JP4838010B2 JP2006046335A JP2006046335A JP4838010B2 JP 4838010 B2 JP4838010 B2 JP 4838010B2 JP 2006046335 A JP2006046335 A JP 2006046335A JP 2006046335 A JP2006046335 A JP 2006046335A JP 4838010 B2 JP4838010 B2 JP 4838010B2
Authority
JP
Japan
Prior art keywords
shell layer
toner
resin
particles
fine powder
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP2006046335A
Other languages
Japanese (ja)
Other versions
JP2006285215A (en
Inventor
英樹 太田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kyocera Document Solutions Inc
Original Assignee
Kyocera Mita Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kyocera Mita Corp filed Critical Kyocera Mita Corp
Priority to JP2006046335A priority Critical patent/JP4838010B2/en
Publication of JP2006285215A publication Critical patent/JP2006285215A/en
Application granted granted Critical
Publication of JP4838010B2 publication Critical patent/JP4838010B2/en
Expired - Fee Related legal-status Critical Current
Anticipated expiration legal-status Critical

Links

Images

Landscapes

  • Developing Agents For Electrophotography (AREA)

Description

本発明は、無機外添剤を添加するのに好適な電子写真用トナーおよびその製造方法に関する。   The present invention relates to an electrophotographic toner suitable for adding an inorganic external additive and a method for producing the same.

一般に、電子写真用トナーには、流動性などを付与する上で外添剤が外添される。この外添剤としては、例えば一次粒子径が5〜20nm程度である二酸化珪素(シリカ)などの無機外添剤が挙げられる。   Generally, an external additive is externally added to the electrophotographic toner in order to impart fluidity and the like. Examples of the external additive include inorganic external additives such as silicon dioxide (silica) having a primary particle diameter of about 5 to 20 nm.

しかし、長期の耐刷などでトナーが現像機中に滞留すると、機内での撹拌ストレスにより、(無機)外添剤がトナーに埋没するという問題がある。これを解決するために、20〜300nm、さらにそれ以上の粒子径を有するシリカ、酸化チタンなどの無機微粉末を、いわゆる大粒径外添剤として併用する方法がある。   However, if the toner stays in the developing machine due to long-term printing durability, there is a problem that the (inorganic) external additive is buried in the toner due to agitation stress in the machine. In order to solve this, there is a method in which inorganic fine powders such as silica and titanium oxide having a particle size of 20 to 300 nm or more are used in combination as a so-called large particle size external additive.

一方、特許文献1では、トナー表面(特に粉砕法トナー)に存在するワックス成分が、トナー流動性の悪化や外添剤埋没の原因であるとして、これを解決すべく、粒子凝集法によるカプセル構造のトナーが提案されている。また、特許文献2では、カプセルトナーにおいて、コア材を形成する樹脂のガラス転移温度(Tg)よりも高いTgを有する樹脂で外殻(シェル)を構成するトナーが提案されている。   On the other hand, in Patent Document 1, the wax component present on the toner surface (particularly the pulverized toner) is considered to be a cause of deterioration in toner fluidity and buried external additive. Toners have been proposed. Patent Document 2 proposes a toner in which an outer shell (shell) is formed of a resin having a Tg higher than the glass transition temperature (Tg) of the resin forming the core material in the capsule toner.

しかし、上記大粒径外添剤を用いた場合や、特許文献1および特許文献2に記載の方法では、外添剤の埋没に対して一定の抑制効果はあるものの、その効果は十分ではない。このため、長期のランニングや印字率の低い印字を継続的に行った場合は、外添剤の埋没を避けられず、現像性の低下(ID低下)、転写効率の低下、現像剤ブロッキング、トナー凝集が発生するという問題点がある。   However, in the case of using the above-mentioned large particle size external additive and the methods described in Patent Document 1 and Patent Document 2, although there is a certain suppression effect on the burying of the external additive, the effect is not sufficient. . For this reason, when long-term running or printing with a low printing rate is performed continuously, burying of external additives cannot be avoided, resulting in a decrease in developability (ID decrease), a decrease in transfer efficiency, developer blocking, toner There is a problem that aggregation occurs.

特許第3141783号公報Japanese Patent No. 3141784 特開2000−147829号公報JP 2000-147829 A

本発明の課題は、長期のランニングや印字率の低い印字を継続的に行った場合でも、外添剤がトナーに埋没するのを抑制して、現像性の低下、転写効率の低下、現像剤ブロッキング、トナー凝集が発生するのを防止することができる電子写真用トナーおよびその製造方法を提供することである。   The object of the present invention is to prevent the external additive from being buried in the toner even when long-term running or printing with a low printing rate is continuously performed, thereby reducing developability, transfer efficiency, and developer. An object of the present invention is to provide an electrophotographic toner capable of preventing the occurrence of blocking and toner aggregation and a method for producing the same.

本発明者らは、上記課題を解決すべく鋭意研究を重ねた結果、以下の知見を得た。すなわち、外添剤がトナーに埋没するのは、外添剤を構成する無機微粉末に対してトナーを構成する樹脂の硬度が不足しているためである。このため、Tgの高い樹脂でカプセルのシェルを構成しても、程度の差はあるものの最終的には外添剤は埋没する。
そこで、トナー表面にシリカと同等の硬度を持つ埋没防止層を設ければ、外添剤の埋没を根本から防止することができることを見出した。
As a result of intensive studies to solve the above problems, the present inventors have obtained the following knowledge. That is, the reason why the external additive is buried in the toner is that the hardness of the resin constituting the toner is insufficient with respect to the inorganic fine powder constituting the external additive. For this reason, even if the shell of the capsule is made of a resin having a high Tg, the external additive is finally buried although there is a difference in degree.
Accordingly, it has been found that if an anti-embedding layer having a hardness equivalent to that of silica is provided on the toner surface, the external additive can be prevented from being buried.

すなわち、本発明の電子写真用トナーおよび電子写真用トナーの製造方法は、以下の構成からなる。
(1)トナー粒子に無機微粉末が外添される電子写真用トナーであり、前記トナー粒子は、少なくとも樹脂、着色剤およびワックスを含有するコア粒子と、該コア粒子の表面に形成される無機微粉末埋没防止用第一シェル層と、該第一シェル層の表面に形成される無機微粉末保持用第二シェル層とを備えたことを特徴とする電子写真用トナー。
(2)前記無機微粉末の粒子径は前記第二シェル層の平均層厚よりも大きい前記(1)記載の電子写真用トナー。
(3)前記コア粒子が、さらに帯電制御剤または帯電制御樹脂を含有する前記(1)または(2)記載の電子写真用トナー。
(4)前記第一シェル層が二酸化珪素を主成分とする前記(1)〜(3)のいずれかに記載の電子写真用トナー。
(5)前記第一シェル層の平均層厚が10nm以上である前記(1)〜(4)のいずれかに記載の電子写真用トナー。
(6)前記第二シェル層が樹脂を主成分とする前記(1)〜(5)のいずれかに記載の電子写真用トナー。
(7)前記第二シェル層の平均層厚が20nm以上である前記(1)〜(6)のいずれかに記載の電子写真用トナー。
(8)前記無機微粉末が二酸化珪素、酸化チタン、酸化アルミニウムおよび磁性粉から選ばれる少なくとも1種である前記(1)〜(7)のいずれかに記載の電子写真用トナー。
(9)前記無機微粉末の粒子径が20nmより大きい前記(1)〜(8)のいずれかに記載の電子写真用トナー。
(10)前記無機微粉末が2種以上からなる前記(1)〜(9)のいずれかに記載の電子写真用トナー。
(11)少なくとも1種の無機微粉末の粒子径が、前記第二シェル層の平均層厚よりも大きい前記(10)記載の電子写真用トナー。
That is, the electrophotographic toner and the method for producing the electrophotographic toner of the present invention have the following configurations.
(1) An electrophotographic toner in which inorganic fine powder is externally added to toner particles. The toner particles include core particles containing at least a resin, a colorant and a wax, and inorganic particles formed on the surface of the core particles. An electrophotographic toner comprising: a first shell layer for preventing burying of fine powder; and a second shell layer for holding fine inorganic powder formed on the surface of the first shell layer.
(2) The toner for electrophotography according to (1), wherein the particle diameter of the inorganic fine powder is larger than the average layer thickness of the second shell layer.
(3) The toner for electrophotography according to (1) or (2), wherein the core particles further contain a charge control agent or a charge control resin.
(4) The electrophotographic toner according to any one of (1) to (3), wherein the first shell layer contains silicon dioxide as a main component.
(5) The electrophotographic toner according to any one of (1) to (4), wherein the average thickness of the first shell layer is 10 nm or more.
(6) The electrophotographic toner according to any one of (1) to (5), wherein the second shell layer contains a resin as a main component.
(7) The toner for electrophotography according to any one of (1) to (6), wherein an average layer thickness of the second shell layer is 20 nm or more.
(8) The electrophotographic toner according to any one of (1) to (7), wherein the inorganic fine powder is at least one selected from silicon dioxide, titanium oxide, aluminum oxide, and magnetic powder.
(9) The toner for electrophotography according to any one of (1) to (8), wherein a particle diameter of the inorganic fine powder is larger than 20 nm.
(10) The electrophotographic toner according to any one of (1) to (9), wherein the inorganic fine powder is composed of two or more kinds.
(11) The electrophotographic toner according to (10), wherein the particle diameter of at least one inorganic fine powder is larger than the average layer thickness of the second shell layer.

(12)少なくとも樹脂、着色剤およびワックスを含有するコア粒子の表面に、二酸化珪素および溶媒を用いて、二酸化珪素を主成分とする第一シェル層を形成する第一シェル層形成工程と、樹脂を含む溶媒を第一シェル層が形成されたコア粒子に添加して、樹脂を主成分とする第二シェル層を第一シェル層の表面に形成する第二シェル層形成工程と、第二シェル層に含有されている樹脂のガラス転移温度以上の温度に加温して、第二シェル層を第一シェル層の表面に固着させて、トナー粒子を得る第二シェル層固着工程と、粒子径が第二シェル層の平均層厚よりも大きい無機微粉末を、トナー粒子に外添する無機微粉末外添工程とを有することを特徴とする電子写真用トナーの製造方法。
(13)前記第一シェル層形成工程が、前記コア粒子と二酸化珪素粒子とを溶媒中で分散させた後、凝集剤にて前記二酸化珪素粒子をコア粒子の表面に付着させる工程と、コア粒子のガラス転移温度以上に加温して、シリカ粒子をコア粒子に固着させる工程と、pH調整により分散系をアルカリ性にして、シリカ粒子同士を固着させる工程と、pH調整により分散系を中性に戻す工程とを含む前記(12)記載の電子写真用トナーの製造方法。
(14)前記第二シェル層形成工程が、樹脂微粒子分散液を調製する工程と、この樹脂微粒子分散液を、第一シェル層が形成されたコア粒子分散液に添加した後、凝集剤にて樹脂微粒子を第一シェル層の表面に付着させる工程とを含む前記(12)または(13)記載の電子写真用トナーの製造方法。
(15)前記コア粒子が、懸濁重合法、乳化重合凝集法および粉砕法から選ばれる方法で得られたものである前記(12)〜(14)のいずれかに記載の電子写真用トナーの製造方法。
(12) a first shell layer forming step of forming a first shell layer containing silicon dioxide as a main component by using silicon dioxide and a solvent on the surface of core particles containing at least a resin, a colorant and a wax; A second shell layer forming step of forming a second shell layer containing a resin as a main component on the surface of the first shell layer by adding a solvent containing A second shell layer fixing step in which toner particles are obtained by heating to a temperature equal to or higher than the glass transition temperature of the resin contained in the layer to fix the second shell layer to the surface of the first shell layer; And an inorganic fine powder external addition step of externally adding an inorganic fine powder larger than the average layer thickness of the second shell layer to the toner particles.
(13) The step of forming the first shell layer includes dispersing the core particles and silicon dioxide particles in a solvent, and then attaching the silicon dioxide particles to the surface of the core particles with a flocculant; The step of fixing the silica particles to the core particles by heating above the glass transition temperature, the step of making the dispersion alkaline by adjusting the pH and fixing the silica particles to each other, and making the dispersion neutral by adjusting the pH The method for producing an electrophotographic toner according to (12), further comprising a returning step.
(14) The second shell layer forming step includes a step of preparing a resin fine particle dispersion, and the resin fine particle dispersion is added to the core particle dispersion on which the first shell layer is formed. The method for producing an electrophotographic toner according to the above (12) or (13), comprising the step of adhering resin fine particles to the surface of the first shell layer.
(15) The toner for electrophotography according to any one of (12) to (14), wherein the core particles are obtained by a method selected from a suspension polymerization method, an emulsion polymerization aggregation method, and a pulverization method. Production method.

本発明によれば、第一シェル層が、無機微粉末の埋没防止層となる。さらに、第二シェル層が、無機微粉末を保持する無機微粉末の保持層となる。その結果、長期のランニングや印字率の低い印字を継続的に行った場合でも、無機微粉末がトナー粒子に埋没するのを第一シェル層で抑制するとともに、無機微粉末をトナー粒子表面で固定化および保持することができる。そして、現像性の低下、転写効率の低下、現像剤ブロッキング、トナー凝集が発生するのを防止することができる。   According to the present invention, the first shell layer becomes the burying prevention layer of the inorganic fine powder. Furthermore, the second shell layer becomes a holding layer for the inorganic fine powder for holding the inorganic fine powder. As a result, even when long-term running or printing with a low printing rate is performed continuously, the first shell layer prevents the inorganic fine powder from being embedded in the toner particles, and the inorganic fine powder is fixed on the toner particle surface. And can be retained. In addition, it is possible to prevent the developability, transfer efficiency, developer blocking, and toner aggregation from occurring.

<電子写真用トナー>
本発明の電子写真用トナーは、トナー粒子に無機微粉末が外添されている。そして、前記トナー粒子は、所定のコア粒子と、該コア粒子の表面に形成される無機微粉末埋没防止用第一シェル層と、該第一シェル層の表面に形成される無機微粉末保持用第二シェル層とを備えている。
<Toner for electrophotography>
In the electrophotographic toner of the present invention, inorganic fine powder is externally added to the toner particles. The toner particles include predetermined core particles, an inorganic fine powder embedding prevention first shell layer formed on the surface of the core particles, and an inorganic fine powder holding surface formed on the surface of the first shell layer. And a second shell layer.

上記のような本発明の電子写真用トナーの一実施形態について、図面を用いて説明する。図1は、本発明の一実施形態にかかる電子写真用トナーの構造を示している。図1に示すように、この電子写真用トナー10は、トナー粒子20と無機微粉末4とで構成されている。トナー粒子20は、コア粒子1と、このコア粒子1の表面に形成されている第一シェル層2と、この第一シェル層2の表面に形成されている第二シェル層3とを有している。したがって、トナー粒子20は、第一シェル層2および第二シェル層3の2層コート構造を備えている。そして、外添された無機微粉末4が第二シェル層3によって保持されている。   One embodiment of the electrophotographic toner of the present invention as described above will be described with reference to the drawings. FIG. 1 shows the structure of an electrophotographic toner according to an embodiment of the present invention. As shown in FIG. 1, this electrophotographic toner 10 is composed of toner particles 20 and inorganic fine powder 4. The toner particle 20 has a core particle 1, a first shell layer 2 formed on the surface of the core particle 1, and a second shell layer 3 formed on the surface of the first shell layer 2. ing. Therefore, the toner particle 20 has a two-layer coat structure of the first shell layer 2 and the second shell layer 3. The externally added inorganic fine powder 4 is held by the second shell layer 3.

コア粒子1は、少なくとも樹脂、着色剤、ワックスを含有する粒子であり、さらに帯電制御剤または帯電制御樹脂を含有するのが好ましい。このコア粒子1は、例えば後述する懸濁重合法、乳化重合凝集法、粉砕法などの方法で製造することができる。   The core particle 1 is a particle containing at least a resin, a colorant, and a wax, and preferably further contains a charge control agent or a charge control resin. The core particle 1 can be produced by a method such as a suspension polymerization method, an emulsion polymerization aggregation method, or a pulverization method described later.

第一シェル層2は、図1に示すように、コア粒子1の表面に形成されており、コア粒子1を覆っている。この第一シェル層2は、外添される無機微粉末4が埋没するのを防止する役割を果たす。つまり、外添される無機微粉末4に外力が働いても、第一シェル層2内に無機微粉末4が埋没するのを防止する無機微粉末4の埋没防止層となる。このため、第一シェル層2は二酸化珪素を主成分とするのが好ましい。これにより、第一シェル層2が外添剤である無機微粉末4とほぼ同等の硬度を持つので、無機微粉末4の埋没を確実に防止することができる。   As shown in FIG. 1, the first shell layer 2 is formed on the surface of the core particle 1 and covers the core particle 1. The first shell layer 2 plays a role of preventing the externally added inorganic fine powder 4 from being buried. In other words, even if an external force is applied to the externally added inorganic fine powder 4, the burying prevention layer of the inorganic fine powder 4 prevents the inorganic fine powder 4 from being buried in the first shell layer 2. For this reason, the first shell layer 2 is preferably composed mainly of silicon dioxide. Thereby, since the 1st shell layer 2 has substantially the same hardness as the inorganic fine powder 4 which is an external additive, the burying of the inorganic fine powder 4 can be prevented reliably.

第二シェル層3は、第一シェル層2の表面に形成されており、第一シェル層2を覆っている。この第二シェル層3は、外添された無機微粉末4に外力が働いた場合、第二シェル層3内に無機微粉末4の一部分が埋没する。つまり、第二シェル層3は、無機微粉末4を埋没させて保持する役割を果たす。このため、第二シェル層3は、樹脂を主成分とするのが好ましい。   The second shell layer 3 is formed on the surface of the first shell layer 2 and covers the first shell layer 2. In the second shell layer 3, when an external force is applied to the externally added inorganic fine powder 4, a part of the inorganic fine powder 4 is buried in the second shell layer 3. That is, the second shell layer 3 plays a role of burying and holding the inorganic fine powder 4. For this reason, it is preferable that the 2nd shell layer 3 has resin as a main component.

無機微粉末4は、電子写真用トナー10の外添剤として使用される微粒子であり、例えば二酸化珪素(シリカ)、酸化チタン、酸化アルミニウム、磁性粉などが挙げられる。前記磁性粉としては、例えばフェライト、マグネタイトをはじめとする鉄、コバルト、ニッケルなどの強磁性を示す金属が挙げられる。特に、無機微粉末4は、二酸化珪素、酸化チタン、酸化アルミニウムおよび磁性粉から選ばれる少なくとも1種であるのが好ましい。   The inorganic fine powder 4 is fine particles used as an external additive of the electrophotographic toner 10, and examples thereof include silicon dioxide (silica), titanium oxide, aluminum oxide, and magnetic powder. Examples of the magnetic powder include metals exhibiting ferromagnetism such as iron, cobalt and nickel including ferrite and magnetite. In particular, the inorganic fine powder 4 is preferably at least one selected from silicon dioxide, titanium oxide, aluminum oxide and magnetic powder.

ここで、図2は、第一シェル層2および第二シェル層3を拡大して示した模式図である。図2に示すt1は第一シェル層2の層厚(平均層厚)を、t2は第二シェル層3の層厚(平均層厚)を、d1は無機微粉末4の粒子径(直径)をそれぞれ示している。   Here, FIG. 2 is a schematic diagram showing the first shell layer 2 and the second shell layer 3 in an enlarged manner. 2, t1 is the layer thickness (average layer thickness) of the first shell layer 2, t2 is the layer thickness (average layer thickness) of the second shell layer 3, and d1 is the particle diameter (diameter) of the inorganic fine powder 4. Respectively.

図2に示すように、本実施形態では、外添される無機微粉末4の粒子径d1は、第二シェル層3の層厚t2よりも大きい。これは、粒子径d1が層厚t2以下の大きさの場合には、第二シェル層3の内部に、無機微粉末4が完全に埋没する可能性があるからである。   As shown in FIG. 2, in this embodiment, the particle diameter d1 of the inorganic fine powder 4 to be externally added is larger than the layer thickness t2 of the second shell layer 3. This is because the inorganic fine powder 4 may be completely buried inside the second shell layer 3 when the particle diameter d1 is not larger than the layer thickness t2.

このトナー10においては、無機微粉末が2種以上からなる場合であってもよい。この場合には、外添される無機微粉末のうち、少なくとも1種の粒子径d1が、第二シェル層3の層厚t2よりも大きいのが好ましい。つまり、本発明においては、t2よりも小さい粒子径を有する外添剤(無機微粉末)と、t2よりも大きい粒子径d1を有する無機微粉末4とを併用してもよい。t2よりも小さい粒子径を有する外添剤(無機微粉末)を併用すると、第一シェル層2に埋没していない外添剤(無機微粉末)により、トナーの流動性が向上する点で好ましい。また、t2よりも大きい粒子径d1を有する無機微粉末4を、2種類以上用いてもよい。   In the toner 10, the inorganic fine powder may be composed of two or more kinds. In this case, it is preferable that at least one particle diameter d1 of the externally added inorganic fine powder is larger than the layer thickness t2 of the second shell layer 3. That is, in the present invention, the external additive (inorganic fine powder) having a particle size smaller than t2 and the inorganic fine powder 4 having a particle size d1 larger than t2 may be used in combination. Use of an external additive (inorganic fine powder) having a particle diameter smaller than t2 is preferable in that the fluidity of the toner is improved by the external additive (inorganic fine powder) not embedded in the first shell layer 2. . Two or more types of inorganic fine powder 4 having a particle diameter d1 larger than t2 may be used.

無機微粉末4の粒子径d1は20nmより大きいのがよく、好ましくは20nmより大きく300nm以下、より好ましくは30〜200nmの無機微粉末(大粒径外添剤)を用いるのがよい。具体例としては、流動性向上の効果が高くd1が30nm以上のシリカ粒子、埋没防止効果が高くd1が40nm以上のシリカ、酸化チタンなどが挙げられる。前記無機微粉末4の「粒子径」は、平均粒子径を意味しており、走査型電子顕微鏡(SEM)より撮影された、10万倍に拡大した写真を測定して得ることができる。   The particle size d1 of the inorganic fine powder 4 should be larger than 20 nm, preferably an inorganic fine powder (large particle size external additive) having a particle size of more than 20 nm and not more than 300 nm, more preferably 30 to 200 nm. Specific examples include silica particles having high fluidity improving effect and d1 of 30 nm or more, silica having high burying prevention effect and d1 of 40 nm or more, and titanium oxide. The “particle diameter” of the inorganic fine powder 4 means an average particle diameter, and can be obtained by measuring a photograph taken with a scanning electron microscope (SEM) and magnified 100,000 times.

第一シェル層2の層厚t1は、特に限定はないが、第一シェル層2が薄すぎる場合は外添剤の埋没ストレスに第一シェル層2が耐えられず、穴が開き、外添剤が埋没してしまう。そのような埋没を防止するためには、t1は10nm以上、好ましくは20nm以上とするのがよい。また、t1を大きくする場合は、トナー重量に対するシリカの添加量を増やす必要があるが、あまりに添加量を多くすれば、定着特性に悪影響が現れる可能性がある。そのため、t1を大きくするためにシリカの添加量を増やす場合でも、トナー総量に対してシリカ重量を10%以下することが好ましい。   The layer thickness t1 of the first shell layer 2 is not particularly limited. However, when the first shell layer 2 is too thin, the first shell layer 2 cannot withstand the burying stress of the external additive, and a hole is formed. The agent will be buried. In order to prevent such burial, t1 is 10 nm or more, preferably 20 nm or more. Further, when t1 is increased, it is necessary to increase the amount of silica added to the toner weight. However, if the amount added is too large, there is a possibility that the fixing characteristics may be adversely affected. Therefore, even when the amount of silica added is increased in order to increase t1, the silica weight is preferably 10% or less with respect to the total amount of toner.

第二シェル層の層厚t2は、無機微粉末4をトナー表面に固定化する役割を果たすためには20nm以上、好ましくは20〜200nmとするのがよい。これにより、粒子径が20nmより大きい外添剤(大粒径外添剤)を添加しても、効果的に外添剤を固定化および保持することができる。これに対し、t2が20nmより小さい場合は、大粒径の無機微粉末4を固定化および保持する能力が低下して、無機微粉末4の脱離が生じ、転写効率の低下、脱離した無機微粉末4による機内汚染が生じる場合がある。一方、第二シェル層の層厚t2の上限については200nm、より好ましくは、使用する大粒子径外添剤の平均粒子径の2/3程度とするのが望ましい。これ以上厚みが大きくなると、外添剤の埋没が進行し、流動性、現像性、転写効率の低下が生じるからである。   The layer thickness t2 of the second shell layer is 20 nm or more, preferably 20 to 200 nm in order to fix the inorganic fine powder 4 on the toner surface. Thereby, even if an external additive having a particle size larger than 20 nm (large particle size external additive) is added, the external additive can be effectively fixed and retained. On the other hand, when t2 is smaller than 20 nm, the ability to immobilize and hold the inorganic fine powder 4 having a large particle diameter is reduced, and the inorganic fine powder 4 is detached, resulting in a decrease in transfer efficiency and desorption. In-machine contamination with the inorganic fine powder 4 may occur. On the other hand, the upper limit of the layer thickness t2 of the second shell layer is preferably 200 nm, more preferably about 2/3 of the average particle size of the large particle size external additive used. This is because if the thickness is increased beyond this, the external additive is buried, resulting in a decrease in fluidity, developability, and transfer efficiency.

前記第一シェル層2の層厚t1および第二シェル層の層厚t2は、トナー粒子20の断面3箇所について、走査型電子顕微鏡(SEM)用いて各層厚を測定し、その平均値を算出して得られた値である。   As for the layer thickness t1 of the first shell layer 2 and the layer thickness t2 of the second shell layer, the thicknesses of the cross sections of the toner particles 20 are measured using a scanning electron microscope (SEM), and the average value is calculated. This is the value obtained.

<電子写真用トナーの製造方法>
次に、上記で説明した電子写真用トナー10の製造方法について説明する。このトナー10の製造方法は、コア粒子1の表面に、二酸化珪素および水系媒体等の溶媒を用いて、二酸化珪素を主成分とする第一シェル層2を形成する第一シェル層形成工程と、樹脂を含む水系媒体等の溶媒を、第一シェル層2が表面に形成されているコア粒子1に添加して、樹脂を主成分とする層(第二シェル層3)を、第一シェル層の表面に形成する第二シェル層形成工程と、第二シェル層3に含有されている樹脂のガラス転移温度以上の温度に加温して、樹脂(第二シェル層3)を固着させ、トナー粒子を得る第二シェル層固着工程と、所定の粒子径を有する無機微粉末を、トナー粒子に外添する無機微粉末外添工程とを有している。
<Method for producing electrophotographic toner>
Next, a method for manufacturing the electrophotographic toner 10 described above will be described. The method for producing the toner 10 includes a first shell layer forming step in which a first shell layer 2 mainly composed of silicon dioxide is formed on the surface of the core particle 1 using a solvent such as silicon dioxide and an aqueous medium, A solvent such as an aqueous medium containing a resin is added to the core particle 1 on which the first shell layer 2 is formed, and a layer containing the resin as a main component (second shell layer 3) is added to the first shell layer. A second shell layer forming step to be formed on the surface of the resin, and heating to a temperature not lower than the glass transition temperature of the resin contained in the second shell layer 3 to fix the resin (second shell layer 3), and A second shell layer fixing step for obtaining particles, and an inorganic fine powder external addition step for externally adding inorganic fine powder having a predetermined particle diameter to the toner particles.

(1)コア粒子
コア粒子1は、前記した通り、少なくとも樹脂、着色剤およびワックスを含有し、さらに帯電制御剤、帯電制御樹脂などを含有するのが好ましい。このコア粒子1の作製に用いることができる樹脂、着色剤、ワックス、帯電制御剤および帯電制御樹脂としては、下記のものが例示される。
(1) Core particle As described above, the core particle 1 preferably contains at least a resin, a colorant, and a wax, and further contains a charge control agent, a charge control resin, and the like. Examples of the resin, colorant, wax, charge control agent, and charge control resin that can be used for the production of the core particle 1 include the following.

(樹脂)
コア粒子1の作製に用いることができる樹脂の種類は、特に制限されるものではないが、例えばポリスチレン系樹脂、ポリアクリル系樹脂、スチレン−アクリル系共重合体、ポリエチレン系樹脂、ポリプロピレン系樹脂、塩化ビニル系樹脂、ポリエステル系樹脂、ポリアミド系樹脂、ポリウレタン系樹脂、ポリビニルアルコール系樹脂、ビニルエーテル系樹脂、N−ビニル系樹脂、スチレン−ブタジエン樹脂などの熱可塑性樹脂が挙げられる。
(resin)
The type of resin that can be used for producing the core particle 1 is not particularly limited. For example, polystyrene resin, polyacrylic resin, styrene-acrylic copolymer, polyethylene resin, polypropylene resin, Examples thereof include thermoplastic resins such as vinyl chloride resin, polyester resin, polyamide resin, polyurethane resin, polyvinyl alcohol resin, vinyl ether resin, N-vinyl resin, and styrene-butadiene resin.

ポリスチレン系樹脂は、スチレンの単独重合体でも、スチレンと共重合可能な他の共重合モノマーとの共重合体でもよい。共重合モノマーとしては、p−クロルスチレン;ビニルナフタレン;エチレン、プロピレン、ブチレン、イソブチレンなどのエチレン不飽和モノオレフィン類;塩化ビニル、臭化ビニル、弗化ビニルなどのハロゲン化ビニル;酢酸ビニル、プロピオン酸ビニル、ベンゾエ酸ビニル、酪酸ビニルなどのビニルエステル類;アクリル酸メチル、アクリル酸エチル、アクリル酸n−ブチル、アクリル酸イソブチル、アクリル酸ドデシル、アクリル酸n−オクチル、アクリル酸2−クロルエチル、アクリル酸フェニル、α−クロルアクリル酸メチル、メタアクリル酸メチル、メタアクリル酸エチル、メタアクリル酸ブチルなどの(メタ)アクリル酸エステル;アクリロニトリル、メタアクリロニトリル、アクリルアミドなどの他のアクリル酸誘導体;ビニルメチルエーテル、ビニルイソブチルエーテルなどのビニルエーテル類;ビニルメチルケトン、ビニルエチルケトン、メチルイソプロペニルケトンなどのビニルケトン類;N−ビニルピロール、N−ビニルカルバゾール、N−ビニルインドール、N−ビニルピロリデンなどのN−ビニル化合物などが挙げられる。   The polystyrene resin may be a styrene homopolymer or a copolymer with another copolymerizable monomer copolymerizable with styrene. As copolymerizable monomers, p-chlorostyrene; vinyl naphthalene; ethylene unsaturated monoolefins such as ethylene, propylene, butylene, and isobutylene; vinyl halides such as vinyl chloride, vinyl bromide, and vinyl fluoride; vinyl acetate, propion Vinyl esters such as vinyl acrylate, vinyl benzoate, vinyl butyrate; methyl acrylate, ethyl acrylate, n-butyl acrylate, isobutyl acrylate, dodecyl acrylate, n-octyl acrylate, 2-chloroethyl acrylate, acrylic (Meth) acrylic acid esters such as phenyl acid, methyl α-chloroacrylate, methyl methacrylate, ethyl methacrylate, butyl methacrylate; other acrylic acid derivatives such as acrylonitrile, methacrylonitrile, acrylamide; Vinyl ethers such as nylmethyl ether and vinyl isobutyl ether; Vinyl ketones such as vinyl methyl ketone, vinyl ethyl ketone and methyl isopropenyl ketone; N-vinyl pyrrole, N-vinyl carbazole, N-vinyl indole, N-vinyl pyrrolidene, etc. N-vinyl compounds of

これら共重合モノマーは、1種を単独でスチレン単量体と共重合させることもできるし、あるいは2種以上を組み合わせてスチレン単量体と共重合させることもできる。なお、ポリスチレン系樹脂は、二つの重量平均分子量ピーク(低分子量ピークおよび高分子量ピーク)を有することが好ましい。具体的には、低分子量ピークが3000〜20000の範囲内であり、もう一つの高分子量ピークが300000〜1500000の範囲内であることが好ましい。さらに、重量平均分子量(Mw)および数平均分子量(Mn)について、Mw/Mnが10以上であることが好ましい。重量平均分子量ピークがこのような範囲内にあれば、トナーを容易に定着させることができ、また、耐オフセット性を向上させることもできる。   One of these copolymerization monomers can be copolymerized alone with the styrene monomer, or two or more of these copolymerization monomers can be copolymerized with the styrene monomer. The polystyrene resin preferably has two weight average molecular weight peaks (low molecular weight peak and high molecular weight peak). Specifically, the low molecular weight peak is preferably in the range of 3000 to 20000, and the other high molecular weight peak is preferably in the range of 300000 to 1500,000. Furthermore, it is preferable that Mw / Mn is 10 or more for the weight average molecular weight (Mw) and the number average molecular weight (Mn). If the weight average molecular weight peak is within such a range, the toner can be easily fixed, and offset resistance can be improved.

ポリエステル系樹脂としては、例えばアルコール成分とカルボン酸成分との縮重合または共縮重合で得られる樹脂が挙げられる。アルコール成分としては、例えば2価または3価以上のアルコール成分が挙げられ、具体例としてはエチレングリコール、ジエチレングリコール、トリエチレングリコール、1,2−プロピレングリコール、1,3−プロピレングリコール、1,4−ブタンジオール、ネオペンチルグリコール、1,4−ブテンジオール、1,5−ペンタンジオール、1,6−ヘキサンジオール、1,4−シクロヘキサンジメタノール、ジプロピレングリコール、ポリエチレングリコール、ポリプロピレングリコール、ポリテトラメチレングリコール等のジオール類;ビスフェノールA、水素添加ビスフェノールA、ポリオキシエチレン化ビスフェノールA、ポリオキシプロピレン化ビスフェノールA等のビスフェノール類;ソルビトール、1,2,3,6−ヘキサンテトロール、1,4−ソルビタン、ペンタエリスリトール、ジペンタエリスリトール、トリペンタエリスリトール、1,2,4−ブタントリオール、1,2,5−ペンタントリオール、グリセロール、ジグリセロール、2−メチルプロパントリオール、2−メチル−1,2,4−ブタントリオール、トリメチロールエタン、トリメチロールプロパン、1,3,5,−トリヒドロキシメチルベンゼン等の3価以上のアルコール類が挙げられる。   Examples of the polyester-based resin include resins obtained by condensation polymerization or co-condensation polymerization of an alcohol component and a carboxylic acid component. Examples of the alcohol component include divalent or trivalent or higher alcohol components, and specific examples include ethylene glycol, diethylene glycol, triethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4- Butanediol, neopentyl glycol, 1,4-butenediol, 1,5-pentanediol, 1,6-hexanediol, 1,4-cyclohexanedimethanol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene glycol Diols such as bisphenol A, hydrogenated bisphenol A, bisphenols such as polyoxyethylenated bisphenol A, polyoxypropylenated bisphenol A; sorbitol, 1,2,3,6- Xanthetrol, 1,4-sorbitan, pentaerythritol, dipentaerythritol, tripentaerythritol, 1,2,4-butanetriol, 1,2,5-pentanetriol, glycerol, diglycerol, 2-methylpropanetriol, Examples include trivalent or higher alcohols such as 2-methyl-1,2,4-butanetriol, trimethylolethane, trimethylolpropane, 1,3,5, -trihydroxymethylbenzene.

カルボン酸成分としては、例えば2価または3価カルボン酸、この酸無水物またはこの低級アルキルエステルが用いられ、マレイン酸、フマール酸、シトラコン酸、イタコン酸、グルタコン酸、フタル酸、イソフタル酸、テレフタル酸、シクロヘキサンジカルボン酸、コハク酸、アジピン酸、セバチン酸、アゼライン酸、マロン酸、あるいはn−ブチルコハク酸、n−ブテニルコハク酸、イソブチルコハク酸、イソブテニルコハク酸、n−オクチルコハク酸、n−オクテニルコハク酸、n−ドデシルコハク酸、n−ドデセニルコハク酸、イソドデシルコハク酸、イソドデセニルコハク酸等のアルキルコハク酸またはアルケニルコハク酸等の2価カルボン酸;1,2,4−ベンゼントリカルボン酸(トリメリット酸)、1,2,5−ベンゼントリカルボン酸、2,5,7−ナフタレントリカルボン酸、1,2,4−ナフタレントリカルボン酸、1,2,4−ブタントリカルボン酸、1,2,5−ヘキサントリカルボン酸、1,3−ジカルボキシル−2−メチル−2−メチレンカルボキシプロパン、1,2,4−シクロヘキサントリカルボン酸、テトラ(メチレンカルボキシル)メタン、1,2,7,8−オクタンテトラカルボン酸、ピロメリット酸、エンポール三量体酸等の3価以上のカルボン酸などが挙げられる。   Examples of the carboxylic acid component include divalent or trivalent carboxylic acids, acid anhydrides or lower alkyl esters thereof, and include maleic acid, fumaric acid, citraconic acid, itaconic acid, glutaconic acid, phthalic acid, isophthalic acid, terephthalic acid. Acid, cyclohexanedicarboxylic acid, succinic acid, adipic acid, sebacic acid, azelaic acid, malonic acid, or n-butyl succinic acid, n-butenyl succinic acid, isobutyl succinic acid, isobutenyl succinic acid, n-octyl succinic acid, n- Divalent carboxylic acids such as alkyl succinic acid or alkenyl succinic acid such as octenyl succinic acid, n-dodecyl succinic acid, n-dodecenyl succinic acid, isododecyl succinic acid and isododecenyl succinic acid; 1,2,4-benzenetricarboxylic acid (Trimellitic acid), 1,2,5-benzene Carboxylic acid, 2,5,7-naphthalenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, 1,2,4-butanetricarboxylic acid, 1,2,5-hexanetricarboxylic acid, 1,3-dicarboxyl- 2-methyl-2-methylenecarboxypropane, 1,2,4-cyclohexanetricarboxylic acid, tetra (methylenecarboxyl) methane, 1,2,7,8-octanetetracarboxylic acid, pyromellitic acid, empole trimer acid, etc. And trivalent or higher carboxylic acids.

樹脂は、定着性が良好な観点から熱可塑性樹脂が好ましいが、ソックスレー抽出器を用いて測定される架橋部分量(ゲル量)が10重量%以下の値、より好ましくは0.1〜10重量%の範囲内の値であれば、熱硬化性樹脂であってもよい。このように一部架橋構造を導入することにより、定着性を低下させることなく、トナーの保存安定性や形態保持性、あるいは耐久性をより向上させることができる。従って、トナーの樹脂として、熱可塑性樹脂を100重量%使用する必要はなく、架橋剤を添加したり、あるいは熱硬化性樹脂を一部使用してもよい。熱硬化性樹脂としては、例えばエポキシ系樹脂やシアネート系樹脂等が使用することができる。より具体的には、ビスフェノールA型エポキシ樹脂、水素化ビスフェノールA型エポキシ樹脂、ノボラック型エポキシ樹脂、ポリアルキレンエーテル型エポキシ樹脂、環状脂肪族型エポキシ樹脂、シアネート樹脂等の1種または2種以上の組み合わせが挙げられる。   The resin is preferably a thermoplastic resin from the viewpoint of good fixability, but the amount of cross-linked portion (gel amount) measured using a Soxhlet extractor is 10% by weight or less, more preferably 0.1 to 10% by weight. If it is a value within the range of%, a thermosetting resin may be used. By introducing a partially crosslinked structure in this way, it is possible to further improve the storage stability, form retention, and durability of the toner without deteriorating the fixability. Therefore, it is not necessary to use 100% by weight of the thermoplastic resin as the toner resin, and a crosslinking agent may be added or a part of the thermosetting resin may be used. As the thermosetting resin, for example, an epoxy resin or a cyanate resin can be used. More specifically, one or more of bisphenol A type epoxy resin, hydrogenated bisphenol A type epoxy resin, novolac type epoxy resin, polyalkylene ether type epoxy resin, cycloaliphatic type epoxy resin, cyanate resin, etc. Combinations are listed.

また、上記樹脂において、ガラス転移温度(Tg)は55〜70℃の範囲内の値とするのが好ましい。樹脂のTgが55℃未満では、得られたトナー同士が融着し、保存安定性が低下する傾向がある。一方、樹脂のTgが70℃を超えると、トナーの定着性が乏しくなる傾向がある。なお、樹脂のTgは、示差走査熱量計(DSC)を用いて、比熱の変化点から求めることができる。   In the resin, the glass transition temperature (Tg) is preferably set to a value within the range of 55 to 70 ° C. When the Tg of the resin is less than 55 ° C., the obtained toners are fused with each other and the storage stability tends to be lowered. On the other hand, when the Tg of the resin exceeds 70 ° C., the fixability of the toner tends to be poor. In addition, Tg of resin can be calculated | required from the change point of specific heat using a differential scanning calorimeter (DSC).

(着色剤)
コア粒子1の作製に用いることができる着色剤は、特に限定されるものではないが、例えばマゼンタ系、シアン系およびイエロー系、ブラック系の着色剤などが挙げられる。
(Coloring agent)
The colorant that can be used for producing the core particle 1 is not particularly limited, and examples thereof include magenta, cyan, yellow, and black colorants.

マゼンタ系着色剤としては、例えばカラーインデックスに記されているC.I.ピグメントレッド81、C.I.ピグメントレッド122、C.I.ピグメントレッド57、C.Iピグメントレッド49、C.I.ソルベントレッド49、C.I.ソルベントレッド19、C.I.ソルベントレッド52、C.I.ベシック(Basic)レッド10、C.I.ディスパーズ(Disperse)レッド15などが挙げられる。   As the magenta colorant, for example, C.I. I. Pigment red 81, C.I. I. Pigment red 122, C.I. I. Pigment red 57, C.I. Pigment Red 49, C.I. I. Solvent Red 49, C.I. I. Solvent Red 19, C.I. I. Solvent Red 52, C.I. I. Basic Red 10, C.I. I. Disperse Red 15 etc. are mentioned.

シアン系着色剤としては、例えばカラーインデックスに記されているC.I.ピグメントブルー15、C.I.ピグメントブルー15−1、C.Iピグメントブルー16、C.I.ソルベントブルー55、C.I.ソルベントブルー70、C.I.ダイレクトブルー86、C.I.ダイレクトブルー25などが挙げられる。   As the cyan colorant, for example, C.I. I. Pigment blue 15, C.I. I. Pigment blue 15-1, C.I. Pigment blue 16, C.I. I. Solvent Blue 55, C.I. I. Solvent Blue 70, C.I. I. Direct Blue 86, C.I. I. Direct Blue 25 etc. are mentioned.

イエロー系着色剤としては、例えばナフトールイエローS等のニトロ系顔料、ハンザイエロー5G、ハンザイエロー3G、ハンザイエローG、ベンジジンイエローG、バルカンファストイエロー5Gなどのアゾ系顔料または黄色酸化鉄、黄土等の無機顔料等があげられる。また、カラーインデックスに記されているC.I.ピグメントイエロー12、C.I.ピグメントイエロー180、C.I.ソルベントイエロー2、C.I.ソルベントイエロー6、C.I.ソルベントイエロー14、C.I.ソルベントイエロー15、C.I.ソルベントイエロー16、C.I.ソルベントイエロー19、C.I.ソルベントイエロー21などが挙げられる。   Examples of the yellow colorant include nitro pigments such as naphthol yellow S, azo pigments such as Hansa Yellow 5G, Hansa Yellow 3G, Hansa Yellow G, Benzidine Yellow G, and Vulcan Fast Yellow 5G, or yellow iron oxide and ocher. And inorganic pigments. In addition, C.C. I. Pigment yellow 12, C.I. I. Pigment yellow 180, C.I. I. Solvent Yellow 2, C.I. I. Solvent Yellow 6, C.I. I. Solvent Yellow 14, C.I. I. Solvent Yellow 15, C.I. I. Solvent Yellow 16, C.I. I. Solvent Yellow 19, C.I. I. Solvent yellow 21 etc. are mentioned.

ブラック系着色剤としては、例えばファーネスブラック、チャンネルブラック、アセチレンブラック、ランブラック、アニリンブラック等のカーボンブラックが挙げられる。また、ブラック系着色剤として、フェライト、マグネタイトをはじめとする鉄、コバルト、ニッケルなどの強磁性を示す金属(磁性粉)を添加してもよい。   Examples of the black colorant include carbon black such as furnace black, channel black, acetylene black, run black, and aniline black. Moreover, you may add the metal (magnetic powder) which shows ferromagnetism, such as iron, cobalt, nickel, such as ferrite and magnetite, as a black type | system | group coloring agent.

(ワックス)
コア粒子1の作製に用いることができるワックスとしては、例えばカルナバワックス、サトウワックス、木ワックス等の植物性ワックス;蜜ワックス、昆虫ワックス、鯨ワックス、羊毛ワックスなどの動物性ワックス;エステルを側鎖に有するフィッシャートロプシュワックスやポリエチレンワックス、ポリプロピレンワックス等の合成炭化水素系ワックスなどが挙げられる。また、ワックスは、示差走査熱量計による吸熱曲線における吸熱メインピークが70〜135℃の範囲であるものが好ましい。吸熱メインピークが70℃未満にある場合、トナーブロッキングおよびホットオフセットが生じるおそれがあり、他方吸熱メインピークが135℃を超える場合、低温定着性が得られないおそれがあるからである。ワックスの添加量は、樹脂100重量部に対して0.1〜20重量部の範囲が好ましい。ワックスの添加量が0.1重量部より少ないと充分なワックスの効果が得られにくく、他方添加量が20重量部より多いと耐ブロッキング性が低下し、またトナーからの脱離が生じるおそれがある。
(wax)
Examples of waxes that can be used to produce the core particles 1 include plant waxes such as carnauba wax, sugar wax, and wood wax; animal waxes such as beeswax, insect wax, whale wax, and wool wax; and ester side chains. And synthetic hydrocarbon waxes such as Fischer-Tropsch wax, polyethylene wax, and polypropylene wax. The wax preferably has an endothermic main peak in a range of 70 to 135 ° C. in an endothermic curve obtained by a differential scanning calorimeter. This is because when the endothermic main peak is less than 70 ° C., toner blocking and hot offset may occur, and when the endothermic main peak exceeds 135 ° C., low-temperature fixability may not be obtained. The amount of the wax added is preferably in the range of 0.1 to 20 parts by weight with respect to 100 parts by weight of the resin. If the addition amount of the wax is less than 0.1 parts by weight, it is difficult to obtain a sufficient effect of the wax. On the other hand, if the addition amount is more than 20 parts by weight, the anti-blocking property is lowered and the toner may be detached. is there.

(帯電制御剤・帯電制御樹脂)
帯電制御剤としては、例えば正帯電性の帯電制御剤が挙げられ、具体例としてはピリダジン、ピリミジン、ピラジン、オルトオキサジン、メタオキサジン、パラオキサジン、オルトチアジン、メタチアジン、パラチアジン、1,2,3−トリアジン、1,2,4−トリアジン、1,3,5−トリアジン、1,2,4−オキサジアジン、1,3,4−オキサジアジン、1,2,6−オキサジアジン、1,3,4−チアジアジン、1,3,5−チアジアジン、1,2,3,4−テトラジン、1,2,4,5−テトラジン、1,2,3,5−テトラジン、1,2,4,6−オキサトリアジン、1,3,4,5−オキサトリアジン、フタラジン、キナゾリン、キノキサリンなどのアジン化合物;アジンファストレッドFC、アジンファストレッド12BK、アジンバイオレットBO、アジンブラウン3G、アジンライトブラウンGR、アジンダ−クグリ−ンBH/C、アジンディ−プブラックEWおよびアジンディーブラック3RLなどのアジン化合物からなる直接染料;ニグロシン、ニグロシン塩、ニグロシン誘導体などのニグロシン化合物;ニグロシンBK、ニグロシンNB、ニグロシンZなどのニグロシン化合物からなる酸性染料;ナフテン酸または高級脂肪酸の金属塩類;アルコキシル化アミン;アルキルアミド;ベンジルメチルヘキシルデシルアンモニウム、デシルトリメチルアンモニウムクロライド等の4級アンモニウム塩を例示することができ、これらは、1種単独でも2種以上を併用して使用することもできる。
(Charge control agent / Charge control resin)
Examples of the charge control agent include positively chargeable charge control agents, and specific examples thereof include pyridazine, pyrimidine, pyrazine, orthooxazine, metaoxazine, paraoxazine, orthothiazine, metathiazine, parathiazine, 1,2,3-triazine. 1,2,4-triazine, 1,3,5-triazine, 1,2,4-oxadiazine, 1,3,4-oxadiazine, 1,2,6-oxadiazine, 1,3,4-thiadiazine, , 3,5-thiadiazine, 1,2,3,4-tetrazine, 1,2,4,5-tetrazine, 1,2,3,5-tetrazine, 1,2,4,6-oxatriazine, 1, Azine compounds such as 3,4,5-oxatriazine, phthalazine, quinazoline, quinoxaline; azine fast red FC, azine fast red 12 Direct dyes composed of azine compounds such as K, azine violet BO, azine brown 3G, azine light brown GR, azinda kugreen BH / C, azine dip black EW and azine black 3RL; nigrosine, nigrosine salt, nigrosine derivative Nigrosine compounds such as: nigrosine BK, nigrosine NB, nigrosine compounds such as nigrosine Z; acid dyes; metal salts of naphthenic acid or higher fatty acids; alkoxylated amines; alkylamides; benzylmethylhexyldecylammonium, decyltrimethylammonium chloride, etc. Quaternary ammonium salts can be exemplified, and these can be used alone or in combination of two or more.

また、4級アンモニウム塩、カルボン酸塩或いはカルボキシル基を官能基として有する樹脂またはオリゴマ−なども正帯電性の帯電制御剤・帯電制御樹脂として使用することができる。より具体的には、4級アンモニウム塩を有するスチレン系樹脂、4級アンモニウム塩を有するアクリル系樹脂、4級アンモニウム塩を有するスチレン−アクリル系樹脂、4級アンモニウム塩を有するポリエステル系樹脂、カルボン酸塩を有するスチレン系樹脂、カルボン酸塩を有するアクリル系樹脂、カルボン酸塩を有するスチレン−アクリル系樹脂、カルボン酸塩を有するポリエステル系樹脂、カルボキシル基を有するポリスチレン系樹脂、カルボキシル基を有するアクリル系樹脂、カルボキシル基を有するスチレン−アクリル系樹脂、カルボキシル基を有するポリエステル系樹脂等の1種または2種以上が挙げられる。   Further, a quaternary ammonium salt, a carboxylate, a resin having a carboxyl group as a functional group, an oligomer, or the like can also be used as a positively chargeable charge control agent / charge control resin. More specifically, a styrene resin having a quaternary ammonium salt, an acrylic resin having a quaternary ammonium salt, a styrene-acrylic resin having a quaternary ammonium salt, a polyester resin having a quaternary ammonium salt, a carboxylic acid Styrene resin with salt, acrylic resin with carboxylate, styrene-acrylic resin with carboxylate, polyester resin with carboxylate, polystyrene resin with carboxyl group, acrylic with carboxyl group 1 type, or 2 or more types, such as resin, the styrene-acrylic resin which has a carboxyl group, and the polyester-type resin which has a carboxyl group, are mentioned.

負帯電性を示す帯電制御剤としては、例えば有機金属錯体、キレート化合物が有効で、その例としてはアルミニウムアセチルアセトナート、鉄(II)アセチルアセトナート、3,5−ジ−tert−ブチルサリチル酸クロム等が挙げられ、特にアセチルアセトン金属錯体、サリチル酸系金属錯体または塩が好ましく、特にサリチル酸系金属錯体またはサリチル酸系金属塩が好ましい。   As the charge control agent exhibiting negative chargeability, for example, organometallic complexes and chelate compounds are effective. Examples thereof include aluminum acetylacetonate, iron (II) acetylacetonate, and 3,5-di-tert-butylsalicylate chromium. In particular, acetylacetone metal complexes, salicylic acid metal complexes or salts are preferable, and salicylic acid metal complexes or salicylic acid metal salts are particularly preferable.

上記で例示した組成からなるコア粒子1の製造方法としては、特に限定されるものではないが、本発明では、懸濁重合法、乳化重合凝集法および粉砕法から選ばれる方法を採用するのが好ましい。これにより、効率よくコア粒子1を得ることができるので、電子写真用トナー10の生産性が向上する。   The production method of the core particle 1 having the composition exemplified above is not particularly limited, but in the present invention, a method selected from a suspension polymerization method, an emulsion polymerization aggregation method and a pulverization method is adopted. preferable. Thereby, since the core particle 1 can be obtained efficiently, the productivity of the electrophotographic toner 10 is improved.

(懸濁重合法)
懸濁重合法を採用する場合には、例えば下記のようにしてコア粒子1を得ることができる。すなわち、重合性単量体、着色剤、重合開始剤および帯電制御剤などを含有する組成物を水相中に撹拌下に加えて造粒し、重合反応後、粒子を濾過・乾燥することによって、コア粒子1を得ることができる。
(Suspension polymerization method)
When employing the suspension polymerization method, for example, the core particles 1 can be obtained as follows. That is, a composition containing a polymerizable monomer, a colorant, a polymerization initiator, a charge control agent and the like is added to an aqueous phase with stirring, and granulated. After the polymerization reaction, the particles are filtered and dried. The core particle 1 can be obtained.

重合性単量体としては、例えばモノビニル芳香族単量体、アクリル系単量体、ビニルエステル系単量体、ビニルエーテル系単量体、ジオレフィン系単量体、モノオレフィン系単量体などが挙げられる。   Examples of the polymerizable monomer include a monovinyl aromatic monomer, an acrylic monomer, a vinyl ester monomer, a vinyl ether monomer, a diolefin monomer, and a monoolefin monomer. Can be mentioned.

着色剤は、上記で例示したものと同様の着色剤を用いることができる。着色剤の添加量は、樹脂100重量部に対して2〜20重量部、好ましくは4〜15重量部の割合で配合されるのがよい。   As the colorant, the same colorant as exemplified above can be used. The added amount of the colorant is 2 to 20 parts by weight, preferably 4 to 15 parts by weight, based on 100 parts by weight of the resin.

重合開始剤としては、例えば過酸化ベンゾイル、過酸化ラウロイル、イソプロピルパーオキシカーボネート、クメンハイドロパーオキサイド、2,4−ジクロリルベンゾイルパーオキサイド、メチルエチルケトンパーオキサイドなどが挙げられる。   Examples of the polymerization initiator include benzoyl peroxide, lauroyl peroxide, isopropyl peroxycarbonate, cumene hydroperoxide, 2,4-dichloroylbenzoyl peroxide, methyl ethyl ketone peroxide, and the like.

帯電制御剤としては、上記で例示したものと同様の帯電制御剤を用いることができ、その添加量は、樹脂100重量部に対して1〜15.0重量部、好ましくは1.5〜8.0重量部とするのがよい。帯電制御剤の添加量が上記範囲よりも少量であると、トナーを安定して帯電することが困難となることがあり、トナーを用いて静電潜像の現像を行って画像形成を行った場合に、画像濃度の低下などが発生する場合がある。一方、帯電制御剤が上記範囲よりも多量であると、耐環境性、特に高温高湿下での帯電不良や画像不良が発生し、感光体の汚染等が生じる場合がある。   As the charge control agent, the same charge control agent as exemplified above can be used, and the addition amount thereof is 1 to 15.0 parts by weight, preferably 1.5 to 8 parts per 100 parts by weight of the resin. 0.0 part by weight is preferable. If the addition amount of the charge control agent is less than the above range, it may be difficult to stably charge the toner, and the electrostatic latent image was developed using the toner to form an image. In some cases, a decrease in image density may occur. On the other hand, if the amount of the charge control agent is larger than the above range, environmental resistance, particularly charging failure or image failure under high temperature and high humidity may occur, and the photoreceptor may be contaminated.

(乳化重合凝集法)
乳化重合凝集法を採用する場合には、例えば下記のようにしてコア粒子1を得ることができる。すなわち、乳化重合で得られた重合体を含有する分散液に、着色剤、帯電制御剤などを添加後、凝集・熟成を行ってコア粒子1を得ればよい。
(Emulsion polymerization aggregation method)
When employing the emulsion polymerization aggregation method, the core particle 1 can be obtained, for example, as follows. That is, a core particle 1 may be obtained by adding a colorant, a charge control agent, and the like to a dispersion containing a polymer obtained by emulsion polymerization, followed by aggregation and aging.

なお、上記方法と異なる方法、例えば乳化重合において、重合体を得る場合に、着色剤をワックスとともに添加してもよい。着色剤としては、上記で例示したものと同様の着色剤を用いればよく、樹脂100重量部に対して3〜20重量部となるように添加することが好ましい。また、帯電制御剤は、上記で例示したものと同様の帯電制御剤を用いればよいが、特に、正荷電性制御剤としては4級アンモニウム塩化合物を、負荷電性制御剤としてはサリチル酸系金属塩などを用いることが好ましい。その使用量は、トナーに所望の帯電量により決定すればよいが、樹脂100重量部に対して0.01〜15重量部、好ましくは0.1〜10重量部用いるのがよい。   In the case of obtaining a polymer in a method different from the above method, for example, emulsion polymerization, a colorant may be added together with the wax. As the colorant, the same colorant as exemplified above may be used, and it is preferable to add 3 to 20 parts by weight with respect to 100 parts by weight of the resin. The charge control agent may be the same charge control agent as exemplified above. In particular, a quaternary ammonium salt compound is used as the positive charge control agent, and a salicylic acid metal is used as the negative charge control agent. It is preferable to use a salt or the like. The amount of use may be determined by the desired charge amount for the toner, but is 0.01 to 15 parts by weight, preferably 0.1 to 10 parts by weight, based on 100 parts by weight of the resin.

(粉砕法)
粉砕法を採用する場合には、例えば下記のようにしてコア粒子1を得ることができる。すなわち、所定量の樹脂、ワックス、帯電制御剤および着色剤などを添加し、これらをヘンシェルミキサーなどの混合装置で攪拌混合する。次に、この混合物を二軸押出機などで溶融混練し、冷却後、ハンマーミルやジェットミルなどの粉砕機で粉砕する。さらに、風力分級機などの分級機を用いれば、所定粒径のコア粒子1を作製することができる。
(Crushing method)
When employing the pulverization method, the core particles 1 can be obtained, for example, as follows. That is, a predetermined amount of resin, wax, charge control agent, colorant and the like are added, and these are stirred and mixed by a mixing device such as a Henschel mixer. Next, the mixture is melt-kneaded with a twin screw extruder or the like, cooled, and then pulverized with a pulverizer such as a hammer mill or a jet mill. Furthermore, if a classifier such as an air classifier is used, the core particle 1 having a predetermined particle size can be produced.

(2)第一シェル層形成工程
第一シェル層形成工程では、上記コア粒子1と、第一シェル層2の原料となるシリカ粒子とを溶媒(例えば水系媒体)中で分散させた後、凝集剤(例えば塩化ナトリウム(NaCl))を添加し、シリカ粒子をコア粒子1の表面に付着させて、シェルを形成する。さらに、コア粒子1のガラス転移温度(Tg)以上に加温して、シリカ粒子をコア粒子1に固着させることが好ましい。その後、pH調整により分散系をアルカリ性(pH=9〜13)にすることにより、シリカ粒子同士を固着させて、第一シェル層2を形成する。さらに分散系を中性に戻して、次の第二シェル層形成工程に移る。
(2) First shell layer forming step In the first shell layer forming step, the core particles 1 and the silica particles as the raw material of the first shell layer 2 are dispersed in a solvent (for example, an aqueous medium), and then aggregated. An agent (for example, sodium chloride (NaCl)) is added to cause silica particles to adhere to the surface of the core particles 1 to form a shell. Furthermore, it is preferable that the silica particles are fixed to the core particles 1 by heating to a temperature higher than the glass transition temperature (Tg) of the core particles 1. Thereafter, the dispersion is made alkaline (pH = 9 to 13) by adjusting the pH, thereby fixing the silica particles to form the first shell layer 2. Further, the dispersion system is returned to neutral, and the process proceeds to the next second shell layer forming step.

(3)第二シェル層形成工程
第二シェル層形成工程では、第一シェル層2上に第二シェル層3を形成する。第二シェル層3を形成する場合、まず、原料樹脂の微粒子と溶媒(例えば水系媒体)とを用いて、樹脂微粒子分散液を調製する。原料樹脂としては、特に制限されるものではないが、例えばポリスチレン系樹脂、ポリアクリル系樹脂、スチレン−アクリル系共重合体、ポリエステル系樹脂などが挙げられる。また、原料樹脂の微粒子としては、例えば乳化重合法により合成した10nmから50nm程度の微粒子、他の重合法で合成した樹脂をアトライタなどの湿式ミルにより微粉砕した樹脂などが挙げられる。
(3) Second Shell Layer Forming Step In the second shell layer forming step, the second shell layer 3 is formed on the first shell layer 2. When forming the second shell layer 3, first, a resin fine particle dispersion is prepared using fine particles of a raw material resin and a solvent (for example, an aqueous medium). Although it does not restrict | limit especially as raw material resin, For example, a polystyrene-type resin, a polyacrylic-type resin, a styrene-acrylic-type copolymer, a polyester-type resin etc. are mentioned. Examples of the fine particles of the raw material resin include fine particles of about 10 nm to 50 nm synthesized by an emulsion polymerization method, and resins obtained by pulverizing a resin synthesized by another polymerization method with a wet mill such as an attritor.

樹脂微粒子分散液の調製後、その樹脂微粒子分散液を第一シェル層が形成されたコア粒子分散液に所定量添加して、ついで凝集剤(例えばNaCl)を添加して、樹脂微粒子を第一シェル層の表面に付着させることにより第二シェル層3(樹脂コート層)を第一シェル層2の表面に形成することができる。   After preparing the resin fine particle dispersion, a predetermined amount of the resin fine particle dispersion is added to the core particle dispersion on which the first shell layer is formed, and then a flocculant (for example, NaCl) is added, and the resin fine particles are added to the first. The second shell layer 3 (resin coat layer) can be formed on the surface of the first shell layer 2 by adhering to the surface of the shell layer.

(4)第二シェル層固着工程
さらに、第二シェル層に含有されている樹脂のTg以上に加温すれば、第二シェル層3を第一シェル層2の表面に固着させることができ、ろ過、洗浄および乾燥の後、トナー粒子20が得られる。
(4) Second shell layer fixing step Further, if the temperature is raised to Tg or more of the resin contained in the second shell layer, the second shell layer 3 can be fixed to the surface of the first shell layer 2, After filtration, washing and drying, toner particles 20 are obtained.

(5)無機微粉末外添工程
その後、乾式で通常の外添処理を行えば、電子写真用トナー10を得ることができる。この工程では、第二シェル層3の平均層厚よりも大きい粒子径を有する無機微粉末4を、トナー粒子20に外添する。外添処理の方法としては、例えば、トナー粒子20と外添剤(無機微粉末4)とを、ヘンシェルミキサーなどを用いて混合する方法が挙げられる。
(5) Inorganic fine powder external addition step Thereafter, a normal external addition process is performed in a dry manner, whereby the electrophotographic toner 10 can be obtained. In this step, the inorganic fine powder 4 having a particle diameter larger than the average layer thickness of the second shell layer 3 is externally added to the toner particles 20. Examples of the external addition method include a method in which the toner particles 20 and the external additive (inorganic fine powder 4) are mixed using a Henschel mixer or the like.

以下、実施例および比較例を挙げて、本発明の電子写真用トナーをさらに詳細に説明するが、本発明は以下の実施例のみに限定されるものではない。   Hereinafter, the toner for electrophotography of the present invention will be described in more detail with reference to Examples and Comparative Examples, but the present invention is not limited only to the following Examples.

[実施例1〜9および比較例1]
<コア粒子の製造例1:懸濁重合法>
スチレン80重量部、2−エチルヘキシルメタクリレート20重量部、カーボンブラック5重量部、低分子量ポリプロピレン3重量部、電荷制御剤(オリエント化学社製の「ボントロンP−51」)2重量部およびジビニルベンゼン(架橋剤)1重量部の混合溶液をボールミルにて十分に分散させた後、重合開始剤2,2−アゾビス(2,4−ジメチルバレロニトリル)2重量部を加え、それをイオン交換水400重量部に加え、更に懸濁安定剤として第三リン酸カルシウム5重量部とドデシルベンゼンスルホン酸ナトリウム0.1重量部とを加え、TKホモミキサ(特殊機化工業社製)を用いて、回転数7000rpmで20分間攪拌し、窒素雰囲気下、70℃、100rpmで10時間重合反応させた。その後、酸洗浄を行い、第三リン酸カルシウムを除去し、体積平均粒径8μmのコア粒子を含む分散液(分散液1)を得た。なお、得られたコア粒子のTgは62℃であった。
[Examples 1 to 9 and Comparative Example 1]
<Production Example of Core Particle 1: Suspension Polymerization Method>
80 parts by weight of styrene, 20 parts by weight of 2-ethylhexyl methacrylate, 5 parts by weight of carbon black, 3 parts by weight of low molecular weight polypropylene, 2 parts by weight of a charge control agent (“Bontron P-51” manufactured by Orient Chemical Co., Ltd.) and divinylbenzene (crosslinking) Agent) After 1 part by weight of the mixed solution is sufficiently dispersed by a ball mill, 2 parts by weight of a polymerization initiator 2,2-azobis (2,4-dimethylvaleronitrile) is added, and 400 parts by weight of ion-exchanged water is added. In addition, 5 parts by weight of tribasic calcium phosphate and 0.1 part by weight of sodium dodecylbenzenesulfonate are added as a suspension stabilizer and TK homomixer (manufactured by Tokushu Kika Kogyo Co., Ltd.) is used for 20 minutes at a rotational speed of 7000 rpm. The mixture was stirred and polymerized at 70 ° C. and 100 rpm for 10 hours under a nitrogen atmosphere. Thereafter, acid washing was performed to remove tricalcium phosphate, and a dispersion liquid (dispersion liquid 1) containing core particles having a volume average particle diameter of 8 μm was obtained. In addition, Tg of the obtained core particle was 62 degreeC.

<コア粒子の製造例2:乳化重合凝集法>
(1)バインダーの乳化重合
スチレン20重量部、アクリル酸ブチル3.5重量部、ジビニルベンゼン0.2重量部、水溶性重合開始剤として過硫酸カリウム0.7重量部、イオン交換水200重量部を丸底フラスコに投入し、アンカー型撹拌翼により100rpm、70℃にて8時間、乳化重合を行い、平均粒子径0.3μmのスチレンアクリルを含む分散液(分散液2)を得た。
<Production Example of Core Particle 2: Emulsion Polymerization Aggregation Method>
(1) Emulsion polymerization of binder 20 parts by weight of styrene, 3.5 parts by weight of butyl acrylate, 0.2 parts by weight of divinylbenzene, 0.7 parts by weight of potassium persulfate as a water-soluble polymerization initiator, 200 parts by weight of ion-exchanged water Was put into a round bottom flask and subjected to emulsion polymerization at 100 rpm and 70 ° C. for 8 hours with an anchor-type stirring blade to obtain a dispersion liquid (dispersion liquid 2) containing styrene acrylic having an average particle diameter of 0.3 μm.

(2)添加剤分散液の調製
カルナバワックス一号(加藤洋行社製)5重量部、ボントロンP−51(オリエント化学社製)2重量部、C.I.Pigment Red 122(大日本インキ社製)4重量部、およびドデシルベンゼンスルホン酸ナトリウム0.1重量部を、イオン交換水200重量部中に投入し、ボールミルにて3時間分散混合し、平均粒子径0.3μmの添加剤を含む分散液(分散液3)を得た。
(2) Preparation of additive dispersion 5 parts by weight of Carnauba wax No. 1 (manufactured by Kato Hiroyuki), 2 parts by weight of Bontron P-51 (manufactured by Orient Chemical Co., Ltd.), 4 parts by weight of CIPigment Red 122 (manufactured by Dainippon Ink and Company) And 0.1 part by weight of sodium dodecylbenzenesulfonate in 200 parts by weight of ion-exchanged water, dispersed and mixed for 3 hours by a ball mill, and a dispersion containing an additive having an average particle size of 0.3 μm (dispersion 3) was obtained.

(3)コア粒子の形成
上記分散液2及び3を混合し、丸底フラスコ内にてアンカー型撹拌翼により100rpm、40℃にて1時間、凝集を成長させた。上記1時間の間に、凝集剤としてNaClを0.5重量部溶解したイオン交換水50重量部を、毎分1重量部の速度で50分間連続投入した。凝集成長の後、70℃に昇温し、100rpmにて30分、融合を行ない、体積平均粒子径8μmのコア粒子を含む分散液(分散液4)を得た。なお、得られたコア粒子のTgは63℃であった。
(3) Formation of core particles The above dispersions 2 and 3 were mixed, and agglomerates were grown in a round bottom flask with an anchor type stirring blade at 100 rpm and 40 ° C for 1 hour. During the above 1 hour period, 50 parts by weight of ion-exchanged water in which 0.5 part by weight of NaCl was dissolved as a flocculant was continuously added for 50 minutes at a rate of 1 part by weight per minute. After the cohesive growth, the temperature was raised to 70 ° C., and fusion was carried out at 100 rpm for 30 minutes to obtain a dispersion liquid (dispersion liquid 4) containing core particles having a volume average particle diameter of 8 μm. In addition, Tg of the obtained core particle was 63 degreeC.

<コア粒子の製造例3:混練粉砕法>
バインダー樹脂(花王社製の「タフトンNE−410」)100重量部と、カーボンブラック(三菱化成社製の「MA−100」)5重量部と、電荷制御剤(オリエント化学社製の「ボントロンP−51」)5重量部と、カルナバワックス一号(加藤洋行社製)4重量部とを、ヘンシェルミキサーに投入・混合した後、二軸押し出し機で溶融混練してドラムフレーカーで冷却し、ハンマーミルで粗粉砕した。次に、機械式ミルで微粉砕し、風力分級機を用いて分級して体積平均粒径8μmのコア粒子を作成した。その後、界面活性剤(ドデシルベンゼンスルホン酸ナトリウム)1.0重量部を加え、イオン交換水500重量部に分散させて、コア粒子の分散液(分散液5)を得た。なお、得られたコア粒子のTgは62℃であった。
<Production Example 3 of Core Particle: Kneading and Crushing Method>
100 parts by weight of a binder resin (“Toughton NE-410” manufactured by Kao), 5 parts by weight of carbon black (“MA-100” manufactured by Mitsubishi Kasei), and a charge control agent (“Bontron P manufactured by Orient Chemical Co., Ltd.”) -51 ") 5 parts by weight and 4 parts by weight of Carnauba Wax No. 1 (manufactured by Kato Yoko Co., Ltd.) were charged into a Henschel mixer, mixed, melt-kneaded with a twin screw extruder, cooled with a drum flaker, Coarsely pulverized with a hammer mill. Next, the mixture was finely pulverized with a mechanical mill and classified using an air classifier to prepare core particles having a volume average particle diameter of 8 μm. Thereafter, 1.0 part by weight of a surfactant (sodium dodecylbenzenesulfonate) was added and dispersed in 500 parts by weight of ion-exchanged water to obtain a core particle dispersion (dispersion 5). In addition, Tg of the obtained core particle was 62 degreeC.

<第二シェル層形成用粒子の乳化重合>
スチレン20重量部、アクリル酸ブチル2重量部、ジビニルベンゼン0.2重量部、水溶性重合開始剤(過硫酸カリウム)0.5重量部、界面活性剤(ドデシルベンゼンスルホン酸ナトリウム)0.4重量部、およびイオン交換水200重量部を、丸底フラスコに投入し、アンカー型撹拌翼により100rpm、70℃にて8時間、乳化重合を行い、スチレンアクリル樹脂粒子の分散液(分散液6)を得た。なお、得られたスチレンアクリル樹脂粒子のTgは75℃、軟化点は140℃、平均粒子径は0.01μmであった。
<Emulsion polymerization of second shell layer forming particles>
20 parts by weight of styrene, 2 parts by weight of butyl acrylate, 0.2 parts by weight of divinylbenzene, 0.5 parts by weight of a water-soluble polymerization initiator (potassium persulfate), 0.4 parts by weight of a surfactant (sodium dodecylbenzenesulfonate) Part and 200 parts by weight of ion-exchanged water are put into a round bottom flask and subjected to emulsion polymerization at 100 rpm and 70 ° C. for 8 hours with an anchor-type stirring blade to obtain a dispersion of styrene acrylic resin particles (Dispersion 6). Obtained. The resulting styrene acrylic resin particles had a Tg of 75 ° C., a softening point of 140 ° C., and an average particle size of 0.01 μm.

<第一シェル層形成工程>
コア粒子を含む分散液1、分散液4または分散液5に、表1に示す添加量の二酸化珪素粉末(シリカ粒子、日本アエロジル社製の「RA200HS」)を添加し、界面活性剤(ドデシルベンゼンスルホン酸ナトリウム)2重量部(対シリカ粒子重量)を用いて水系内に十分に分散させた。その後、凝集剤(NaCl)0.5重量部(対シリカ粒子重量)を加え、丸底フラスコ内にてアンカー型撹拌翼により100rpm、70℃にて30分間、シリカ粒子の固着化処理を行った。その後、さらに2NのNaOH水溶液を10ml滴下してシリカの融着を行った後、2Nの塩酸水溶液により水系のpHを中性に戻し、第一シェル層が形成された粒子の分散液を調製した。
<First shell layer forming step>
Addition amount of silicon dioxide powder (silica particles, “RA200HS” manufactured by Nippon Aerosil Co., Ltd.) shown in Table 1 is added to dispersion 1, dispersion 4 or dispersion 5 containing core particles, and a surfactant (dodecylbenzene) is added. 2 parts by weight (sodium sulfonate) (relative to the weight of silica particles) was used and sufficiently dispersed in the aqueous system. Thereafter, 0.5 part by weight of a flocculant (NaCl) (weight of silica particles) was added, and the silica particles were fixed in the round bottom flask with an anchor-type stirring blade at 100 rpm and 70 ° C. for 30 minutes. . Thereafter, 10 ml of a 2N NaOH aqueous solution was further dropped to fuse the silica, and then the aqueous pH was returned to neutral with a 2N hydrochloric acid aqueous solution to prepare a dispersion of particles on which the first shell layer was formed. .

<第二シェル層形成工程>
上記第一シェル層形成工程で調製した分散液に、表1に示す各種添加量にて第二シェル層形成用粒子(分散液6)を加え、その後、凝集剤(NaCl)0.5重量部(対第二シェル層形成用粒子重量)を加えて、第二シェル層形成用粒子を第一シェル層の表面に形成した。
<Second shell layer forming step>
To the dispersion prepared in the first shell layer forming step, the second shell layer forming particles (dispersion 6) are added at various addition amounts shown in Table 1, and then 0.5 parts by weight of a flocculant (NaCl). (Particle weight for forming the second shell layer) was added to form particles for forming the second shell layer on the surface of the first shell layer.

<第二シェル層固着工程>
その後、丸底フラスコ内にてアンカー型撹拌翼により100rpm、75℃にて30分の時間で第二シェル層形成用粒子の固着化処理を行い、組成物を得た。その後、得られた組成物をろ過、洗浄、および乾燥して、原粉(トナー粒子)を得た。
<Second shell layer fixing step>
Thereafter, the second shell layer forming particles were fixed in a round bottom flask with an anchor type stirring blade at 100 rpm and 75 ° C. for 30 minutes to obtain a composition. Thereafter, the obtained composition was filtered, washed, and dried to obtain a raw powder (toner particles).

<無機微粉末外添工程(トナーの調製)>
原粉100重量部と、シリカRA200HS(日本アエロジル製、平均粒子径12nm)0.8重量部と、無機微粉末(大粒径外添剤)とをヘンシェルミキサーにて2分間混合し、トナーを得た。なお、無機微粉末(大粒径外添剤)の種類およびその添加量、用いたコア粒子(分散液1、4または5)の種類といったトナーの処方については、表1に示す。また、表1中、大粒径外添剤の「粒子径」は、平均粒子径を意味する。さらに、第一シェル層および第二シェル層の各平均層厚は、トナー粒子の断面3箇所について、走査型電子顕微鏡(SEM)用いて各層厚を測定し、その平均値を算出して得た。
<Inorganic fine powder external addition step (preparation of toner)>
100 parts by weight of raw powder, 0.8 parts by weight of silica RA200HS (manufactured by Nippon Aerosil Co., Ltd., average particle size 12 nm) and inorganic fine powder (large particle size external additive) are mixed for 2 minutes using a Henschel mixer, and toner is added. Obtained. Table 1 shows toner prescriptions such as the type and amount of inorganic fine powder (large particle size external additive) and the type of core particles (dispersion 1, 4, or 5) used. In Table 1, “particle diameter” of the large particle size external additive means an average particle diameter. Furthermore, each average layer thickness of the first shell layer and the second shell layer was obtained by measuring each layer thickness using a scanning electron microscope (SEM) and calculating an average value thereof at three cross sections of the toner particles. .

Figure 0004838010
Figure 0004838010

<評価用現像剤の作製>
上記表1に示す処方で作製した各種トナー35gと、京セラミタ製FS−8008C用キャリア700gとを500mlのポリプロピレン製の容器に入れ、100rpmにて30分間混合し評価用現像剤を作製した。
<Preparation of developer for evaluation>
35 g of various toners prepared according to the formulation shown in Table 1 above and 700 g of Kyocera Mita FS-8008C carrier were placed in a 500 ml polypropylene container and mixed at 100 rpm for 30 minutes to prepare a developer for evaluation.

<評価試験>
上記現像剤と、画像形成装置(京セラミタ社製FS−8008C)とを用いて、初期性能(1枚目)および印字率1%で5000枚の連続印字後について評価試験を行った。なお、画像濃度は、ソリッド画像をグレタグマクベス濃度計で測定した。転写効率は、ソリッド印字部のドラム上の現像トナー量と、転写後のドラム上残存トナー量とを測定し、下記式により転写効率を求めた。結果を表2に示す。
<Evaluation test>
Using the developer and an image forming apparatus (FS-8008C manufactured by Kyocera Mita Co., Ltd.), an evaluation test was performed on 5000 sheets after continuous printing with an initial performance (first sheet) and a printing rate of 1%. The image density was measured with a Gretag Macbeth densitometer on a solid image. The transfer efficiency was determined by measuring the amount of developed toner on the drum of the solid printing portion and the amount of residual toner on the drum after transfer, and obtaining the transfer efficiency by the following formula. The results are shown in Table 2.

Figure 0004838010
Figure 0004838010

なお、表2における総合判定の基準を以下に示す。
○:画像濃度が1.30以上かつ転写効率が85%以上である場合
△:画像濃度が1.25〜1.29または転写効率が80〜84%である場合
×:画像濃度が1.24以下または転写効率が79%以下である場合
The criteria for comprehensive judgment in Table 2 are shown below.
◯: When the image density is 1.30 or more and the transfer efficiency is 85% or more Δ: When the image density is 1.25 to 1.29 or the transfer efficiency is 80 to 84% ×: The image density is 1.24 Or when the transfer efficiency is 79% or less

Figure 0004838010
Figure 0004838010

表1および2によれば、第一シェル層と第二シェル層とが形成され、第二シェル層の平均層厚が無機微粉末(大粒径外添剤)の粒子径よりも大きい場合、つまり実施例1〜9の場合は、総合判定が「○」または「△」で、良好な結果を示している。   According to Tables 1 and 2, when the first shell layer and the second shell layer are formed, and the average layer thickness of the second shell layer is larger than the particle diameter of the inorganic fine powder (large particle size external additive), That is, in Examples 1 to 9, the overall determination is “◯” or “Δ”, indicating a good result.

特に、第二シェル層の平均層厚が20nm以上の実施例1〜7では、すべて総合判定が「○」であり、極めて良好な結果が得られたことが分かる。これは、第二シェル層の平均層厚を20nm以上とすることによって、トナー粒子の表面で大粒径外添剤を固定化する能力が高まったためと考えられる。   In particular, in Examples 1 to 7 in which the average thickness of the second shell layer is 20 nm or more, the overall judgment is “◯”, and it can be seen that extremely good results were obtained. This is presumably because the ability to fix the large particle size external additive on the surface of the toner particles was increased by setting the average thickness of the second shell layer to 20 nm or more.

一方、第一シェル層が形成されていない比較例1では、大粒径外添剤の埋没により、画像濃度および転写効率が低下した。   On the other hand, in Comparative Example 1 in which the first shell layer was not formed, the image density and the transfer efficiency were lowered due to the embedding of the large particle size external additive.

本発明の一実施形態にかかる電子写真用トナーの構造を示す模式図である。FIG. 3 is a schematic diagram illustrating a structure of an electrophotographic toner according to an embodiment of the present invention. 本発明の一実施形態にかかる電子写真用トナーの表面を示す模式図である。FIG. 3 is a schematic diagram illustrating a surface of an electrophotographic toner according to an embodiment of the present invention.

符号の説明Explanation of symbols

1 コア粒子
2 第一シェル層
3 第二シェル層
4 無機微粉末
10 電子写真用トナー
20 トナー粒子
DESCRIPTION OF SYMBOLS 1 Core particle 2 1st shell layer 3 2nd shell layer 4 Inorganic fine powder 10 Toner for electrophotography 20 Toner particle

Claims (14)

トナー粒子に無機微粉末が外添される電子写真用トナーであり、前記トナー粒子は、少なくとも樹脂、着色剤およびワックスを含有するコア粒子と、該コア粒子の表面に形成される二酸化珪素を主成分とする無機微粉末埋没防止用第一シェル層と、該第一シェル層の表面に形成される樹脂を主成分とする無機微粉末保持用第二シェル層とを備えたことを特徴とする電子写真用トナー。 An electrophotographic toner in which inorganic fine powder is externally added to toner particles, the toner particles mainly comprising core particles containing at least a resin, a colorant and a wax, and silicon dioxide formed on the surface of the core particles. An inorganic fine powder embedding prevention first shell layer as a component and an inorganic fine powder retaining second shell layer mainly composed of a resin formed on the surface of the first shell layer are provided. Toner for electrophotography. 前記無機微粉末の粒子径は前記第二シェル層の平均層厚よりも大きい請求項1記載の電子写真用トナー。   The electrophotographic toner according to claim 1, wherein a particle diameter of the inorganic fine powder is larger than an average layer thickness of the second shell layer. 前記コア粒子が、さらに帯電制御剤または帯電制御樹脂を含有する請求項1または2記載の電子写真用トナー。   The toner for electrophotography according to claim 1, wherein the core particles further contain a charge control agent or a charge control resin. 前記第一シェル層の平均層厚が10nm以上である請求項1〜のいずれかに記載の電子写真用トナー。 The toner for electrophotography according to any one of claims 1 to 3 average layer thickness of the first shell layer is 10nm or more. 前記第二シェル層が樹脂を主成分とする請求項1〜のいずれかに記載の電子写真用トナー。 The toner for electrophotography according to any one of claims 1 to 4 wherein said second shell layer is composed mainly of resin. 前記第二シェル層の平均層厚が20nm以上である請求項1〜のいずれかに記載の電子写真用トナー。 The toner for electrophotography according to any one of claims 1 to 5 average layer thickness of the second shell layer is 20nm or more. 前記無機微粉末が二酸化珪素、酸化チタン、酸化アルミニウムおよび磁性粉から選ばれる少なくとも1種である請求項1〜のいずれかに記載の電子写真用トナー。 The inorganic fine powder is silicon dioxide, titanium oxide, toner for electrophotography according to any one of claims 1 to 6 at least one selected from aluminum oxide and magnetic powder. 前記無機微粉末の粒子径が20nmより大きい請求項1〜のいずれかに記載の電子写真用トナー。 The toner for electrophotography according to any one of the particle diameter of the inorganic fine powder is 20nm greater claims 1-7. 前記無機微粉末が2種以上からなる請求項1〜のいずれかに記載の電子写真用トナー。 The toner for electrophotography according to any one of claims 1 to 8, wherein said inorganic fine powder is composed of two or more. 少なくとも1種の無機微粉末の粒子径が、前記第二シェル層の平均層厚よりも大きい請求項記載の電子写真用トナー。 The toner for electrophotography according to claim 9 , wherein the particle diameter of at least one inorganic fine powder is larger than the average layer thickness of the second shell layer. 少なくとも樹脂、着色剤およびワックスを含有するコア粒子の表面に、二酸化珪素および溶媒を用いて、二酸化珪素を主成分とする第一シェル層を形成する第一シェル層形成工程と、
樹脂を含む溶媒を第一シェル層が形成されたコア粒子に添加して、樹脂を主成分とする第二シェル層を第一シェル層の表面に形成する第二シェル層形成工程と、
第二シェル層に含有されている樹脂のガラス転移温度以上の温度に加温して、第二シェル層を第一シェル層の表面に固着させて、トナー粒子を得る第二シェル層固着工程と、
粒子径が第二シェル層の平均層厚よりも大きい無機微粉末を、トナー粒子に外添する無機微粉末外添工程とを有することを特徴とする電子写真用トナーの製造方法。
A first shell layer forming step of forming a first shell layer mainly composed of silicon dioxide using silicon dioxide and a solvent on the surface of core particles containing at least a resin, a colorant and a wax;
A second shell layer forming step of adding a solvent containing a resin to the core particles on which the first shell layer is formed, and forming a second shell layer containing the resin as a main component on the surface of the first shell layer;
A second shell layer fixing step in which toner particles are obtained by heating to a temperature equal to or higher than the glass transition temperature of the resin contained in the second shell layer to fix the second shell layer to the surface of the first shell layer; ,
A method for producing an electrophotographic toner, comprising: adding an inorganic fine powder having a particle diameter larger than an average layer thickness of the second shell layer to the toner particles.
前記第一シェル層形成工程が、前記コア粒子と二酸化珪素粒子とを溶媒中で分散させた後、凝集剤にて前記二酸化珪素粒子をコア粒子の表面に付着させる工程と、コア粒子のガラス転移温度以上に加温して、シリカ粒子をコア粒子に固着させる工程と、pH調整により分散系をアルカリ性にして、シリカ粒子同士を固着させる工程と、pH調整により分散系を中性に戻す工程とを含む請求項11記載の電子写真用トナーの製造方法。 In the first shell layer forming step, after the core particles and silicon dioxide particles are dispersed in a solvent, the silicon dioxide particles are adhered to the surface of the core particles with a flocculant, and the glass transition of the core particles A step of heating above the temperature to fix the silica particles to the core particles, a step of making the dispersion alkaline by pH adjustment, fixing the silica particles to each other, and a step of returning the dispersion to neutrality by pH adjustment The method for producing an electrophotographic toner according to claim 11 , comprising: 前記第二シェル層形成工程が、樹脂微粒子分散液を調製する工程と、この樹脂微粒子分散液を、第一シェル層が形成されたコア粒子分散液に添加した後、凝集剤にて樹脂微粒子を第一シェル層の表面に付着させる工程とを含む請求項11または12記載の電子写真用トナーの製造方法。 The second shell layer forming step includes a step of preparing a resin fine particle dispersion, and the resin fine particle dispersion is added to the core particle dispersion on which the first shell layer is formed. method for producing a toner for electrophotography according to claim 11 or 12, wherein and the step of attaching to the surface of the first shell layer. 前記コア粒子が、懸濁重合法、乳化重合凝集法および粉砕法から選ばれる方法で得られたものである請求項1113のいずれかに記載の電子写真用トナーの製造方法。 The method for producing an electrophotographic toner according to any one of claims 11 to 13 , wherein the core particles are obtained by a method selected from a suspension polymerization method, an emulsion polymerization aggregation method, and a pulverization method.
JP2006046335A 2005-03-10 2006-02-23 Toner for electrophotography and method for producing the same Expired - Fee Related JP4838010B2 (en)

Priority Applications (1)

Application Number Priority Date Filing Date Title
JP2006046335A JP4838010B2 (en) 2005-03-10 2006-02-23 Toner for electrophotography and method for producing the same

Applications Claiming Priority (3)

Application Number Priority Date Filing Date Title
JP2005067446 2005-03-10
JP2005067446 2005-03-10
JP2006046335A JP4838010B2 (en) 2005-03-10 2006-02-23 Toner for electrophotography and method for producing the same

Publications (2)

Publication Number Publication Date
JP2006285215A JP2006285215A (en) 2006-10-19
JP4838010B2 true JP4838010B2 (en) 2011-12-14

Family

ID=37407158

Family Applications (1)

Application Number Title Priority Date Filing Date
JP2006046335A Expired - Fee Related JP4838010B2 (en) 2005-03-10 2006-02-23 Toner for electrophotography and method for producing the same

Country Status (1)

Country Link
JP (1) JP4838010B2 (en)

Families Citing this family (9)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
DE102008021005A1 (en) 2008-04-25 2009-10-29 Byk-Chemie Gmbh Particular wax composites with core / shell structure and process for their preparation and their use
JP6011046B2 (en) * 2012-06-12 2016-10-19 コニカミノルタ株式会社 Method for producing toner for developing electrostatic image
JP2014209207A (en) * 2013-03-26 2014-11-06 三菱化学株式会社 Toner for electrostatic charge image development
JP6332082B2 (en) * 2015-03-02 2018-05-30 京セラドキュメントソリューションズ株式会社 Toner for electrostatic latent image development
JP6387951B2 (en) * 2015-12-16 2018-09-12 京セラドキュメントソリューションズ株式会社 Toner for electrostatic latent image development
JP6447485B2 (en) * 2015-12-22 2019-01-09 京セラドキュメントソリューションズ株式会社 Toner for electrostatic latent image development
WO2017170030A1 (en) * 2016-03-30 2017-10-05 日本ゼオン株式会社 Magenta toner for electrostatic charge image development
JP6497364B2 (en) * 2016-07-21 2019-04-10 京セラドキュメントソリューションズ株式会社 Toner for developing electrostatic latent image and two-component developer
JP6520866B2 (en) * 2016-08-24 2019-05-29 京セラドキュメントソリューションズ株式会社 Toner for developing electrostatic latent image

Family Cites Families (4)

* Cited by examiner, † Cited by third party
Publication number Priority date Publication date Assignee Title
JPH06282107A (en) * 1993-03-25 1994-10-07 Toshiba Corp Production of developer, developer and image forming device using the same
JP2001083735A (en) * 1999-09-14 2001-03-30 Fuji Xerox Co Ltd Toner with external additive, image forming device and method of forming image
JP2005099233A (en) * 2003-09-24 2005-04-14 Konica Minolta Business Technologies Inc Toner for developing electrostatic charge image and its production method
JP2005301178A (en) * 2004-04-16 2005-10-27 Konica Minolta Business Technologies Inc Electrostatic charge image developing toner

Also Published As

Publication number Publication date
JP2006285215A (en) 2006-10-19

Similar Documents

Publication Publication Date Title
JP4838010B2 (en) Toner for electrophotography and method for producing the same
KR100191289B1 (en) A toner for static charge image and method for manufacture thereof
US8252495B2 (en) Electrophotographic toner and manufacturing method thereof
JP6493301B2 (en) Toner for developing electrostatic latent image and method for producing the same
JP2006178093A (en) Electrophotographic toner and its manufacturing method
US10768542B2 (en) Positively chargeable toner
JP6443287B2 (en) Toner for electrostatic latent image development
JP6372446B2 (en) Toner for electrostatic latent image development
JP6504132B2 (en) Toner for developing electrostatic latent image and method for producing the same
JP6358228B2 (en) Toner for electrostatic latent image development
JP6237677B2 (en) Toner for electrostatic latent image development
US8980516B2 (en) Electrostatic charge image development toner
JP2017151255A (en) Positively chargeable toner
JP2016167018A (en) Toner for electrostatic latent image development, two-component developer, image forming apparatus, and image forming method
JP6390635B2 (en) Toner for electrostatic latent image development
US11262667B2 (en) Magnetic toner
JP6493031B2 (en) Positively charged toner
JP4175969B2 (en) Toner for electrostatic latent image development
JP6332127B2 (en) Toner for developing electrostatic latent image and method for producing the same
JP4511332B2 (en) Full color image forming method
JP2017068167A (en) Image forming apparatus and image forming method
JP2017107076A (en) Toner for electrostatic latent image development
JP2006184693A (en) Toner for electrophotographic development and method for manufacturing same
JP6269526B2 (en) Method for producing two-component developer
JP6010010B2 (en) Wax masterbatch, toner, and toner production method

Legal Events

Date Code Title Description
A621 Written request for application examination

Free format text: JAPANESE INTERMEDIATE CODE: A621

Effective date: 20090203

A977 Report on retrieval

Free format text: JAPANESE INTERMEDIATE CODE: A971007

Effective date: 20101208

A131 Notification of reasons for refusal

Free format text: JAPANESE INTERMEDIATE CODE: A131

Effective date: 20110201

TRDD Decision of grant or rejection written
A01 Written decision to grant a patent or to grant a registration (utility model)

Free format text: JAPANESE INTERMEDIATE CODE: A01

Effective date: 20110906

A01 Written decision to grant a patent or to grant a registration (utility model)

Free format text: JAPANESE INTERMEDIATE CODE: A01

A61 First payment of annual fees (during grant procedure)

Free format text: JAPANESE INTERMEDIATE CODE: A61

Effective date: 20110929

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20141007

Year of fee payment: 3

R150 Certificate of patent or registration of utility model

Ref document number: 4838010

Country of ref document: JP

Free format text: JAPANESE INTERMEDIATE CODE: R150

Free format text: JAPANESE INTERMEDIATE CODE: R150

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20141007

Year of fee payment: 3

S533 Written request for registration of change of name

Free format text: JAPANESE INTERMEDIATE CODE: R313533

FPAY Renewal fee payment (event date is renewal date of database)

Free format text: PAYMENT UNTIL: 20141007

Year of fee payment: 3

R350 Written notification of registration of transfer

Free format text: JAPANESE INTERMEDIATE CODE: R350

LAPS Cancellation because of no payment of annual fees