[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP4759907B2 - Cosmetic material - Google Patents

Cosmetic material Download PDF

Info

Publication number
JP4759907B2
JP4759907B2 JP2003271265A JP2003271265A JP4759907B2 JP 4759907 B2 JP4759907 B2 JP 4759907B2 JP 2003271265 A JP2003271265 A JP 2003271265A JP 2003271265 A JP2003271265 A JP 2003271265A JP 4759907 B2 JP4759907 B2 JP 4759907B2
Authority
JP
Japan
Prior art keywords
layer
resin
isocyanate compound
pattern printing
ionomer resin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP2003271265A
Other languages
Japanese (ja)
Other versions
JP2005028769A (en
Inventor
中村  剛
孝教 松沢
智司 長澤
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Toppan Inc
Original Assignee
Toppan Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toppan Inc filed Critical Toppan Inc
Priority to JP2003271265A priority Critical patent/JP4759907B2/en
Publication of JP2005028769A publication Critical patent/JP2005028769A/en
Application granted granted Critical
Publication of JP4759907B2 publication Critical patent/JP4759907B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

本発明は、住宅や店舗、オフィスビル等の建築物における壁材や天井材、床材等の内外装材や、建具、造作材等の建築資材、家具什器類、住設機器や家電製品等の外装材、車両等の輸送機器の内外装材等として使用される化粧材に関するものである。   The present invention relates to interior and exterior materials such as wall materials, ceiling materials, and floor materials in buildings such as houses, stores, and office buildings, building materials such as joinery and construction materials, furniture fixtures, housing equipment, and home appliances. The present invention relates to a decorative material used as an exterior material, an interior / exterior material of a transportation device such as a vehicle.

上記した各種用途の化粧材としては、古くは例えば天然木の無垢板や突板、天然石材、天然皮革、織物等が用いられたが、より意匠品質の安定した製品を安価に大量生産可能なものとして、紙や合成樹脂フィルム等の人工素材に印刷によって各種意匠の絵柄を付与したものを用いるのが、現在では一般的になっている。係る化粧材における絵柄印刷層は、通常の書籍等の印刷物と異なり、長年に亘って光に曝される条件下で使用されても、変退色等により絵柄の意匠性が著しく劣化したり、印刷インキの劣化により表面強度や層間密着強度が著しく低下したりすることがないように、優れた耐候性が要求される。   In the past, for example, solid wood and veneer, natural stone, natural leather, and woven fabric were used as decorative materials for various applications. However, products with more stable design quality can be mass-produced at low cost. Currently, it is common to use artificial materials such as paper and synthetic resin films provided with various design patterns by printing. The pattern printed layer in such a decorative material is different from the printed material such as a normal book, and even if it is used under conditions exposed to light for many years, the design of the pattern is significantly deteriorated due to discoloration, etc. Excellent weather resistance is required so that the surface strength and interlaminar adhesion strength do not significantly decrease due to ink deterioration.

この様な厳しい要求に堪える印刷インキとしては種々開発されているが、それらの中でも、イソシアネート化合物と反応可能な活性水素基を有する樹脂を主剤とし、イソシアネート化合物を硬化剤として両者を配合し、前者の活性水素基と後者のイソシアネート基とのウレタン化反応により架橋させて硬化させる、イソシアネート硬化型ウレタン系樹をバインダーとする印刷インキは、極めて耐候性に優れた印刷インキ被膜を形成し得るものとして、各種の化粧材に既に広く用いられている(特許文献1〜4)。
特公昭55−7378号公報 特開平11−179858号公報 特開2000−135771号公報 特開2001−353815号公報 しかし、近年になって、係る人工素材からなる化粧材に対する諸物性の要求が益々厳しくなると共に、限りある資源の有効利用の観点から、住宅の長寿命化、延いては化粧材の長寿命化が要求されるようになり、また、資源保護及び外観の高意匠化の観点から、従来は内装用途が中心であった印刷化粧材の外装用途への展開が要求されるようになる等、化粧材の耐候性向上の要求が益々強まりつつある中で、上記したイソシアネート硬化型ウレタン系樹脂をバインダーとする印刷インキをもってしても、化粧材における絵柄印刷層に要求される耐候性を十分に満足させることは困難になりつつあるのが現実である。
A variety of printing inks have been developed that can meet such strict requirements. Among them, a resin having an active hydrogen group capable of reacting with an isocyanate compound is used as a main agent, and both are blended using an isocyanate compound as a curing agent. Printing inks that are crosslinked and cured by the urethanization reaction between the active hydrogen group and the latter isocyanate group, using an isocyanate-cured urethane tree as a binder, can form a printing ink film with extremely excellent weather resistance. Have already been widely used in various cosmetic materials (Patent Documents 1 to 4).
Japanese Patent Publication No.55-7378 Japanese Patent Laid-Open No. 11-179858 Japanese Patent Laid-Open No. 2000-135771 However, in recent years, demands for various physical properties of cosmetic materials made of such artificial materials have become increasingly severe, and from the viewpoint of effective use of limited resources, the lifespan of houses has been extended and extended. The use of cosmetic materials has been required to extend the service life, and from the viewpoints of resource protection and high appearance design, it has been required to expand the use of printed cosmetic materials, which had been mainly used for interior applications. As the demand for improving the weather resistance of cosmetic materials is becoming stronger, even with printing inks containing the above-mentioned isocyanate-curable urethane resins as binders, there is a demand for pattern printing layers in cosmetic materials. In reality, it is becoming difficult to sufficiently satisfy the weather resistance.

例えば、店舗等の内装用の床タイルとしては従来、ポリ塩化ビニル樹脂製のものが主流であったが、ポリ塩化ビニル樹脂は火災時や焼却処分時等の燃焼時に塩化水素ガスやダイオキシン類等の有害物質を発生するおそれがあるため、これに代わるものとして、ポリ塩化ビニル樹脂に近似した物性を有する非ハロゲン系熱可塑性樹脂である、アイオノマー樹脂を用いた床タイルが提案され、ポリ塩化ビニル樹脂製の床タイルに対する置き換えが進行しつつある(特許文献5〜8)。
特表平9−504584号公報 特開平9−207276号公報 特開平10−315422号公報 特開2003−53920号公報 しかし、従来のポリ塩化ビニル樹脂製の床タイルは、透明表面層、絵柄印刷層及びバッカー層の全てがポリ塩化ビニル樹脂からなり、熱ラミネーションにより融着一体化するため、事実上、層間密着性の問題がないのに対し、アイオノマー樹脂を用いた床材は、必然的に異種の樹脂からなる多層積層体となるため、層間密着強度の確保が難しい。
For example, for floor tiles for interiors in stores, for example, those made of polyvinyl chloride resin have been the mainstream, but polyvinyl chloride resin, hydrogen chloride gas, dioxins, etc. during combustion in the event of a fire or incineration As a substitute for this, floor tiles using ionomer resin, a non-halogen thermoplastic resin having properties similar to polyvinyl chloride resin, have been proposed. Replacement of resin floor tiles is in progress (Patent Documents 5 to 8).
JP-T 9-504484 JP-A-9-207276 JP-A-10-315422 However, in the conventional floor tile made of polyvinyl chloride resin, the transparent surface layer, the pattern printing layer, and the backer layer are all made of polyvinyl chloride resin and are fused and integrated by thermal lamination. In fact, there is no problem of interlayer adhesion, but a flooring material using an ionomer resin inevitably becomes a multilayer laminate composed of different kinds of resins, so it is difficult to ensure interlayer adhesion strength.

この問題に関し、本発明者らは既に、絵柄印刷層にイソシアネート硬化型ウレタン系樹脂をバインダーとする印刷インキを使用すると共に、該絵柄印刷層上にプライマー層として、末端に水酸基、アミノ基またはカルボキシル基を有するオレフィン系樹脂と、エチレン−酢酸ビニル共重合体樹脂との混合物を主成分とする樹脂の層を設けることによって、床タイルとして十分な層間密着強度が得られることを見出している。   In connection with this problem, the present inventors have already used a printing ink having an isocyanate curable urethane resin as a binder for the pattern printing layer, and used as a primer layer on the pattern printing layer, a hydroxyl group, an amino group or a carboxyl at the terminal. It has been found that by providing a resin layer mainly composed of a mixture of an olefin-based resin having a group and an ethylene-vinyl acetate copolymer resin, sufficient interlayer adhesion strength as a floor tile can be obtained.

上記の床タイルは、製造直後には優れた層間密着強度を有することは勿論のこと、サンシャインウェザオメーターにて1000時間程度の促進耐候性試験後にも、層間密着強度の低下が殆ど認められないだけの耐候性が確認されており、室内用の床タイルとしては一定の水準にあると言えるものである。   Of course, the above floor tiles have excellent interlayer adhesion strength immediately after production, and almost no decrease in interlayer adhesion strength is observed even after an accelerated weathering test of about 1000 hours with a sunshine weatherometer. It can be said that it is at a certain level as a floor tile for indoor use.

しかし、サンシャインウェザオメーターにて1000時間を越えると、層間密着強度が徐々に低下を始め、2000時間後には当初の半分以下にまで低下してしまうことが判明した。これは、室内用の床タイルとして直ちに使用不可という水準では決してないが、室内床面の中でも窓際等で直射日光が当たることのある場所に使用された場合や、想定寿命を超えて長期間使用された場合などを考慮すると、十分に満足すべき水準にあるとは言い難いものである。   However, it was found that when the sunshine weatherometer exceeded 1000 hours, the interlaminar adhesion strength began to gradually decrease, and after 2000 hours, it decreased to less than half of the original. This is not at the level that it cannot be used immediately as a floor tile for indoor use, but it is used for a long period of time exceeding the expected life when used in a place where the floor is exposed to direct sunlight, etc. Considering such cases, it is difficult to say that the level is sufficiently satisfactory.

そこで、促進耐候性試験によって層間密着強度が低下した床タイルの剥離面を調査したところ、絵柄印刷層のバインダーであるイソシアネート硬化型ウレタン系樹脂が劣化したために、絵柄印刷層が凝集破壊を起こしていることが判明した。従って、上記床タイルの層間密着強度の経時による低下を抑制し、より厳しい条件における長期に亘る耐候性や耐久性を確保するためには、絵柄印刷層の耐候性の向上は、避けて通ることのできない最重要課題である。   Therefore, when the peeled surface of the floor tile whose interlaminar adhesion strength was reduced by the accelerated weather resistance test was investigated, the design printing layer caused cohesive failure because the isocyanate curable urethane resin that was the binder of the design printing layer was deteriorated. Turned out to be. Therefore, in order to suppress the deterioration of the interlayer adhesion strength of the floor tile over time and to ensure long-term weather resistance and durability under more severe conditions, improvement of the weather resistance of the pattern printing layer should be avoided. It is the most important issue that cannot be done.

また、以上に例示した床タイル以外の各種の化粧材においても、絵柄印刷層の劣化は、化粧材の層間密着強度や表面強度等の低下に直結するから、化粧材の耐候性や耐久性の向上の為には、絵柄印刷層の耐候性の向上が不可欠であることは、広く一般の化粧材に共通の技術課題であると言うことができる。   Also, in various decorative materials other than the floor tiles exemplified above, the deterioration of the pattern printing layer directly leads to a decrease in the interlayer adhesion strength, surface strength, etc. of the decorative material, so that the weather resistance and durability of the decorative material are reduced. It can be said that the improvement of the weather resistance of the pattern printing layer is indispensable for the improvement, which is a technical problem common to general cosmetics.

本発明は、上記従来技術の問題点に鑑み為されたもので、その技術的課題とするところは、イソシアネート硬化型ウレタン系樹脂をバインダーとする絵柄印刷層を少なくとも有する化粧材において、絵柄印刷層の耐候性をさらに向上させ、化粧材の層間密着強度または表面強度等の物性をさらに長期間に亘り持続させることのできる、耐候性や耐久性の改善された化粧材を提供することにある。   The present invention has been made in view of the above-mentioned problems of the prior art, and the technical problem is that in a cosmetic material having at least a pattern printing layer having an isocyanate-curable urethane resin as a binder, the pattern printing layer An object of the present invention is to provide a cosmetic material with improved weather resistance and durability, which can further improve the weather resistance of the cosmetic material and maintain physical properties such as interlayer adhesion strength or surface strength of the cosmetic material for a longer period of time.

上記課題を解決するため、本発明の化粧材は、アイオノマー樹脂層と、ポリオレフィン系樹脂又はポリエステル系樹脂からなる中間樹脂層からなり、前記中間層上にイソシアネート硬化型ウレタン系樹脂をバインダーとする絵柄印刷層を設けた化粧材において、前記絵柄印刷層は、ブロックされていないイソシアネート化合物と、ブロックイソシアネート化合物とが配合された硬化剤として用いたイソシアネート硬化型ウレタン系樹脂をバインダーとする印刷インキ組成物によって形成されており、かつ、前記イソシアネート硬化型ウレタン系樹脂は、前記ブロックされていないイソシアネート化合物を架橋剤としたウレタン化反応により架橋硬化していると共に、前記ブロックイソシアネート化合物が未解離の状態で残存していることを特徴とするものである。 In order to solve the above problems, the decorative material of the present invention comprises an ionomer resin layer and an intermediate resin layer made of a polyolefin resin or a polyester resin. In the decorative material provided with a printing layer, the pattern printing layer is a printing ink composition comprising an isocyanate curable urethane resin used as a curing agent in which an unblocked isocyanate compound and a blocked isocyanate compound are blended. And the isocyanate curable urethane resin is crosslinked and cured by a urethanization reaction using the unblocked isocyanate compound as a crosslinking agent, and the blocked isocyanate compound is in an undissociated state. That it remains It is an.

また本発明は、上記の化粧材において、さらに、前記アイオノマー樹脂層上に、他のアイオノマー樹脂層、前記絵柄印刷層上に、プライマー層を介して無機充填剤を含有する熱可塑性樹脂からなるバッカー層とが積層されてなることを特徴とするものである。 Further, the present invention provides a backer comprising the thermoplastic resin containing an inorganic filler via a primer layer on the ionomer resin layer, another ionomer resin layer, and the pattern printing layer on the decorative material. The layer is laminated .

本発明の化粧材は、上記したとおり、絵柄印刷層のバインダーであるイソシアネート硬化型ウレタン系樹脂が、イソシアネート化合物を架橋剤としたウレタン化反応により既に架橋硬化しているのみならず、該架橋硬化しているイソシアネート硬化型ウレタン系樹脂の内部に、未解離のブロックイソシアネート化合物が未反応の状態で含有されている。   As described above, the decorative material of the present invention is not only crosslinked and cured by the urethanization reaction using an isocyanate compound as a crosslinking agent, but also the crosslinked and cured isocyanate-based urethane resin that is a binder of the pattern printing layer. An undissociated blocked isocyanate compound is contained in an unreacted state inside the isocyanate-curable urethane resin.

この未解離のブロックイソシアネート化合物は、化粧材の製造から施工にかけての期間内には殆ど解離しないが、化粧材の施工後の使用期間という長い時間的尺度で見れば徐々に解離が進行し、該解離により生成したイソシアネート化合物は、絵柄印刷層のバインダーである既に架橋硬化されたイソシアネート硬化型ウレタン系樹脂と更に反応して、架橋密度を更に向上させる作用をなす。   Although this undissociated blocked isocyanate compound hardly dissociates within the period from the production of the cosmetic material to the construction, the dissociation gradually proceeds on a long time scale of the usage period after the construction of the cosmetic material. The isocyanate compound produced by the dissociation further reacts with the already crosslinked and cured isocyanate-based urethane resin, which is a binder for the pattern printing layer, to further improve the crosslinking density.

従って、使用中の長期間の経時及び紫外線等の作用によって、イソシアネート硬化型ウレタン系樹脂が劣化して分子鎖が分断されても、上記解離により生成したイソシアネート化合物との反応により再度架橋されることにより、架橋密度の低下が抑えられ、絵柄印刷層の内部凝集力が維持される。こうして、化粧材の層間密着強度や表面強度を、従来よりも長期間に亘り持続させることが可能となる。   Therefore, even if the isocyanate curable urethane resin deteriorates and the molecular chain is broken due to long-term aging during use and the action of ultraviolet rays, it is cross-linked again by the reaction with the isocyanate compound generated by the above dissociation. As a result, the decrease in the crosslink density is suppressed, and the internal cohesive force of the picture print layer is maintained. In this way, it is possible to maintain the interlaminar adhesion strength and surface strength of the decorative material for a longer period than before.

本発明の化粧材の具体的構成に関しては、少なくとも絵柄印刷層を含むことを必須とすることを除けば、一切制限はない。一般的には、絵柄印刷層の支持体としての適当な基材の片面又は両面に、絵柄印刷層が形成される。この絵柄印刷層を保護するために、該絵柄印刷層の前記基材と反対側に、表面保護層が形成されたり、他の基材が積層されたりする場合もあるし、更にいずれか一方又は両方の側に1層又は複数層の材料層が積層されて多層化される場合もある。勿論、絵柄印刷層の少なくとも一方の側に積層される層は全て透明又は半透明とされて、絵柄印刷層は化粧材の少なくとも片面側から観察可能とされる。   The specific configuration of the decorative material of the present invention is not limited at all except that it is essential to include at least a pattern printing layer. Generally, a pattern printing layer is formed on one or both sides of a suitable base material as a support for the pattern printing layer. In order to protect this pattern printing layer, a surface protective layer may be formed on the opposite side of the pattern printing layer from the substrate, or another substrate may be laminated, and either one or the other In some cases, one or more material layers are laminated on both sides to be multilayered. Of course, all layers laminated on at least one side of the pattern printing layer are all transparent or translucent, and the pattern printing layer can be observed from at least one side of the decorative material.

本発明の化粧材における基材の材質には一切制限はなく、従来の化粧材の基材として使用されて来たものと同様のものが使用可能である。具体的には、例えば、薄葉紙、チタン紙、上質紙、クラフト紙、樹脂含浸紙、樹脂混抄紙、紙間強化紙等の紙類や、織布、不織布、編布等の繊維質基材、ポリオレフィン系樹脂、ポリエステル系樹脂、アクリル系樹脂、ポリスチレン系樹脂、ポリビニル系樹脂等の熱可塑性樹脂、不飽和ポリエステル系樹脂、エポキシ系樹脂、メラミン系樹脂、尿素系樹脂、フェノール系樹脂、ポリウレタン系樹脂等の熱硬化性樹脂、繊維強化プラスチック等の合成樹脂系基材、木材単板、合板、集成材、中質繊維板、パーティクルボード等の木質系基材、ガラス、陶磁器、石膏ボード、スレート板、珪酸カルシウム板、スラグ石膏板、木毛セメント板、ガラス繊維強化コンクリート板、軽量気泡コンクリート板等の無機質系基材、鋼鉄、真鍮、ステンレス、アルミニウム等の金属系基材等、或いはそれらの複数種からなる複合系基材等であり、その形態もシート状、板状、各種成形体状等、一切問わない。また、多層積層体とする場合には、これらから選ばれる任意の材料を任意の組み合わせで用いることができる。   There is no restriction | limiting in the material of the base material in the decorative material of this invention, The thing similar to what has been used as a base material of the conventional decorative material can be used. Specifically, for example, paper such as thin paper, titanium paper, fine paper, kraft paper, resin-impregnated paper, resin mixed paper, inter-paper reinforced paper, and fibrous base materials such as woven fabric, non-woven fabric, knitted fabric, Thermoplastic resins such as polyolefin resin, polyester resin, acrylic resin, polystyrene resin, polyvinyl resin, unsaturated polyester resin, epoxy resin, melamine resin, urea resin, phenol resin, polyurethane resin Thermosetting resins such as, synthetic resin base materials such as fiber reinforced plastic, wood single board, plywood, laminated wood, medium fiber board, wood base materials such as particle board, glass, ceramics, gypsum board, slate board , Calcium silicate board, slag gypsum board, wood wool cement board, glass fiber reinforced concrete board, lightweight cellular concrete board and other inorganic base materials, steel, brass, stainless steel, Metallic substrates such as aluminum, or a composite-based substrate or the like consisting of a plurality of types, the form also a sheet, plate, various molded articles like an interpreter, or at all. Moreover, when setting it as a multilayer laminated body, the arbitrary materials chosen from these can be used by arbitrary combinations.

本発明の化粧材における絵柄印刷層のバインダーとして用いるイソシアネート硬化型ウレタン系樹脂は、イソシアネート化合物と反応可能な活性水素基を有する樹脂を主剤とし、イソシアネート化合物を硬化剤として配合し、ウレタン化反応により架橋硬化させるものであって、本発明においては特に、前記イソシアネート化合物として少なくともブロックイソシアネート化合物を配合すると共に、前記架橋硬化の際に、該ブロックイソシアネート化合物の少なくとも一部を未反応のまま未解離の状態で残存させる必要がある。   The isocyanate-curable urethane resin used as a binder for the pattern printing layer in the decorative material of the present invention is mainly composed of a resin having an active hydrogen group that can react with an isocyanate compound, and the isocyanate compound as a curing agent. In the present invention, in particular, at least a blocked isocyanate compound is blended as the isocyanate compound, and at the time of the crosslinking and curing, at least a part of the blocked isocyanate compound remains unreacted and undissociated. It needs to remain in a state.

主剤のイソシアネート化合物と反応可能な活性水素基を有する樹脂としては、例えばアミノ基、イミノ基、カルボキシル基等を有する樹脂も可能であるが、一般的には水酸基を有する樹脂、すなわちポリオール化合物が用いられる場合が多い。係るポリオール化合物としては、例えばポリエステルポリオール化合物、ポリエーテルポリオール化合物、ポリウレタンポリオール化合物、アクリルポリオール化合物等が用いられる。これらを複数種混合して用いても勿論良い。   As the resin having an active hydrogen group capable of reacting with the main isocyanate compound, for example, a resin having an amino group, an imino group, a carboxyl group, or the like can be used. In general, a resin having a hydroxyl group, that is, a polyol compound is used. It is often done. Examples of such polyol compounds include polyester polyol compounds, polyether polyol compounds, polyurethane polyol compounds, acrylic polyol compounds, and the like. Of course, a mixture of a plurality of these may be used.

ブロックイソシアネート化合物としては、例えばトリレンジイソシアネート、ジフェニルメタンジイソシアネート、キシリレンジイソシアネート、ナフタレンジイソシアネート、イソホロンジイソシアネート、ヘキサメチレンジイソシアネート等のイソシアネート化合物、又はこれらのビューレット体、アダクト体、イソシアヌレート体等に含有されている遊離のイソシアネート基を、例えばフェノール、クレゾール等のフェノール系ブロック剤や、メチルエチルケトンオキシム、アセトンオキシム等のオキシム系ブロック剤、ε−カプロラクタム、γ−ブチロラクタム等のラクタム系ブロック剤、アセト酢酸エチル、アセチルアセトン、マロン酸エチル等の活性メチレン系ブロック剤、メタノール、エタノール等のアルコール系ブロック剤、アミン系ブロック剤、イミン系ブロック剤、イミド系ブロック剤、イミダゾール系ブロック剤、メルカプタン系ブロック剤等のブロック剤でブロックしてなる化合物を使用することができる。これらを複数種混合して用いても勿論良い。   Examples of the blocked isocyanate compound include tolylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and the like, or their burettes, adducts, isocyanurates and the like. The free isocyanate group is, for example, a phenol blocking agent such as phenol or cresol, an oxime blocking agent such as methyl ethyl ketone oxime or acetone oxime, a lactam blocking agent such as ε-caprolactam or γ-butyrolactam, ethyl acetoacetate or acetylacetone. Active methylene blocking agents such as ethyl malonate, alcohol blocking agents such as methanol and ethanol, A compound formed by blocking with a blocking agent such as an amine blocking agent, an imine blocking agent, an imide blocking agent, an imidazole blocking agent, or a mercaptan blocking agent can be used. Of course, a mixture of a plurality of these may be used.

上記両者の配合物をウレタン化反応により架橋硬化させると共に、未解離のブロックイソシアネート化合物を残存させる為には、硬化剤であるブロックイソシアネート化合物を過剰に配合すると共に、架橋硬化時の加熱温度や加熱時間等の処理条件を適宜調整することにより、主剤の活性水素基と見合う量のブロックイソシアネート化合物のみを解離させて架橋反応させる方法や、硬化剤であるブロックイソシアネート化合物として、解離温度の異なる複数種類のものを配合し、その各解離温度の中間の温度で硬化処理を行うことによって、解離温度の低いもののみを解離させて架橋反応させ、解離温度の高いものを未解離の状態で残存させる方法なども考えられる。   In order to crosslink and cure the blend of both of the above by a urethanization reaction and to leave the undissociated blocked isocyanate compound, the block isocyanate compound as a curing agent is excessively blended, and the heating temperature and heating at the time of crosslinking and curing are also included. By appropriately adjusting the processing conditions such as time, a method of dissociating only a blocked isocyanate compound in an amount corresponding to the active hydrogen group of the main agent and a crosslinking reaction, or a plurality of different dissociation temperatures as a blocked isocyanate compound as a curing agent A method in which only those having a low dissociation temperature are dissociated and subjected to a crosslinking reaction, and those having a high dissociation temperature are left in an undissociated state by performing a curing treatment at a temperature intermediate between the respective dissociation temperatures. Etc. are also conceivable.

しかし、上記の様な方法では、加熱温度や加熱時間等の処理条件のばらつきによって反応量がばらつき、得られる化粧材の物性が不安定になり易い。そこで、硬化剤として、ブロックされていないイソシアネート化合物と、ブロックイソシアネート化合物とを併用し、このうちブロックされていないイソシアネート化合物のみを架橋反応させて、ブロックイソシアネート化合物を解離させずに残存させる方法を用いれば、反応量はブロックされていないイソシアネート化合物とブロックイソシアネート化合物との配合比率で決定されるので、得られる化粧材の物性を安定させるためには有利である。ブロックされていないイソシアネート化合物による架橋反応は、常温ないし50℃以下程度の低温で数日程度で完結するので、この間にブロックイソシアネート化合物が解離して反応してしまうおそれがないからである。なお、化粧材の製造工程において、絵柄印刷層の形成後に加熱工程を含む場合には、その加熱の温度及び時間の条件では殆ど解離することがない様に、解離温度の高いブロックイソシアネート化合物を使用することが望ましい。   However, in the method as described above, the reaction amount varies due to variations in processing conditions such as heating temperature and heating time, and the physical properties of the resulting cosmetic material are likely to be unstable. Therefore, as a curing agent, a method is used in which an unblocked isocyanate compound and a blocked isocyanate compound are used in combination, and only the unblocked isocyanate compound is subjected to a crosslinking reaction to leave the blocked isocyanate compound without dissociation. For example, the reaction amount is determined by the blending ratio of the unblocked isocyanate compound and the blocked isocyanate compound, which is advantageous for stabilizing the physical properties of the resulting cosmetic material. This is because the crosslinking reaction with the unblocked isocyanate compound is completed within a few days at room temperature or a low temperature of about 50 ° C. or less, so that there is no possibility that the blocked isocyanate compound will dissociate and react during this time. In addition, when a heating process is included after the pattern printed layer is formed in the manufacturing process of the decorative material, a blocked isocyanate compound having a high dissociation temperature is used so that it hardly dissociates under the conditions of the heating temperature and time. It is desirable to do.

ブロックされていないイソシアネート化合物としては、例えばトリレンジイソシアネート、ジフェニルメタンジイソシアネート、キシリレンジイソシアネート、ナフタレンジイソシアネート、イソホロンジイソシアネート、ヘキサメチレンジイソシアネート等のイソシアネート化合物、又はこれらのビューレット体、アダクト体、イソシアヌレート体等を使用することができる。   Non-blocked isocyanate compounds include, for example, tolylene diisocyanate, diphenylmethane diisocyanate, xylylene diisocyanate, naphthalene diisocyanate, isophorone diisocyanate, hexamethylene diisocyanate and the like, or their burettes, adducts, isocyanurates and the like. Can be used.

但し、耐候性を考慮すると、黄変の原因となる芳香環を有しない脂肪族又は脂環式のイソシアネート化合物を使用することが望ましい。例えば、イソホロンジイソシアネート、ヘキサメチレンジイソシアネート、シクロヘキサンジイソシアネート、メチルヘキサンジイソシアネート、トリメチルヘキサメチレンジイソシアネート、水素添加ジフェニルメタンジイソシアネート、水素添加キシリレンジイソシアネート等又はこれらの誘導体等である。これはブロックイソシアネート、ブロックされていないイソシアネートに共通である。   However, in consideration of weather resistance, it is desirable to use an aliphatic or alicyclic isocyanate compound that does not have an aromatic ring that causes yellowing. For example, isophorone diisocyanate, hexamethylene diisocyanate, cyclohexane diisocyanate, methylhexane diisocyanate, trimethylhexamethylene diisocyanate, hydrogenated diphenylmethane diisocyanate, hydrogenated xylylene diisocyanate, etc., or derivatives thereof. This is common for blocked and unblocked isocyanates.

ブロックされていないイソシアネート化合物の配合量は、活性水素基を有する樹脂の活性水素基の量にほぼ見合う量とするのが良いが、厳密に一致させる必要性は必ずしもなく、活性水素基の数とイソシアネート基の数との比率が概ね1:0.9〜1:1.4程度の範囲内となる様な配合比率が選ばれるのが一般的である。通例、活性水素基を有する樹脂100重量部に対し、1〜10重量部程度の配合とすることが好ましい。   The blending amount of the unblocked isocyanate compound is preferably an amount substantially commensurate with the amount of active hydrogen groups of the resin having active hydrogen groups, but it is not always necessary to exactly match the number of active hydrogen groups. In general, the blending ratio is selected such that the ratio to the number of isocyanate groups is approximately in the range of about 1: 0.9 to 1: 1.4. In general, it is preferable to add about 1 to 10 parts by weight per 100 parts by weight of the resin having active hydrogen groups.

ブロックイソシアネート化合物の配合量は、化粧材に所望される耐候性や耐久性の程度によって適宜設計され、その量を増す程耐候性や耐久性の面では有利であるが、反面、あまり多すぎると、製造直後の初期状態において絵柄印刷層のバインダーが未反応の低分子量成分を多く含むことになるため、初期状態における層間密着性の物性が低下したり、或いは、経時によりブロックイソシアネート化合物が解離して生成したイソシアネート化合物による架橋反応が進み過ぎて、絵柄印刷層のバインダーの架橋密度が極端に高くなり過ぎたりして、却って層間密着性等の物性の低下の原因となる場合もある。従って、ブロックイソシアネート化合物の配合量は、前述したブロックされていないイソシアネート化合物の配合量の2倍以下の程度とすることが好ましい。一般的には、ブロックされていないイソシアネート化合物とほぼ同等程度の配合量とすることが好ましく、通例、活性水素基を有する樹脂100重量部に対し、1〜10重量部程度の配合とすることが好ましい。   The blending amount of the blocked isocyanate compound is appropriately designed depending on the degree of weather resistance and durability desired for the cosmetic material. Increasing the amount is more advantageous in terms of weather resistance and durability. In the initial state immediately after production, the binder of the pattern printing layer contains many unreacted low molecular weight components, so that the physical properties of interlayer adhesion in the initial state are reduced, or the blocked isocyanate compound is dissociated over time. In some cases, the cross-linking reaction by the isocyanate compound thus produced proceeds too much, and the cross-linking density of the binder of the picture print layer becomes extremely high, which may cause a decrease in physical properties such as interlayer adhesion. Therefore, the blending amount of the blocked isocyanate compound is preferably about twice or less than the blending amount of the unblocked isocyanate compound. In general, the blending amount is preferably about the same as that of an unblocked isocyanate compound. Generally, the blending amount is about 1 to 10 parts by weight with respect to 100 parts by weight of the resin having an active hydrogen group. preferable.

ちなみに、ブロックされていないイソシアネート化合物を全く配合せず、ブロックイソシアネート化合物を単独で使用し、これを全く解離させずに絵柄印刷層中に残存させる構成とすることは、化粧材の完成時点において絵柄印刷層のバインダーが架橋硬化していないので、初期の層間密着強度に劣るほか、印刷後の印刷インキ組成物の乾燥性が悪く、印刷物の巻取り又は積重ね保管時にブロッキング現象を発生し易いことなどの問題がある。   By the way, it is possible to use a blocked isocyanate compound alone without blending any unblocked isocyanate compound and leave it in the pattern print layer without dissociating it at the time of completion of the cosmetic material. Since the binder of the printing layer is not cross-linked and cured, the initial interlayer adhesion strength is inferior, the drying property of the printing ink composition after printing is poor, and a blocking phenomenon is likely to occur during winding or stacking of printed materials. There is a problem.

本発明の化粧材のより具体的な実施の形態の例を挙げれば、図1に示したのは、上側から順に、アイオノマー樹脂層1と、ポリオレフィン系樹脂又はポリエステル系樹脂からなる中間樹脂層2と、絵柄印刷層3と、プライマー層4と、バッカー層5とが積層されてなる、床タイル等の用途に好適な化粧材である。この化粧材の絵柄印刷層3は、既に説明した通りの、イソシアネート化合物を架橋剤としたウレタン化反応により架橋硬化していると共に、未解離のブロックイソシアネート化合物を含有する、イソシアネート硬化型ウレタン系樹脂をバインダーとして形成されているものである。   To give an example of a more specific embodiment of the decorative material of the present invention, FIG. 1 shows an ionomer resin layer 1 and an intermediate resin layer 2 made of a polyolefin resin or a polyester resin in order from the upper side. And a decorative material suitable for applications such as floor tiles, in which the pattern printing layer 3, the primer layer 4, and the backer layer 5 are laminated. This decorative material pattern print layer 3 is an isocyanate-cured urethane resin that has been crosslinked and cured by the urethanization reaction using an isocyanate compound as a crosslinking agent as described above, and contains an undissociated blocked isocyanate compound. Are formed using a binder.

アイオノマー樹脂層1に使用されるアイオノマー樹脂とは、一般に有機及び無機の成分が共有結合とイオン結合によって結合されている樹脂のことである。そして、上記化粧材に特に好ましく使用されるアイオノマー樹脂としては、共重合体の分子間を金属イオンで架橋した樹脂が挙げられ、この場合の共重合体としてはアクリレート系共重合体、例えばエチレン−メタクリル酸共重合体などが挙げられる。金属イオンとしては、例えばNa、K、Mg、Zn等のイオンが挙げられる。   The ionomer resin used for the ionomer resin layer 1 is a resin in which organic and inorganic components are generally bonded by covalent bonds and ionic bonds. Examples of the ionomer resin particularly preferably used for the decorative material include resins in which the copolymer molecules are cross-linked with metal ions. Examples of the copolymer in this case include acrylate copolymers such as ethylene- A methacrylic acid copolymer etc. are mentioned. Examples of metal ions include ions such as Na, K, Mg, and Zn.

アイオノマー樹脂を得るには、例えば、カルボキシル基を側鎖に有する単量体、例えばアクリル酸、メタクリル酸、マレイン酸、イタコン酸等、を共重合させたエチレン系のポリマーにNa、K、Mg、Zn等の水酸化物、アルコキシド、低級脂肪酸塩等を加えて酸基を中和する方法が挙げられる。これにより、分子鎖に沿って分布するカルボキシル陰イオンが分子間に存在する金属陽イオンと静電的に結合して一種の架橋を形成し、共重合体の分子間を金属イオンで架橋した構造のアイオノマー樹脂が得られる。   In order to obtain an ionomer resin, for example, Na, K, Mg, an ethylene polymer copolymerized with a monomer having a carboxyl group in the side chain, such as acrylic acid, methacrylic acid, maleic acid, itaconic acid, etc. A method of neutralizing an acid group by adding a hydroxide such as Zn, an alkoxide, a lower fatty acid salt or the like can be mentioned. As a result, a structure in which carboxyl anions distributed along the molecular chain are electrostatically combined with metal cations existing between the molecules to form a kind of cross-links, and the copolymer molecules are cross-linked with metal ions. The ionomer resin can be obtained.

上述のアイオノマー樹脂は、主鎖の共重合組成によってシートの硬さが任意に選択でき、また金属イオンによる架橋結合は、過熱により結合力が弱められ、冷却すると結合力が回復するという、ポリ塩化ビニル樹脂等の熱可塑性樹脂と近似した性質を有するので、熱ラミネーション及びエンボス加工により製造されていた従来のポリ塩化ビニル樹脂製の化粧材の製造ライン等に適用しやすいという利点がある。   The above-mentioned ionomer resin can be arbitrarily selected in terms of sheet hardness depending on the copolymer composition of the main chain, and the cross-linking by metal ions is weakened by overheating, and the bonding strength is restored by cooling. Since it has properties similar to those of a thermoplastic resin such as vinyl resin, it has an advantage that it can be easily applied to a conventional production line for decorative materials made of polyvinyl chloride resin, which has been manufactured by thermal lamination and embossing.

アイオノマー樹脂層1は、上記のアイオノマー樹脂に適当な添加剤を添加したものをシート化することにより得られる。アイオノマー樹脂層1の厚さは本発明において特に限定されるわけではないが、通常は200〜1000μm程度の厚さが適当である。   The ionomer resin layer 1 is obtained by forming a sheet obtained by adding an appropriate additive to the above ionomer resin. The thickness of the ionomer resin layer 1 is not particularly limited in the present invention, but a thickness of about 200 to 1000 μm is usually appropriate.

アイオノマー樹脂層1は、2層以上の複数層が積層されていてもよい。図1に示す例では、アイオノマー樹脂層1は、表面側の第1アイオノマー樹脂層11と、下側の第2アイオノマー樹脂層12との2層から構成されている。この様に構成すると、印刷基材である中間樹脂層2とアイオノマー樹脂層1との直接熱ラミネートが困難な場合であっても、中間樹脂層2の表面側に予め、厚さ10〜100μm程度の薄い第2アイオノマー樹脂層12を、例えばドライラミネート法、エクストルージョンラミネート法、共押出法等の手法により積層しておけば、該積層体の第2アイオノマー樹脂層12面に第1アイオノマー樹脂層11を容易に熱ラミネート可能となる利点がある。   The ionomer resin layer 1 may be a laminate of two or more layers. In the example shown in FIG. 1, the ionomer resin layer 1 is composed of two layers of a first ionomer resin layer 11 on the surface side and a second ionomer resin layer 12 on the lower side. If comprised in this way, even if it is a case where the direct thermal lamination of the intermediate resin layer 2 which is a printing base material and the ionomer resin layer 1 is difficult, about 10-100 micrometers in thickness on the surface side of the intermediate resin layer 2 beforehand. If the thin second ionomer resin layer 12 is laminated by, for example, a dry lamination method, an extrusion lamination method, a coextrusion method, or the like, the first ionomer resin layer 12 is formed on the second ionomer resin layer 12 surface of the laminate. There is an advantage that 11 can be easily heat laminated.

中間樹脂層2は、耐溶剤性に劣り印刷適性が良くないアイオノマー樹脂層1に代わって印刷基材となると共に、化粧材の使用中に使用されるワックスや洗浄剤等に含有される化学成分がアイオノマー樹脂層1中を浸透して来て絵柄印刷層3やプライマー層4を侵すのを防止する、化学成分の浸透遮断機能をも目的として設けられるもので、ポリオレフィン系樹脂又はポリエステル系樹脂が好適に使用される。   The intermediate resin layer 2 serves as a printing substrate in place of the ionomer resin layer 1 having poor solvent resistance and poor printability, and is a chemical component contained in a wax or a detergent used during use of a cosmetic material. Is provided for the purpose of blocking the penetration of chemical components, preventing penetration of the ionomer resin layer 1 and invading the pattern printing layer 3 and the primer layer 4. Preferably used.

ポリオレフィン系樹脂としては、例えばポリエチレン、ポリプロピレン、ポリブテン−1、ポリ−4−メチルペンテン−1、エチレン−プロピレン共重合体、エチレン−プロピレン−ブテン−1共重合体等、ポリエステル系樹脂としては、例えばポリエチレンテレフタレート、ポリブチレンテレフタレート、ポリエチレンイソフタレート、ポリエチレンナフタレート等を使用することができる。   Examples of the polyolefin resin include polyethylene, polypropylene, polybutene-1, poly-4-methylpentene-1, ethylene-propylene copolymer, and ethylene-propylene-butene-1 copolymer. Polyethylene terephthalate, polybutylene terephthalate, polyethylene isophthalate, polyethylene naphthalate and the like can be used.

中間樹脂層2の裏面に絵柄印刷層3を形成する際には、公知の任意の印刷方法を適用して行うことができる。例えば、グラビア印刷法、オフセット印刷法、フレキソ印刷法、スクリーン印刷法、転写印刷法、インクジェット印刷法等である。中でも化粧材においてはグラビア印刷法が最も一般的である。また絵柄印刷層3の印刷を行う前に、中間樹脂層2の裏面に予め例えばコロナ放電処理、プラズマ処理、オゾン処理、電離放射線処理、火炎処理、酸又はアルカリ処理等の易接着化のための表面処理を施してもよい。   When the pattern printing layer 3 is formed on the back surface of the intermediate resin layer 2, any known printing method can be applied. For example, a gravure printing method, an offset printing method, a flexographic printing method, a screen printing method, a transfer printing method, an inkjet printing method, and the like. Of these, the gravure printing method is the most common for decorative materials. Further, before printing the pattern printing layer 3, for example, corona discharge treatment, plasma treatment, ozone treatment, ionizing radiation treatment, flame treatment, acid or alkali treatment, etc. on the back surface of the intermediate resin layer 2 in advance. A surface treatment may be applied.

中間樹脂層2の厚さは、薄過ぎると各種化学物質に対する遮断性が不足し、厚過ぎるとアイオノマー樹脂層1の柔軟性や弾力性を減殺して化粧材の特性を損なうので、通常10〜100μm程度の範囲内とすることが望ましい。   If the thickness of the intermediate resin layer 2 is too thin, the barrier property against various chemical substances is insufficient, and if it is too thick, the flexibility and elasticity of the ionomer resin layer 1 are diminished and the properties of the cosmetic material are impaired. It is desirable to be within a range of about 100 μm.

これらアイオノマー樹脂層1や中間樹脂層2には、必要に応じて、その透明性を著しく減殺しない範囲において、各種の添加剤を添加してもよい。添加剤としては、例えば紫外線吸収剤、光安定剤、熱安定剤、着色剤、充填剤、滑剤、難燃剤、帯電防止剤、抗菌剤、防黴剤等を任意の組み合わせで用いることができる。   Various additives may be added to the ionomer resin layer 1 and the intermediate resin layer 2 as necessary, as long as the transparency is not significantly diminished. As additives, for example, ultraviolet absorbers, light stabilizers, heat stabilizers, colorants, fillers, lubricants, flame retardants, antistatic agents, antibacterial agents, antifungal agents and the like can be used in any combination.

プライマー層4は、中間樹脂層2及び絵柄印刷層3とバッカー層5とを、相互に強固に接着させるために設けられるものであり、その材質は、中間樹脂層2、絵柄印刷層3、バッカー層5の構成材料との接着性を勘案して適宜決定すればよい。必要なことは、アイオノマー樹脂層1からバッカー層5までを熱ラミネーションする温度及び圧力の条件で十分な接着性を発現するホットメルトタイプのものであることと、化粧材として実用に堪える接着力を有することである。   The primer layer 4 is provided to firmly bond the intermediate resin layer 2 and the pattern printing layer 3 and the backer layer 5 to each other, and the materials thereof are the intermediate resin layer 2, the pattern printing layer 3, and the backer layer. What is necessary is just to determine suitably considering the adhesiveness with the constituent material of the layer 5. FIG. What is necessary is that it is a hot melt type that exhibits sufficient adhesiveness under conditions of temperature and pressure for thermal lamination from the ionomer resin layer 1 to the backer layer 5, and has an adhesive strength that can withstand practical use as a cosmetic material. Is to have.

プライマー層4に用いるプライマーの好適な例を挙げれば、例えばエチレン−酢酸ビニル共重合体樹脂(EVA)、オレフィン系樹脂、またはそれらの混合物を主成分とした樹脂等であり、特に30〜50℃で溶解する性質を有するものが好ましい。また特に、該オレフィン系樹脂として、末端に例えば水酸基、アミノ基またはカルボキシル基等の官能基を有する樹脂を使用すると、隣接する層に含有されるカルボキシル基やエステル結合等の官能基との間に、水素結合やアミド結合、エステル結合等の化学結合を生成し、接着性を飛躍的に向上させることができるので好適である。   A suitable example of the primer used for the primer layer 4 is, for example, an ethylene-vinyl acetate copolymer resin (EVA), an olefin resin, or a resin mainly composed of a mixture thereof, particularly 30 to 50 ° C. Those having the property of being dissolved in are preferable. Further, in particular, when a resin having a functional group such as a hydroxyl group, an amino group or a carboxyl group at the terminal is used as the olefin-based resin, it is between the functional group such as a carboxyl group or an ester bond contained in an adjacent layer. It is preferable because a chemical bond such as a hydrogen bond, an amide bond or an ester bond can be generated and the adhesiveness can be drastically improved.

プライマー層4の形成方法は特に限定されず、従来公知の任意の塗工方法を適宜適用して形成することができる。具体的には、例えばグラビアコート法、ロールコート法、ナイフコート法、エアナイフコート法、バーコート法、ディップコート法、キスコート法、スプレーコート法、ダイコート法等であり、このほか絵柄印刷層3の形成方法として例示した各種の印刷方法によることもできる。   The formation method of the primer layer 4 is not specifically limited, It can form by applying conventionally well-known arbitrary coating methods suitably. Specific examples include a gravure coating method, a roll coating method, a knife coating method, an air knife coating method, a bar coating method, a dip coating method, a kiss coating method, a spray coating method, a die coating method, and the like. Various printing methods exemplified as the forming method can also be used.

なお、プライマー層4として、上述の様にホットメルトタイプのものを使用する場合には、プライマー層4の形成はホットメルトコーティング法によるのが最も適当である。すなわち、樹脂の固形分比NVを5〜30%程度に調整した塗液を加温させながら塗工する。塗工方法は、上掲した従来公知の任意の手段を任意に適用して行うことができる。プライマー層4の塗布量(乾燥後)は、0.1〜10g/m程度が適当であるが、勿論この範囲に限定されるものではない。 When the primer layer 4 is a hot melt type as described above, the primer layer 4 is most preferably formed by a hot melt coating method. That is, it coats, heating the coating liquid which adjusted solid content ratio NV of resin to about 5-30%. The coating method can be carried out by arbitrarily applying any conventionally known means described above. The amount of the primer layer 4 applied (after drying) is suitably about 0.1 to 10 g / m 2 , but of course is not limited to this range.

バッカー層5は、この化粧材の支持体となるものであり、従来の類似の化粧材においてバッカー層として使用されていたものと同様のものを使用すれば良い。一般的には熱可塑性樹脂を主成分とし、該熱可塑性樹脂として具体的には、例えばエチレン?アクリル酸メチル共重合体樹脂(EMA)、エチレン?アクリル酸エチル共重合体樹脂(EEA)、エチレン?メタクリル酸共重合体樹脂(EMAA)、エチレン?アクリル酸共重合体樹脂(EAA)、エチレンジアクリレート樹脂(EDA)、アイオノマー樹脂等のアクリレート系共重合体樹脂や、エチレン−酢酸ビニル共重合体樹脂(EVA)、エチレン−酪酸ビニル共重合体樹脂(EVB)等のビニルエステル系共重合体樹脂、或いはそれらの混合物などの樹脂が挙げられる。このような共重合樹脂は、共重合組成によりシートの硬さが任意に変えられる利点がある。   The backer layer 5 serves as a support for the decorative material, and the same material as that used as the backer layer in the conventional similar decorative material may be used. In general, a thermoplastic resin is the main component, and specific examples of the thermoplastic resin include ethylene-methyl acrylate copolymer resin (EMA), ethylene-ethyl acrylate copolymer resin (EEA), ethylene, and the like. Methacrylic acid copolymer resin (EMAA), ethylene-acrylic acid copolymer resin (EAA), ethylene diacrylate resin (EDA), ionomer resin and other acrylate copolymer resins, and ethylene-vinyl acetate copolymer Examples thereof include resins such as a resin (EVA), a vinyl ester copolymer resin such as an ethylene-vinyl butyrate copolymer resin (EVB), or a mixture thereof. Such a copolymer resin has an advantage that the hardness of the sheet can be arbitrarily changed by the copolymer composition.

バッカー層5を構成する熱可塑性樹脂には、化粧材の支持体として要求される剛性や寸法安定性を付与したり、製造原価を低減したりする目的で、無機充填剤が添加されるのが一般的である。この無機充填剤として具体的には、例えば炭酸カルシウム、硫酸バリウム、タルク、マイカ、カオリン、焼成クレー、シリカ、アルミナ、マグネシア、酸化チタン、酸化亜鉛、珪酸マグネシウム、チタン酸カリウム、水酸化アルミニウム、水酸化マグネシウム等を任意に組み合わせて用いることができる。無機充填剤の添加量は、熱可塑性樹脂100重量部当たり5〜500重量部程度の範囲で適宜設計される。   An inorganic filler is added to the thermoplastic resin constituting the backer layer 5 for the purpose of imparting rigidity and dimensional stability required as a support for a decorative material or reducing the manufacturing cost. It is common. Specific examples of the inorganic filler include calcium carbonate, barium sulfate, talc, mica, kaolin, calcined clay, silica, alumina, magnesia, titanium oxide, zinc oxide, magnesium silicate, potassium titanate, aluminum hydroxide, water Any combination of magnesium oxide and the like can be used. The addition amount of the inorganic filler is appropriately designed in the range of about 5 to 500 parts by weight per 100 parts by weight of the thermoplastic resin.

その他、必要に応じて、例えば紫外線吸収剤、光安定剤、熱安定剤、着色剤、有機充填剤、金属粉、滑剤、難燃剤、帯電防止剤、抗菌剤、防黴剤等の各種の添加剤を任意の組み合わせで添加することも勿論差し支えない。バッカー層5の厚さは特に限定はなく任意であるが、化粧材全体の厚み等を考慮すると、通常0.5〜5mm程度の厚さが適当である。   In addition, various additions such as UV absorbers, light stabilizers, heat stabilizers, colorants, organic fillers, metal powders, lubricants, flame retardants, antistatic agents, antibacterial agents, antifungal agents, etc., as necessary Of course, the agents may be added in any combination. The thickness of the backer layer 5 is not particularly limited and is arbitrary. However, considering the thickness of the entire decorative material, a thickness of about 0.5 to 5 mm is usually appropriate.

バッカー層5は、2層以上の多層積層体から構成されていてもよい。図1に示す例では、バッカー層5は、上側のエチレンジアクリレート樹脂からなる表層51と、下側の無機充填剤を含むエチレン−酢酸ビニル共重合体樹脂からなる基層52とから構成されている。このようにバッカー層5が多層積層体から構成されている場合には、無機充填剤は全ての層に含まれている必要は必ずしもなく、一部の層のみに含まれていてもよい。   The backer layer 5 may be composed of a multilayer stack of two or more layers. In the example shown in FIG. 1, the backer layer 5 includes a surface layer 51 made of an upper ethylene diacrylate resin and a base layer 52 made of an ethylene-vinyl acetate copolymer resin containing a lower inorganic filler. . Thus, when the backer layer 5 is comprised from the multilayer laminated body, the inorganic filler does not necessarily need to be contained in all the layers, and may be contained only in one part layer.

上記の化粧材の製造方法について説明すると、まず、ポリオレフィン系樹脂又はポリエステル系樹脂からなる中間樹脂層2と、第2アイオノマー樹脂層12との積層フィルムを、ドライラミネート法、エクストルージョンラミネート法又は共押出製膜法等の公知の手法で作製し、その中間樹脂層2面に、活性水素基を有する樹脂からなる主剤と、ブロックイソシアネート化合物及びブロックされていないイソシアネート化合物の混合物からなる硬化剤との配合組成物である、イソシアネート硬化型ポリウレタン樹脂をバインダーとする印刷インキ組成物を使用して、適宜の印刷方法により絵柄印刷層3を形成し、さらに、プライマー層4を塗工形成する。若しくは、中間樹脂層2の片面に絵柄印刷層3を形成してから、その反対側の面に第2アイオノマー樹脂層12をドライラミネート法又はエクストルージョンラミネート法等により積層してもよい。   The method for producing the decorative material will be described. First, a laminated film of the intermediate resin layer 2 made of polyolefin resin or polyester resin and the second ionomer resin layer 12 is formed by dry lamination, extrusion lamination, Produced by a known method such as an extrusion film forming method, on the intermediate resin layer 2 surface, a main agent composed of a resin having an active hydrogen group, and a curing agent composed of a mixture of a blocked isocyanate compound and an unblocked isocyanate compound Using the printing ink composition having an isocyanate curable polyurethane resin as a binder, which is a blended composition, the pattern printing layer 3 is formed by an appropriate printing method, and the primer layer 4 is formed by coating. Alternatively, after the pattern printing layer 3 is formed on one surface of the intermediate resin layer 2, the second ionomer resin layer 12 may be laminated on the opposite surface by a dry laminating method or an extrusion laminating method.

次に、この積層フィルムの第2アイオノマー樹脂層12面に第1アイオノマー樹脂層11を、プライマー層4面にバッカー層5を配置させて、これを熱ラミネーション法により貼り合わせて一体化した積層体を作製する。ラミネーションの方法としては、一般に枚葉による多段プレス方式、あるいは連続ラミネーション方式があるが、上記の化粧材の作製にはこのいずれの方式を用いても構わない。   Next, a laminated body in which the first ionomer resin layer 11 is disposed on the second ionomer resin layer 12 surface of the laminated film and the backer layer 5 is disposed on the primer layer 4 surface, which are bonded together by a thermal lamination method. Is made. As a lamination method, there are generally a multi-stage press method using single wafers or a continuous lamination method, and any of these methods may be used for producing the above-mentioned decorative material.

出来た積層体の表面には意匠性をさらに向上させるためエンボス加工を施し凹凸形状を形成してもよい。エンボス加工を施す手段としては、凹凸面を有するエンボスロールまたはエンボス版を加圧する従来公知の方法を用いて行うことができる。エンボス加工は上記の熱ラミネーションとは別に行っても構わないが、同時に行う方が製造工程を短縮できて有利である。以上の熱ラミネーションやエンボス加工には、従来のポリ塩化ビニル樹脂製の化粧材の製造ライン等をそのまま適用することも可能であり、安価な製造が可能である。   The surface of the resulting laminate may be embossed to form a concavo-convex shape in order to further improve the design. As the means for embossing, a conventionally known method of pressurizing an embossing roll or an embossing plate having an uneven surface can be used. The embossing may be performed separately from the thermal lamination described above, but it is advantageous to perform the embossing simultaneously because the manufacturing process can be shortened. For the above thermal lamination and embossing, it is possible to apply a conventional production line of a polyvinyl chloride resin decorative material as it is, and inexpensive production is possible.

以下に本発明の化粧材の具体的な実施例及び比較例を示して更に詳細に説明する。   Hereinafter, specific examples and comparative examples of the decorative material of the present invention will be shown and described in more detail.

実施例1
厚さ50μmのポリプロピレン樹脂層と厚さ30μmのアイオノマー樹脂層(三井デュポンポリケミカル社製「ハイミラン」)とからなる総厚80μmの共押出フィルムを作製し、そのポリプロピレン樹脂層面に、イソシアネート硬化型ウレタン系樹脂(主剤:水酸基含有ウレタン−塩化酢酸ビニル系樹脂100重量部、硬化剤:イソホロンジイソシアネート(IPDI)−ヘキサメチレンジイソシアネート(HMDI)系イソシアネート硬化剤(ブロックされていないもの)3重量部及びヘキサメチレンジイソシアネート(HMDI)系ブロックイソシアネート硬化剤3重量部)をバインダーとする印刷インキ組成物を使用して、グラビア印刷法により絵柄を印刷し(乾燥後の平均塗布量約1g/m)、さらに、エチレン−酢酸ビニル共重合体樹脂と、末端にカルボキシル基を有するオレフィン系樹脂との混合物を主成分(EVA/オレフィン=1/3)としたプライマー塗料をグラビアコーターにて乾燥後の塗布量が1.5g/mとなるように塗布し、乾燥させた。
Example 1
A co-extruded film having a total thickness of 80 μm comprising a polypropylene resin layer having a thickness of 50 μm and an ionomer resin layer having a thickness of 30 μm (“HIMILAN” manufactured by Mitsui DuPont Polychemical Co., Ltd.) was prepared. Resin (main agent: hydroxyl group-containing urethane-vinyl chloride resin 100 parts by weight, curing agent: isophorone diisocyanate (IPDI) -hexamethylene diisocyanate (HMDI) isocyanate curing agent (unblocked) 3 parts by weight and hexamethylene Using a printing ink composition having a diisocyanate (HMDI) block isocyanate curing agent (3 parts by weight) as a binder, a pattern is printed by a gravure printing method (average coating amount after drying is about 1 g / m 2 ), Ethylene-vinyl acetate And coalescing the resin, the coating amount after drying by gravure coater mixture main component (EVA / olefin = 1/3) and the primer coating of an olefin-based resin having a carboxyl group at the terminal with 1.5 g / m 2 It was applied and dried.

次に、この絵柄印刷とプライマー塗布を行った共押出フィルムのアイオノマー樹脂層面に、厚さ600μmのアイオノマー樹脂シート(三井デュポンポリケミカル社製「ハイミラン」)を、また、プライマー塗布面に、エチレンジアクリレート(EDA)樹脂からなる厚さ80μmの表層と、無機充填剤を含有するエチレン−酢酸ビニル共重合体(EVA)樹脂からなる厚さ1mmの基層との積層体からなるバッカー層の表層面を向けて重ね合わせ、ラミネート温度120℃の条件で連続ラミネーション方式により積層して貼り合わせて、本発明の化粧材を作製した。   Next, an ionomer resin sheet (“HIMILAN” manufactured by Mitsui DuPont Polychemical Co., Ltd.) having a thickness of 600 μm is formed on the surface of the ionomer resin layer of the coextruded film on which the pattern printing and the primer have been applied. A surface layer surface of a backer layer made of a laminate of a surface layer made of acrylate (EDA) resin having a thickness of 80 μm and a base layer made of ethylene-vinyl acetate copolymer (EVA) resin containing an inorganic filler and made of 1 mm thick. The decorative material according to the present invention was manufactured by laminating and laminating by a continuous lamination method under a lamination temperature of 120 ° C.

比較例1
上記実施例1において、絵柄の印刷に用いる印刷インキ組成物からブロックイソシアネート硬化剤を除き、他は同一の条件で化粧材を作製した。
Comparative Example 1
In Example 1 described above, a decorative material was prepared under the same conditions except that the blocked isocyanate curing agent was removed from the printing ink composition used for pattern printing.

性能評価
上記実施例1及び比較例1の化粧材について、サンシャインウェザオメーターにて促進耐候性試験を実施し、その500時間後、1000時間後及び2000時間後の化粧材の層間剥離強度を測定したところ、下表のとおりの結果であった。但し、剥離箇所は、比較例1の2000時間後のみが絵柄印刷層の凝集破壊であり、その他は全てバッカー層における表層と基層との層間剥離であった。
Performance Evaluation The decorative material of Example 1 and Comparative Example 1 was subjected to an accelerated weather resistance test with a sunshine weatherometer, and the delamination strength of the decorative material after 500 hours, 1000 hours and 2000 hours was measured. The results were as shown in the table below. However, as for the peeling part, only after 2000 hours of Comparative Example 1 was the cohesive failure of the pattern printing layer, and all the others were delaminations between the surface layer and the base layer in the backer layer.

促進耐候性試験後の層間剥離強度の測定結果(単位:[N/mm])
経過時間 0時間 500時間 1000時間 2000時間
実施例1 3.2 3.1 3.2 3.1
比較例1 3.2 3.2 3.3 0.9
Measurement result of delamination strength after accelerated weathering test (unit: [N / mm])
Elapsed time 0 hours 500 hours 1000 hours 2000 hours
Example 1 3.2 3.1 3.2 3.1
Comparative Example 1 3.2 3.2 3.3 0.9 0.9

本発明の化粧材の実施の形態を示す側断面図である。It is a sectional side view which shows embodiment of the decorative material of this invention.

符号の説明Explanation of symbols

1 アイオノマー樹脂層
11 第1アイオノマー樹脂層
12 第2アイオノマー樹脂層
2 中間樹脂層
3 絵柄印刷層
4 プライマー層
5 バッカー層
51 表層
52 基層
DESCRIPTION OF SYMBOLS 1 Ionomer resin layer 11 1st ionomer resin layer 12 2nd ionomer resin layer 2 Intermediate resin layer 3 Picture printing layer 4 Primer layer 5 Backer layer 51 Surface layer 52 Base layer

Claims (2)

アイオノマー樹脂層と、ポリオレフィン系樹脂又はポリエステル系樹脂からなる中間樹脂層からなり、前記中間層上にイソシアネート硬化型ウレタン系樹脂をバインダーとする絵柄印刷層を設けた化粧材において、前記絵柄印刷層は、ブロックされていないイソシアネート化合物と、ブロックイソシアネート化合物とが配合された硬化剤として用いたイソシアネート硬化型ウレタン系樹脂をバインダーとする印刷インキ組成物によって形成されており、かつ、前記イソシアネート硬化型ウレタン系樹脂は、前記ブロックされていないイソシアネート化合物を架橋剤としたウレタン化反応により架橋硬化していると共に、前記ブロックイソシアネート化合物が未解離の状態で残存していることを特徴とする化粧材。In a cosmetic material comprising an ionomer resin layer and an intermediate resin layer made of a polyolefin resin or a polyester resin, and a pattern printing layer having an isocyanate curable urethane resin as a binder on the intermediate layer, the pattern printing layer is , Formed by a printing ink composition having an isocyanate curable urethane resin used as a curing agent in which an unblocked isocyanate compound and a blocked isocyanate compound are blended, and the isocyanate curable urethane system The resin is crosslinked and cured by a urethanization reaction using the unblocked isocyanate compound as a crosslinking agent, and the blocked isocyanate compound remains in an undissociated state.
さらに、前記アイオノマー樹脂層上に、他のアイオノマー樹脂層、前記絵柄印刷層上に、プライマー層を介して無機充填剤を含有する熱可塑性樹脂からなるバッカー層とが積層されてなることを特徴とする請求項1に記載の化粧材 Furthermore, another ionomer resin layer on the ionomer resin layer, and a backer layer made of a thermoplastic resin containing an inorganic filler via a primer layer are laminated on the pattern printing layer. The cosmetic material according to claim 1 .
JP2003271265A 2003-07-07 2003-07-07 Cosmetic material Expired - Fee Related JP4759907B2 (en)