面における水の接触角は、別途サンプル基板で洗浄及び測定を行い洗浄条件を定め、その条件で洗浄を行った。
Ultraviolet ozone cleaning was performed using a dry cleaning 200 W low pressure mercury lamp (manufactured by Sen Special Light Source Co., Ltd.). As shown in Table 1, by adjusting the irradiation distance and irradiation time, a first electrode forming substrate was prepared by changing the contact angle of water on the substrate electrode surface. 1-1 to 1-12. In addition, the contact angle of water on the surface of the substrate electrode was separately cleaned and measured with a sample substrate to determine cleaning conditions, and cleaning was performed under those conditions.

また、水の接触角の測定は、JIS R 3257規格の試験法に基づき、接触角計(協和界面科学(株)製DropMaster700)で行った。   The contact angle of water was measured with a contact angle meter (DropMaster 700 manufactured by Kyowa Interface Science Co., Ltd.) based on the test method of JIS R 3257 standard.

Figure 0005168762
Figure 0005168762

乾式洗浄を行った各第一電極形成基板No.1−1〜1−12を、湿式洗浄した。この後、乾燥処理を行い、再度乾式洗浄を行った。   Each of the first electrode forming substrates No. 1 subjected to the dry cleaning. 1-1 to 1-12 were wet cleaned. Thereafter, drying treatment was performed, and dry cleaning was performed again.

湿式洗浄
流水式高周波超音波洗浄機(本多電子(株)製W−357−P25)を用い、流水式シャワー洗浄により洗浄を行った。発振周波数は1MHz、高周波出力は60W、水量1.5リットル/分とし、電極表面に5分間吹きつけた。洗浄に用いた溶媒は、超純水とした。
Wet cleaning Using a flowing water type high frequency ultrasonic cleaning machine (W-357-P25 manufactured by Honda Electronics Co., Ltd.), cleaning was performed by flowing water type shower cleaning. The oscillation frequency was 1 MHz, the high frequency output was 60 W, the amount of water was 1.5 liters / minute, and the electrode surface was sprayed for 5 minutes. The solvent used for washing was ultrapure water.

乾燥処理
湿式洗浄後の基板を回転テーブル上に保持し、回転数3000r/min、回転時間30秒にてスピン乾燥を行った。
Drying treatment The substrate after wet cleaning was held on a rotary table, and spin drying was performed at a rotation speed of 3000 r / min and a rotation time of 30 seconds.

乾式洗浄
乾燥処理後の基板を200W低圧水銀ランプ(セン特殊光源(株)製)を用い、照射距離10mm、照射時間60秒にて紫外線オゾン洗浄を行った。
Dry cleaning The substrate after the drying treatment was subjected to ultraviolet ozone cleaning using a 200 W low-pressure mercury lamp (manufactured by Sen Special Light Source Co., Ltd.) at an irradiation distance of 10 mm and an irradiation time of 60 seconds.

<有機EL素子の作製>
洗浄を行った各第一電極形成基板No.1−1〜1−12上に、以下に示す方法で正孔輸送層、発光層、電子注入層、第二電極、封止膜を順次形成し有機EL素子を作製し試料NO.101〜112とした。
<Production of organic EL element>
Each cleaned first electrode forming substrate No. A hole transport layer, a light emitting layer, an electron injection layer, a second electrode, and a sealing film are sequentially formed on the 1-1 to 1-12 by the method described below to produce an organic EL element, and sample NO. 101-112.

<正孔輸送層の形成>
第一電極形成基板を真空蒸着機にセットし、真空槽内を1×10-4Paまで排気後、N,N’−ジフェニル−N,N’−m−トリル4,4’−ジアミノ−1,1’−ビフェニル(以下、TPD)を蒸着速度0.3nm/秒で厚さ50nmに真空蒸着し、正孔輸送層を形成した。
<Formation of hole transport layer>
The first electrode forming substrate is set in a vacuum vapor deposition machine, the inside of the vacuum chamber is evacuated to 1 × 10 −4 Pa, and then N, N′-diphenyl-N, N′-m-tolyl 4,4′-diamino-1 1,1′-biphenyl (hereinafter, TPD) was vacuum-deposited to a thickness of 50 nm at a deposition rate of 0.3 nm / second to form a hole transport layer.

<発光層の形成>
正孔輸送層を形成した基板を真空蒸着機にセットし、真空槽内を1×10-4Paまで排気後、発光材料としてAlq3を使用し、蒸着速度0.3nm/秒で厚さ50nmに真空蒸着した。
<Formation of light emitting layer>
The substrate on which the hole transport layer is formed is set in a vacuum vapor deposition machine, the inside of the vacuum chamber is evacuated to 1 × 10 −4 Pa, Alq 3 is used as a light emitting material, and the thickness is 50 nm at a vapor deposition rate of 0.3 nm / second. Was vacuum evaporated.

<電子注入層の形成>
発光層を形成した基板を真空蒸着機にセットし、真空槽内を1×10-4Paまで排気後、電子注入層材料としてLiFを使用し、蒸着速度0.03nm/秒で厚さ1nmに真空蒸着した。
<Formation of electron injection layer>
The substrate on which the light emitting layer is formed is set in a vacuum vapor deposition machine, the inside of the vacuum chamber is evacuated to 1 × 10 −4 Pa, LiF is used as an electron injection layer material, and the thickness is 1 nm at a vapor deposition rate of 0.03 nm / second. Vacuum deposited.

<第二電極の形成>
電子注入層を形成した基板を真空蒸着機にセットし、真空槽内を1×10-4Paまで排気後、第二電極材料としてAlを使用し、電子注入層の上に第一電極と直行する方向に、第一電極が形成された領域に、蒸着速度0.3nm/秒で100nmの厚さに真空蒸着し、幅2.0mm、間隔1.0mm、3本の第二電極を形成した。
<Formation of second electrode>
The substrate on which the electron injection layer is formed is set in a vacuum vapor deposition machine, the inside of the vacuum chamber is evacuated to 1 × 10 −4 Pa, Al is used as the second electrode material, and the first electrode is placed directly on the electron injection layer. In the direction where the first electrode was formed, vacuum deposition was performed to a thickness of 100 nm at a deposition rate of 0.3 nm / second to form a width of 2.0 mm, a spacing of 1.0 mm, and three second electrodes. .

<封止膜の形成>
第二電極を形成した基板を真空蒸着機にセットし、1×10-4Paまで排気後、封止膜材料としてSiOxを使用し、第一電極、第二電極の接続端子となる領域以外にスパッタリング法により、成膜速度0.3nm/秒で300nmの厚さに成膜し封止膜を形成した。
<Formation of sealing film>
The substrate on which the second electrode is formed is set in a vacuum vapor deposition machine, evacuated to 1 × 10 −4 Pa, and then SiOx is used as a sealing film material, except for the region that becomes the connection terminal of the first electrode and the second electrode. A sealing film was formed by sputtering to a thickness of 300 nm at a deposition rate of 0.3 nm / second.

(評価)
作製した各試料No.101〜112に付き、リーク電流特性を以下に示す試験方法により試験し、以下に示す評価ランクに従って評価した結果を表2に示す。
(Evaluation)
Each prepared sample No. Table 2 shows the results of the leak current characteristics tested by the test method shown below and evaluated according to the evaluation rank shown below.

リーク電流特性の試験方法
定電圧電源を用いて、逆方向の電圧(逆バイアス)を5Vを5秒間印加し、その時素子に流れる電流を測定した。9ドット(発光領域)全てにおいて測定を行い、最大電流値をリーク電流とした。
リーク電流の評価ランク
◎:1×10-8A未満
○:1×10-8A以上、1×10-6A未満
△:1×10-6A以上、1×10-4A未満
×:1×10-4A以上
Test Method for Leakage Current Characteristics Using a constant voltage power source, a reverse voltage (reverse bias) was applied at 5 V for 5 seconds, and the current flowing through the device at that time was measured. Measurement was performed for all 9 dots (light emitting region), and the maximum current value was defined as a leakage current.
Evaluation rank of leakage current ◎: Less than 1 × 10 −8 A ○: 1 × 10 −8 A or more, less than 1 × 10 −6 A △: 1 × 10 −6 A or more, less than 1 × 10 −4 A ×: 1 × 10 -4 A or more

Figure 0005168762
Figure 0005168762

本発明の有効性が確認された。   The effectiveness of the present invention was confirmed.

乾式洗浄と湿式洗浄を組み合わせた洗浄工程の模式図である。It is a schematic diagram of the cleaning process combining dry cleaning and wet cleaning. 枚葉シート状基板の紫外線オゾン乾式洗浄の模式図である。It is a schematic diagram of ultraviolet ozone dry cleaning of a single wafer sheet-like substrate. 流水式超音波シャワー湿式洗浄の模式図である。It is a schematic diagram of flowing water type ultrasonic shower wet cleaning. 連続シート状基板をロールツーロール方式で洗浄を行い、同一のウェブ搬送ラインで有機層の成膜を行う工程の模式図である。It is a schematic diagram of the process which cleans a continuous sheet-like board | substrate by a roll-to-roll system, and forms the organic layer into a film by the same web conveyance line. パッシブマトリックスのフルカラー有機EL素子の層構成を示す模式図である。It is a schematic diagram which shows the layer structure of the full color organic EL element of a passive matrix.

符号の説明Explanation of symbols

1 基板
1A 連続シート状基板
21、24 乾式洗浄装置
22、22A、22B 湿式洗浄装置
211 低圧水銀ランプ光源
221 洗浄槽
222 シャワーノズル
223 超音波発生装置
224 溶媒貯水容器
225 フィルター
23 乾燥装置
3 有機層成膜装置
51 粒子数測定手段(LPC)
52 分析部
53 演算部
54 制御部
C1 コンベア
B1 溶媒
P1 供給ポンプ
P2 循環ポンプ
DESCRIPTION OF SYMBOLS 1 Substrate 1A Continuous sheet-like substrate 21, 24 Dry cleaning device 22, 22A, 22B Wet cleaning device 211 Low-pressure mercury lamp light source 221 Cleaning tank 222 Shower nozzle 223 Ultrasonic generator 224 Solvent storage container 225 Filter 23 Drying device 3 Organic layer formation Membrane device 51 Particle number measuring means (LPC)
52 Analysis Unit 53 Calculation Unit 54 Control Unit C1 Conveyor B1 Solvent P1 Supply Pump P2 Circulation Pump

Claims (6)

基板上に少なくとも第一電極と有機物質からなる一層以上の発光層と第二電極を成膜してなる有機エレクトロルミネッセンス素子の製造方法において、
前記基板上に第一電極が成膜してなる基板の前記第一電極を洗浄する乾式洗浄と湿式洗浄からなる洗浄工程を具備するとともに、前記洗浄工程は前記乾式洗浄工程、前記湿式洗浄工程及び前記乾式洗浄工程をこの順に連続して行い、前記湿式洗浄に使用する溶媒が超純水であることを特徴とする有機エレクトロルミネッセンス素子の製造方法。
In the method for producing an organic electroluminescent element, wherein at least a first electrode and a light emitting layer composed of an organic substance and a second electrode are formed on a substrate.
A cleaning process comprising a dry cleaning process and a wet cleaning process for cleaning the first electrode of a substrate formed by forming a first electrode on the substrate; and the cleaning process includes the dry cleaning process, the wet cleaning process, and the dry cleaning process the have rows successively in this order, the method of manufacturing the organic electroluminescent device solvent used for the wet cleaning, characterized in that ultrapure water.
前記乾式洗浄で基板電極表面における水の接触角を45°以下とし、前記湿式洗浄を行うことを特徴とする請求項1に記載の有機エレクトロルミネッセンス素子の製造方法。 The method for producing an organic electroluminescent element according to claim 1, wherein the wet cleaning is performed by setting the contact angle of water on the surface of the substrate electrode to 45 ° or less in the dry cleaning. 前記乾式洗浄の方法は、紫外線オゾン洗浄、プラズマ洗浄の少なくとも何れか1つであることを特徴とする請求項1または2に記載の有機エレクトロルミネッセンス素子の製造方法。   3. The method of manufacturing an organic electroluminescence element according to claim 1, wherein the dry cleaning method is at least one of ultraviolet ozone cleaning and plasma cleaning. 前記湿式洗浄の方法は、洗浄浴槽浸漬、超音波洗浄浴槽浸漬、流水式洗浄浴槽浸漬、流水式超音波洗浄浴槽浸漬、流水式シャワー及び流水式超音波シャワー方式の少なくとも何れか1つであることを特徴とする請求項1乃至3の何れか1項に記載の有機エレクトロルミネッセンス素子の製造方法。   The wet cleaning method is at least one of cleaning bath immersion, ultrasonic cleaning bath immersion, flowing water cleaning bath immersion, flowing water ultrasonic cleaning bath immersion, flowing water shower, and flowing water ultrasonic shower method. The manufacturing method of the organic electroluminescent element of any one of Claims 1 thru | or 3 characterized by these. 前記洗浄工程は、連続シート状基板をロールツーロール方式でウェブ搬送しながら前記連続シート状基板を洗浄することを特徴とする請求項1乃至の何れか1項に記載の有機エレクトロルミネッセンス素子の製造方法。 The washing step, the organic electroluminescent device according to any one of claims 1 to 4, characterized in that washing the continuous sheet-like substrate while web transport the continuous sheet-like substrate in a roll-to-roll method Production method. 前記洗浄工程と同一のウェブ搬送ライン上に有機層成膜工程とを具備するとともに、前記洗浄工程で洗浄した後、同一のウェブ搬送ラインで連続シート状基板電極上に少なくとも1層以上の有機層を成膜することを特徴とする請求項に記載の有機エレクトロルミネッセンス素子の製造方法。 An organic layer film forming step on the same web conveyance line as the washing step, and after washing in the washing step, at least one organic layer on the continuous sheet-like substrate electrode in the same web conveyance line The method of manufacturing an organic electroluminescence element according to claim 5 , wherein the film is formed.
JP2005222683A 2005-08-01 2005-08-01 Method for manufacturing organic electroluminescence element Expired - Fee Related JP5168762B2 (en)