JP5045780B2 - Method of manufacturing cutting blade member of cutting tool and press molding die of green compact used in the manufacturing method - Google Patents

Method of manufacturing cutting blade member of cutting tool and press molding die of green compact used in the manufacturing method Download PDF

Info

Publication number
JP5045780B2
JP5045780B2 JP2010101486A JP2010101486A JP5045780B2 JP 5045780 B2 JP5045780 B2 JP 5045780B2 JP 2010101486 A JP2010101486 A JP 2010101486A JP 2010101486 A JP2010101486 A JP 2010101486A JP 5045780 B2 JP5045780 B2 JP 5045780B2
Authority
JP
Japan
Prior art keywords
die
green compact
punch
main
press
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Lifetime
Application number
JP2010101486A
Other languages
Japanese (ja)
Other versions
JP2010158723A (en
Inventor
義一 岡田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Mitsubishi Materials Corp
Original Assignee
Mitsubishi Materials Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Mitsubishi Materials Corp filed Critical Mitsubishi Materials Corp
Priority to JP2010101486A priority Critical patent/JP5045780B2/en
Publication of JP2010158723A publication Critical patent/JP2010158723A/en
Application granted granted Critical
Publication of JP5045780B2 publication Critical patent/JP5045780B2/en
Anticipated expiration legal-status Critical
Expired - Lifetime legal-status Critical Current

Description

本発明は、切刃を備えて切削工具の本体に着脱可能に装着されるスローアウェイチップのような切削工具の切刃部材の製造方法、およびこのような切刃部材を、その原料粉末を圧縮した圧粉体から製造する場合の該製造方法に用いられる圧粉体のプレス成形金型に関するものである。   The present invention relates to a method for manufacturing a cutting blade member of a cutting tool such as a throw-away tip that is provided with a cutting blade and is detachably attached to the main body of the cutting tool, and compresses the raw material powder of such a cutting blade member. The present invention relates to a green compact press-molding die used in the manufacturing method in the case of manufacturing from a green compact.

このような切削工具の切刃部材の製造方法としては、例えば特許文献1に上記スローアウェイチップの製造方法として、図24に示すような方形平板状のチップ本体1を備えて、その方形をなす平板面2の周囲に配置される4つの周面のうち、互いに反対側に位置する一対の周面がすくい面3とされ、このすくい面3と逃げ面とされる上記平板面2との交差稜線が切刃4とされた所謂縦刃式のスローアウェイチップの製造方法が提案されている。すなわち、この特許文献1記載の製造方法では、チップ本体1の厚さ方向(図24において上下方向)に対応する方向に垂直な方向に互いに対向して離接(上下動)する上下のパンチと、上下動して接近したこれら上下パンチの周囲を取り囲むように配設されて該上下パンチとの間にキャビティーを画成するダイとを備えたプレス成形金型を用いて、上記キャビティー内に投入した超硬合金等のスローアウェイチップの原料粉末を、上下パンチによって圧縮して圧粉体をプレス成形するようにしている。   As a manufacturing method of the cutting blade member of such a cutting tool, for example, as a manufacturing method of the above throwaway tip in Patent Document 1, a rectangular flat plate-shaped chip body 1 as shown in FIG. Of the four peripheral surfaces arranged around the flat plate surface 2, a pair of peripheral surfaces positioned on the opposite sides is a rake surface 3, and the rake surface 3 intersects the flat plate surface 2 as a flank surface. A so-called vertical blade type throw-away tip manufacturing method in which the ridge line is the cutting edge 4 has been proposed. That is, in the manufacturing method described in Patent Document 1, the upper and lower punches that face each other in the direction perpendicular to the direction corresponding to the thickness direction (vertical direction in FIG. Using a press molding die provided with a die which is arranged so as to surround the upper and lower punches which are moved up and down and which surrounds the upper and lower punches to define a cavity between the upper and lower punches. The raw powder of the throw-away tip such as cemented carbide introduced in is compressed by upper and lower punches, and the green compact is press-molded.

なお、上記スローアウェイチップにおいては、そのチップ本体1の上記周面のうちすくい面3に隣接する残りの一対の他の周面5と該すくい面3との交差稜線も切刃6として使用されることがあり、この場合にはこの他の周面5は該切刃6の逃げ面とされるとともに、上記切刃4と切刃6が形成された交差稜線同士が交差するすくい面3の角部には、これらの切刃4,6に滑らかに連なる1/4凸円弧状のコーナ部7が形成され、これに伴い切刃6の逃げ面となる上記他の周面5と上記平板面2との交差稜線部は断面1/4凸円弧等の凸曲面状のコーナ稜線部8とされる。また、この特許文献1に記載されたスローアウェイチップは、上記すくい面3と逃げ面とされる平板面2および他の周面5が切刃4,6を介して直交する方向に配設されたネガティブタイプとされ、しかも上記すくい面3にチップブレーカ9が形成されたブレーカ付きのスローアウェイチップとされている。さらに、この特許文献1では、上記キャビティー内にダイからピンを上記厚さ方向に対応する方向に出没可能に設けて、スローアウェイチップの工具本体への取り付けの際にクランプネジ等が挿入される取付穴10となる貫通孔を圧粉体に形成するようにしている。   In the throw-away tip, the crossed ridge line between the other peripheral surface 5 adjacent to the rake face 3 of the peripheral surface of the tip body 1 and the rake face 3 is also used as the cutting edge 6. In this case, the other peripheral surface 5 is used as a flank of the cutting edge 6, and the rake face 3 where the intersecting ridgelines where the cutting edge 4 and the cutting edge 6 are formed intersect each other is formed. In the corner portion, a 1/4 convex arc-shaped corner portion 7 smoothly connected to the cutting edges 4 and 6 is formed, and accordingly, the other peripheral surface 5 and the flat plate serving as a flank of the cutting edge 6. The intersecting ridge line portion with the surface 2 is a corner ridge line portion 8 having a convex curved surface shape such as a quarter convex arc. In addition, the throw-away tip described in Patent Document 1 is arranged in a direction in which the rake face 3 and the flat plate surface 2 and the other peripheral surface 5 serving as the flank face are orthogonal to each other via the cutting edges 4 and 6. Further, it is a throw-away tip with a breaker in which a chip breaker 9 is formed on the rake face 3. Further, in Patent Document 1, a pin is provided in the cavity so as to be able to protrude and retract in a direction corresponding to the thickness direction, and a clamp screw or the like is inserted when the throw-away tip is attached to the tool body. A through hole to be the mounting hole 10 is formed in the green compact.

特開平10−146695号公報Japanese Patent Laid-Open No. 10-146695

ところが、上記特許文献1に記載のように、縦刃式スローアウェイチップに形成される圧粉体を、チップ本体1の厚さ方向に対応する方向に垂直な方向に互いに対向して上下動する上下パンチによって圧縮してプレス成形すると、この圧縮される方向の圧粉体の寸法が圧粉体の厚さ寸法よりも大きくなるため、原料粉末を均一に圧縮するのが困難となるおそれがあった。特に、この特許文献1記載の製造方法およびプレス成形金型では、チップ本体1をその厚さ方向に貫通する取付穴10を形成するため、上述のようにこの厚さ方向に対応する方向、すなわち上下パンチによる圧縮方向に垂直な方向にピンをキャビティー内に出没可能に設けており、原料粉末の圧縮時にはこのピンの周りで原料粉末の圧縮比が僅かながら変化してしまうので、焼結後に製造されたスローアウェイチップにおいてもその取付穴10の周囲で微小な凹凸等の変形が生じたり、取付穴10の穴形状自体が楕円になったりするおそれもある。   However, as described in Patent Document 1, the green compact formed on the vertical blade type throw-away tip moves up and down facing each other in a direction perpendicular to the direction corresponding to the thickness direction of the tip body 1. If the upper and lower punches are used for press molding, the size of the green compact in the direction of compression becomes larger than the thickness of the green compact, which may make it difficult to uniformly compress the raw material powder. It was. In particular, in the manufacturing method and press-molding die described in Patent Document 1, the mounting hole 10 that penetrates the chip body 1 in the thickness direction is formed, so that the direction corresponding to the thickness direction as described above, that is, A pin is provided in the cavity in a direction perpendicular to the compression direction by the upper and lower punches, and when the raw material powder is compressed, the compression ratio of the raw material powder changes slightly around this pin. Even in the manufactured throw-away tip, there is a possibility that deformation such as minute irregularities may occur around the mounting hole 10 or the hole shape itself of the mounting hole 10 may become an ellipse.

また、例えば溝入れ用の縦刃式スローアウェイチップのように、略三角形や四角形あるいはそれ以上の多角形平板状のチップ本体において、三面や四面あるいはそれ以上の周面がすくい面とされる場合には、こうしてチップ本体の厚さ方向に対応する方向に垂直な方向に原料粉末を圧縮して圧粉体をプレス成形することは甚だ困難であり、概ね外形を合わせてプレス成形した圧粉体を焼結した後にすくい面等を砥石によって所望の形状に研削加工したり、あるいは射出成形法によって焼結素材を成形したりしなければならない。しかしながら、前者の場合には研削加工に多大な時間と労力とを要し、また後者の場合には焼結素材中に原料粉末とともに含有されるバインダーにより、製造後のスローアウェイチップにおいて高い形状、寸法精度を得ることができなくなるおそれがある。   In addition, in the case of a substantially triangular, quadrilateral or more polygonal flat plate-like chip body such as a vertical blade type throwaway tip for grooving, the peripheral surface of three, four or more is a rake face. Therefore, it is extremely difficult to press-mold the green compact by compressing the raw material powder in a direction perpendicular to the direction corresponding to the thickness direction of the chip body. After sintering, the rake face or the like must be ground into a desired shape with a grindstone, or a sintered material must be molded by an injection molding method. However, in the former case, it takes a lot of time and labor for grinding, and in the latter case, the binder contained together with the raw material powder in the sintered material, a high shape in the throw-away tip after production, There is a possibility that dimensional accuracy cannot be obtained.

また、上記縦刃式のスローアウェイチップに限らず、切削工具に用いられる切刃部材としては近年より複雑な形状のものが使用されるようになってきており、そのような切刃部材は上記射出成形法によって成形された焼結素材からしか製造できないものとされていたが、かかる射出成形法では上述のように高い形状、寸法精度の切刃部材を製造することが困難であるとともに、射出成形金型や成形装置が高コストとなることから、プレス成形金型による圧粉体のプレス成形によってこのような切刃部材を製造することが求められるようになってきている。 Further, not only the above-mentioned vertical blade type throw-away tip, but also a cutting blade member used in a cutting tool has been used in more complex shapes in recent years, such a cutting blade member Although it was supposed that it could only be manufactured from a sintered material molded by the injection molding method, it is difficult to manufacture a cutting blade member with a high shape and dimensional accuracy as described above, and injection Due to the high cost of a molding die and a molding apparatus, it has been required to manufacture such a cutting blade member by press molding of a green compact with a press molding die.

本発明は、このような背景の下になされたもので、上述のような縦刃式のスローアウェイチップは勿論のこと、より複雑な形状の切削工具の切刃部材でも、原料粉末のプレス成形による圧粉体から極めて高精度に製造することが可能な切削工具の切刃部材の製造方法を提供し、またかかる製造方法に用いて好適な圧粉体のプレス成形金型を提供することを目的としている。   The present invention has been made under such a background. In addition to the above-described vertical blade type throw-away tip, the present invention is capable of press forming raw material powder even with a cutting blade member of a cutting tool having a more complicated shape. The present invention provides a method for manufacturing a cutting blade member of a cutting tool that can be manufactured with extremely high accuracy from a green compact produced by the above-mentioned method, and provides a green compact press mold suitable for use in such a manufacturing method. It is aimed.

上記課題を解決して、このような目的を達成するために、本発明の切削工具の切刃部材の製造方法は、互いに対向して相対的に離接させられる複数の主パンチと、接近したこれら主パンチの周囲を取り囲むように配設されるダイとを備えたプレス成形金型を用いて、このプレス成形金型に投入した原料粉末を圧縮することにより、切削工具の切刃部材に製造される圧粉体をプレス成形する切削工具の切刃部材の製造方法であって、上記ダイに、上記プレス成形金型のキャビティーを間にして分割されて離接可能とされる分割ダイと、上記キャビティーに対して固定された分割固定ダイとを備え、一体化された上記分割ダイと上記分割固定ダイとによって上記ダイを構成して上記圧粉体をプレス成形し、上記分割ダイを分割して該圧粉体を取り出すことを特徴とする。また、本発明の圧粉体のプレス成形金型は、このような切削工具の切刃部材の製造方法に用いられる圧粉体のプレス成形金型であって、互いに対向して相対的に離接させられる複数の主パンチと、接近したこれら主パンチの周囲を取り囲むように配設されるダイとを備え、このダイは、上記プレス成形金型のキャビティーを間にして分割されて離接可能とされる分割ダイと、上記キャビティーに対して固定された分割固定ダイとを備えていることを特徴とする。 In order to solve the above-described problems and achieve such an object, a method for manufacturing a cutting blade member of a cutting tool according to the present invention is close to a plurality of main punches that are opposed to each other and relatively separated from each other. Manufactured into a cutting blade member of a cutting tool by compressing the raw material powder put into this press molding die using a press molding die provided with a die arranged so as to surround the periphery of these main punches A method of manufacturing a cutting blade member of a cutting tool for press-molding a green compact to be formed, wherein the die is divided with a cavity of the press-molding die in between, and can be separated and contacted A split fixing die fixed to the cavity, the die is constituted by the integrated split die and the split fixing die, and the green compact is press-molded. Divide and remove the green compact And wherein the nest. The green compact press-molding die of the present invention is a green compact press-molding die used in such a method of manufacturing a cutting blade member of a cutting tool, and is relatively opposed to each other. A plurality of main punches to be brought into contact with each other, and a die arranged so as to surround the adjacent main punches, and the die is divided with the cavity of the press molding die in between and separated It is characterized by comprising a split die that can be made and a split fixed die fixed to the cavity .

このような切削工具の切刃部材の製造方法および該製造方法に用いられる圧粉体のプレス成形金型では例えば上記切刃部材が、略平板状を呈するチップ本体を有して、該チップ本体の厚さ方向を向く平板面とこの平板面の周りに配置される周面とを備え、この周面に形成されたすくい面と上記平板面との交差稜線と、このすくい面に隣接する他の周面と該すくい面との交差稜線との少なくとも一方に切刃が形成された上述のような縦刃式のスローアウェイチップである場合には、上記主パンチを上記厚さ方向に対応する方向に離接させて、上記圧粉体において上記チップ本体の平板面に対応する面の少なくとも一部を成形することにより、寸法の小さい上記厚さ方向に対応する方向に原料粉末が圧縮されて圧粉体がプレス成形されるのでこの主パンチの離接方向について原料粉末の圧縮の均一化を図ることができるとともに、様々な平面視形状のスローアウェイチップを製造可能となる。また、プレス成形金型において、主パンチに、この主パンチの離接方向に上記キャビティー内に出没可能なピンを備えることにより、チップ本体をその厚さ方向に貫通する取付穴を形成することができ、この場合でも原料粉末はピンの突出する方向に圧縮されるので、ピンの周辺における圧縮比の変化を抑えることができる。 In such a manufacturing method of a cutting blade member of a cutting tool and a press mold of a green compact used in the manufacturing method , for example, the cutting blade member has a chip body having a substantially flat plate shape, and the chip A flat plate surface facing the thickness direction of the main body and a peripheral surface arranged around the flat plate surface, and a ridge line between the rake surface formed on the peripheral surface and the flat plate surface, and adjacent to the rake surface. In the case of the above-described vertical blade type throw-away tip in which a cutting edge is formed on at least one of the other peripheral surface and the crossing ridge line of the rake face, the main punch corresponds to the thickness direction. The raw material powder is compressed in the direction corresponding to the small thickness direction by forming at least part of the surface corresponding to the flat plate surface of the chip body in the green compact. since the green compact Te is press-molded, The disjunction direction of the main punch it is possible to achieve uniform raw material powder compression, enables production of throw-away tip of different shape in plan view. Further, in the press molding die, a mounting hole penetrating the chip body in the thickness direction is formed by providing the main punch with a pin that can be projected and retracted in the cavity in the direction of separation of the main punch. Even in this case, since the raw material powder is compressed in the protruding direction of the pin, the change in the compression ratio around the pin can be suppressed.

また、ダイを、上記キャビティーを間にして分割される分割ダイを備えて離接可能とすることにより、プレス成形された圧粉体を容易に取り出すことが可能となる。ただし、この場合ダイの設計の容易さを考慮すると、この分割ダイは、上記主パンチの離接方向と平行な方向、または該主パンチの離接方向に垂直な方向に離接可能とされるのが望ましい。 Further, by providing the die with a split die that is split with the cavity in between, the pressed compact can be easily taken out. However, in this case , considering the ease of die design, this split die can be detached / attached in a direction parallel to the main punch separation / contact direction or a direction perpendicular to the main punch separation / contact direction. Is desirable.

本発明のプレス成形金型の第1の参考例を示す主パンチ11,12の離接方向と副パンチ15の離接方向とに沿った断面図である。FIG. 3 is a cross-sectional view of the first reference example of the press-molding die of the present invention along the separation / contact direction of the main punches 11 and 12 and the separation / contact direction of the sub punch 15. 図1に示す参考例において主パンチ11,12の離接方向に沿って副パンチ15の離接方向に直交する断面図である。FIG. 2 is a cross-sectional view orthogonal to the direction of contact of the sub punch 15 along the direction of contact of the main punches 11 and 12 in the reference example shown in FIG. 1. 図2における鎖線A部分の拡大図であって、(a)〜(c)は参考例、(d)は凹部16をダイ13側に設けなかった場合の例である。It is an enlarged view of the chain line A part in FIG. 2, (a)-(c) is a reference example , (d) is an example when the recessed part 16 is not provided in the die | dye 13 side. 第1の参考例のプレス成形金型を用いた製造方法によって製造される縦刃式スローアウェイチップの斜視図である。It is a perspective view of the vertical blade type throwaway tip manufactured by the manufacturing method using the press molding die of the 1st reference example . 図1に示す参考例のプレス成形金型によって圧粉体をプレス成形して切刃部材を製造する場合の本発明の製造方法の第1の参考例を示す図である。It is a figure which shows the 1st reference example of the manufacturing method of this invention in the case of manufacturing a cutting blade member by press-molding green compact with the press molding die of the reference example shown in FIG. 第1の参考例のプレス成形金型の変形例を示す主パンチ11,12の離接方向と副パンチ15の離接方向とに沿った断面図である。FIG. 5 is a cross-sectional view taken along the direction of separation of the main punches 11 and 12 and the direction of separation of the sub-punch 15 showing a modification of the press mold of the first reference example . 図6に示す変形例において主パンチ11,12の離接方向に沿って副パンチ15の離接方向に直交する断面図である。7 is a cross-sectional view orthogonal to the direction of contact of the sub punch 15 along the direction of contact of the main punches 11 and 12 in the modification shown in FIG. 図6に示す変形例により製造される縦刃式スローアウェイチップの(a)は切刃4,6またはコーナ部7に直交する断面図、(b)は取付穴10の断面図である。6A is a cross-sectional view orthogonal to the cutting blades 4 and 6 or the corner portion 7, and FIG. 6B is a cross-sectional view of the mounting hole 10. 第1の参考例のプレス成形金型の他の変形例を示す主パンチ11,12の離接方向と副パンチ15の離接方向とに沿った断面図である。It is sectional drawing along the separation / contact direction of the main punches 11 and 12 and the separation / contact direction of the subpunch 15 which show the other modification of the press molding die of a 1st reference example . 第1の参考例のプレス成形金型の変形例を示す、(a)は主パンチ11,12の離接方向と副パンチ15の離接方向とに沿った断面図、(b)は(a)におけるZZ断面図の一例、(c)は(a)におけるZZ断面図の他の例である。A modification of the press-molding die of the first reference example is shown, (a) is a sectional view along the direction of separation of the main punches 11 and 12 and the direction of separation of the sub-punch 15, and (b) is (a) ) Is an example of a ZZ cross-sectional view in (), and (c) is another example of a ZZ cross-sectional view in (a). 本発明のプレス成形金型の第2の参考例を示す主パンチ11,12の離接方向と副パンチ23の離接方向とに沿った断面図である。It is sectional drawing along the separation / contact direction of the main punches 11 and 12 and the separation / contact direction of the subpunch 23 which show the 2nd reference example of the press molding die of this invention. 図11に示す参考例において主パンチ11,12の離接方向に沿って副パンチ23の離接方向に直交する断面図である。12 is a cross-sectional view perpendicular to the direction of contact of the sub punch 23 along the direction of contact of the main punches 11 and 12 in the reference example shown in FIG. 図11における鎖線B部分の例を示す拡大図である。It is an enlarged view which shows the example of the dashed-dotted line B part in FIG. 第2の参考例のプレス成形金型の変形例、およびこの変形例のプレス成形金型によって圧粉体をプレス成形して切刃部材を製造する場合の本発明の製造方法の第2の参考例の変形例を示す、主パンチ11,12の離接方向と副パンチ23の離接方向とに沿った断面図である。Modification of the press-molding die of the second reference example, and a second reference for the manufacturing method of the present invention in the case of producing the cutting member by press-forming a green compact by press molding die of the modification It shows a modification of the embodiment, a cross-sectional view along the and disjunction direction disjunctive direction and sub punch 23 of the main punch 11 and 12. 図14(c)における鎖線C部分の例を示す拡大図である。It is an enlarged view which shows the example of the chain line C part in FIG.14 (c). 第2の参考例のプレス成形金型の他の変形例、およびこの他の変形例のプレス成形金型によって圧粉体をプレス成形して切刃部材を製造する場合の本発明の製造方法の第2の参考例の他の変形例を示す、主パンチ11,12の離接方向と副パンチ23の離接方向とに沿った断面図である。Another modification of the press-molding die of the second reference example , and the manufacturing method of the present invention in the case of producing a cutting blade member by press-molding a green compact with a press-molding die of another modification It is sectional drawing along the separation / contact direction of the main punches 11 and 12 and the separation / contact direction of the sub punch 23 which shows the other modification of a 2nd reference example . 図16(c)における鎖線D部分の例を示す拡大図である。It is an enlarged view which shows the example of the dashed-dotted line D part in FIG.16 (c). 本発明のプレス成形金型の実施形態を示す横断面図(図19におけるZZ断面図)である。FIG. 20 is a transverse sectional view (ZZ sectional view in FIG. 19) showing an embodiment of the press-molding die of the present invention. 図18におけるZZ断面図である。It is ZZ sectional drawing in FIG. 図18に示す実施形態のプレス成形金型を用いた製造方法によって製造される縦刃式スローアウェイチップの平面図である。 It is a top view of the vertical blade type throwaway tip manufactured by the manufacturing method using the press molding die of embodiment shown in FIG. 図20における矢線Y方向視の側面図である。It is a side view of the arrow line Y direction view in FIG. 図20に示した縦刃式スローアウェイチップの(a)すくい面3の拡大側面図、(b)切刃6周辺部分の拡大平面図、(c)他の周面5側から見た切刃6周辺部分の他の拡大側面図である。20A is an enlarged side view of the rake face 3, FIG. 20B is an enlarged plan view of a peripheral portion of the cutting edge 6, and FIG. 20C is a cutting edge viewed from the other peripheral face 5 side. FIG. 6 is another enlarged side view of the peripheral portion. 図20に示した縦刃式スローアウェイチップの取付穴10の拡大断面図である。It is an expanded sectional view of the attachment hole 10 of the vertical blade type | formula throwaway tip shown in FIG. チップブレーカ9付きの方形平板状の縦刃式スローアウェイチップを示す斜視図である。It is a perspective view showing a rectangular flat plate type vertical blade type throwaway tip with a tip breaker 9.

図1ないし図3は、本発明のプレス成形金型の実施形態を説明する上での第1の参考例を示すものであり、図4は、かかるプレス成形金型を用いた切削工具の切刃部材の製造方法により製造される切刃部材を示すものである。ここで、この切刃部材は、図24に示した縦刃式のスローアウェイチップと略同様の構成を有するものであって、略方形平板状のチップ本体1を有し、このチップ本体1の厚さ方向(図4において上下方向)を向いて方形をなす一対の平板面2と、この平板面2の周りに配置される4つの周面とを備えていて、上記一対の平板面2間の間隔、すなわちチップ本体1の厚さ方向の寸法が、上記4つの周面のうち互いに反対側に位置するもの同士の間隔、すなわちチップ本体1の幅寸法および長さ寸法よりも小さくされている。 FIGS. 1 to 3 show a first reference example for explaining an embodiment of a press molding die of the present invention. FIG. 4 shows a cutting tool cutting using the press molding die. The cutting blade member manufactured by the manufacturing method of a blade member is shown. Here, the cutting blade member has substantially the same configuration as the vertical blade type throw-away tip shown in FIG. 24, and has a substantially rectangular flat plate-shaped tip body 1. A pair of flat plate surfaces 2 that form a square shape in the thickness direction (vertical direction in FIG. 4) and four peripheral surfaces arranged around the flat plate surface 2 are provided. , That is, the dimension in the thickness direction of the chip body 1 is made smaller than the distance between the four peripheral surfaces located on opposite sides, that is, the width dimension and the length dimension of the chip body 1. .

さらに、これら4つの周面のうち、互いに反対側に位置する一対の周面(図4において左手前と右奥の周面)はすくい面3とされるとともに、このすくい面3と上記平板面2との交差稜線には切刃4が、また該すくい面3と残りの一対の他の周面(図4において左右の周面)5との交差稜線に切刃6がそれぞれ形成されていて、上記平板面2および他の周面5がそれぞれこれら切刃4,6に対する逃げ面とされている。また、切刃4,6が交差するコーナ部7は1/4凸円弧状とされ、これに伴い平板面2と他の周面5との交差稜線部も、すくい面3に平行な断面が1/4凸円弧をなす凸曲面状のコーナ稜線部8とされている。ただし、すくい面3は、図24のようなチップブレーカ9が形成されてはおらず、逃げ面とされる平板面2、他の周面5、およびコーナ稜線部8に直交する平坦面とされている。さらに、一対の平板面2の中央間にはチップ本体1を厚さ方向に貫通する取付穴10が形成されている。そして、このようなスローアウェイチップは、チップ本体1と同形で焼結の際の収縮代分だけ各寸法が大きくされた圧粉体を、超硬合金等の切刃部材の原料粉末から本参考例の上記プレス成形金型によってプレス成形して焼結することにより製造される。 Further, of these four peripheral surfaces, a pair of peripheral surfaces (peripheral surfaces on the left front side and the right rear side in FIG. 4) which are opposite to each other are used as a rake face 3, and the rake face 3 and the flat plate surface. The cutting edge 4 is formed on the intersecting ridge line with 2, and the cutting edge 6 is formed on the intersecting ridge line between the rake face 3 and the remaining pair of other peripheral surfaces (left and right peripheral surfaces in FIG. 4). The flat plate surface 2 and the other peripheral surface 5 are flank surfaces for the cutting edges 4 and 6, respectively. Further, the corner portion 7 where the cutting edges 4 and 6 intersect is formed in a ¼ convex arc shape, and accordingly, the intersecting ridge line portion between the flat plate surface 2 and the other peripheral surface 5 also has a cross section parallel to the rake face 3. The corner ridge line portion 8 has a convex curved surface forming a ¼ convex arc. However, the rake face 3 is not formed with the chip breaker 9 as shown in FIG. 24, and is a flat face perpendicular to the flat plate face 2, the other peripheral face 5, and the corner ridge line portion 8 as a flank face. Yes. Further, an attachment hole 10 that penetrates the chip body 1 in the thickness direction is formed between the centers of the pair of flat plate surfaces 2. Then, such throw-away tip, the shrinkage allowance only green compact dimensions is large during sintering in the tip body 1 and the same shape, this reference from the raw material powder of the cutting member of hard metal It is produced by sintering by press-forming by the press molding die example.

このような圧粉体をプレス成形して切刃部材としてのスローアウェイチップを製造するための本参考例のプレス成形金型は、図1および図2に示すように、互いに対向して図示されない駆動手段により相対的に離接させられる複数の主パンチ11,12と、接近したこれら主パンチ11,12の周囲を取り囲むように配設されるダイ13と、そしてこのダイ13に設けられて、接近した主パンチ11,12間に画成されるキャビティー14に向けて主パンチ11,12の離接方向とは異なる方向から離接させられる副パンチ15とを備えている。ここで、本参考例では主パンチ11,12は図示の通り上下方向に離接させられるように配設される一方、副パンチ15はこの主パンチ11,12の離接方向に垂直な方向、すなわち水平方向にキャビティー14に向けて離接させられる。また、本参考例では一対の副パンチ15が間にキャビティー14を挟むように一直線上に互いに対向して、このキャビティー14に向けて該直線に沿って離接するように配設させられている。 As shown in FIGS. 1 and 2, the press-molding dies of this reference example for producing a throw-away tip as a cutting blade member by press-molding such a green compact are not shown facing each other. A plurality of main punches 11 and 12 that are relatively separated from each other by the driving means, a die 13 disposed so as to surround the main punches 11 and 12 that are close to each other, and the die 13 are provided. A sub-punch 15 that is separated from a direction different from the direction in which the main punches 11 and 12 are separated from each other toward the cavity 14 defined between the adjacent main punches 11 and 12 is provided. Here, in this reference example , the main punches 11 and 12 are arranged so as to be separated from each other in the vertical direction as shown in the figure, while the sub punch 15 is in a direction perpendicular to the separation and contact direction of the main punches 11 and 12. That is, they are separated from each other toward the cavity 14 in the horizontal direction. In this reference example , the pair of sub-punches 15 are arranged so as to face each other in a straight line so as to sandwich the cavity 14 therebetween, and are arranged so as to be in contact with and separated from the cavity 14 along the straight line. Yes.

そして、主パンチ11,12が離接する上下方向は、プレス成形される圧粉体においてチップ本体1に焼結させられたときの上記厚さ方向に対応する方向とされており、これら主パンチ11,12が接近することにより、主パンチ11,12間に投入された上記原料粉末が該主パンチ11,12の互いに対向するプレス面11A,12Aによって押圧されて圧縮され、圧粉体においてチップ本体1の上記平板面2に対応する面が成形される。また、本参考例では上記一対の副パンチ15が離接する方向は、上記圧粉体においてチップ本体1のすくい面3が形成される周面に対応する面に対向する方向とされており、従ってこれら一対の副パンチ15がキャビティー14に向けて接近することにより、圧粉体において上記すくい面3に対応する面が成形される。従って、この副パンチ15のキャビティー14側を向くプレス面15Aは、圧粉体においてチップ本体1のすくい面3に対応する面と略等しい寸法形状とされ、すなわち横長の長方形の4隅のコーナ部が1/4凸円弧によって面取りされたような形状とされる。 The vertical direction in which the main punches 11 and 12 are separated from each other is the direction corresponding to the thickness direction when the chip body 1 is sintered in the green compact to be press-molded. , 12 approach, the raw material powder introduced between the main punches 11, 12 is pressed and compressed by the press surfaces 11A, 12A of the main punches 11, 12 facing each other, and the chip body in the green compact A surface corresponding to the flat plate surface 2 is formed. Further, in this reference example , the direction in which the pair of sub punches 15 are separated from each other is the direction facing the surface corresponding to the peripheral surface on which the rake face 3 of the chip body 1 is formed in the green compact. When the pair of sub-punches 15 approach toward the cavity 14, a surface corresponding to the rake surface 3 is formed in the green compact. Accordingly, the pressing surface 15A facing the cavity 14 side of the sub punch 15 has a shape substantially equal to the surface corresponding to the rake face 3 of the chip body 1 in the green compact, that is, the corners of the four corners of the horizontally long rectangle. The part is shaped to be chamfered by a 1/4 convex arc.

一方、圧粉体においてチップ本体1の上記他の周面5に対応する面側は、本参考例ではダイ13によって成形される。すなわち、図2に示すように上記ダイ13には、接近した主パンチ11,12間に画成されるキャビティー14に対して、該主パンチ11,12の離接方向と副パンチ15の離接方向とに垂直な方向(図2における左右方向。図1においては図面に直交する方向)に外側に向けて凹となる凹部16が形成されており、この凹部16のキャビティー14内側を向く底面16Aは主パンチ11,12の離接方向と副パンチ15の離接方向とに平行な平坦面とされていて、この底面16Aにより圧粉体においてチップ本体1の上記他の周面5に対応する面が成形される。また、上記主パンチ11,12の離接方向側における凹部16の両縁部には、底面16Aに滑らかに連なる断面凹円弧状をなしてキャビティー14の内側に延びる凹曲面状の壁面16Bがそれぞれ形成されており、プレス成形の際に主パンチ11,12が接近して位置決めされることによりキャビティー14が形成された時点で、これらの壁部16Bは主パンチ11,12の上記プレス面11A,12Aに滑らかに連なるようにされていて、圧粉体においてチップ本体1の上記コーナ稜線部8に対応する部分が成形される。 On the other hand, the surface side corresponding to the other peripheral surface 5 of the chip body 1 in the green compact is formed by the die 13 in this reference example . That is, as shown in FIG. 2, the die 13 has a cavity 14 defined between the adjacent main punches 11 and 12, and the separation direction of the main punches 11 and 12 and the separation of the sub punch 15. A recessed portion 16 that is recessed outward is formed in a direction perpendicular to the contact direction (the left-right direction in FIG. 2, the direction orthogonal to the drawing in FIG. 1), and faces the inside of the cavity 14 of the recessed portion 16. The bottom surface 16A is a flat surface parallel to the contact / separation direction of the main punches 11 and 12 and the contact / separation direction of the sub-punch 15, and the bottom surface 16A forms the green compact on the other peripheral surface 5 of the chip body 1. The corresponding surface is molded. Further, on both edges of the concave portion 16 on the side of the main punches 11 and 12 in the direction of separation, a concave curved wall surface 16B extending inwardly of the cavity 14 is formed in a concave arc shape that is smoothly connected to the bottom surface 16A. These wall portions 16B are formed on the press surfaces of the main punches 11 and 12 when the cavities 14 are formed when the main punches 11 and 12 are positioned close to each other during press molding. The portion corresponding to the corner ridgeline portion 8 of the chip body 1 is molded in the green compact.

ここで、この壁面16Bは、図3(a)に示すようにその断面が1/4円弧に満たないものとされていてもよく、この場合には、主パンチ11,12のプレス面11A,12Aの凹部16側の両側縁部に、該主パンチ11,12が上述のように位置決めされてキャビティ14が形成された状態で壁面16Bに滑らかに連なる断面円弧状の凹曲面部17が形成され、この凹曲面部17と壁面16Bとにより、圧粉体において上記コーナ稜線部8に対応する断面1/4円弧の凸曲面が成形される。従って、この場合には、圧粉体においてチップ本体1の上記平板面2の全部とこの平板面2側のコーナ稜線部8の一部に対応する部分が主パンチ11,12によって成形され、コーナ稜線部8の残りと他の周面5に対応する部分とがダイ13によって成形される。なお、この場合において、上記凹曲面部17側でダイ13に摺接する主パンチ11,12の外周面18と凹曲面部17とがなす交差角αは45°以上とされるのが望ましく、これよりも交差角αが小さいとこれら凹曲面部17と外周面18との交差稜線部分が鋭角になりすぎて欠損を生じるおそれがある。   Here, as shown in FIG. 3A, the wall surface 16B may have a cross section of less than ¼ arc, and in this case, the press surfaces 11A of the main punches 11 and 12 A concave curved surface portion 17 having an arcuate cross section that is smoothly connected to the wall surface 16B in a state where the main punches 11 and 12 are positioned as described above and the cavity 14 is formed is formed on both side edges on the concave portion 16 side of 12A. The concave curved surface portion 17 and the wall surface 16B form a convex curved surface having a ¼ arc in cross section corresponding to the corner ridge line portion 8 in the green compact. Therefore, in this case, in the green compact, all of the flat plate surface 2 of the chip body 1 and a portion corresponding to a part of the corner ridge line portion 8 on the flat plate surface 2 side are formed by the main punches 11 and 12, and the corners are formed. The remainder of the ridge line portion 8 and the portion corresponding to the other peripheral surface 5 are formed by the die 13. In this case, it is desirable that the crossing angle α formed by the outer peripheral surface 18 of the main punches 11 and 12 slidably contacting the die 13 on the concave curved surface portion 17 side and the concave curved surface portion 17 is 45 ° or more. If the crossing angle α is smaller than the above, the crossing ridge line portion between the concave curved surface portion 17 and the outer peripheral surface 18 becomes too acute, and there is a possibility that a defect is generated.

また、上記壁面16Bは、図3(b)に示すようにその断面が丁度1/4円弧となるような凹曲面とされていてもよく、この場合には主パンチ11,12のプレス面11A,12Aに上述のような凹曲面部17は形成されず、このプレス面11A,12Aと主パンチ11,12の上記外周面18との交差角αは90°となり、圧粉体において他の周面5から丁度コーナ稜線部8の全体に対応する部分までがダイ13の上記凹部16によって成形される。さらに、この壁面16Bは、図3(c)に示すようにその断面が1/4円弧を越えて主パンチ11,12の離接方向に垂直な方向に延びるように形成されていてもよく、この場合にも主パンチ11,12のプレス面11A,12Aに上述のような凹曲面部17は形成されずに、プレス面11A,12Aと外周面18との交差角αは90°となる。そして、この場合には、圧粉体においては他の周面5からコーナ稜線部8を越えて平板面2の他の周面5側の縁部に対応する部分までがダイ13の上記凹部16によって成形されることとなり、主パンチ11,12は圧粉体において平板面2の上記縁部間の一部に対応する部分のみを成形することになる。   Further, the wall surface 16B may be a concave curved surface whose cross section is exactly a ¼ arc as shown in FIG. 3B. In this case, the press surface 11A of the main punches 11 and 12 is used. , 12A is not formed, and the crossing angle α between the press surfaces 11A, 12A and the outer peripheral surface 18 of the main punches 11, 12 is 90 °. From the surface 5 to the portion corresponding to the entire corner ridge line portion 8 is formed by the concave portion 16 of the die 13. Further, the wall surface 16B may be formed so that its cross section extends over a 1/4 arc and extends in a direction perpendicular to the contact / separation direction of the main punches 11 and 12, as shown in FIG. Also in this case, the concave curved surface portion 17 as described above is not formed on the press surfaces 11A and 12A of the main punches 11 and 12, and the crossing angle α between the press surfaces 11A and 12A and the outer peripheral surface 18 is 90 °. In this case, in the green compact, the concave portion 16 of the die 13 extends from the other peripheral surface 5 to the portion corresponding to the edge on the other peripheral surface 5 side beyond the corner ridgeline portion 8. Thus, the main punches 11 and 12 form only a portion corresponding to a part between the edges of the flat plate surface 2 in the green compact.

なお、これら主パンチ11,12のうち、本参考例では下側の主パンチ12に、主パンチ11,12の上記離接方向に向けて上記キャビティー14内に出没可能とされるピン19が備えられている。このピン19は、チップ本体1の取付穴10に対応する貫通穴を圧粉体に形成するものであって、円柱状をなし、下側の主パンチ12の上記プレス面12A中央部に開口するように形成された円孔12Bに嵌挿され、該主パンチ12とは独立して駆動されてプレス面12Aから上向きに突出するように出没可能とされている。一方、上側の主パンチ11には、そのプレス面11Aの中央部に開口するように円孔11Bが形成されており、接近した主パンチ11,12間に画成されたキャビティー14内に突出したピン19の先端(上端)部は、この上側の主パンチ11の円孔11B内に嵌挿されて収容される。 Of these main punches 11 and 12, in the present reference example , the lower main punch 12 has a pin 19 that can be projected and retracted in the cavity 14 in the direction in which the main punches 11 and 12 are separated from each other. Is provided. The pin 19 forms a through hole corresponding to the mounting hole 10 of the chip body 1 in the green compact, has a cylindrical shape, and opens at the center of the press surface 12A of the lower main punch 12. It is inserted into the circular hole 12B formed as described above, and is driven independently of the main punch 12 so as to protrude and protrude upward from the press surface 12A. On the other hand, a circular hole 11B is formed in the upper main punch 11 so as to open in the center of the press surface 11A, and protrudes into a cavity 14 defined between the main punches 11 and 12 that are close to each other. The tip (upper end) portion of the pin 19 is inserted and accommodated in the circular hole 11B of the upper main punch 11.

また、上記ダイ13は、キャビティー14を間にして分割されて離接可能とされている。すなわち、本参考例では、ダイ13は、図2に示すように主パンチ11,12の離接方向においてキャビティー14の略中央に位置する分割面Pによりこれら主パンチ11,12の離接方向と平行な方向に分割される一対の分割ダイ13A,13Bによって構成されており、上記分割面Pは主パンチ11,12の離接方向に垂直な平面とされている。そして、これらの分割ダイ13A,13Bは、主パンチ11,12の離接やピン19の出没とは独立して、該主パンチ11,12の離接方向と平行な方向に相対的に離接可能とされる。なお、このうち一方の分割ダイ(例えば、下側の分割ダイ13B)は上記副パンチ15とともに主パンチ11,12の離接方向の位置を固定しておき、他方の分割ダイ(例えば、上側の分割ダイ13A)のみを離接させるようにしてもよい。 The die 13 is divided with the cavity 14 therebetween, and can be separated from and connected to the die 13. That is, in the present reference example , the die 13 is separated from the main punches 11 and 12 by the dividing surface P located substantially at the center of the cavity 14 in the direction of separation of the main punches 11 and 12, as shown in FIG. The split surface P is a plane perpendicular to the contact / separation direction of the main punches 11 and 12. These divided dies 13A and 13B are separated from each other in a direction parallel to the direction of separation of the main punches 11 and 12 independently of the separation and contact of the main punches 11 and 12 and the protrusions and depressions of the pins 19. It is possible. One of the divided dies (for example, the lower divided die 13B) fixes the position of the main punches 11 and 12 together with the sub-punch 15 and fixes the other divided die (for example, the upper divided die 13B). Only the split die 13A) may be separated.

次に、このように構成されたプレス成形金型により、上記縦刃式スローアウェイチップに製造される圧粉体を成形する場合の切削工具の切刃部材の製造方法の参考例について図5により説明すると、まず図5(a)に示されるように分割ダイ13A,13Bを接近させてダイ13を構成し、下側の主パンチ12をキャビティー14が形成される位置から離間させるとともに副パンチ15はキャビティー14の位置まで接近させた状態で、上側の主パンチ11をダイ13から離間させておいてその開口部から、WCを主成分とする超硬合金やTiC−TiNを主成分とするサーメット等の原料粉末を投入して、所定量が充填されるようにする。なお、このときピン19は、その上端が投入された原料粉末と略等しい高さとなるように下側の主パンチ12のプレス面12Aから突出させられている。 Next, a reference example of a method for manufacturing a cutting blade member of a cutting tool in the case of forming a green compact manufactured on the above-mentioned vertical blade type throw-away tip by the press molding die configured as described above will be described with reference to FIG. First, as shown in FIG. 5A, the divided dies 13A and 13B are brought close to each other to form the die 13, and the lower main punch 12 is separated from the position where the cavity 14 is formed and the auxiliary die 13 is formed. The punch 15 is close to the position of the cavity 14, the upper main punch 11 is separated from the die 13, and a cemented carbide containing WC as a main component or TiC-TiN as a main component from its opening. A raw material powder such as cermet is added to fill a predetermined amount. At this time, the pin 19 is protruded from the press surface 12A of the lower main punch 12 so that the upper end of the pin 19 has a height substantially equal to the charged raw material powder.

次いで、図5(b)に示すように、上側の主パンチ11が下側主パンチ12に向けて接近してピン19を円孔11B内に嵌挿しつつダイ13に挿入されて前進(降下)してゆくが、このとき下側の主パンチ12は接近する上側主パンチ11に対して離間するように後退するとともに副パンチ15もキャビティー14側から離間するように後退し、これにより投入された原料粉末はこれら主パンチ12および副パンチ15が後退した空間へと引き込まれるように充填され、圧縮工程前の原料粉末の移送工程の終了となる。そして、上側の主パンチ11が所定の位置まで前進したところで、下側の主パンチ12も上側主パンチ11に向けて接近して前進(上昇)するとともに、副パンチ15もキャビティー14側に向けて接近するように前進して主パンチ11,12とともに原料粉末を圧縮し、図5(c)に示されるように所定の形状のキャビティー14を画成するとともに、その内部にこのキャビティー14の形状に対応した圧粉体をプレス成形する。すなわち、主パンチ11,12によって圧粉体におけるチップ本体1の上記平板面2に対応する面の少なくとも一部を成形するとともに、副パンチ15によってすくい面3に対応する面を成形し、残りの他の周面5に対応する面等の部分はダイ13によって成形する。   Next, as shown in FIG. 5 (b), the upper main punch 11 approaches the lower main punch 12 and is inserted into the die 13 while being inserted into the circular hole 11B to move forward (lower). At this time, however, the lower main punch 12 is retracted away from the approaching upper main punch 11 and the sub punch 15 is also retracted away from the cavity 14 side. The raw material powder is filled so that the main punch 12 and the sub punch 15 are drawn into the retracted space, and the raw material powder transfer step before the compression step is completed. Then, when the upper main punch 11 advances to a predetermined position, the lower main punch 12 approaches and moves upward (rises) toward the upper main punch 11, and the sub punch 15 also faces the cavity 14 side. The raw powder is compressed together with the main punches 11 and 12 by moving forward so that a cavity 14 having a predetermined shape is defined as shown in FIG. The green compact corresponding to the shape is pressed. That is, at least a part of the surface corresponding to the flat plate surface 2 of the chip body 1 in the green compact is formed by the main punches 11 and 12, and the surface corresponding to the rake face 3 is formed by the sub punch 15, and the remaining portions are formed. Portions such as surfaces corresponding to other peripheral surfaces 5 are formed by the die 13.

なお、このとき、上記副パンチ15のキャビティー14への接近による原料粉末の圧縮は、主パンチ11,12が原料粉末を圧縮し始めてから圧縮を終了するまでに接近する移動量の50%以上を移動した後に終了するように設定されている。すなわち、図5(b)に示したように上側の主パンチ11が降下する一方で下側の主パンチ12が後退して原料粉末を引き込んでから前進(上昇)に転じた時点を主パンチ11,12による圧縮の開始とし、図5(c)に示したようにこれら上下の主パンチ11,12が互いに接近して上記所定の形状のキャビティー14を画成した時点を圧縮の終了としたとき、圧縮の開始からの主パンチ11,12の移動量が、これら圧縮開始と終了の間に主パンチ11,12が移動する移動量L(図5(b)参照)の1/2に達した後に、副パンチ15が上記キャビティー14を画成する位置に達して停止し、該副パンチ15による原料粉末の圧縮が終了するようになされている。従って、副パンチ15による圧縮終了は主パンチ11,12による圧縮終了と同時(主パンチ11,12の移動量が上記移動量Lに達した時点)でもよく、またそれ以降であってもよい。   At this time, the compression of the raw material powder due to the approach of the sub punch 15 to the cavity 14 is 50% or more of the moving amount approaching from the time when the main punches 11 and 12 start to compress the raw material powder to the end of the compression. Is set to end after moving. That is, as shown in FIG. 5 (b), the time when the upper main punch 11 descends while the lower main punch 12 recedes and pulls in the raw material powder and then moves forward (rises), the main punch 11 , 12 is started, and as shown in FIG. 5C, the upper and lower main punches 11 and 12 approach each other to define the cavity 14 having the predetermined shape, and the compression ends. At this time, the amount of movement of the main punches 11 and 12 from the start of compression reaches half of the amount of movement L (see FIG. 5B) that the main punches 11 and 12 move between the start and end of compression. After that, the sub punch 15 reaches the position defining the cavity 14 and stops, and the compression of the raw material powder by the sub punch 15 is finished. Therefore, the compression end by the sub punch 15 may be simultaneous with the end of the compression by the main punches 11 and 12 (when the movement amount of the main punches 11 and 12 reaches the movement amount L) or after that.

そして、こうして圧粉体が成形されたなら、ピン19を後退させてキャビティー14から下側主パンチ12内に没入させるとともに、ダイ13を分割して分割ダイ13A,13Bを離間させ、さらに上側の主パンチ11と副パンチ15を離間(後退)させることにより、成形された圧粉体は下側の主パンチ12上に載置されただけの状態となるので、これを取り出して焼結することにより、図4に示したような縦刃式スローアウェイチップすなわち切削工具の切刃部材を製造することができる。   When the green compact is formed in this way, the pin 19 is retracted to be immersed in the lower main punch 12 from the cavity 14, and the die 13 is divided to separate the divided dies 13A and 13B. By separating (retracting) the main punch 11 and the sub punch 15, the formed green compact is merely placed on the lower main punch 12, and is taken out and sintered. Thus, a vertical blade type throwaway tip as shown in FIG. 4, that is, a cutting blade member of a cutting tool can be manufactured.

従って、このような製造方法およびプレス成形金型においては、主パンチ11,12と、これら主パンチ11,12の離接方向とは異なる方向に離接する副パンチ15とによって原料粉末が圧縮されるので、これら主パンチ11,12の離接方向と副パンチ15の離接方向との多方向から擬似的にキャビティー14内において原料粉末を等方的に圧縮して圧粉体をプレス成形することができる。このため、単に互いに対向して離接する一対のパンチによって原料粉末を圧縮する場合などに比べ、圧粉体において原料粉末を満遍なくより均一に圧縮することができるので、こうしてプレス成形された圧粉体を焼結しても微少な変形や歪みすら生じることがなく、圧粉体のプレス成形によっても極めて高精度の切刃部材を製造することが可能となる。   Therefore, in such a manufacturing method and press molding die, the raw material powder is compressed by the main punches 11 and 12 and the sub-punch 15 that comes in contact with and separates from the direction in which the main punches 11 and 12 come in contact with each other. Therefore, the raw material powder is pseudo-compressed in the cavity 14 in a pseudo manner from the multiple directions of the separation and contact directions of the main punches 11 and 12 and the separation and contact direction of the sub punch 15 to press-mold the green compact. be able to. For this reason, since the raw material powder can be uniformly and evenly compressed in the green compact as compared with the case where the raw powder is simply compressed by a pair of punches facing and separating from each other, the green compact thus press-molded is possible. Sintering does not cause even slight deformation or distortion, and it becomes possible to manufacture a cutting blade member with extremely high accuracy by press molding of a green compact.

例えば、本参考例では、上述のような縦刃式スローアウェイチップに製造される圧粉体を成形するのに際し、ダイ13の凹部16によって圧粉体の他の周面5に対応する面とコーナ稜線部8の一部(図3(a)の場合)、または全部(図3(b)の場合)、またはコーナ稜線部8の全部と平板面2の一部(図3(c)の場合)に対応する面とが成形されるようになされているが、特に図3(c)のように凹部16の後退量が大きい場合には、上下の主パンチ11,12による圧縮だけではこの凹部16内で原料粉末を極めて均一に圧縮するのは困難となる。ところが、これに対して本参考例によれば、副パンチ15が主パンチ11,12の離接方向と垂直な上記凹部16の延びる方向にキャビティ14に向けて接近して原料粉末を圧縮することにより、この凹部16内に充填された原料粉末をも十分に圧縮することができ、圧粉体の全体においてその原料粉末の圧縮の確実な均一化を図ることが可能となるので、こうしてプレス成形された圧粉体を焼結したスローアウェイチップにおいては、特に上記他の周面5からコーナ稜線部8にかけての部分を所望の形状寸法とすることができ、これに伴い切削工具の切刃部材として重要な切刃6からコーナ部7にかけての部分も極めて高精度に形成することができる。 For example, in this reference example , when forming the green compact manufactured in the above-described vertical blade type throw-away tip, the surface corresponding to the other peripheral surface 5 of the green compact by the concave portion 16 of the die 13 Part of the corner ridgeline 8 (in the case of FIG. 3A) or all (in the case of FIG. 3B), or all of the corner ridgeline 8 and part of the flat plate surface 2 (in FIG. 3C) In the case where the recess 16 has a large retraction amount as shown in FIG. 3C, the compression by the upper and lower main punches 11 and 12 is sufficient. It becomes difficult to compress the raw material powder very uniformly in the recess 16. On the other hand, according to the present reference example , the sub punch 15 approaches the cavity 14 in the direction in which the concave portion 16 extends perpendicularly to the direction in which the main punches 11 and 12 are separated from each other, and compresses the raw material powder. Thus, the raw material powder filled in the recess 16 can be sufficiently compressed, and it becomes possible to ensure uniform compression of the raw material powder in the whole green compact. In the throw-away tip in which the green compact is sintered, the portion from the other peripheral surface 5 to the corner ridge line portion 8 can be made to have a desired shape dimension, and accordingly, the cutting blade member of the cutting tool The important part from the cutting edge 6 to the corner part 7 can be formed with extremely high accuracy.

これは、例えば上記すくい面3にチップブレーカ9が形成された図24に示したような縦刃式スローアウェイチップを製造する場合も同様であり、本参考例においてこのようなスローアウェイチップに製造される圧粉体を成形するには、図6および図7に示す変形例のプレス成形金型のように、副パンチ15のプレス面15Aに、圧粉体におけるチップブレーカ9に対応した形状に応じて凹凸が逆になるように、凹部15Bや凸部15Cを形成すればよい。ここで、図8(a)は、この変形例によって製造される縦刃式スローアウェイチップのチップブレーカ9部分の断面図であり、このチップブレーカ9は、切刃4.6またはコーナ部7に、平板面2、他の周面5、およびコーナ稜線部8に垂直な幅の短いランド部20を介して、すくい面3の内側(図8(a)において右側)に向かうに従い漸次後退した後に隆起する凹溝状とされており、さらにその内側には平板面2、他の周面5、およびコーナ稜線部8に垂直で切刃4,6およびコーナ部7よりも突出した平坦面21が形成されて、チップ本体1の一対のすくい面3のうち一方のすくい面3周縁の切刃4,6、およびコーナ部7を切削に用いる際に、他方のすくい面3の平坦面21が切削工具のチップ取付座壁面に当接して着座させられるようになされている。 This is the same as the case of manufacturing a vertical blade type throwaway tip as shown in FIG. 24 in which the chip breaker 9 is formed on the rake face 3, for example. In this reference example , such a throwaway tip is manufactured. In order to mold the green compact to be formed, the shape corresponding to the chip breaker 9 in the green compact is formed on the press surface 15A of the sub punch 15 as in the press molding die of the modification shown in FIGS. Accordingly, the concave portions 15B and the convex portions 15C may be formed so that the concave and convex portions are reversed. Here, FIG. 8A is a cross-sectional view of the tip breaker 9 portion of the vertical blade type throw-away tip manufactured according to this modification, and this tip breaker 9 is attached to the cutting edge 4.6 or the corner portion 7. After retreating gradually toward the inner side of the rake face 3 (right side in FIG. 8A) through the flat surface 2, the other peripheral surface 5, and the land portion 20 having a short width perpendicular to the corner ridgeline portion 8. Further, a flat surface 21 that is perpendicular to the flat plate surface 2, the other peripheral surface 5, and the corner ridgeline portion 8 and protrudes from the cutting edges 4, 6 and the corner portion 7 is formed inside. When the cutting edges 4 and 6 on the periphery of one rake face 3 of the pair of rake faces 3 of the chip body 1 and the corner portion 7 are used for cutting, the flat face 21 of the other rake face 3 is cut. It can be seated against the wall surface of the tool mounting seat Uninasa are.

そして、これに応じて図6に示すように副パンチ15のプレス面15Aにも、その外周縁に当該副パンチ15の離接方向に垂直な幅狭枠状の平坦面15Dが形成されるとともに、その内側には該プレス面15Aの内側に向かうに従い漸次隆起する上記凸部15Cと、この凸部15Cから副パンチ15が離間する方向に後退してキャビティー14に対し凹となる上記凹部15Bとが形成され、この凹部15Bの底面15Eは上記平坦面15Dよりも副パンチ15の離間する方向に後退した平坦面とされる。なお、この変形例によって製造される縦刃式スローアウェイチップでは、図8(b)に示すように取付穴10が、上記厚さ方向中央部においてこの厚さ方向中央部に向かうに従い漸次縮径する縮径部10Aを有したいわゆるベル穴構造とされており、これに伴い主パンチ11,12のプレス面11A,12Aにおいて上記円孔11B,12Bの周りには、それぞれ先端に上記縮径部10Aに対応する部分を圧粉体の貫通穴に成形する縮径部22Aが形成された概略円筒状の突部22が形成され、ピン19はこれらの突部22の内径部に嵌挿されるようにして出没可能とされる。   Accordingly, as shown in FIG. 6, a narrow frame-like flat surface 15 </ b> D perpendicular to the direction of separation of the sub punch 15 is formed on the outer peripheral edge of the press surface 15 </ b> A of the sub punch 15. On the inner side, the convex portion 15C that gradually rises toward the inner side of the press surface 15A, and the concave portion 15B that recedes in a direction in which the auxiliary punch 15 is separated from the convex portion 15C and becomes concave with respect to the cavity 14. And the bottom surface 15E of the recess 15B is a flat surface that is recessed in the direction in which the sub punch 15 is separated from the flat surface 15D. In the vertical blade type throw-away tip manufactured according to this modification, as shown in FIG. 8 (b), the mounting hole 10 is gradually reduced in diameter toward the central portion in the thickness direction in the central portion in the thickness direction. In accordance with this, a so-called bell hole structure having a reduced diameter portion 10A is formed, and on the press surfaces 11A and 12A of the main punches 11 and 12, the reduced diameter portion is provided at the tip of the circular holes 11B and 12B. A substantially cylindrical projection 22 is formed in which a reduced diameter portion 22A is formed to mold a portion corresponding to 10A into a through hole of the green compact, and the pin 19 is inserted into the inner diameter portion of these projection 22 It is possible to appear and disappear.

従って、このような変形例においても、図7に示すようにダイ13に形成された凹部16によってチップ本体1の他の周面5に対応する圧粉体の面の周辺が成形される場合に、主パンチ11,12の離接方向とは異なる水平方向から離接する副パンチ15により、該凹部16に充填された原料粉末を均一に圧縮することができる。そして、さらに当該変形例では、上記他の周面5とは異なるすくい面3となる周面に上述のような凹状のチップブレーカ9や凸状の平坦面21が形成される場合でも、この副パンチ15に上述のような凸部15Cや凹部15Bを形成することにより、これらチップブレーカ9や平坦面21に応じた凹凸を圧粉体のすくい面3に対応する面が確実かつ均一に圧縮されるように成形することができる。なお、すくい面3に形成されるチップブレーカ9が切刃4,6やコーナ部7から突出するものだけである場合には、これに応じて上記プレス面15Aに凹部のみを形成すればよく、逆にチップブレーカ9がすくい面3に凹状に形成されるものだけである場合にはプレス面15Aにも凸部のみを形成すればよい。   Therefore, even in such a modified example, when the periphery of the surface of the green compact corresponding to the other peripheral surface 5 of the chip body 1 is formed by the recess 16 formed in the die 13 as shown in FIG. The raw material powder filled in the concave portion 16 can be uniformly compressed by the sub punch 15 that comes in contact with and separates from the horizontal direction different from the direction of separation of the main punches 11 and 12. Further, in this modified example, even when the above-described concave chip breaker 9 or the convex flat surface 21 is formed on the peripheral surface to be the rake surface 3 different from the other peripheral surface 5, By forming the convex portions 15C and the concave portions 15B as described above in the punch 15, the surface corresponding to the chip breaker 9 and the flat surface 21 corresponding to the rake face 3 of the green compact is reliably and uniformly compressed. It can be shaped as follows. In addition, when the chip breaker 9 formed on the rake face 3 is only the one that protrudes from the cutting blades 4 and 6 and the corner portion 7, it is only necessary to form only the concave portion on the press surface 15A accordingly. On the contrary, when the chip breaker 9 is only formed in a concave shape on the rake face 3, only the convex portion may be formed on the press surface 15A.

しかるに、例えばこのような凹部15Bや凸部15Cを上記凹部16と同様にダイ13側に形成しておくことも考えられるが、特に上記縦刃式スローアウェイチップのようにすくい面3の外周側を周回する凹溝状のチップブレーカ9の内側に切刃4,6やコーナ部7より凸となる平坦面21が形成されるのに伴い、枠状に周回する凸部15Cの内側に大きく凹んだ凹部15Bが形成される場合には、主パンチ11,12による圧縮だけではこの凹部15Bの底面近傍に原料粉末を確実に回り込ませて他の部分と均一に圧縮するのは困難となるおそれがある。ところが、これ対して、本参考例の上記変形例によれば、副パンチ15に形成された凹凸部15B,15Cが凹凸する方向に該副パンチ15が離接させられることとなるので、たとえ凹部15Bの底面近傍でも原料粉末を確実かつ均一に圧縮して圧粉体を成形することができ、従ってチップ本体1において着座の基準となる上記平坦面21をより高精度に形成することが可能となる。 However, for example, it is conceivable to form such concave portions 15B and convex portions 15C on the die 13 side in the same manner as the concave portion 16, but particularly on the outer peripheral side of the rake face 3 like the vertical blade type throwaway tip. As the flat surface 21 that protrudes from the cutting blades 4 and 6 and the corner portion 7 is formed inside the recessed groove-shaped chip breaker 9 that circulates, it is greatly recessed inside the convex portion 15C that circulates in a frame shape. In the case where the recess 15B is formed, it may be difficult to make the raw material powder surely wrap around the bottom surface of the recess 15B and compress it uniformly with other portions only by compression by the main punches 11 and 12. is there. On the other hand, according to the modification of the present reference example , the sub punch 15 is brought into contact with the concave and convex portions 15B and 15C formed on the sub punch 15 in the direction in which the concave and convex portions are uneven. Even in the vicinity of the bottom surface of 15B, it is possible to reliably and uniformly compress the raw material powder to form a green compact. Therefore, it is possible to form the flat surface 21 serving as a reference for seating in the chip body 1 with higher accuracy. Become.

また、この変形例も含めた上記参考例では、平板状のチップ本体1に製造される圧粉体のうち最も面積の大きくなる上記平板面2に対応する面の少なくとも一部が上下方向に離接する主パンチ11,12によって成形されて、これら主パンチ11,12により原料粉末がチップ本体1の寸法の小さい厚さ方向に対応する方向に圧縮されて圧粉体が成形されるようになされており、より均一な原料粉末の圧縮を図ることができる。特に、本参考例のように取付穴10とされる貫通穴が圧粉体に成形される場合でも、この貫通穴を成形するピン19は、主パンチ11,12の離接方向すなわち主パンチ11,12による圧縮方向に沿ってキャビティー14内に突出させられるので、このピン19の周辺においても均一な原料粉末圧縮比を得ることができる。しかも、変形例のように上記突部22によってベル穴状の貫通穴を成形する場合でも、本参考例ではこの主パンチ11,12による圧縮に加えて副パンチ15によりピン19の突出方向に垂直な方向からも原料粉末が圧縮されるので、主パンチ11,12の両突部22間の環状に凹となる部分にも確実に原料粉末を押し込んで圧縮の均一化を図ることができる。 In the reference example including this modification, at least a part of the surface corresponding to the flat plate surface 2 having the largest area among the green compacts manufactured on the flat plate-shaped chip body 1 is separated in the vertical direction. Molded by the main punches 11 and 12 in contact with each other, the raw powder is compressed by the main punches 11 and 12 in a direction corresponding to the thickness direction in which the size of the chip body 1 is small, thereby forming a green compact. Therefore, the raw material powder can be compressed more uniformly. In particular, even when the through hole which is the mounting hole 10 is formed into a green compact as in this reference example , the pin 19 for forming the through hole is in the direction in which the main punches 11 and 12 are separated, that is, the main punch 11. , 12 is projected into the cavity 14 along the compression direction, so that a uniform raw material powder compression ratio can be obtained also around the pin 19. Moreover, even when a bell hole-shaped through hole is formed by the protrusion 22 as in the modification, in the present reference example , in addition to the compression by the main punches 11 and 12, the sub punch 15 causes the pin 19 to be perpendicular to the protruding direction. Since the raw material powder is compressed from any direction, the raw material powder can be surely pushed into the annularly concave portion between the protrusions 22 of the main punches 11 and 12 to achieve uniform compression.

さらに、こうして副パンチ15によって主パンチ11,12とともに原料粉末を圧縮するのに際して、本参考例の製造方法では、主パンチ11,12が原料粉末を圧縮し始めてから圧縮を終了するまでの移動量Lの50%以上移動して接近した後に、副パンチ15による原料粉末の圧縮が終了するようになされており、主パンチ11,12による圧縮が十分になされないうちに副パンチ15がキャビティー14を画成する位置に達して圧縮を終了することにより、あたかもこの副パンチ15部分がダイ13の一部となったところに主パンチ11,12による圧縮が行われるような状態となるのを防ぐことができ、この副パンチ15の圧縮による圧粉体の圧縮の均一化効果を確実に奏することが可能となる。なお、この副パンチ15による原料粉末の圧縮終了は、当該製造方法における圧縮工程時間の短縮等を考慮すると主パンチ11,12による圧縮の終了と略同時までの間とされるのが望ましいが、上述のようにこの主パンチ11,12による原料粉末の圧縮の終了後とされていてもよい。 Further, when the raw powder is compressed together with the main punches 11 and 12 by the sub punch 15 in this way, in the manufacturing method of the present reference example , the movement amount from when the main punches 11 and 12 start to compress the raw material powder until the compression ends. After moving closer than 50% of L, compression of the raw material powder by the sub punch 15 is completed, and before the compression by the main punches 11 and 12 is sufficiently performed, the sub punch 15 is inserted into the cavity 14. Is reached and the compression is terminated, so that it is prevented that the main punches 11 and 12 are compressed as if the sub-punch 15 portion becomes a part of the die 13. Therefore, it is possible to reliably achieve the effect of compressing the green compact by the compression of the sub punch 15. In addition, it is desirable that the compression of the raw material powder by the sub punch 15 is approximately until the end of the compression by the main punches 11 and 12 in consideration of shortening of the compression process time in the manufacturing method. As described above, it may be after the compression of the raw material powder by the main punches 11 and 12 is completed.

さらにまた、本参考例の製造方法では、主パンチ11,12の間に原料粉末が投入された後に、副パンチ15がキャビティー14を画成する位置から一旦離間し、しかる後に再び接近して原料粉末を圧縮するようになされており、これにより投入された原料粉末を副パンチ15が離間して後退する際に形成される空間に十分に引き込んでから圧縮することができるので、圧粉体における一層確実な原料粉末の圧縮の均一化を図ることができる。また、本参考例では同時に下側の主パンチ12も上側の主パンチ11に対して離間(後退)して下降することにより、この下側主パンチ12の上の空間にも原料粉末を引き込んでから上側主パンチ11との間で圧縮することができるので、この主パンチ11,12の離接方向にも圧縮の均一化を図ることができる。ただし、上記副パンチ15による原料粉末圧縮のための移動量が小さい場合には、上述のように副パンチ15を一旦離間させることなく、例えば下側の主パンチ12による引き込みが終了して上側の主パンチ11とによる圧縮が開始された時点で同時に、あるいはそれより後などに、そのままキャビティー14側に向けて接近させて圧縮を行うようにしてもよい。 Furthermore, in the manufacturing method of the present reference example , after the raw material powder is put between the main punches 11 and 12, the sub punch 15 is once separated from the position defining the cavity 14, and then approaches again. The raw material powder is compressed, so that the charged raw material powder can be sufficiently drawn into the space formed when the sub punch 15 is separated and retracted, and then compressed. It is possible to achieve more uniform compression of the raw material powder. In this reference example , the lower main punch 12 is also moved away from (retracted from) the upper main punch 11 at the same time, so that the raw material powder is drawn into the space above the lower main punch 12. To the upper main punch 11, the compression can be made uniform in the direction in which the main punches 11 and 12 are separated from each other. However, when the amount of movement for compressing the raw material powder by the sub punch 15 is small, the pulling by the lower main punch 12 is completed, for example, without the sub punch 15 being temporarily separated as described above. At the time when the compression by the main punch 11 is started, the compression may be performed by approaching the cavity 14 as it is at the same time or after that.

一方、本参考例のプレス成形金型では、主パンチ11,12の離接方向に対して副パンチ15の離接方向が垂直とされており、特に主パンチ11,12が上下方向に離接させられるのに対して副パンチ15は水平に離接させられるので、これら主パンチ11,12と副パンチ15を離接させるための駆動手段を該離接方向に沿った直交座標に基づいて設計すればよく、設計の簡略化を図ってより低廉なプレス成形金型を提供することができ、従って切刃部材(縦刃式スローアウェイチップ)の製造コストの一層の低減を図ることができる。また、本参考例ではプレス成形された圧粉体を取り出すのに、ダイ13もこのキャビティー14を間にして複数の分割ダイ13A,13Bに分割されて離接可能とされており、しかもこのダイ13の分割方向が主パンチ11,12の離接方向と平行な方向、すなわち上下方向とされているので、このダイ13を分割して離接させるための駆動手段についても設計の簡略化を図りつつ、成形された圧粉体を容易に金型から取り出すことが可能となる。 On the other hand, in the press molding die of this reference example, the contact direction of the sub punch 15 is perpendicular to the contact direction of the main punches 11 and 12, and in particular, the main punches 11 and 12 are contacted in the vertical direction. In contrast to this, since the sub punch 15 is horizontally separated, the drive means for separating the main punches 11 and 12 and the sub punch 15 is designed based on the orthogonal coordinates along the separation direction. Therefore, it is possible to provide a more inexpensive press mold by simplifying the design, and therefore it is possible to further reduce the manufacturing cost of the cutting blade member (vertical blade type throw-away tip). Further, in this reference example , in order to take out the press-molded green compact, the die 13 is also divided into a plurality of divided dies 13A and 13B with the cavity 14 in between, and can be separated and connected. Since the dividing direction of the die 13 is a direction parallel to the separating / contacting direction of the main punches 11 and 12, that is, the vertical direction, the design of the driving means for dividing and separating the die 13 can be simplified. The molded green compact can be easily taken out from the mold while being planned.

ただし、本参考例ではこのようにダイ13を分割して圧粉体を取り出すようにしているが、例えば図1および図2に示した参考例のように主パンチ11,12のプレス面11A,12Aに変形例のような突部22や逆に凹部などが形成されていない場合には、ダイ13を分割することなく、圧縮終了後にピン19を後退させてプレス面12Aから没入させてから、一対の副パンチ15のうち一方をキャビティー14に対して離間させるとともに、他方をこの一方の副パンチ15が離間する側に圧粉体ごと押し出して取り出すことも可能である。また、ダイ13を分割するにしても、上記参考例のように主パンチ11,12の離接する方向と平行な方向の他に、この離接方向と垂直な、例えば副パンチ15の離接方向に平行な方向(図1における左右方向)や、主、副パンチ11,12,15の離接方向に双方に垂直な方向(図2における左右方向)にダイ13を分割して離接させるようにしてもよく、場合によっては圧粉体に対して抜き勾配が与えられる方向に斜めにダイ13を2またはそれ以上の分割ダイに分割して離接させてもよい。 However, in this reference example , the die 13 is divided in this way so that the green compact is taken out. For example , as in the reference example shown in FIGS. In the case where the protrusion 22 as in the modified example or the concavity or the like is not formed in 12A, the pin 19 is retracted after the compression is completed and the press surface 12A is immersed without dividing the die 13, One of the pair of sub-punches 15 can be separated from the cavity 14 and the other can be pushed out together with the green compact to the side where the one sub-punch 15 is separated. Even when the die 13 is divided, in addition to the direction parallel to the direction in which the main punches 11 and 12 are separated from each other as in the above-described reference example , the direction in which the sub punch 15 is separated, for example, perpendicular to this direction. The die 13 is divided and separated in a direction parallel to the horizontal direction (left and right direction in FIG. 1) and in a direction perpendicular to both directions of the main and sub punches 11, 12, and 15 (left and right direction in FIG. 2). In some cases, the die 13 may be divided into two or more divided dies and separated from each other in a direction in which a draft is given to the green compact.

なお、こうしてダイ13を分割するのと同様に、上記主パンチ11,12や副パンチ15についても、その少なくとも1つを上記ダイ13と同様に複数の分割パンチによって構成するようにしてもよい。ただし、この場合に複数の分割パンチによって構成される主パンチ11,12と副パンチ15とのうちの少なくとも一つは、その離接方向に沿った分割面によって分割されて、各分割パンチがこの分割面で摺接しながら該離接方向に互いに独立して離接させられることとなる。   As in the case of dividing the die 13 in this way, at least one of the main punches 11 and 12 and the sub punch 15 may be constituted by a plurality of divided punches as in the die 13. However, in this case, at least one of the main punches 11 and 12 and the sub-punch 15 constituted by a plurality of divided punches is divided by a dividing surface along the separation / contact direction, and each divided punch is While being slidably contacted with the dividing surface, they are separated from each other independently in the separating direction.

そして、このように主パンチ11,12や副パンチ15を複数の分割パンチで構成したときには、この分割されたパンチによって成形される圧粉体の面のなかでもその離接方向における原料粉末充填量や圧縮比の細かな制御を行うことができ、より均一な密度の圧粉体を得ることが可能となる。例えば、上記参考例において、副パンチ15の離接方向にキャビティー14側から見て上記ピン19が投影される副パンチ15の中央部分では、該離接方向にピン19が位置するため、単一の副パンチ15によって圧縮するとその両側の部分に比べて原料粉末の充填量が相違して圧縮比も変化してしまうのに対し、この中央部分と両側部分とで副パンチ15を分割してこれらを独立して離接させることにより、このような原料粉末充填量の相違に応じて圧縮比が均一化するように中央部分と両側部分とで充填量を制御することが可能となる。 When the main punches 11 and 12 and the sub-punch 15 are constituted by a plurality of divided punches as described above, the raw material powder filling amount in the separating direction among the surfaces of the green compact formed by the divided punches. Further, it is possible to finely control the compression ratio and obtain a green compact with a more uniform density. For example, in the above reference example , the pin 19 is located in the center of the sub punch 15 where the pin 19 is projected when viewed from the cavity 14 side in the direction of separation of the sub punch 15. When compression is performed with one sub punch 15, the filling amount of the raw material powder is different compared to the portions on both sides thereof, and the compression ratio also changes. On the other hand, the sub punch 15 is divided at the center portion and both side portions. By independently separating them, it is possible to control the filling amount between the central portion and both side portions so that the compression ratio becomes uniform according to the difference in the filling amount of the raw material powder.

さらに、本参考例では、チップ本体1の他の周面5に対応する圧粉体の面と、この他の周面5と上記平板面2との交差稜線部に形成される断面1/4凸円弧状のコーナ稜線部8に対応する部分の一部または全部、あるいはその全部と平板面2のコーナ稜線部8側の縁部とが、図3(a)〜(c)に示したようにダイ13に形成された凹部16によって成形されるようになされている。しかるに、この点、例えばこのような凹部16をダイ13側に設けずに、図3(d)に示すように平板面2からコーナ稜線部8の全部に対応する圧粉体部分を上記主パンチ11,12によって成形しようとすると、この主パンチ11,12のプレス面11A,12Aの縁部に形成される凹曲面部17と主パンチ11,12のダイ13に摺接する外周面18とがなす交差角αが限りなく0°に近くなり、その交差稜線部分の強度が損なわれて欠損を生じてしまうおそれがあるが、上述のようにコーナ稜線部8の少なくとも一部に対応する部分をダイ13によって成形するようにした本参考例では、この交差角αを望ましくは45°以上と大きく確保することができて、このような主パンチ11,12の欠損を防止することが可能となる。 Furthermore, in this reference example , the cross-section 1/4 formed on the surface of the green compact corresponding to the other peripheral surface 5 of the chip body 1 and the intersecting ridge line portion between the other peripheral surface 5 and the flat plate surface 2. As shown in FIGS. 3A to 3C, a part or all of the portion corresponding to the convex arcuate corner ridge line portion 8 or all of the portion and the edge portion on the corner ridge line portion 8 side of the flat plate surface 2 are shown in FIGS. It is made to be formed by a recess 16 formed in the die 13. However, in this respect, for example, without providing the concave portion 16 on the die 13 side, the green compact portion corresponding to the entire corner ridge line portion 8 from the flat plate surface 2 as shown in FIG. 11 and 12, the concave curved surface portion 17 formed at the edge of the press surfaces 11A and 12A of the main punches 11 and 12 and the outer peripheral surface 18 in sliding contact with the die 13 of the main punches 11 and 12 are formed. The crossing angle α may be as close to 0 ° as possible, and the strength of the crossing ridge line portion may be impaired and a defect may occur. However, as described above, a portion corresponding to at least a part of the corner ridgeline portion 8 is die-shaped. In the present reference example formed by No. 13, this crossing angle α can be ensured to be as large as 45 ° or more, and it is possible to prevent the main punches 11 and 12 from being lost.

ところで、このような主パンチ11,12や、あるいは副パンチ15の欠損のおそれは、互いに異なる方向から離接するこれら主パンチ11,12と副パンチ15とがそれぞれ接近してキャビティー14を画成する際に、例えば主パンチ11,12や副パンチ15の駆動手段の制御誤差等により、該主パンチ11,12と副パンチ15とがともに所定のキャビティー14を画成する位置よりも内側に接近しすぎて互いに干渉あるいは接触することによっても生じうる。そこで、このような干渉や接触による主パンチ11,12や副パンチ15の欠損を確実に防ぐには、図9に示す本参考例の他の変形例や図10に示すその他の変形例のように、上記プレス成形金型において、これら主パンチ11,12と副パンチ15とを、上記キャビティー14が画成される原料粉末の圧縮終了位置において互いに間隔をあけて配置されるようにすればよい。そして、この場合にも本参考例の製造方法においては、この間隔をあけた部分では圧粉体の表面がダイ13によって成形されることとなる。 By the way, there is a possibility that the main punches 11 and 12 or the sub-punch 15 may be lost, so that the main punches 11 and 12 and the sub-punch 15 that are separated from each other approach each other to define the cavity 14. In this case, the main punches 11 and 12 and the sub punch 15 are both inside the position defining the predetermined cavity 14 due to, for example, a control error of the driving means of the main punches 11 and 12 and the sub punch 15. It can also be caused by too close to interfere or contact each other. Therefore, in order to reliably prevent the main punches 11 and 12 and the sub punch 15 from being lost due to such interference and contact, other modified examples of this reference example shown in FIG. 9 and other modified examples shown in FIG. In addition, in the press mold, the main punches 11 and 12 and the sub punch 15 are arranged at a distance from each other at the compression end position of the raw material powder in which the cavity 14 is defined. Good. In this case as well, in the manufacturing method of the present reference example , the surface of the green compact is formed by the die 13 at the portion where the gap is provided.

ここで、図9に示す変形例では、主パンチ11,12のプレス面11A,12Aが、副パンチ15の圧縮終了時におけるそのプレス面15Aの位置よりも該副パンチ15の離接方向(図9における左右方向)においてキャビティ14の内側に位置するように、圧粉体において成形されるチップ本体1の上記平板面2に対応する面よりもこの副パンチ15の離接方向に小さくされることにより、原料粉末の圧縮終了位置においてこれら主パンチ11,12と副パンチ15との間に間隔Xがあけられるようにされている。従って、この場合にも主パンチ11,12は、圧粉体における上記平板面2に対応する面の間隔X部分を除いた一部のみを成形することとなり、この間隔X部分すなわちチップ本体1の少なくとも平板面2のうち切刃4に連なる部分に対応する圧粉体部分は、主パンチ11,12の離接方向を向いて該間隔Xの幅を有するダイ13側の成形面13Cによって成形されることとなる。   Here, in the modification shown in FIG. 9, the press surfaces 11 </ b> A and 12 </ b> A of the main punches 11 and 12 are in contact with and separated from the position of the press surface 15 </ b> A at the end of compression of the sub punch 15 (FIG. 9 in the direction of the contact of the sub punch 15 with respect to the surface corresponding to the flat plate surface 2 of the chip body 1 formed in the green compact so as to be located inside the cavity 14 in the horizontal direction in FIG. Thus, an interval X is provided between the main punches 11 and 12 and the sub punch 15 at the compression end position of the raw material powder. Accordingly, in this case as well, the main punches 11 and 12 are formed only on a part of the green compact excluding the interval X portion of the surface corresponding to the flat plate surface 2. At least the green compact portion corresponding to the portion of the flat plate surface 2 connected to the cutting edge 4 is formed by the forming surface 13C on the die 13 side facing the separating contact direction of the main punches 11 and 12 and having the width X. The Rukoto.

また、これとは逆に図10に示す変形例では、図10(a)に示すように副パンチ15のプレス面15Aが、主パンチ11,12の圧縮終了時におけるそのプレス面11A,12Aの位置よりも該主パンチ11,12の離接方向(図10(a)〜(c)における上下方向)においてキャビティ14の内側に位置するように、圧粉体におけるチップ本体1のすくい面3に対応する面よりも小さくされることにより、原料粉末の圧縮終了位置においてこれら主パンチ11,12と副パンチ15との間に間隔Xがあけられるようにされている。従って、この場合には、副パンチ15は圧粉体における上記すくい面3に対応する面の一部のみを成形することとなり、残りのすくい面3に対応する面は副パンチ15の離接方向を向くダイ13の成形面13Dによって成形される。   On the contrary, in the modification shown in FIG. 10, the press surface 15 </ b> A of the sub-punch 15 is formed on the press surfaces 11 </ b> A and 12 </ b> A at the end of compression of the main punches 11 and 12, as shown in FIG. On the rake face 3 of the chip body 1 in the green compact so as to be located inside the cavity 14 in the direction of separation of the main punches 11 and 12 (the vertical direction in FIGS. 10A to 10C) rather than the position. By making it smaller than the corresponding surface, an interval X is provided between the main punches 11 and 12 and the sub punch 15 at the compression end position of the raw material powder. Accordingly, in this case, the sub punch 15 forms only a part of the surface corresponding to the rake face 3 in the green compact, and the surface corresponding to the remaining rake face 3 is in the direction of contact / separation of the sub punch 15. Is formed by the forming surface 13D of the die 13 facing the surface.

ただし、この図10に示す変形例においてプレス面15Aは、図10(b)に示すようにすくい面3に対応する面から全周に亙って間隔X分だけ一回り小さくなるようにされていてもよく、この場合に上記成形面13Dは、副パンチ15の離接方向から見て上記間隔Xの幅で周回する概略窓枠状とされる。また、プレス面15Aは図10(c)に示すように主パンチ11,12との接触のおそれがある部分だけ間隔Xで小さくされていてもよく、この場合に成形面13Dは、副パンチ15の離接方向から見て主パンチ11,12の圧縮終了時におけるプレス面11A,12Aの位置から内側に上記間隔Xの幅で該プレス面11A,12Aに沿って延びる帯状に形成される。   However, in the modification shown in FIG. 10, the press surface 15A is made smaller by an interval X over the entire circumference from the surface corresponding to the rake face 3 as shown in FIG. 10 (b). In this case, the molding surface 13 </ b> D has a substantially window frame shape that circulates with the width of the interval X as seen from the separation / contact direction of the sub punch 15. Further, as shown in FIG. 10C, the press surface 15A may be made smaller by an interval X only at a portion where there is a possibility of contact with the main punches 11 and 12. In this case, the molding surface 13D is formed by the sub punch 15 When the compression of the main punches 11 and 12 is finished, the strips are formed in strips extending along the press surfaces 11A and 12A with the width of the interval X inward from the positions of the press surfaces 11A and 12A when the main punches 11 and 12 are compressed.

従って、これらのような第1の参考例の変形例によれば、上述のようにキャビティー14が画成された状態で原料粉末の圧縮終了位置における主パンチ11,12と副パンチ15との間に間隔Xがあけられるので、たとえその離接のための駆動手段に制御誤差等が生じたりして該主パンチ11,12と副パンチ15とが所定の圧縮終了位置より接近しすぎてキャビティ14内に突出してしまったとしても、図9に示した変形例では副パンチ15の突出量が上記間隔X以下であれば、また図10に示した変形例では主パンチ11,12の突出量が間隔X以下であれば、これら主パンチ11,12と副パンチ15とが接触したり干渉したりすることはなく、その欠損を防止することができる。 Therefore, according to the modifications of the first reference example as described above, the main punches 11 and 12 and the sub punch 15 at the compression end position of the raw material powder in the state where the cavity 14 is defined as described above. Since there is a gap X between them, even if a control error or the like occurs in the drive means for the separation and contact, the main punches 11 and 12 and the sub punch 15 are too close to the predetermined compression end position, and the cavity 9, even if the amount of protrusion of the sub-punch 15 is equal to or smaller than the distance X in the modification shown in FIG. 9, the amount of protrusion of the main punches 11 and 12 in the modification shown in FIG. If the distance is equal to or less than the distance X, the main punches 11 and 12 and the sub punch 15 do not come into contact with each other or interfere with each other, and the loss can be prevented.

しかも、図9に示した変形例では、主パンチ11,12の突出量に関わらず副パンチ15の突出量が上記間隔X未満であれば、圧粉体においてチップ本体1の切刃4,6およびコーナ部7に対応する稜線部は副パンチ15のプレス面15Aの外周縁そのままに所定の輪郭を描くように成形されることとなり、また図10に示した変形例でも、図10(b)に示した例の場合には、主パンチ11,12の圧縮終了位置が所定の位置であれば、圧粉体における切刃4,6およびコーナ部7に対応する稜線部は、副パンチ15の突出量に関わらずダイ13に形成されたプレス面15Aより一回り大きな成形面13Dの辺稜部と主パンチ11,12のプレス面11A,12Aの副パンチ15側辺稜部とによって成形される。すなわち、これらの変形例、特に図9に示した変形例では、切削工具の切刃部材として重要なチップ本体1の切刃4,6およびコーナ部7となる部分を圧粉体において確実に所定の形状、寸法に成形することができるので、切削加工に用いて高精度の加工を行うことが可能な切刃部材(スローアウェイチップ)を提供することができる。   In addition, in the modification shown in FIG. 9, the cutting edges 4 and 6 of the chip body 1 in the green compact if the protruding amount of the sub punch 15 is less than the interval X regardless of the protruding amount of the main punches 11 and 12. The ridge line portion corresponding to the corner portion 7 is formed so as to draw a predetermined outline as it is on the outer peripheral edge of the press surface 15A of the sub punch 15, and also in the modification shown in FIG. In the case of the example shown in FIG. 5, if the compression end position of the main punches 11 and 12 is a predetermined position, the ridge line portions corresponding to the cutting edges 4 and 6 and the corner portion 7 in the green compact are Regardless of the amount of protrusion, it is formed by the side ridge portion of the molding surface 13D that is slightly larger than the press surface 15A formed on the die 13 and the side ridge portion of the main punches 11 and 12 on the secondary punch 15 side of the press surfaces 11A and 12A. . That is, in these modified examples, particularly in the modified example shown in FIG. 9, the portions that become the cutting blades 4 and 6 and the corner portion 7 of the chip body 1 that are important as the cutting blade member of the cutting tool are reliably specified in the green compact. Therefore, it is possible to provide a cutting blade member (throw away tip) that can be used for cutting and can be processed with high accuracy.

ただし、上記間隔Xは、これが小さすぎると、主、副パンチ11,12,15の駆動手段の制御誤差によってはこれら主パンチ11,12と副パンチ15との接触や干渉を確実に防ぐことができなくなるおそれがある。一方、逆にこの間隔Xが大きすぎると上記成形面13C,13Dの幅も大きくなり、すなわち離接しないダイ13によって圧粉体が成形される部分が大きくなって、異なる方向から離接する上記主パンチ11,12と副パンチ15とによって原料粉末を圧縮することにより圧粉体において圧縮の均一化を図るという効果を十分に奏することができなくなるおそれが生じる。このため、上記間隔Xは0.01mm〜5mmの範囲に設定されるのが望ましい。   However, if the distance X is too small, contact or interference between the main punches 11 and 12 and the sub punch 15 can be reliably prevented depending on the control error of the driving means of the main and sub punches 11, 12 and 15. There is a risk that it will not be possible. On the other hand, if the distance X is too large, the widths of the molding surfaces 13C and 13D also increase, that is, the portion where the green compact is molded by the die 13 that does not come into contact / separate becomes large. By compressing the raw material powder by the punches 11 and 12 and the sub punch 15, there is a possibility that the effect of achieving uniform compression in the green compact cannot be sufficiently achieved. For this reason, it is desirable that the interval X is set in a range of 0.01 mm to 5 mm.

なお、これら図9と図10に示した変形例は適宜組み合わせてもよく、すなわち副パンチ15の少なくとも一方と、主パンチ11,12の一方とには図9の変形例を適用して間隔Xをあけるとともに、主パンチ11,12の他方とには図10の変形例を適用するようにしてもよい。また、これら図9、図10の変形例の双方を組み合わせて、主パンチ11,12のプレス面11A,12Aは、圧縮終了時の副パンチ15のプレス面15Aの位置よりもその離接方向おいてキャビティ14内側に位置するようにして、圧粉体における上記平板面2に対応する面よりも副パンチ15の離接方向に小さくするとともに、副パンチ15のプレス面15Aも、主パンチ11,12の圧縮終了時のプレス面11A,12Aの位置よりその離接方向おいてキャビティ14内側に位置するようにして、圧粉体におけるすくい面3に対応する面よりも全周に亙ってあるいは部分的に小さくなるようにしてもよい。この場合において上記間隔Xは、上記圧縮終了位置における主パンチ11,12のプレス面11A,12Aと副パンチ15のプレス面15Aとの隣接する辺稜部同士の間隔とすればよい。   9 and FIG. 10 may be combined as appropriate, that is, at least one of the sub punches 15 and one of the main punches 11 and 12 may be applied by applying the modification of FIG. 10 may be applied to the other of the main punches 11 and 12. Further, by combining both of the modified examples of FIGS. 9 and 10, the press surfaces 11A and 12A of the main punches 11 and 12 are closer to and away from the position of the press surface 15A of the sub punch 15 at the end of compression. And is located in the cavity 14 so as to be smaller in the direction in which the sub punch 15 is separated from the surface corresponding to the flat plate surface 2 of the green compact, and the press surface 15A of the sub punch 15 is also formed in the main punch 11, 12 so that it is located inside the cavity 14 in the direction of separation from the position of the press surfaces 11A, 12A at the end of compression, or over the entire circumference of the surface corresponding to the rake face 3 in the green compact. It may be partially reduced. In this case, the interval X may be an interval between adjacent edge portions of the press surfaces 11A and 12A of the main punches 11 and 12 and the press surface 15A of the sub punch 15 at the compression end position.

さらに、上記図10(b)に示した変形例においては、上述のようにダイ13の成形面13Dが副パンチ15の離接方向から見て上記間隔Xの幅で周回する概略窓枠状とされていて、その内側に望むように接近した副パンチ15のプレス面15Aと該成形面13Dとにより、圧粉体においてチップ本体1のすくい面3に対応する面が成形されるようになされている。そこで、このような変形例によって、例えば図24および図8(a)に示したようにチップ本体1のすくい面3において切刃4,6およびコーナ部7の内側にランド部20を介して凹溝状のチップブレーカ9や平坦面21が形成された縦刃式スローアウェイチップを製造する場合には、図6に示した変形例において副パンチ15のプレス面15A側に形成されていた平坦面15Dや、この平坦面15Dと凸部15C、あるいはこれらに加えて凹部15Bの底面15E周縁までの部分を、上記ダイ13側の成形面13Dに形成するようにしてもよい。   Furthermore, in the modified example shown in FIG. 10B, as described above, a substantially window frame shape in which the molding surface 13D of the die 13 circulates with the width of the interval X when viewed from the contact / separation direction of the sub punch 15; The surface corresponding to the rake face 3 of the chip body 1 is molded in the green compact by the pressing surface 15A of the sub punch 15 and the molding surface 13D which are close to each other as desired. Yes. Therefore, according to such a modification, for example, as shown in FIG. 24 and FIG. 8A, the rake face 3 of the chip body 1 is recessed via the land portion 20 inside the cutting edges 4 and 6 and the corner portion 7. In the case of manufacturing a vertical blade type throwaway tip in which the groove-shaped chip breaker 9 or the flat surface 21 is formed, the flat surface formed on the press surface 15A side of the sub punch 15 in the modification shown in FIG. 15D, the flat surface 15D and the convex portion 15C, or a portion up to the periphery of the bottom surface 15E of the concave portion 15B may be formed on the molding surface 13D on the die 13 side.

なお、このような場合においては、上記ダイ13側の成形面13Dと副パンチ15のプレス面15Aとの境界が、平坦面15Dと凸部15Cとの境界、またはこの凸部15Cの突端、あるいは凹部15Bの底面15Eの周縁などに位置するように設定するのが望ましい。これにより、チップ本体1のすくい面3においてランド部20とチップブレーカ9との境界、または凹溝状のチップブレーカ9の溝底、あるいはこのチップブレーカ9が隆起して平坦面21と交差する交差稜線部など、このすくい面3が曲折する折れ線部分に対応する部分に成形面13Dとプレス面15Aとの境界を位置させるようにして圧粉体をプレス成形することができるので、例えば上述のように副パンチ15の駆動手段に制御誤差が生じたりしてプレス面15Aの位置がずれた場合でも、このプレス面15Aと成形面13Dとのずれによって圧粉体に形成される段差が、チップ本体1においてランド部20上や平坦面21上、あるいはチップブレーカ9の傾斜面上に形成されたりするのを避けることができる。   In such a case, the boundary between the molding surface 13D on the die 13 side and the pressing surface 15A of the sub punch 15 is the boundary between the flat surface 15D and the convex portion 15C, or the protruding end of the convex portion 15C, or It is desirable to set so that it may be located in the periphery of the bottom face 15E of the recessed part 15B. As a result, at the rake face 3 of the chip body 1, the boundary between the land portion 20 and the chip breaker 9, the groove bottom of the concave chip breaker 9, or the intersection where the chip breaker 9 rises and intersects the flat surface 21. Since the green compact can be press-molded such that the boundary between the molding surface 13D and the pressing surface 15A is located at a portion corresponding to the broken line portion where the rake face 3 bends, such as a ridge line portion, for example, as described above Even when a control error occurs in the driving means of the sub punch 15 and the position of the press surface 15A is displaced, the step formed on the green compact due to the displacement between the press surface 15A and the molding surface 13D is not possible. 1 can be prevented from being formed on the land portion 20, the flat surface 21, or the inclined surface of the chip breaker 9.

次に、図11ないし図17は、本発明の切削工具の切刃部材の製造方法および該製造方法に用いられる圧粉体のプレス成形金型の第2の参考例を示すものであり、この第2の参考例のプレス成形金型において上記第1の参考例のプレス成形金型と共通する部分には同一の符号を配して説明を省略する。本参考例では、第1の参考例と同様に図4に示した方形平板状の縦刃式のスローアウェイチップを製造するのに際して、圧粉体においてチップ本体1の上記平板面2に対応する面を主パンチ11,12によって成形するとともに、他の周面5に対応する面をこの主パンチ11,12の離接方向とは異なる方向から離接する副パンチ23によって成形するものである。 Next, FIG. 11 to FIG. 17 show a second reference example of a method for manufacturing a cutting blade member of a cutting tool of the present invention and a press molding die of a green compact used in the manufacturing method. In the press-molding die of the second reference example , the same reference numerals are assigned to portions common to the press-molding die of the first reference example , and description thereof is omitted. In this reference example , when the rectangular flat plate type vertical blade type throwaway tip shown in FIG. 4 is manufactured as in the first reference example , the green compact corresponds to the flat plate surface 2 of the chip body 1 in the green compact. The surface is formed by the main punches 11 and 12, and the surface corresponding to the other peripheral surface 5 is formed by the sub-punch 23 that is separated from the direction in which the main punches 11 and 12 are separated from each other.

すなわち、図11および図12に示すように、本参考例においても主パンチ11,12は上下方向に離接させられるとともに、これら上下の主パンチ11,12間に画成されるキャビティー14に向けては一対の上記副パンチ23が、そのプレス面23Aを互いに対向させて1直線上に水平方向に離接させられる。そして、これらの副パンチ23のプレス面23Aには、第1の参考例においてダイ13に形成されたのと同様に、圧粉体においてチップ本体1の他の周面5に対応する面を成形する底面16Aと、コーナ稜線部8に対応する部分の少なくとも一部を成形する断面円弧をなす凹曲面状の壁面16Bとを備えた凹部16が形成されており、これらの副パンチ23が主パンチ11,12とともに上記キャビティー14に投入された原料粉末を圧縮することにより、上記縦刃式スローアウェイチップに製造される圧粉体がプレス成形される。 That is, as shown in FIGS. 11 and 12, also in this reference example , the main punches 11 and 12 are separated from each other in the vertical direction, and the cavity 14 defined between the upper and lower main punches 11 and 12 is formed. The pair of sub-punches 23 are separated from each other in the horizontal direction on one straight line with their press surfaces 23A facing each other. Then, a surface corresponding to the other peripheral surface 5 of the chip body 1 in the green compact is formed on the press surface 23A of these sub punches 23 in the same manner as that formed on the die 13 in the first reference example . A recess 16 having a bottom surface 16A and a concave curved wall 16B having a cross-sectional arc forming at least a part of a portion corresponding to the corner ridgeline portion 8 is formed. By compressing the raw material powder charged into the cavity 14 together with 11 and 12, the green compact produced in the vertical blade type throwaway tip is press-molded.

なお、キャビティー14内の主パンチ11,12の離接方向と副パンチ23の離接方向との双方に直交する方向(図11においては図面に垂直な方向。図12においては左右方向)を向く面はダイ13に形成され、この直交方向に垂直すなわち主、副パンチ11,12,23の離接方向に平行な平坦面とされて、圧粉体におけるチップ本体1の上記すくい面3に対応する面を成形するダイ13側の成形面24とされる。従って、この成形面24に、キャビティー14に対して後退する凹部とキャビティー14に向けて突出する凸部とのうち少なくとも一方を形成しておけば、この凹凸部を反転させた形状のチップブレーカに対応する凸凹部を圧粉体の上記すくい面3に対応する面に成形することができる。   Note that the direction perpendicular to both the contact / separation direction of the main punches 11 and 12 in the cavity 14 and the contact / separation direction of the sub punch 23 (the direction perpendicular to the drawing in FIG. 11 and the left-right direction in FIG. 12). The facing surface is formed on the die 13 and is a flat surface perpendicular to the orthogonal direction, that is, parallel to the contact / separation direction of the main and sub-punches 11, 12, and 23. The corresponding surface is formed as a forming surface 24 on the die 13 side. Accordingly, if at least one of a concave portion retreating with respect to the cavity 14 and a convex portion protruding toward the cavity 14 is formed on the molding surface 24, a chip having a shape in which the concave and convex portions are inverted. Convex and concave portions corresponding to the breaker can be formed on a surface corresponding to the rake surface 3 of the green compact.

また、このダイ13も、キャビティー14を間にして図12に示す分割面Pから主パンチ11,12の離接方向に平行な上下方向に分割される複数の分割ダイ13A,13Bにより構成される。勿論、主パンチ11,12の離接方向に垂直な水平方向、例えば図11における左右方向や図12における左右方向にダイ13を分割するようにしてもよい。ただし、上述のようにダイ13側の成形面24に凹部や凸部が形成される場合には、ダイ13はこの凹部や凸部が凹凸する上記主パンチ11,12の離接方向と副パンチ23の離接方向との双方に直交する水平方向に分割される。また、この参考例のプレス成形金型によって圧粉体をプレス成形する際の第2の参考例の製造方法における主パンチ11,12および副パンチ23の離接動作は、図5(a)〜(c)に示した第1の参考例の場合と同様でよい。 Further, the die 13 is also constituted by a plurality of divided dies 13A and 13B which are divided in the vertical direction parallel to the contact / separation direction of the main punches 11 and 12 from the divided surface P shown in FIG. The Of course, the die 13 may be divided in a horizontal direction perpendicular to the direction in which the main punches 11 and 12 are separated from each other, for example, in the left-right direction in FIG. However, when a concave portion or a convex portion is formed on the molding surface 24 on the die 13 side as described above, the die 13 is separated from the main punches 11 and 12 where the concave portion and the convex portion are concave and convex and the sub punch. It is divided in the horizontal direction orthogonal to both of the separation / contact directions of 23. Further, the operation of separating the main punches 11 and 12 and the sub punch 23 in the manufacturing method of the second reference example when the green compact is press-molded by the press molding die of this reference example is shown in FIGS. It may be the same as the case of the first reference example shown in (c).

従って、このような第2の参考例においても、第1の参考例と同様にキャビティー14に投入される原料粉末が、主パンチ11,12とこれら主パンチ11,12の離接方向とは異なる方向に離接させられる副パンチ23とによって圧縮されて圧粉体がプレス成形されるので、この圧粉体において原料粉末の圧縮の均一化を図ることができ、こうして成形された圧粉体を焼結することにより、微少な変形や歪みを抑えて極めて高精度の切刃部材(縦刃式スローアウェイチップ)を製造することが可能となる。すなわち、本参考例では、チップ本体1の他の周面5とコーナ稜線部8の少なくとも一部に対応する部分を圧粉体に成形するキャビティー14に対して後退した凹部16が、この主パンチ11,12とは異なる方向にキャビティー14に向けて離接する副パンチ23のキャビティー14側を向くプレス面23Aに形成されており、該副パンチ23が原料粉末の投入されたキャビティー14に向けて接近することにより、この凹部16の後退量が大きくても該凹部16内に原料粉末を十分に充填しつつ主パンチ11,12とともに圧縮して原料粉末が均一に圧縮された圧粉体を成形することができる。 Therefore, in the second reference example as well, the raw powder charged into the cavity 14 is the main punches 11 and 12 and the contact / separation direction of the main punches 11 and 12 as in the first reference example. Since the green compact is compressed and pressed by the sub-punch 23 separated and contacted in different directions, it is possible to make the compression of the raw material powder uniform in this green compact. By sintering, it becomes possible to manufacture a cutting blade member (vertical blade type throw-away tip) with extremely high accuracy while suppressing slight deformation and distortion. That is, in the present reference example , the concave portion 16 that is recessed with respect to the cavity 14 that molds the portion corresponding to at least a part of the other peripheral surface 5 of the chip body 1 and the corner ridgeline portion 8 into the green compact is the main portion. It is formed on the press surface 23A facing the cavity 14 side of the sub punch 23 that is separated from and coming into contact with the cavity 14 in a direction different from the punches 11 and 12, and the sub punch 23 is a cavity 14 into which raw material powder is charged. Even when the recess 16 has a large retraction amount, it is compressed together with the main punches 11 and 12 while the raw material powder is sufficiently filled in the recess 16, and the raw powder is uniformly compressed. The body can be shaped.

ところで、このように凹部16が副パンチ23に形成された第2の参考例においても、特に該凹部16の上記壁面16Bが上述のように断面円弧の凹曲面状に形成されていると、この壁面16Bとダイ13と摺接する副パンチ23の外周面25とがなす交差角βが小さすぎる場合、例えば上記壁面16Bが断面1/4凹円弧状とされていて交差角βが限りなく0°に近くなる場合には、この壁面16Bと外周面25との交差稜線部分の強度が著しく損なわれてしまう。そして、このように上記交差稜線部分の強度が損なわれた副パンチ23と主パンチ11,12が、それぞれの駆動手段の制御誤差等によって接触したり干渉を生じたりすると、この交差稜線部分が容易に欠損してしまう結果となる。 By the way, also in the second reference example in which the concave portion 16 is formed in the sub punch 23 in this way, particularly when the wall surface 16B of the concave portion 16 is formed in a concave curved surface shape having a cross-section arc as described above, When the intersection angle β formed by the wall surface 16B and the outer peripheral surface 25 of the sub punch 23 that is in sliding contact with the die 13 is too small, for example, the wall surface 16B has a ¼ concave arc shape in cross section and the intersection angle β is infinitely 0 °. In the case of approaching, the strength of the intersecting ridge line portion between the wall surface 16B and the outer peripheral surface 25 is significantly impaired. Then, when the sub punch 23 and the main punches 11 and 12 whose strengths of the intersecting ridge portions are thus damaged are brought into contact or cause interference due to control errors of the respective driving means, the intersecting ridge portions are easily formed. Result in loss.

そこで、このような副パンチ23の欠損を防止するのに、1つには、上記第1の参考例の場合と同様に、この副パンチ23と主パンチ11,12とを、図13(a)〜(c)に示す変形例のようにその圧縮終了位置において互いに間隔Xをあけて配置されるようにすればよい。ここで、図13(a)に示す変形例では、副パンチ23のプレス面23Aに、圧粉体においてチップ本体1の上記他の周面5に対応する面全部を成形する底面16Aと、コーナ稜線部8のうちこの他の周面5側の一部に対応する面を成形する断面凹円弧状の壁面16Bとが形成される一方、主パンチ11,12のプレス面11A,12Aにも、第1の参考例の図3(a)に示したのと同じように、副パンチ23側の両側縁部に断面円弧状の凹曲面部17が形成され、これら主パンチ11,12と副パンチ23とが圧縮終了位置に達したところで、副パンチ23の上記壁面16と外周面25との交差稜線部と、主パンチ11,12の上記凹曲面部17の突端との間に図示のような間隔Xがあけられる。従って、この変形例では、圧粉体においてチップ本体1のコーナ稜線部8のうちの一部に対応する部分が、上記間隔X部分においてキャビティ14を画成することとなるダイ13側の成形面13Eによって成形される。 Therefore, in order to prevent such a loss of the secondary punch 23, as in the case of the first reference example , the secondary punch 23 and the main punches 11 and 12 are connected to each other as shown in FIG. ) To (c) as in the modification examples, the compression end positions may be arranged with an interval X therebetween. Here, in the modification shown in FIG. 13 (a), a bottom surface 16A for molding the entire surface corresponding to the other peripheral surface 5 of the chip body 1 in the green compact on the press surface 23A of the sub punch 23, and a corner While the ridgeline portion 8 is formed with a concave arcuate wall surface 16B that forms a surface corresponding to a part of the other peripheral surface 5 side, on the press surfaces 11A and 12A of the main punches 11 and 12, As shown in FIG. 3A of the first reference example , concave curved surface portions 17 having an arc cross section are formed on both side edges on the side of the sub punch 23, and these main punches 11 and 12 and the sub punches are formed. 23, when the compression end position is reached, between the intersecting ridge line portion of the wall surface 16 and the outer peripheral surface 25 of the sub punch 23 and the protruding end of the concave curved surface portion 17 of the main punches 11 and 12, as shown in the figure. An interval X is provided. Therefore, in this modification, a portion corresponding to a part of the corner ridge line portion 8 of the chip body 1 in the green compact defines the cavity 14 in the interval X portion, and the molding surface on the die 13 side. Molded by 13E.

また、図13(b)に示す変形例では、副パンチ23のプレス面23Aは、上記凹部16のうち圧粉体においてチップ本体1の他の周面5に対応する面全部を成形する底面16Aのみが形成されて平面状とされるとともに、主パンチ11,12のプレス面11A,12Aも図3(b)に示したのと同様に、圧粉体においてチップ本体1の上記平板面2に対応する面の全部のみを成形する平面状とされており、従ってこれら主パンチ11,12のプレス面11A,12Aと外周面18との交差角αおよび副パンチ23のプレス面23Aと外周面25との交差角βは90°とされ、圧粉体においてチップ本体1のコーナ稜線部8の全部に対応する部分が、これら主パンチ11,12と副パンチ23との間隔X部分においてダイ13側の成形面13Eにより成形される。さらに、図13(c)に示す変形例では、主、副パンチ11,12,23のプレス面11A,12A,23Aが、圧粉体においてチップ本体1の平板面2と他の周面5のうちコーナ稜線部8側の縁部を除いた一部に対応する部分を成形するように平面状に形成されており、やはり外周面18,25との交差角α,βは90°とされるとともに、圧粉体においてコーナ稜線部8とこのコーナ稜線部8側の平板面2および他の周面5の縁部とに対応する部分は、主パンチ11,12と副パンチ23との間隔X部分に臨むダイ13の成形面13Eにより成形される。   Further, in the modification shown in FIG. 13B, the press surface 23A of the sub punch 23 is a bottom surface 16A that forms the entire surface of the recess 16 corresponding to the other peripheral surface 5 of the chip body 1 in the green compact. Only the press surfaces 11A and 12A of the main punches 11 and 12 are formed on the flat plate surface 2 of the chip body 1 in the green compact as shown in FIG. 3B. Accordingly, only the corresponding surfaces are formed into a flat shape. Therefore, the cross angle α between the press surfaces 11A and 12A of the main punches 11 and 12 and the outer peripheral surface 18 and the press surface 23A and the outer peripheral surface 25 of the sub punch 23 are used. Is 90 °, and the portion of the green compact corresponding to the entire corner ridge portion 8 of the chip body 1 is on the die 13 side in the space X between the main punches 11 and 12 and the sub punch 23. Molding surface 13E It is more molded. Furthermore, in the modification shown in FIG. 13C, the press surfaces 11A, 12A, and 23A of the main and sub punches 11, 12, and 23 are formed between the flat surface 2 of the chip body 1 and the other peripheral surface 5 in the green compact. Of these, it is formed in a flat shape so as to form a portion corresponding to a part excluding the edge on the corner ridge line portion 8 side, and the crossing angles α and β with the outer peripheral surfaces 18 and 25 are also 90 °. In addition, in the green compact, the portions corresponding to the corner ridgeline portion 8 and the edges of the flat plate surface 2 and the other peripheral surface 5 on the corner ridgeline portion 8 side are the distance X between the main punches 11 and 12 and the sub punch 23. It is molded by the molding surface 13E of the die 13 facing the part.

なお、これらの変形例においても、上記間隔Xは第1の参考例と同様に0.01mm〜5mmの範囲とされるのが望ましく、また上記交差角βも45°以上とされるのが望ましい。また、これら図13(a)〜(c)に示した変形例は、その主パンチ11,12側の構成と副パンチ23側の構成とを適宜組み替えて採用するようにしてもよく、例えば副パンチ23のプレス面23Aには図13(a)のように凹部16の底面16Aと断面凹円弧状の壁面16Bとを形成する一方で、主パンチ11,12のプレス面11A,12Aは図13(b)、(c)のように平面状として、圧粉体においてコーナ稜線部8に対応する部分のうち上記壁面16Bにより成形される部分以外の部分や平板面2の縁部に対応する部分をダイ13の成形面13Eによって成形するようにしてもよく、逆に主パンチ11,12のプレス面11A,12Aには図13(a)のように凹曲面部17を形成する一方で、副パンチ23のプレス面23Aは図13(b)、(c)のように平面状として、圧粉体においてコーナ稜線部8に対応する部分のうち凹曲面部17により成形される部分以外の部分や、圧粉体の他の周面5のコーナ稜線部8側の縁部に対応する部分を成形面13Eによって成形するようにしてもよい。さらに、上下の主パンチ11,12同士の間や一対の副パンチ23同士の間でも異なる構成を採用してもよい。 In these modifications, the interval X is preferably in the range of 0.01 mm to 5 mm as in the first reference example, and the intersection angle β is preferably 45 ° or more. . Further, in the modified examples shown in FIGS. 13A to 13C, the configuration on the main punches 11 and 12 side and the configuration on the sub punch 23 side may be appropriately combined and employed. On the press surface 23A of the punch 23, as shown in FIG. 13A, a bottom surface 16A of the recess 16 and a wall surface 16B having a concave arcuate cross section are formed, while the press surfaces 11A and 12A of the main punches 11 and 12 are shown in FIG. (B) As a flat shape as in (c), a portion corresponding to the corner ridgeline portion 8 in the green compact other than a portion formed by the wall surface 16B or a portion corresponding to an edge portion of the flat plate surface 2 May be formed by the molding surface 13E of the die 13, and conversely, the concave surfaces 17 are formed on the press surfaces 11A and 12A of the main punches 11 and 12 as shown in FIG. The press surface 23A of the punch 23 is 13 (b) and 13 (c) have a flat shape, the portion corresponding to the corner ridgeline portion 8 in the green compact, the portion other than the portion formed by the concave curved surface portion 17, and the other circumference of the green compact You may make it shape | mold the part corresponding to the edge by the side of the corner ridgeline part 8 of the surface 5 by the molding surface 13E. Furthermore, a different configuration may be adopted between the upper and lower main punches 11 and 12 or between the pair of sub punches 23.

一方、上述のような副パンチ23の欠損や主パンチ11,12の欠損を防止する手段の他の1つとして、本参考例では図14ないし図17に示す変形例のように、これら主パンチ11,12と副パンチ23のうちの一方のパンチに、その原料粉末の圧縮終了位置において他方のパンチの周面に摺接する摺接面を、この他方のパンチの離接方向に延びるように形成するようにしてもよい。ここで、図14および図15に示す変形例は副パンチ23が上記一方のパンチ、主パンチ11,12が他方のパンチとなる場合であって、副パンチ23のプレス面23Aには凹部16が形成されるとともに、この凹部16とダイ13に摺接する副パンチ23の外周面25との間に、主パンチ11,12の離接方向(上下方向)に延びる平面状の摺接面26が形成されている。また、図16および図17に示す変形例では、逆に主パンチ11,12が一方のパンチ、副パンチ23が他方のパンチとされて、主パンチ11,12のプレス面11A,12Aには凹曲面部17の少なくとも一部が形成されるとともに、その突端の上記外周面18との間に、副パンチ23の離接方向(図16,17における左右方向)に延びる平面状の摺接面27が形成される。 On the other hand, as another means for preventing the loss of the sub-punch 23 and the loss of the main punches 11 and 12 as described above, in this reference example , as shown in the modifications shown in FIGS. A slidable contact surface slidably contacting the peripheral surface of the other punch at the compression end position of the raw material powder is formed on one of the punches 11 and 12 and the sub punch 23 so as to extend in the direction of separating and contacting the other punch. You may make it do. Here, the modification shown in FIGS. 14 and 15 is a case where the sub punch 23 is the one punch and the main punches 11 and 12 are the other punch, and the concave surface 16 is formed on the press surface 23A of the sub punch 23. A flat slidable contact surface 26 is formed between the concave portion 16 and the outer peripheral surface 25 of the sub punch 23 that is in slidable contact with the die 13. Has been. 16 and 17, the main punches 11 and 12 are used as one punch and the sub punch 23 is used as the other punch, and the press surfaces 11A and 12A of the main punches 11 and 12 are recessed. At least a part of the curved surface portion 17 is formed, and a planar sliding contact surface 27 extending between the protruding end and the outer peripheral surface 18 in the direction of separating and contacting the sub punch 23 (left and right direction in FIGS. 16 and 17). Is formed.

これらのような変形例のプレス成形金型においては、原料粉末の圧縮終了前に、まず上記一方のパンチがその圧縮終了位置に達して位置決めされ、次いで他方のパンチがその外周面を一方のパンチの摺接面に摺接させつつ圧縮終了位置に達して位置決めされ、キャビティー14を画成する。すなわち、副パンチ23が摺接面26の形成された一方のパンチとされる場合には、図14(a)に示すように互いに異なる離接方向から主、副パンチ11,12,23が接近して原料粉末を圧縮しつつも、まず先に図14(b)に示すように副パンチ23が圧縮終了位置に達し、その摺接面26が、主パンチ11,12の外周面18と摺接するダイ13の摺接面13Fと面一となった状態で位置決めされる。なお、この時点で主パンチ11,12は、その離接方向に副パンチ23の外周面25を越えて接近してはいない。そして、このように副パンチ23が位置決めされた後で、主パンチ11,12が、その外周面18をダイ側の上記摺接面13Fから副パンチ23の摺接面26に摺接させつつ接近し、プレス面11A、12Aが凹部16の壁面16Bに滑らかに連なったところで圧縮終了位置に達して位置決めされることにより、図14(c)に示すようにキャビティー14が画成されて原料粉末の圧縮が終了し、圧粉体がプレス成形される。   In the press-molding dies of these modified examples, before the compression of the raw material powder, the one punch first reaches the compression end position, and then the other punch touches the outer peripheral surface of one punch. The compression end position is reached while being in sliding contact with the sliding contact surface, and the cavity 14 is defined. That is, when the sub punch 23 is one punch on which the sliding contact surface 26 is formed, the main and sub punches 11, 12, and 23 are approached from different contact directions as shown in FIG. Then, while compressing the raw material powder, first, as shown in FIG. 14B, the sub punch 23 first reaches the compression end position, and its sliding contact surface 26 slides on the outer peripheral surface 18 of the main punches 11 and 12. Positioning is performed in a state where it is flush with the sliding contact surface 13F of the die 13 in contact therewith. At this time, the main punches 11 and 12 are not approaching beyond the outer peripheral surface 25 of the sub punch 23 in the direction of separation. After the sub punch 23 is positioned in this way, the main punches 11 and 12 approach while the outer peripheral surface 18 is slidably contacted with the slidable contact surface 26 of the sub punch 23 from the slidable contact surface 13F on the die side. Then, when the press surfaces 11A and 12A are smoothly connected to the wall surface 16B of the recess 16, the compression end position is reached and positioned, whereby the cavity 14 is defined as shown in FIG. Is finished, and the green compact is press-molded.

また、摺接面27が形成された一方のパンチが主パンチ11,12である図16の変形例の場合には、図16(a)に示すようにやはり主、副パンチ11,12,23が異なる離接方向から接近して原料粉末を圧縮しつつ、まず図16(b)に示すように主パンチ11,12が先に圧縮終了位置に達して位置決めされることにより、上記摺接面27が副パンチ23の外周面25と摺接するダイ13側の摺接面13Gと面一とされる。そして、その後に副パンチ23が、その離接方向に主パンチ11,12の外周面18の位置を越えて接近して、そのプレス面23Aが主パンチ11,12の上記凹曲面部17と滑らかに連なったところで圧縮終了位置に達して位置決めされ、これにより図16(c)に示すようにキャビティー14が画成されて原料粉末の圧縮が終了するとともに圧粉体がプレス成形される。   Further, in the case of the modified example of FIG. 16 in which one of the punches on which the slidable contact surface 27 is formed is the main punches 11 and 12, as shown in FIG. The main punches 11 and 12 first reach the compression end position and are positioned as shown in FIG. 16B while compressing the raw material powder approaching from different separation directions. 27 is flush with the slidable contact surface 13G on the die 13 side that is in slidable contact with the outer peripheral surface 25 of the sub punch 23. Thereafter, the sub punch 23 approaches the separation / contact direction beyond the position of the outer peripheral surface 18 of the main punch 11, 12, and the press surface 23 A is smooth with the concave curved surface portion 17 of the main punch 11, 12. As shown in FIG. 16 (c), the cavity 14 is defined and the compression of the raw material powder is completed, and the green compact is press-molded.

なお、図14に示す変形例において、上記副パンチ23における摺接面26が凹部16に交差する位置は、図15(a)に示すように該凹部16における壁面16Bが、圧粉体においてチップ本体1のコーナ稜線部8の断面がなす1/4円弧の一部に対応する部分を成形するような位置とされていてもよく、この場合に上記1/4円弧の残りの一部に対応する部分は主パンチ11,12のプレス面11A,12Aに形成された凹曲面部17によって成形される。また、図15(b)に示すようにこの壁面16Bが上記1/4円弧の全部に対応する部分を成形したり、図15(c)に示すように壁面16Bがこの1/4円弧の全部とチップ本体1の平板面2におけるコーナ稜線部8側の縁部とに対応する部分を成形したりするような位置とされていてもよく、これらの場合には主パンチ11,12のプレス面11A,12Aは凹曲面部17を備えない平面状とされて、図15(b)の場合はチップ本体1における平板面2に対応する部分の全部が、また図15(c)の場合は上記縁部を除いた平板面2の一部に対応する部分が、圧粉体においてこれらプレス面11A,12Aによって成形される。   In the modification shown in FIG. 14, the position where the slidable contact surface 26 of the sub punch 23 intersects the recess 16 is such that the wall surface 16B of the recess 16 is a chip in the green compact as shown in FIG. The position corresponding to a part of the ¼ arc formed by the cross section of the corner ridge line portion 8 of the main body 1 may be formed, and in this case, the part corresponds to the remaining part of the ¼ arc. The portion to be formed is formed by a concave curved surface portion 17 formed on the press surfaces 11A and 12A of the main punches 11 and 12. Further, as shown in FIG. 15 (b), the wall surface 16B forms a portion corresponding to the entire ¼ arc, or as shown in FIG. 15 (c), the wall surface 16B forms the entire ¼ arc. And a position corresponding to the edge of the flat plate surface 2 of the chip body 1 on the corner ridge line portion 8 side may be formed. In these cases, the press surfaces of the main punches 11 and 12 may be used. 11A and 12A have a flat shape without the concave curved surface portion 17. In the case of FIG. 15B, all of the portions corresponding to the flat plate surface 2 in the chip body 1 and in the case of FIG. A portion corresponding to a part of the flat plate surface 2 excluding the edge portion is formed by the press surfaces 11A and 12A in the green compact.

一方、図16に示した変形例においても、主パンチ11,12における摺接面27が凹曲面部17に交差する位置は、図17(a)に示すように圧粉体においてチップ本体1のコーナ稜線部8の断面がなす1/4円弧の一部に対応する部分をこの凹曲面部17が成形するような位置とされていてもよく、この場合に上記1/4円弧の残りの一部に対応する部分は副パンチ23に形成された凹部16の壁面16Bにより成形される。また、図17(b)に示すように凹曲面部17が上記1/4円弧の全部に対応する部分を成形したり、図17(c)に示すように凹曲面部17がこの1/4円弧の全部とチップ本体1の他の周面5におけるコーナ稜線部8側の縁部とに対応する部分を成形したりするような位置とされていてもよく、これらの場合に副パンチ23のプレス面23Aは図16に示したように凹部16が形成されることのない平面状とされて、図17(b)の場合はチップ本体1の他の周面5に対応する圧粉体部分の全部が、また図17(c)の場合は上記縁部を除いた他の周面5の一部に対応する圧粉体部分がこのプレス面23Aによって成形される。   On the other hand, also in the modification shown in FIG. 16, the position where the slidable contact surface 27 of the main punches 11 and 12 intersects the concave curved surface portion 17 is the position of the chip body 1 in the green compact as shown in FIG. A portion corresponding to a part of a ¼ arc formed by the cross section of the corner ridge line portion 8 may be set to a position where the concave curved surface portion 17 is formed. In this case, the remaining one part of the ¼ arc is formed. A portion corresponding to the portion is formed by a wall surface 16 </ b> B of the recess 16 formed in the sub punch 23. Further, as shown in FIG. 17 (b), the concave curved surface portion 17 forms a portion corresponding to the entire ¼ arc, or as shown in FIG. The portion corresponding to the entire arc and the edge of the other peripheral surface 5 of the chip body 1 on the corner ridge line portion 8 side may be formed. In these cases, the sub punch 23 As shown in FIG. 16, the pressing surface 23A has a flat shape with no recess 16 formed. In the case of FIG. 17B, the green compact portion corresponding to the other peripheral surface 5 of the chip body 1 is used. In addition, in the case of FIG. 17C, a green compact portion corresponding to a part of the other peripheral surface 5 excluding the edge portion is formed by the press surface 23A.

従って、これらの変形例においては、主、副パンチ11,12,23の駆動手段の制御には高い精度が要求されるものの、摺接面26,27が形成されることにより、主パンチ11,12や副パンチ23のプレス面11A,12A,23Aと外周面18,25との交差稜線部に先端が鋭利となる強度の弱い部分が形成されるのを避けることができ、かかる部分における欠損の発生を防止することが可能となる。また、これらの変形例のプレス成形金型を用いた本参考例の製造方法の変形例では、上記図14(a)〜(c)や図16(a)〜(c)に示したように、原料粉末の圧縮終了前にまず上記一方のパンチがその圧縮終了位置に達して位置決めされ、次いで他方のパンチがその離接方向に一方のパンチの外周面の位置を越えて接近し、この一方のパンチの上記摺接面に摺接しながら圧縮終了位置に達して位置決めされることにより、キャビティー14が画成されて圧粉体がプレス成形されるので、一方のパンチの摺接面と他方のパンチの外周面との間に原料粉末が噛み込まれて詰まりを生じたりすることがない。すなわち、図14、15に示した変形例で副パンチ23が位置決めされる前に主パンチ11,12がダイ13からキャビティー14側に突出したり、図16、17に示した変形例で主パンチ11,12が位置決めされる前に副パンチ23が突出したりすると、外周面18,25と摺接面26,27との間に原料粉末が詰まりを生じ、副パンチ23または主パンチ11,12を所定の圧縮終了位置まで接近させることができなくなるおそれがある。 Therefore, in these modified examples, although high accuracy is required for controlling the driving means of the main and sub punches 11, 12, 23, the main punches 11, 26 are formed by forming the slidable contact surfaces 26, 27. 12 and the press surfaces 11A, 12A, 23A of the sub punch 23 and the outer peripheral surfaces 18, 25 can be prevented from forming a weak portion having a sharp tip, and defects in such portions can be prevented. Occurrence can be prevented. Moreover, in the modified example of the manufacturing method of this reference example using the press-molding die of these modified examples, as shown in FIGS. 14 (a) to (c) and FIGS. 16 (a) to (c). First, before the compression of the raw material powder, the one punch reaches the compression end position and is positioned, and then the other punch approaches the disengagement direction beyond the position of the outer peripheral surface of the one punch. Since the cavity 14 is defined and the green compact is press-molded by slidably contacting the above-mentioned slidable contact surface of the punch, the cavity 14 is defined, and the green compact is press-molded. The raw material powder is not caught between the outer peripheral surfaces of the punches and no clogging occurs. That is, the main punches 11 and 12 protrude from the die 13 toward the cavity 14 before the sub punch 23 is positioned in the modification shown in FIGS. 14 and 15, or the main punches in the modification shown in FIGS. If the auxiliary punch 23 protrudes before the positioning of the auxiliary punch 11 or 12, the raw material powder is clogged between the outer peripheral surfaces 18 and 25 and the sliding contact surfaces 26 and 27. There is a risk that it will not be possible to approach the predetermined compression end position.

なお、上記他方のパンチ(図14、15に示す変形例では主パンチ11,12、図16、17に示す変形例では副パンチ23)の離接方向における上記摺接面26,27の幅Wは、これが小さすぎると、一方のパンチ(図14、15に示す変形例では副パンチ23、図16、17に示す変形例では主パンチ11,12)において、その外周面18,25とプレス面11A,12A,23Aに形成された凹曲面部17や壁面16Bとの間隔すなわち上記交差稜線部の先端周辺の肉厚が小さくなり、十分な強度を確保することができずに欠損等を防止できなくなるおそれがある。しかしながら、この幅Wが大きすぎても、一方のパンチが圧縮終了位置に達して位置決めされてから、その摺接面26,27に他方のパンチが摺接しつつこの他方のパンチの圧縮終了位置に達するまでの移動量が大きくなってしまい、一方のパンチとともに原料粉末を圧縮することによる圧粉体の均一圧縮効果が損なわれてしまうおそれがあるので、上記摺接面26,27の幅Wは0.1mm〜5mmの範囲とされるのが望ましい。   The width W of the slidable contact surfaces 26 and 27 in the separating direction of the other punch (the main punches 11 and 12 in the modification shown in FIGS. 14 and 15 and the sub-punch 23 in the modification shown in FIGS. 16 and 17). If this is too small, the outer peripheral surfaces 18 and 25 and the press surface of one of the punches (sub punch 23 in the modification shown in FIGS. 14 and 15 and main punches 11 and 12 in the modification shown in FIGS. 16 and 17). The distance between the concave curved surface portion 17 and the wall surface 16B formed on 11A, 12A, and 23A, that is, the wall thickness around the tip of the intersecting ridge line portion is reduced, and sufficient strength cannot be ensured to prevent defects and the like. There is a risk of disappearing. However, even if the width W is too large, after one punch reaches the compression end position and is positioned, the other punch comes into sliding contact with the sliding contact surfaces 26 and 27 and reaches the compression end position of the other punch. Since the amount of movement until reaching a large value and the uniform compression effect of the green compact by compressing the raw material powder together with one of the punches may be impaired, the width W of the sliding contact surfaces 26 and 27 is It is desirable to be in the range of 0.1 mm to 5 mm.

ところで、図1ないし図10に示した第1の参考例では方形平板状の縦刃式スローアウェイチップに製造される圧粉体においてチップ本体1のすくい面3に対応する周面を副パンチ15によって成形する場合を、また図11ないし図17に示した第2の参考例では上記すくい面3に隣接する他の周面に対応する面を副パンチ23によって成形する場合をそれぞれ説明したが、これらを組み合わせて、主パンチ11,12の離接方向とも異なり、かつ互いにも異なる方向に離接させられる複数の副パンチ15,23により、主パンチ11,12とともに原料粉末を圧縮して圧粉体を成形するように構成してもよく、これによって原料粉末をより多方向から等方的に圧縮してさらに圧縮の均一な圧粉体を成形することが可能になり、従って一層高精度の寸法形状を有するスローアウェイチップすなわち切刃部材を製造することができる。なお、この場合においても圧粉体の一部はダイ13によって成形するようにしてもよく、また例えば図14ないし図17に示した第2の参考例の変形例において主パンチ11,12と副パンチ23とによって画成されたキャビティー14に、これら主パンチ11,12の離接方向と副パンチ23の離接方向との双方に直交する方向(図14ないし図17の図面に直交する方向)から、圧粉体においてすくい面3に対応する面を成形する副パンチ15が嵌挿されるように離接させれば、圧粉体のすべての面をこれら主、副パンチ11,12,15,23のプレス面11A,12A,15A,23Aによって成形することも可能となる。 By the way, in the first reference example shown in FIG. 1 to FIG. 10, the peripheral surface corresponding to the rake face 3 of the chip body 1 in the green compact manufactured to the vertical flat plate type throw-away chip is formed as the sub punch 15. In the second reference example shown in FIGS. 11 to 17, the case where the surface corresponding to the other peripheral surface adjacent to the rake face 3 is formed by the sub punch 23 has been described. Combining these, the raw powder is compressed together with the main punches 11 and 12 by a plurality of sub-punches 15 and 23 that are different from the contacting / separating directions of the main punches 11 and 12 in different directions. It may be configured to form the body, which makes it possible to compress the raw material powder isotropically from more directions to form a green compact with more uniform compression. It can be produced indexable i.e. cutting member having a degree of size and shape. In this case as well, a part of the green compact may be formed by the die 13, and the main punches 11 and 12 and the auxiliary punches are modified in the second reference example shown in FIGS. In the cavity 14 defined by the punch 23, a direction perpendicular to both the separation / contact direction of the main punches 11 and 12 and the separation / contact direction of the sub-punch 23 (direction orthogonal to the drawings of FIGS. 14 to 17). ) From the green compact, all the surfaces of the green compact are connected to the main and secondary punches 11, 12, and 15 so that the secondary punch 15 for forming the surface corresponding to the rake face 3 in the green compact is inserted and inserted. , 23 can be formed by the press surfaces 11A, 12A, 15A, 23A.

最後に、このような第1、第2の参考例およびその変形例を踏まえて、図18および図19は本発明のプレス成形金型の実施形態を示すものであり、この実施形態のプレス成形金型は、図20ないし図23に示すような略正三角形平板状の溝入れ加工等に使用される縦刃式スローアウェイチップに製造される圧粉体を成形するためのものである。すなわち、このスローアウェイチップにおいては、そのチップ本体1の厚さ方向を向く三角形状の平板面2のうち、一方の平板面2(図21において上側の平板面2)ではその中央部2Aが一段突出するようにされて、この中央部2Aと他方の平板面2(図21において下側の平板面2)の略全体とが上記厚さ方向に垂直な平坦面とされるとともに、これらの平板面2がなす三角形の3つの角部分においては、それぞれ該角部で交差する一対の周面の一方にすくい面3が形成されるとともに他の周面5が逃げ面とされ、これらすくい面3と逃げ面とされる他の周面5との交差稜線が切刃6とされている。なお、このすくい面3と逃げ面とされる上記他の周面5とは、図21に示すように上記他方の平板面2がなす平坦面の延長面Qに対して90°よりも僅かに大きい傾斜角θをなし、一方の平板面2側に向かうに従い上記中央部2Aに傾斜して延びるように形成されている。 Finally, such first, second reference example and in light of its modification, 18 and 19 show one embodiment of a press-molding die of the present invention, the press of this embodiment The molding die is for molding a green compact manufactured on a vertical blade type throw-away tip used for grooving processing of a substantially equilateral triangular flat plate shape as shown in FIGS. That is, in this throw-away tip, of the triangular flat plate surface 2 facing the thickness direction of the chip body 1, one flat plate surface 2 (the upper flat plate surface 2 in FIG. 21) has a central portion 2A that is one step. The central portion 2A and the other flat plate surface 2 (the lower flat plate surface 2 in FIG. 21) are formed as flat surfaces perpendicular to the thickness direction, and these flat plates are projected. In the three corners of the triangle formed by the surface 2, the rake face 3 is formed on one of a pair of peripheral faces intersecting at the corner, and the other peripheral face 5 is a flank face. The cutting edge 6 is an intersecting ridge line with the other peripheral surface 5 that is a flank. The rake face 3 and the other peripheral face 5 as a flank are slightly less than 90 ° with respect to the flat extension surface Q formed by the other flat plate face 2 as shown in FIG. A large inclination angle θ is formed, and the first flat plate surface 2 is formed so as to be inclined and extend toward the central portion 2A.

また、この切刃6の両端には凸円弧状をなすコーナ部7が形成されており、これらのコーナ部7に連なる上記他の周面5と両平板面2の上記角部分との交差稜線部は、この交差稜線部が延びる方向に直交する断面が該平板面2と他の周面5とに滑らかに連なる凸円弧等をなすように形成された凸曲面状のコーナ稜線部8とされている。さらに、このコーナ稜線部8に交差する平板面2の上記角部分のうち上記一方の平板面2側の部分は、コーナ稜線部8からこの一方の平板面2中央部の上記平坦面側に向かうに従い、反対側の上記他方の平板面2に向けて傾斜する傾斜面2Bとされている。また、チップ本体1の周面のうち上記三角形の角部分以外の部分、すなわち周方向に隣接する角部の一方に形成されたすくい面3と他方に形成された上記逃げ面となる他の周面5との間の部分は、上記一方の平板面2の中央部側の部分が上記厚さ方向に沿った平面28とされるとともに、この平面28から他方の平板面2側の部分は、該他方の平板面2側に向かうに従いチップ本体1の内側に傾斜する傾斜面29とされている。   Further, a corner portion 7 having a convex arc shape is formed at both ends of the cutting edge 6, and an intersecting ridge line between the other peripheral surface 5 connected to the corner portion 7 and the corner portions of both flat plate surfaces 2. The section is a convex curved corner ridge line portion 8 formed so that a cross section perpendicular to the direction in which the intersecting ridge line portion extends forms a convex arc or the like smoothly connected to the flat plate surface 2 and the other peripheral surface 5. ing. Further, of the corner portions of the flat plate surface 2 intersecting with the corner ridge line portion 8, the portion on the one flat plate surface 2 side is directed from the corner ridge line portion 8 toward the flat surface side of the central portion of the one flat plate surface 2. Accordingly, the inclined surface 2B is inclined toward the other flat plate surface 2 on the opposite side. Further, the peripheral surface of the chip body 1 other than the corners of the triangle, that is, the rake face 3 formed on one of the corners adjacent in the circumferential direction and the other periphery serving as the flank formed on the other side. The portion between the plane 5 and the portion on the central portion side of the one flat plate surface 2 is a flat surface 28 along the thickness direction, and the portion on the other flat plate surface 2 side from the flat surface 28 is It is set as the inclined surface 29 which inclines inside the chip | tip main body 1 as it goes to this other flat plate surface 2 side.

さらにまた、図22(a)〜(c)に示されるように、上記すくい面3は切刃6から該すくい面3の奥側に向けて(図22(a)、(b)において切刃6から上側に向けて)、またすくい面3と上記両平板面2との交差稜線部からそれぞれチップ本体1の厚さ方向(図22(a)、(c)において左右方向)の内側に向けて、これら切刃6や両平板面2との交差稜線部に対して漸次後退する凹面状に形成されている一方、該すくい面3の中央部には略四角錐台形の凸状チップブレーカ30が形成されていて、このチップブレーカ30の突端は切刃6や上記交差稜線部よりも突出した位置に形成されている。また、このスローアウェイチップの取付穴10は、図23に示すように上記一方の平板面2側(図23において上側)が小径とされるとともに他方の平板面2側(図23において下側)は大径とされ、チップ本体1の厚さ方向(図23における上下方向)の中央部に他方の平板面2側から一方の平板面2側に向かうに従い漸次縮径する縮径部10Aが形成されたベル穴形状とされている。   Furthermore, as shown in FIGS. 22A to 22C, the rake face 3 is directed from the cutting edge 6 toward the back side of the rake face 3 (the cutting edge in FIGS. 22A and 22B). 6 toward the upper side) and from the intersecting ridge line portion of the rake face 3 and the two flat plate faces 2 to the inside of the thickness direction of the chip body 1 (left and right direction in FIGS. 22A and 22C), respectively. The cutting edge 6 and the two flat plate surfaces 2 are formed in a concave shape that gradually recedes with respect to the intersecting ridge line portions, while the rake face 3 has a substantially quadrangular pyramid-shaped convex chip breaker 30 at the center. The tip of the chip breaker 30 is formed at a position protruding from the cutting edge 6 and the intersecting ridge line portion. Further, as shown in FIG. 23, the mounting hole 10 of the throw-away tip has a small diameter on the one flat plate surface 2 side (upper side in FIG. 23) and the other flat plate surface 2 side (lower side in FIG. 23). Is formed in a central portion in the thickness direction (vertical direction in FIG. 23) of the chip body 1 and a reduced diameter portion 10A that gradually decreases in diameter from the other flat plate surface 2 side toward the one flat plate surface 2 side is formed. The bell hole shape.

従って、このような三角形平板状のスローアウェイチップを粉末プレス成形による圧粉体から製造しようとすると圧粉体も三角形平板状となるため、例えば特許文献1に記載のように原料粉末を上記チップ本体1の厚さ方向に対応する方向に垂直に圧縮して圧粉体を成形する方法および金型では、原料粉末を均一に圧縮することがますます困難となって現実的には製造することができない。そこで、本実施形態のプレス成形金型では、主パンチ11,12によって原料粉末を上記チップ本体1の厚さ方向に対応する方向に圧縮するとともに、これら主パンチ11,12とは異なる方向に離接する複数(本実施形態では3つ)の副パンチ15によっても原料粉末を圧縮して、図1ないし図10に示した第1の参考例のプレス成形金型と同様に圧粉体においてチップ本体1の上記すくい面3に対応する面をそれぞれ成形するようにしている。 Therefore, when such a triangular flat plate-shaped throw-away tip is manufactured from a green compact by powder press molding, the green compact also becomes a triangular flat plate shape. In the method and mold in which the green compact is molded by compressing perpendicularly to the direction corresponding to the thickness direction of the main body 1, it becomes increasingly difficult to uniformly compress the raw material powder, and it is practically manufactured. I can't. Therefore, in the press mold of this embodiment, the raw powder is compressed by the main punches 11 and 12 in a direction corresponding to the thickness direction of the chip body 1 and separated in a direction different from the main punches 11 and 12. The raw material powder is also compressed by a plurality of (three in this embodiment) auxiliary punches 15 in contact with each other, and the chip body in the green compact is the same as in the press mold of the first reference example shown in FIGS. Each of the surfaces corresponding to the rake surface 3 of 1 is formed.

ここで、本実施形態では、まずダイ13が、上下方向に離接する主パンチ11,12の離接方向と平行な方向、すなわち上下方向にキャビティー14を間にして分割面Pから分割される3組の分割ダイ13A,13Bと、周方向においてこれら分割ダイ13A,13Bの組の間にそれぞれ配設されて、主、副パンチ11,12,15によって画成されるキャビティ14に対して固定された3つの分割固定ダイ13Hとから構成されており、図19に示すように、一体化された上記分割ダイ13A,13Bに形成される凹部16により、圧粉体においてチップ本体1の切刃6に連なって逃げ面とされる他の周面5に対応する部分が成形され、また上記分割固定ダイ13Hにより周面のうちの上記平面28および傾斜面29に対応する部分が成形される。なお、チップ本体1のすくい面3および逃げ面とされる他の周面5が上述のような傾斜を有していることから、このチップ本体1と相似の形状を有して成形される圧粉体に対して抜き勾配を与えるために、分割ダイ13A,13Bの上記分割面Pは、成形される圧粉体において上記コーナ稜線部8のうち上記チップ本体1の厚さ方向に対応する方向に垂直な方向に最も突出した部分、すなわち図19に示すようにダイ13においては凹部16のうち最も凹んだ部分を境界として分割ダイ13A,13Bが分割されるように配設される。   Here, in the present embodiment, first, the die 13 is divided from the dividing plane P in the direction parallel to the contact / separation direction of the main punches 11 and 12 that contact / separate in the vertical direction, that is, in the vertical direction. Three sets of divided dies 13A, 13B and circumferentially arranged between these divided dies 13A, 13B are fixed to a cavity 14 defined by main and sub punches 11, 12, 15 respectively. As shown in FIG. 19, the cutting edge of the chip body 1 in the green compact is formed by the concave portion 16 formed in the integrated divided dies 13A and 13B, as shown in FIG. 6, a portion corresponding to the other peripheral surface 5 which is a flank is formed, and a portion corresponding to the flat surface 28 and the inclined surface 29 of the peripheral surface is formed by the split fixing die 13 </ b> H. It is. Since the rake face 3 of the chip body 1 and the other peripheral surface 5 as the flank face have the inclination as described above, the pressure formed with a shape similar to that of the chip body 1 is obtained. In order to give a draft to the powder, the divided surface P of the divided dies 13A and 13B is a direction corresponding to the thickness direction of the chip body 1 in the corner ridgeline portion 8 in the green compact to be molded. As shown in FIG. 19, the die 13 is arranged so that the divided dies 13A and 13B are divided with the most concave portion of the concave portion 16 as a boundary.

また、本実施形態では主パンチ11,12も、当該主パンチ11,12の離接方向(上下方向)に沿った分割面Rにより分割される複数の分割パンチによってそれぞれ構成されている。すなわち、上側の主パンチ11は、チップ本体1の上記一方の平板面2のうち厚さ方向に垂直な上記中央部2Aに対応する部分を成形する内主パンチ11Cと、この一方の平板面2がなす三角形の角部側の3つの上記傾斜面2Bに対応する部分をそれぞれ成形する3つの外主パンチ11Dとにより分割可能に構成されるとともに、下側の主パンチ12も、上記他方の平板面2のうち上記中央部2Aと反対側の部分に対応する部分を成形する内主パンチ12Cと、上記傾斜面2Bの反対側の部分に対応する部分を成形する3つの外主パンチ12Dとにより分割可能に構成されている。   Further, in the present embodiment, the main punches 11 and 12 are also constituted by a plurality of divided punches that are divided by a dividing surface R along the contact / separation direction (vertical direction) of the main punches 11 and 12. That is, the upper main punch 11 includes an inner main punch 11 </ b> C for forming a portion corresponding to the central portion 2 </ b> A perpendicular to the thickness direction of the one flat plate surface 2 of the chip body 1, and the one flat plate surface 2. And the three outer main punches 11D that respectively mold the portions corresponding to the three inclined surfaces 2B on the corner side of the triangle, and the lower main punch 12 also has the other flat plate. An inner main punch 12C for forming a portion corresponding to the portion opposite to the central portion 2A of the surface 2 and three outer main punches 12D for forming a portion corresponding to the portion opposite to the inclined surface 2B. It is configured to be splittable.

従って、上側の上記内主パンチ11Cのプレス面11Aと下側の内、外主パンチ12C,12Dのプレス面12Aとは、チップ本体1の厚さ方向に対応した主パンチ11,12の離接方向に垂直な平面とされる一方、上側の外主パンチ11Dのプレス面11Aは上記分割面R側に向かうに従いキャビティー14側に向かう傾斜面とされる。さらに、これら上側の内、外主パンチ11C,11D同士と下側の内、外主パンチ12C,12D同士とは、それぞれ上記分割面Rで互いに摺接しながらその離接方向(上下方向)に独立して離接可能とされている。ただし、上側の3つの外主パンチ11D同士と下側の3つの外主パンチ12D同士は、それぞれに互いに同期して一体に離接させられる。また、下側の内主パンチ12Cのプレス面12A中央部には、チップ本体1の上述のようなベル穴形状の取付穴10を形成するための突部22が、ピン19が出没する円孔12Bの周りに形成されている。   Therefore, the press surface 11A of the upper inner main punch 11C and the lower inner press surface 12A of the outer main punches 12C and 12D are separated from the main punches 11 and 12 corresponding to the thickness direction of the chip body 1. On the other hand, the press surface 11A of the upper outer main punch 11D is an inclined surface toward the cavity 14 side toward the dividing surface R side. Furthermore, the outer main punches 11C and 11D on the upper side and the outer main punches 12C and 12D on the lower side are independent in the separating direction (vertical direction) while being in sliding contact with each other on the dividing surface R. It is possible to connect and disconnect. However, the upper three outer main punches 11D and the lower three outer main punches 12D are brought into and out of contact with each other in synchronization with each other. Further, a protrusion 22 for forming the bell hole-shaped mounting hole 10 as described above of the chip body 1 is formed in the central portion of the press surface 12A of the lower inner main punch 12C, and the circular hole in which the pin 19 protrudes and retracts. It is formed around 12B.

なお、一体化された上記分割ダイ13A,13Bと上記分割固定ダイ13Hとによって構成されるダイ13には3つの副パンチ15が嵌挿されて、上記主パンチ11,12間に画成されるキャビティー14に向け、本実施形態では図18に示すように平面視に略三角形状をなす該キャビティー14の各辺に略直交する方向に、かつ主パンチ11,12が離接する上下方向に垂直な方向である水平方向に離接させられる。従って、本実施形態でも、これら主パンチ11,12と副パンチ15とがキャビティー14に向けて接近することにより該キャビティー14に投入された原料粉末が圧縮されて圧粉体が成形され、このとき圧粉体においてチップ本体1の周面のうち3つの上記すくい面3に対応する部分が、これら3つの副パンチ15によってそれぞれ成形される。さらに、この副パンチ15の各プレス面15Aには、チップ本体1のすくい面3がなす凹面に対応してキャビティー14に向け突出する凸部15Cがプレス面15Aの外周側に枠状に形成されるとともに、プレス面15Aの中央部には上記凸状チップブレーカ30に対応してキャビティー14に対して後退する凹部15Bが形成されている。 In addition, three sub punches 15 are inserted into the die 13 constituted by the integrated divided dies 13A and 13B and the divided fixed die 13H, and are defined between the main punches 11 and 12. Toward the cavity 14, in this embodiment, as shown in FIG. 18, in a direction substantially perpendicular to each side of the cavity 14 having a substantially triangular shape in plan view, and in a vertical direction in which the main punches 11 and 12 are separated from each other. It is separated from the horizontal direction which is a vertical direction. Therefore, also in this embodiment, when the main punches 11 and 12 and the sub punch 15 approach toward the cavity 14, the raw material powder charged into the cavity 14 is compressed to form a green compact, At this time, portions of the green compact corresponding to the three rake faces 3 in the peripheral surface of the chip body 1 are formed by the three sub punches 15, respectively. Further, on each press surface 15A of the sub punch 15, a convex portion 15C protruding toward the cavity 14 corresponding to the concave surface formed by the rake surface 3 of the chip body 1 is formed in a frame shape on the outer peripheral side of the press surface 15A. In addition, a concave portion 15B that recedes from the cavity 14 corresponding to the convex chip breaker 30 is formed in the central portion of the press surface 15A.

このように構成された本発明の一実施形態のプレス成形金型および該プレス成形金型を用いた切削工具の切刃部材の製造方法によれば、第1、第2の参考例のように方形平板状の切刃部材(縦刃式スローアウェイチップ)以外の、上述のような三角形平板状のものも原料粉末のプレス成形による圧粉体から製造することができ、この圧粉体が主パンチ11,12と、その離接方向とは異なる方向から離接させられる副パンチ15とによって多方向から等方的に原料粉末を圧縮して成形されるものであるので、その原料粉末の圧縮の均一化を図ることができて、焼結の際の微少な変形や歪みのない高精度の寸法形状を有する切刃部材を製造することが可能となる。そして、本発明によれば、このような三角形平板状や、第1、第2の参考例のような方形平板状の切刃部材のみならず、それ以上の多角形平板状のものや星形のように周面自体が凹凸する形状のもの、あるいは平板状以外の複雑な形状を有する切刃部材などでも、射出成形等によらずにプレス成形による圧粉体から高精度に製造することが可能となる。 According to the press molding die of one embodiment of the present invention configured as described above and the method for manufacturing a cutting blade member of a cutting tool using the press molding die, as in the first and second reference examples . Other than the rectangular flat plate cutting edge member (vertical blade type throw-away tip), the triangular flat plate as described above can also be manufactured from green compact by press molding of raw material powder. Since the raw material powder is formed by isotropically compressing from multiple directions by the punches 11 and 12 and the sub punch 15 separated from the direction different from the separation direction, the compression of the raw material powder is performed. Therefore, it is possible to manufacture a cutting blade member having a highly accurate dimensional shape without any slight deformation or distortion during sintering. According to the present invention, not only such a triangular flat plate shape, but a rectangular flat plate-shaped cutting blade member as in the first and second reference examples , a polygonal flat plate shape or a star shape larger than that is used. Even if the peripheral surface itself has a shape that is uneven, or a cutting blade member that has a complicated shape other than a flat plate shape, it can be manufactured with high precision from a green compact by press molding without using injection molding etc. It becomes possible.

また、上述のように主パンチ11,12がそれぞれ複数の内主パンチ11C,12Cと外主パンチ11D,12Dとに分割されて互いに独立して離接可能とされた実施形態のプレス成形金型では、上記一方の平板面2の中央部2Aと傾斜面2B部分とで図21に示すように厚さの異なるチップ本体1に製造される圧粉体を成形する場合でも、圧縮開始時の内主パンチ11C,12C間の間隔と外主パンチ11D,12D間の間隔とを適宜調整したりして充填される原料粉末量を制御したりすることにより、原料粉末圧縮比を確実に均一化することができる。なお、本実施形態では、圧粉体の上記すくい面3に対応する部分を副パンチ15によって成形するようにしているが、第2の参考例のように切刃6の逃げ面とされる他の周面5に対応する部分を副パンチによって成形してもよく、さらにこれらすくい面3と他の周面5とに対応する部分を、主パンチ11,12の離接方向と異なり、かつ互いにも異なる方向に離接させられる複数の副パンチによってそれぞれ成形するようにしてもよい。 The main punch 11 and 12 each of the plurality of main punch 11C as described above, 12C and outer major punch 11D, the press molding die of the present embodiment that can be disjunction and independently from each other is divided into a 12D In the mold, even when the green compact manufactured on the chip body 1 having a different thickness as shown in FIG. 21 is formed between the central portion 2A and the inclined surface 2B of the one flat plate surface 2, By appropriately adjusting the distance between the inner main punches 11C and 12C and the distance between the outer main punches 11D and 12D and controlling the amount of the raw material powder to be filled, the raw material powder compression ratio is surely made uniform. can do. In the present embodiment, the portion corresponding to the rake face 3 of the green compact is formed by the sub punch 15, but other than the flank face of the cutting edge 6 as in the second reference example. The portion corresponding to the peripheral surface 5 may be formed by the sub punch, and further, the portions corresponding to the rake surface 3 and the other peripheral surface 5 are different from the contact / separation direction of the main punches 11 and 12, and Alternatively, the molding may be performed by a plurality of sub-punches that are separated from each other in different directions.

また、本発明では、上述のようにプレス成形による圧粉体において原料粉末の圧縮の均一化を図ることにより、かかる圧粉体を焼結するだけで極めて高精度の切刃部材を製造することを可能としているが、さらに切刃部材の精度の向上等が必要な場合などには、焼結後のスローアウェイチップにおいてそのチップ本体の周面や平板面の少なくとも一部に砥石によって研削加工を施したり、切刃にホーニング加工を施したりしてもよい。   Further, in the present invention, as described above, by compressing the raw material powder in the green compact by press molding, an extremely accurate cutting blade member can be produced simply by sintering the green compact. However, when further improvement in the accuracy of the cutting blade member is required, etc., grinding is performed with a grindstone on at least a part of the peripheral surface of the chip body or the flat plate surface in the throw-away tip after sintering. It may be applied, or the cutting blade may be subjected to honing.

1 チップ本体
2 平板面
3 すくい面
4,6 切刃
5 チップ本体1の他の周面
7 コーナ部
8 コーナ稜線部
9,30 チップブレーカ
10 取付穴
11,12 主パンチ
11A,12A 主パンチ11,12のプレス面
11C,12C 内主パンチ(分割パンチ)
11D,12D 外主パンチ(分割パンチ)
13 ダイ
13A,13B 分割ダイ
13C,13D,13E,24 ダイ13の成形面
14 キャビティー
15,23 副パンチ
15A,23A 副パンチ15,23のプレス面
15B,16 凹部
15C 凸部
19 ピン
26 副パンチ23の摺接面
27 主パンチ11,12の摺接面
L 主パンチ11,12が原料粉末を圧縮し始めてから圧縮を終了するまでに接近する移動量
X 原料粉末の圧縮終了位置において主パンチ11,12と副パンチ15,23との間にあけられる間隔
W 摺接面26,27の幅
DESCRIPTION OF SYMBOLS 1 Tip body 2 Flat surface 3 Rake face 4,6 Cutting edge 5 Other peripheral surface of the chip body 1 7 Corner part 8 Corner ridge part 9, 30 Chip breaker 10 Mounting hole 11, 12 Main punch 11A, 12A Main punch 11, 12 press faces 11C, 12C Main punch (split punch)
11D, 12D outer main punch (split punch)
13 Die 13A, 13B Split Die 13C, 13D, 13E, 24 Die 13 Molding Surface 14 Cavity 15, 23 Sub Punch 15A, 23A Press Surface of Sub Punch 15, 23 15B, 16 Concave 15C Convex 19 Pin 26 Sub Punch 23 Sliding contact surface 27 Sliding contact surface of main punches 11 and 12 L Amount of movement that main punches 11 and 12 approach from the start of compression of raw material powder to the end of compression X Main punch 11 at the end point of compression of raw material powder , 12 and the sub-punches 15 and 23 are spaced apart. W The width of the sliding surfaces 26 and 27

Claims (9)

互いに対向して相対的に離接させられる複数の主パンチと、接近したこれら主パンチの周囲を取り囲むように配設されるダイとを備えたプレス成形金型を用いて、このプレス成形金型に投入した原料粉末を圧縮することにより、切削工具の切刃部材に製造される圧粉体をプレス成形する切削工具の切刃部材の製造方法であって、上記ダイに、上記プレス成形金型のキャビティーを間にして分割されて離接可能とされる分割ダイと、上記キャビティーに対して固定された分割固定ダイとを備え、一体化された上記分割ダイと上記分割固定ダイとによって上記ダイを構成して上記圧粉体をプレス成形し、上記分割ダイを分割して該圧粉体を取り出すことを特徴とする切削工具の切刃部材の製造方法。 Using this press-molding die comprising a press-molding die comprising a plurality of main punches that are opposed to each other and relatively separated from each other and a die that is disposed so as to surround the adjacent main punches A method for producing a cutting tool member for a cutting tool, in which a green compact produced on a cutting tool member of a cutting tool is press-molded by compressing the raw material powder charged into the die, wherein the die is formed on the die. A split die that can be separated from and separated from the cavity, and a split fixed die that is fixed to the cavity. The integrated split die and the split fixed die A method for producing a cutting blade member of a cutting tool, comprising: forming the die, press-molding the green compact, dividing the divided die, and taking out the green compact . 上記切刃部材は、略平板状を呈するチップ本体を有して、該チップ本体の厚さ方向を向く平板面とこの平板面の周りに配置される周面とを備え、この周面に形成されたすくい面と上記平板面との交差稜線と、このすくい面に隣接する他の周面と該すくい面との交差稜線との少なくとも一方に切刃が形成されたスローアウェイチップであって、上記主パンチは上記厚さ方向に対応する方向に離接させられて、上記圧粉体において上記チップ本体の平板面に対応する面の少なくとも一部を成形することを特徴とする請求項1に記載の切削工具の切刃部材の製造方法。 The cutting blade member has a chip body having a substantially flat plate shape, and includes a flat plate surface facing the thickness direction of the chip main body and a peripheral surface disposed around the flat plate surface, and formed on the peripheral surface A throw-away tip having a cutting edge formed on at least one of an intersecting ridge line between the rake face and the flat plate surface, and an intersecting ridge line between the other peripheral surface adjacent to the rake face and the rake face, The said main punch is made to contact / separate in the direction corresponding to the said thickness direction, and at least one part of the surface corresponding to the flat plate surface of the said chip body is shape | molded in the said green compact. The manufacturing method of the cutting-blade member of the cutting tool of description. 上記分割ダイにより構成される上記ダイ側の成形面に、上記キャビティーに対して後退する凹部と上記キャビティーに向けて突出する凸部とのうち少なくとも一方を形成して、この凹凸部を反転させた形状の凸凹部を上記圧粉体に成形することを特徴とする請求項1または請求項2に記載の切削工具の切刃部材の製造方法。 Forming at least one of a concave portion retreating with respect to the cavity and a convex portion projecting toward the cavity on the molding surface on the die side constituted by the divided dies, and reversing the uneven portion. The manufacturing method of the cutting blade member of the cutting tool according to claim 1 or 2, wherein the convex-concave portion having the shape is formed into the green compact . 上記主パンチに、この主パンチの離接方向に上記キャビティー内に出没可能なピンを備えて、上記切刃部材の取付穴とされる貫通穴を上記圧粉体に成形することを特徴とする請求項1から請求項3のいずれかに記載の切削工具の切刃部材の製造方法。 The main punch is provided with a pin that can be projected and retracted in the cavity in the direction of separation of the main punch, and a through hole to be a mounting hole of the cutting blade member is formed in the green compact. The manufacturing method of the cutting-blade member of the cutting tool in any one of Claim 1 to 3 to do . 上記分割ダイは、上記主パンチの離接方向と平行な方向、または該主パンチの離接方向に垂直な方向に離接可能とされていることを特徴とする請求項1から請求項4のいずれかに記載の切削工具の切刃部材の製造方法。 5. The split die is separable in a direction parallel to the main punch separation / contact direction or in a direction perpendicular to the main punch separation / contact direction. The manufacturing method of the cutting-blade member of the cutting tool in any one . 請求項1ないし請求項5のいずれかに記載の切削工具の切刃部材の製造方法に用いられる圧粉体のプレス成形金型であって、互いに対向して相対的に離接させられる複数の主パンチと、接近したこれら主パンチの周囲を取り囲むように配設されるダイとを備え、このダイは、上記プレス成形金型のキャビティーを間にして分割されて離接可能とされる分割ダイと、上記キャビティーに対して固定された分割固定ダイとを備えていることを特徴とする圧粉体のプレス成形金型。 Claims 1 a press-molding die of the green compact used in the production method of cutting member of the cutting tool according to claim 5, a plurality of which are allowed to relatively disjunction facing each other A main punch, and a die disposed so as to surround the adjacent main punches, and the die is divided with the cavity of the press molding die in between so as to be separable A green compact press-molding die comprising a die and a split fixed die fixed to the cavity . 上記分割ダイにより構成される上記ダイ側の成形面には、上記キャビティーに対して後退する凹部と上記キャビティーに向けて突出する凸部とのうち少なくとも一方が形成されていることを特徴とする請求項6に記載の圧粉体のプレス成形金型。 The molding surface on the die side constituted by the divided dies is characterized in that at least one of a concave portion retreating with respect to the cavity and a convex portion protruding toward the cavity is formed. The press molding die of the green compact according to claim 6 . 上記主パンチには、この主パンチの離接方向に上記キャビティー内に出没可能なピンが備えられていることを特徴とする請求項6または請求項7に記載の圧粉体のプレス成形金型。 The green compact press-molding metal according to claim 6 or 7 , wherein the main punch is provided with a pin that can be projected and retracted in the cavity in a direction in which the main punch is separated from and coming into contact with the main punch. Type. 上記分割ダイは、上記主パンチの離接方向と平行な方向、または該主パンチの離接方向に垂直な方向に離接可能とされていることを特徴とする請求項6から請求項8のいずれかに記載の圧粉体のプレス成形金型。 9. The split die is separable in a direction parallel to the main punch separation / contact direction or a direction perpendicular to the main punch separation / contact direction . A green compact press mold according to any one of the above.
JP2010101486A 2010-04-26 2010-04-26 Method of manufacturing cutting blade member of cutting tool and press molding die of green compact used in the manufacturing method Expired - Lifetime JP5045780B2 (en)