JP4650060B2 - Hollow molded container - Google Patents

Hollow molded container Download PDF

Info

Publication number
JP4650060B2
JP4650060B2 JP2005098193A JP2005098193A JP4650060B2 JP 4650060 B2 JP4650060 B2 JP 4650060B2 JP 2005098193 A JP2005098193 A JP 2005098193A JP 2005098193 A JP2005098193 A JP 2005098193A JP 4650060 B2 JP4650060 B2 JP 4650060B2
Authority
JP
Japan
Prior art keywords
ethylene
component
hollow molded
polymerization
olefin copolymer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
JP2005098193A
Other languages
Japanese (ja)
Other versions
JP2006273404A (en
Inventor
晋 江尻
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Sumitomo Chemical Co Ltd
Original Assignee
Sumitomo Chemical Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Sumitomo Chemical Co Ltd filed Critical Sumitomo Chemical Co Ltd
Priority to JP2005098193A priority Critical patent/JP4650060B2/en
Publication of JP2006273404A publication Critical patent/JP2006273404A/en
Application granted granted Critical
Publication of JP4650060B2 publication Critical patent/JP4650060B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Description

本発明は、エチレン−α−オレフィン共重合体を中空成形してなる中空成形容器に関するものである。   The present invention relates to a hollow molded container formed by hollow molding an ethylene-α-olefin copolymer.

マヨネーズやケチャップなどの食品、シャンプーやリンスなどの界面活性剤などに用いられる容器には、エチレン−α−オレフィン共重合体を中空成形してなる中空成形容器が多く用いられている。例えば、特定のメタロセン錯体とメチルアルミノキサンとを触媒成分とする重合触媒を用いて製造されたエチレン−1−オクテン共重合体からなる中空成形体(例えば、特許文献1参照。)、特定のメタロセン錯体と特定のホウ素化合物とトリイソブチルアルミニウムとを触媒成分とする重合触媒を用いて製造されたエチレン−1−ヘキセン共重合体と、低密度ポリエチレンとの樹脂組成物からなる中空成形体(例えば、特許文献2参照。)、メタロセン系重合触媒で製造されたエチレン−α−オレフィン共重合体と高密度ポリエチレンとの樹脂組成物からなる中空成形体(例えば、特許文献3参照。)などが提案されている。   As containers used for foods such as mayonnaise and ketchup, and surfactants such as shampoo and rinse, hollow molded containers formed by hollow molding of ethylene-α-olefin copolymers are often used. For example, a hollow molded body made of an ethylene-1-octene copolymer produced using a polymerization catalyst having a specific metallocene complex and methylaluminoxane as catalyst components (for example, see Patent Document 1), a specific metallocene complex A hollow molded body made of a resin composition of an ethylene-1-hexene copolymer produced using a polymerization catalyst containing a specific boron compound and triisobutylaluminum as catalyst components and low-density polyethylene (for example, patents) Reference 2), and a hollow molded body made of a resin composition of an ethylene-α-olefin copolymer and a high-density polyethylene produced with a metallocene polymerization catalyst (for example, see Patent Document 3) have been proposed. Yes.

特開平9−12634号公報Japanese Patent Laid-Open No. 9-12634 特開平10−25376号公報Japanese Patent Laid-Open No. 10-25376 特開2002−80531号公報JP 2002-80531 A

しかしながら、従来のエチレン−α−オレフィン共重合体を中空成形してなる中空成形容器は、メルトフラクチャーにより外観が低下することがあり、透明性や光沢において十分満足のいくものではなく、また、落下強度についても十分満足のいくものではなかった。
かかる状況のもと、本発明が解決しようとする課題は、外観、透明性、光沢および落下強度に優れる中空成形体を提供することにある。
However, a hollow molded container formed by hollow molding a conventional ethylene-α-olefin copolymer may deteriorate in appearance due to melt fracture, and is not sufficiently satisfactory in transparency and gloss. The strength was not satisfactory.
Under such circumstances, the problem to be solved by the present invention is to provide a hollow molded article excellent in appearance, transparency, gloss and drop strength.

本発明により、外観、透明性、光沢および落下強度に優れる中空成形体を提供することができる。   According to the present invention, it is possible to provide a hollow molded article excellent in appearance, transparency, gloss, and drop strength.

すなわち、本発明は、下記成分(A)を中空成形してなる中空成形容器にかかるものである。
成分(A):流動の活性化エネルギー(Ea)が40kJ/mol以上であり、JIS K7210に規定された温度190℃、荷重21.18Nの条件で測定されるメルトフローレート(MFR)が0.1〜100g/10分であり、分子量分布(Mw/Mn)が6〜25であるエチレン−α−オレフィン共重合体
That is, the present invention relates to a hollow molded container formed by hollow molding the following component (A).
Component (A): The flow activation energy (Ea) is 40 kJ / mol or more, the melt flow rate (MFR) measured under the conditions of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210 is 0.1. An ethylene-α-olefin copolymer having a molecular weight distribution (Mw / Mn) of 6 to 25 and 1 to 100 g / 10 minutes

本発明の成分(A)のエチレン−α−オレフィン共重合体は、エチレンと炭素原子数3〜20のα−オレフィンとを共重合して得られるエチレン−α−オレフィン共重合体である。炭素原子数3〜20のα−オレフィンとしては、例えば、プロピレン、1−ブテン、1−ペンテン、1−ヘキセン、1−ヘプテン、1−オクテン、1−ノネン、1−デセン、1−ドデセン、4−メチル−1−ペンテン、4−メチル−1−ヘキセン等があげられ、好ましくは1−ブテン、1−ヘキセン、1−オクテンである。また、上記の炭素原子数3〜20のα−オレフィンは単独で用いてもよく、2種以上を併用してもよい。   The component (A) ethylene-α-olefin copolymer of the present invention is an ethylene-α-olefin copolymer obtained by copolymerizing ethylene and an α-olefin having 3 to 20 carbon atoms. Examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 4 -Methyl-1-pentene, 4-methyl-1-hexene and the like can be mentioned, and 1-butene, 1-hexene and 1-octene are preferable. Moreover, said C3-C20 alpha olefin may be used independently and may use 2 or more types together.

成分(A)のエチレン−α−オレフィン共重合体としては、例えば、エチレン−プロピレン共重合体、エチレン−1−ブテン共重合体、エチレン−1−ヘキセン共重合体、エチレン−1−オクテン共重合体等があげられ、好ましくはエチレン−1−ブテン共重合体、エチレン−1−ヘキセン共重合体、エチレン−1−ブテン−1−ヘキセン共重合体、エチレン−1−ブテン−1−オクテン共重合体である。   Examples of the ethylene-α-olefin copolymer of component (A) include an ethylene-propylene copolymer, an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, and an ethylene-1-octene copolymer. Preferred are ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-butene-1-hexene copolymer, ethylene-1-butene-1-octene copolymer. It is a coalescence.

成分(A)のエチレン−α−オレフィン共重合体中のエチレンに基づく単量体単位の含有量は、エチレン−α−オレフィン共重合体の全重量(100重量%)に対して、通常50〜99重量%である。炭素原子数3〜12のα−オレフィンに基づく単量体単位の含有量は、エチレン−α−オレフィン共重合体の全重量(100重量%)に対して、通常1〜50重量%である。   The content of the monomer unit based on ethylene in the ethylene-α-olefin copolymer of the component (A) is usually from 50 to 50% based on the total weight (100% by weight) of the ethylene-α-olefin copolymer. 99% by weight. The content of the monomer unit based on the α-olefin having 3 to 12 carbon atoms is usually 1 to 50% by weight with respect to the total weight (100% by weight) of the ethylene-α-olefin copolymer.

成分(A)のエチレン−α−オレフィン共重合体は長鎖分岐を有し、このようなエチレン−α−オレフィン共重合体は、中空成形用に知られた従来のエチレン−α−オレフィン共重合体に比して、流動の活性化エネルギー(Ea)が高く、通常40kJ/mol以上である。従来から知られている中空成形用のエチレン−α−オレフィン共重合体のEaは、通常40kJ/molよりも低い値であり、中空成形品の透明性や光沢が劣ることがある。   The ethylene-α-olefin copolymer of component (A) has long chain branching, and such an ethylene-α-olefin copolymer is a conventional ethylene-α-olefin copolymer known for hollow molding. Compared with coalescence, the flow activation energy (Ea) is high, and is usually 40 kJ / mol or more. The Ea of the ethylene-α-olefin copolymer for hollow molding that has been conventionally known is usually lower than 40 kJ / mol, and the transparency and gloss of the hollow molded article may be inferior.

成分(A)のエチレン−α−オレフィン共重合体の流動の活性化エネルギー(Ea)として、中空成形体の透明性や光沢を高める観点から、好ましくは45kJ/mol以上であり、より好ましくは50kJ/mol以上であり、さらに好ましくは60kJ/mol以上である。また、中空成形体の落下強度を高める観点から、Eaは、好ましくは100kJ/mol以下であり、より好ましくは90kJ/mol以下である。   The flow activation energy (Ea) of the ethylene-α-olefin copolymer of component (A) is preferably 45 kJ / mol or more, more preferably 50 kJ, from the viewpoint of enhancing the transparency and gloss of the hollow molded body. / Mol or more, more preferably 60 kJ / mol or more. Further, from the viewpoint of increasing the drop strength of the hollow molded body, Ea is preferably 100 kJ / mol or less, more preferably 90 kJ / mol or less.

エチレン−α−オレフィン共重合体(A)の流動の活性化エネルギー(Ea)は、温度−時間重ね合わせ原理に基づいて、190℃での溶融複素粘度(単位:Pa・sec)の角周波数(単位:rad/sec)依存性を示すマスターカーブを作成する際のシフトファクター(aT)からアレニウス型方程式により算出される数値であって、以下に示す方法で求められる値である。すなわち、130℃、150℃、170℃、190℃、210℃の温度の中から、190℃を含む4つの温度について、夫々の温度(T、単位:℃)におけるエチレン−α−オレフィン共重合体の溶融複素粘度−角周波数曲線(溶融複素粘度の単位はPa・sec、角周波数の単位はrad/secである。)を、温度−時間重ね合わせ原理に基づいて、各温度(T)での溶融複素粘度−角周波数曲線毎に、190℃でのエチレン系共重合体の溶融複素粘度−角周波数曲線に重ね合わせた際に得られる各温度(T)でのシフトファクター(aT)を求め、夫々の温度(T)と、各温度(T)でのシフトファクター(aT)とから、最小自乗法により[ln(aT)]と[1/(T+273.16)]との一次近似式(下記(I)式)を算出する。次に、該一次式の傾きmと下記式(II)とからEaを求める。
ln(aT) = m(1/(T+273.16))+n (I)
Ea = |0.008314×m| (II)
T :シフトファクター
Ea:流動の活性化エネルギー(単位:kJ/mol)
T :温度(単位:℃)
上記計算は、市販の計算ソフトウェアを用いてもよく、該計算ソフトウェアとしては、Rheometrics社製 Rhios V.4.4.4などがあげられる。
なお、シフトファクター(aT)は、夫々の温度(T)における溶融複素粘度−角周波数の両対数曲線を、log(Y)=−log(X)軸方向に移動させて(但し、Y軸を溶融複素粘度、X軸を角周波数とする。)、190℃での溶融複素粘度−角周波数曲線に重ね合わせた際の移動量であり、該重ね合わせでは、夫々の温度(T)における溶融複素粘度−角周波数の両対数曲線は、角周波数をaT倍に、溶融複素粘度を1/aT倍に移動させる。
また、130℃、150℃、170℃、190℃、210℃の中から190℃を含む4つの温度でのシフトファクターと温度から得られる一次近似式(I)式を最小自乗法で求めるときの相関係数は、通常、0.99以上である。
The activation energy (Ea) of the flow of the ethylene-α-olefin copolymer (A) is an angular frequency (unit: Pa · sec) at 190 ° C. based on the temperature-time superposition principle. (Unit: rad / sec) It is a numerical value calculated by the Arrhenius equation from the shift factor (a T ) at the time of creating a master curve showing dependency, and is a value obtained by the following method. That is, an ethylene-α-olefin copolymer at each temperature (T, unit: ° C.) for four temperatures including 190 ° C. among temperatures of 130 ° C., 150 ° C., 170 ° C., 190 ° C., and 210 ° C. The melt complex viscosity-angular frequency curve (melt melt viscosity unit is Pa · sec, angular frequency unit is rad / sec) based on the temperature-time superposition principle at each temperature (T). For each melt complex viscosity-angular frequency curve, the shift factor (a T ) at each temperature (T) obtained when superimposed on the melt complex viscosity-angular frequency curve of the ethylene copolymer at 190 ° C. is obtained. , and each of the temperature (T), the primary approximate expression because the shift factor (a T) at each temperature (T), by the method of least squares [ln (aT)] and [1 / (T + 273.16) ] (Equation (I) below) is calculated. Next, Ea is obtained from the slope m of the linear expression and the following expression (II).
ln (a T ) = m (1 / (T + 273.16)) + n (I)
Ea = | 0.008314 × m | (II)
a T : Shift factor Ea: Activation energy of flow (unit: kJ / mol)
T: Temperature (unit: ° C)
For the calculation, commercially available calculation software may be used. As the calculation software, Rheos V. 4.4.4.
The shift factor (a T ) is obtained by moving the logarithmic curve of the melt complex viscosity-angular frequency at each temperature (T) in the log (Y) = − log (X) axis direction (however, the Y axis Is the complex viscosity of the melt, and the X axis is the angular frequency.), And the amount of movement when superposed on the melt complex viscosity-angular frequency curve at 190 ° C., in the superposition, melting at each temperature (T) The logarithmic curve of complex viscosity-angular frequency moves the angular frequency aT times and the melt complex viscosity 1 / aT times.
In addition, when obtaining the linear approximation formula (I) obtained from the shift factors and temperatures at four temperatures including 190 ° C. from 130 ° C., 150 ° C., 170 ° C., 190 ° C., and 210 ° C. by the method of least squares. The correlation coefficient is usually 0.99 or more.

上記の溶融複素粘度−角周波数曲線の測定は、粘弾性測定装置(例えば、Rheometrics社製Rheometrics Mechanical Spectrometer RMS−800など。)を用い、通常、ジオメトリー:パラレルプレート、プレート直径:25mm、プレート間隔:1.5〜2mm、ストレイン:5%、角周波数:0.1〜100rad/秒の条件で行われる。なお、測定は窒素雰囲気下で行われ、また、測定試料には予め酸化防止剤を適量(例えば1000ppm)を配合することが好ましい。   The above-mentioned melt complex viscosity-angular frequency curve is measured using a viscoelasticity measuring apparatus (for example, Rheometrics Mechanical Spectrometer RMS-800 manufactured by Rheometrics). Usually, geometry: parallel plate, plate diameter: 25 mm, plate interval: It is performed under the conditions of 1.5 to 2 mm, strain: 5%, angular frequency: 0.1 to 100 rad / sec. The measurement is performed in a nitrogen atmosphere, and it is preferable that an appropriate amount of an antioxidant (for example, 1000 ppm) is blended in advance with the measurement sample.

成分(A)のエチレン−α−オレフィン共重合体のJIS K7210−1995に規定された、温度190℃および荷重21.18Nの条件で測定されるメルトフローレート(MFR)は、0.01〜100g/10分である。該MFRが高すぎると中空成形体の落下強度が低下することがある。好ましくは0.1g/10分以上であり、より好ましくは0.5g/10分以上である。また、該MFRは、中空成形性を高める観点から、好ましくは100g/10分以下であり、より好ましくは10g/10分以下であり、更に好ましくは2g/10分以下であり、特に好ましくは1g/10分以下である。   The melt flow rate (MFR) measured under the conditions of a temperature of 190 ° C. and a load of 21.18 N as defined in JIS K7210-1995 of the ethylene-α-olefin copolymer of component (A) is 0.01 to 100 g. / 10 minutes. If the MFR is too high, the drop strength of the hollow molded body may decrease. Preferably it is 0.1 g / 10 minutes or more, More preferably, it is 0.5 g / 10 minutes or more. The MFR is preferably 100 g / 10 min or less, more preferably 10 g / 10 min or less, still more preferably 2 g / 10 min or less, and particularly preferably 1 g from the viewpoint of improving hollow moldability. / 10 minutes or less.

成分(A)のエチレン−α−オレフィン共重合体のメルトフローレート比(MFRR)は、通常40〜300である。該MFRRは、中空成形体の外観をより高める観点から、好ましくは50以上であり、より好ましくは55以上である。また、該MFRRは、中空成形体の落下強度をより高める観点から、好ましくは250以下であり、より好ましくは200以下である。なお、該MFRRは、JIS K7210−1995に規定された温度190℃および荷重211.8Nの条件で測定されるメルトフローレートを、JIS K7210−1995に規定された温度190℃および荷重21.18Nの条件で測定されるメルトフローレートで除した値である。   The melt flow rate ratio (MFRR) of the ethylene-α-olefin copolymer of component (A) is usually 40 to 300. The MFRR is preferably 50 or more, more preferably 55 or more, from the viewpoint of further enhancing the appearance of the hollow molded body. Further, the MFRR is preferably 250 or less, more preferably 200 or less, from the viewpoint of further increasing the drop strength of the hollow molded body. The MFRR is a melt flow rate measured at a temperature of 190 ° C. and a load of 211.8 N specified in JIS K7210-1995, and at a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210-1995. It is the value divided by the melt flow rate measured under the conditions.

成分(A)のエチレン−α−オレフィン共重合体の密度は、通常、890〜960kg/m3である。該密度は、中空成形体の落下強度をより高める観点から、好ましくは940kg/m3以下であり、より好ましくは935kg/m3以下であり、さらに好ましくは930kg/m3以下である。また、該密度は、中空成形容器の剛性を高める観点から、好ましくは900kg/m3以上であり、より好ましくは910kg/m3以上であり、さらに好ましくは912kg/m3以上である。なお、該密度は、JIS K6760−1995に記載のアニーリングを行い、JIS K7112−1980に規定された方法に従って測定される。 The density of the ethylene-α-olefin copolymer of component (A) is usually 890 to 960 kg / m 3 . Said seal degree, in order to further improve the drop strength of hollow molded body is preferably 940 kg / m 3 or less, more preferably 935 kg / m 3 or less, more preferably 930 kg / m 3 or less. Moreover, said seal degree, from the viewpoint of enhancing the rigidity of the hollow molded container, preferably 900 kg / m 3 or more, more preferably 910 kg / m 3 or more, more preferably 912 kg / m 3 or more. The density is measured according to the method defined in JIS K7112-1980 after annealing described in JIS K6760-1995.

成分(A)のエチレン−α−オレフィン共重合体の分子量分布(Mw/Mn)は、中空成形体の外観を高める観点から、好ましくは6以上であり、より好ましくは7以上である。また、該Mw/Mnは、中空成形体の透明性、光沢、落下強度を高める観点から、好ましくは25以下であり、より好ましくは20以下であり、更に好ましくは17以下である。なお、該分子量分布(Mw/Mn)は、ゲル・パーミエイション・クロマトグラフ測定によってポリスチレン換算の重量平均分子量(Mw)と数平均分子量(Mn)とを求め、MwをMnで除した値(Mw/Mn)である。   The molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer of component (A) is preferably 6 or more, more preferably 7 or more, from the viewpoint of enhancing the appearance of the hollow molded article. The Mw / Mn is preferably 25 or less, more preferably 20 or less, and still more preferably 17 or less, from the viewpoint of enhancing the transparency, gloss, and drop strength of the hollow molded body. The molecular weight distribution (Mw / Mn) is a value obtained by obtaining a weight average molecular weight (Mw) and a number average molecular weight (Mn) in terms of polystyrene by gel permeation chromatography, and dividing Mw by Mn ( Mw / Mn).

成分(A)のエチレン−α−オレフィン共重合体は、中空成形容器の透明性、光沢、落下強度を高める観点から、JIS K7210−1995に規定された、温度190℃、荷重21.18Nの条件で測定されるメルトフローレートをMFR(単位:g/10分)とし、極限粘度を[η](単位:dl/g)として、下記式(1)を充足することが好ましい。
0.80×MFR-0.094 < [η] < 1.50×MFR-0.156 (1)
中空成形容器の落下強度を高める観点から、エチレン−α−オレフィン共重合体(A)は、下記式(1−2)を充足することがより好ましく、
0.90×MFR-0.094 < [η] (1−2)
下記式(1−3)を充足することが更に好ましい。
1.00×MFR-0.094 < [η] (1−3)
また、中空成形体の透明性、光沢を高める観点から、エチレン−α−オレフィン共重合体は、下記式(1−4)を充足することがより好ましく、
[η] < 1.40×MFR-0.156 (1−4)
下記式(1−5)を充足することが更に好ましい。
[η] < 1.35×MFR-0.156 (1−5)
なお、JIS K7210−1995に規定された、温度190℃、荷重21.18Nの条件で測定されるメルトフローレートが同じ値である従来のエチレン−α−オレフィン共重合体と本発明のエチレン−α−オレフィン共重合体とを比較した場合、従来のエチレン−α−オレフィン共重合体の極限粘度は、本発明のエチレン−α−オレフィン共重合体の極限粘度よりも、通常高い値である。
The component (A) ethylene-α-olefin copolymer is a condition of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210-1995 from the viewpoint of enhancing the transparency, gloss, and drop strength of the hollow molded container. It is preferable to satisfy the following formula (1), where the melt flow rate measured in is MFR (unit: g / 10 min) and the intrinsic viscosity is [η] (unit: dl / g).
0.80 × MFR −0.094 <[η] <1.50 × MFR −0.156 (1)
From the viewpoint of increasing the drop strength of the hollow molded container, the ethylene-α-olefin copolymer (A) more preferably satisfies the following formula (1-2):
0.90 × MFR −0.094 <[η] (1-2)
It is more preferable to satisfy the following formula (1-3).
1.00 × MFR −0.094 <[η] (1-3)
Moreover, from the viewpoint of enhancing the transparency and gloss of the hollow molded body, the ethylene-α-olefin copolymer more preferably satisfies the following formula (1-4):
[Η] <1.40 × MFR −0.156 (1-4)
It is more preferable that the following formula (1-5) is satisfied.
[Η] <1.35 × MFR −0.156 (1-5)
In addition, the conventional ethylene-α-olefin copolymer having the same melt flow rate measured under the conditions of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210-1995 and the ethylene-α of the present invention. When comparing with an olefin copolymer, the intrinsic viscosity of the conventional ethylene-α-olefin copolymer is usually higher than the intrinsic viscosity of the ethylene-α-olefin copolymer of the present invention.

成分(A)のエチレン−α−オレフィン共重合体は、中空成形容器の透明性、光沢、落下強度を高める観点から、JIS K7210−1995に規定された、温度190℃、荷重21.18Nの条件で測定されるメルトフローレートをMFR(単位:g/10分)とし、190℃における溶融張力をMT(単位:cN)として、下記式(2)を充足することが好ましい。
2×MFR-0.59 < MT < 20×MFR-0.59 (2)
中空成形体の透明性、光沢を高める観点から、エチレン−α−オレフィン共重合体は、下記式(2−2)を充足することがより好ましく、
2.2×MFR-0.59 < MT (2−2)
下記式(2−3)を充足することが更に好ましい。
2.5×MFR-0.59 < MT (2−3)
また、中空成形体の落下強度を高める観点から、エチレン−α−オレフィン共重合体は、下記式(2−4)を充足することがより好ましく、
MT < 10×MFR-0.59 (2−4)
下記式(2−5)を充足することが更に好ましい。
MT < 5×MFR-0.59 (2−5)
The component (A) ethylene-α-olefin copolymer is a condition of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210-1995 from the viewpoint of enhancing the transparency, gloss, and drop strength of the hollow molded container. It is preferable to satisfy the following formula (2) where MFR (unit: g / 10 minutes) is the melt flow rate measured in step (1) and MT (unit: cN) is 190 ° C.
2 x MFR -0.59 <MT <20 x MFR -0.59 (2)
From the viewpoint of increasing the transparency and gloss of the hollow molded body, the ethylene-α-olefin copolymer more preferably satisfies the following formula (2-2):
2.2 x MFR -0.59 <MT (2-2)
It is more preferable to satisfy the following formula (2-3).
2.5 × MFR -0.59 <MT (2-3)
Moreover, from the viewpoint of increasing the drop strength of the hollow molded body, the ethylene-α-olefin copolymer more preferably satisfies the following formula (2-4),
MT <10 × MFR -0.59 (2-4)
It is more preferable to satisfy the following formula (2-5).
MT <5 x MFR -0.59 (2-5)

成分(A)のエチレン−α−オレフィン共重合体は、中空成形体の外観、透明性、光沢を高める観点から、温度190℃、角周波数100rad/secでの溶融複素粘度をη*(単位:Pa・sec)とし、JIS K7210に規定された、温度190℃、荷重21.18Nの条件で測定されるメルトフローレートをMFR(単位:g/10分)として、下記式(3)を充足するものが好ましく、
η* < 1550×MFR-0.25−420 (3)
下記式(3−2)を充足することがより好ましく、
η* < 1500×MFR-0.25−420 (3−2)
下記式(3−3)を充足することが更に好ましく、
η* < 1450×MFR-0.25−420 (3−3)
下記式(3−4)を充足することが特に好ましい。
η* < 1350×MFR-0.25−420 (3−4)
The component (A) ethylene-α-olefin copolymer has a melt complex viscosity of η * (unit: unit) at a temperature of 190 ° C. and an angular frequency of 100 rad / sec from the viewpoint of enhancing the appearance, transparency and gloss of the hollow molded body. Pa · sec), and the melt flow rate measured under conditions of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210 is MFR (unit: g / 10 minutes), and the following formula (3) is satisfied. Is preferred,
η * <1550 × MFR -0.25 -420 (3)
More preferably, the following formula (3-2) is satisfied,
η * <1500 × MFR -0.25 -420 (3-2)
More preferably, the following formula (3-3) is satisfied,
η * <1450 × MFR -0.25 -420 (3-3)
It is particularly preferable that the following formula (3-4) is satisfied.
η * <1350 × MFR -0.25 -420 (3-4)

溶融複素粘度η*は、エチレン−α−オレフィン共重合体(A)の流動の活性化エネルギー(Ea)を求めるために行われる測定のうち、190℃の溶融複素粘度−角周波数の測定において得られた、角周波数100rad/secにおける溶融複素粘度である。 The melt complex viscosity η * is obtained in the measurement of the melt complex viscosity-angular frequency at 190 ° C. among the measurements performed for obtaining the activation energy (Ea) of the flow of the ethylene-α-olefin copolymer (A). The melt complex viscosity at an angular frequency of 100 rad / sec.

成分(A)のエチレン−α−オレフィン共重合体の製造方法としては、例えば、有機アルミニウム化合物、有機アルミニウムオキシ化合物、ホウ素化合物、有機亜鉛化合物などの助触媒成分を粒子状担体に担持させてなる固体粒子状の助触媒成分(以下、成分(イ)と称する。)と、アルキレン基やシリレン基等の架橋基で2つのシクロペンタジエニル型アニオン骨格が結合した構造を持つ配位子を有するメタロセン錯体(以下、成分(ロ)と称する。)とを触媒成分として用いてなる重合触媒の存在下、エチレンとα−オレフィンとを共重合する方法があげられる。   As a method for producing the ethylene-α-olefin copolymer of component (A), for example, a promoter component such as an organoaluminum compound, an organoaluminum oxy compound, a boron compound, and an organozinc compound is supported on a particulate carrier. It has a solid particulate promoter component (hereinafter referred to as component (i)) and a ligand having a structure in which two cyclopentadienyl type anion skeletons are bonded to each other by a crosslinking group such as an alkylene group or a silylene group. Examples thereof include a method in which ethylene and an α-olefin are copolymerized in the presence of a polymerization catalyst using a metallocene complex (hereinafter referred to as component (b)) as a catalyst component.

上記固体粒子状の助触媒成分としては、メチルアルモキサンを多孔質シリカと混合させた成分、ジエチル亜鉛と水とフッ化フェノールを多孔質シリカと混合させた成分等をあげることができる。   Examples of the solid particulate promoter component include a component in which methylalumoxane is mixed with porous silica, a component in which diethyl zinc, water, and fluorinated phenol are mixed with porous silica.

上記固体粒子状の助触媒成分のより具体例として、成分(a)ジエチル亜鉛、成分(b)フッ素化フェノール、成分(c)水、成分(d)多孔質シリカおよび成分(e)トリメチルジシラザン(((CH33Si)2NH)を接触させてなる助触媒担体成分(イ)をあげることができる。 More specific examples of the solid particulate promoter component include component (a) diethylzinc, component (b) fluorinated phenol, component (c) water, component (d) porous silica and component (e) trimethyldisilazane. The promoter support component (a) obtained by contacting (((CH 3 ) 3 Si) 2 NH) can be mentioned.

成分(b)のフッ素化フェノールとしては、ペンタフルオロフェノール、3,5−ジフルオロフェノール、3,4,5−トリフルオロフェノール、2,4,6−トリフルオロフェノール等をあげることができる。成分(A)の流動活性化エネルギー(Ea)、分子量分布(Mw/Mn)を高める観点から、フッ素数の異なる2種類のフッ素化フェノールを用いることが好ましく、この場合、フッ素数が多いフェノールとフッ素数が少ないフェノールとのモル比としては、通常、20/80〜80/20であり、該モル比は高い方が好ましい。   Examples of the fluorinated phenol of component (b) include pentafluorophenol, 3,5-difluorophenol, 3,4,5-trifluorophenol, 2,4,6-trifluorophenol and the like. From the viewpoint of increasing the fluid activation energy (Ea) and molecular weight distribution (Mw / Mn) of the component (A), it is preferable to use two types of fluorinated phenols having different fluorine numbers. The molar ratio of phenol with a small number of fluorine is usually 20/80 to 80/20, and it is preferable that the molar ratio is high.

上記成分(a)、成分(b)および成分(c)の使用量としては、各成分の使用量のモル比率を成分(a):成分(b):成分(c)=1:y:zとすると、yおよびzが下記の式を満足することが好ましい。
|2−y−2z|≦1
上記の式におけるyとして、好ましくは0.01〜1.99の数であり、より好ましくは0.10〜1.80の数であり、さらに好ましくは0.20〜1.50の数であり、最も好ましくは0.30〜1.00の数である。
The amount of component (a), component (b) and component (c) used is the molar ratio of the amount of each component used: component (a): component (b): component (c) = 1: y: z Then, it is preferable that y and z satisfy the following formula.
| 2-y-2z | ≦ 1
Y in the above formula is preferably a number of 0.01 to 1.99, more preferably a number of 0.10 to 1.80, and still more preferably a number of 0.20 to 1.50. Most preferably, the number is 0.30 to 1.00.

成分(a)に対して使用する成分(d)の量としては、成分(a)と成分(d)との接触により得られる粒子に含まれる亜鉛原子のモル数が、該粒子1gあたり0.1mmol以上となる量であることが好ましく、0.5〜20mmolとなる量であることがより好ましい。成分(d)に対して使用する成分(e)の量としては、成分(d)1gあたり成分(e)0.1mmol以上となる量であることが好ましく、0.5〜20mmolとなる量であることがより好ましい。   The amount of the component (d) used relative to the component (a) is such that the number of moles of zinc atoms contained in the particles obtained by contacting the component (a) and the component (d) is 0.00 per gram of the particles. The amount is preferably 1 mmol or more, and more preferably 0.5 to 20 mmol. The amount of the component (e) to be used with respect to the component (d) is preferably an amount that makes the component (e) 0.1 mmol or more per 1 g of the component (d), and an amount that becomes 0.5 to 20 mmol. More preferably.

上記メタロセン錯体としては、2つのインデニル基が、エチレン基、ジメチルメチレン基またはジメチルシリレン基で結合したジルコノセン錯体、2つのメチルインデニル基が、エチレン基、ジメチルメチレン基またはジメチルシリレン基で結合したジルコノセン錯体、2つのメチルシクロペンタジエニル基が、エチレン基、ジメチルメチレン基またはジメチルシリレン基で結合したジルコノセン錯体、2つのジメチルシクロペンタジエニル基が、エチレン基、ジメチルメチレン基またはジメチルシリレン基で結合したジルコノセン錯体等をあげることができる。また、成分(ロ)の金属原子としては、ジルコニウムとハフニウムが好ましく、さらに金属原子が有する残りの置換基としては、ジフェノキシ基やジアルコキシ基が好ましい。成分(ロ)として、好ましくは、エチレンビス(1−インデニル)ジルコニウムジフェノキシドがあげられる。   The metallocene complex includes a zirconocene complex in which two indenyl groups are bonded by an ethylene group, a dimethylmethylene group or a dimethylsilylene group, and a zirconocene in which two methylindenyl groups are bonded by an ethylene group, a dimethylmethylene group or a dimethylsilylene group. Complex A zirconocene complex in which two methylcyclopentadienyl groups are bonded by ethylene, dimethylmethylene or dimethylsilylene groups, and two dimethylcyclopentadienyl groups are bonded by ethylene, dimethylmethylene or dimethylsilylene groups The zirconocene complex etc. which were made can be mention | raise | lifted. Moreover, as a metal atom of a component (b), a zirconium and hafnium are preferable, and also as a remaining substituent which a metal atom has, a diphenoxy group and a dialkoxy group are preferable. The component (b) is preferably ethylenebis (1-indenyl) zirconium diphenoxide.

上記の固体粒子状の助触媒成分とメタロセン錯体とを用いてなる重合触媒においては、適宜、有機アルミニウム化合物を触媒成分として併用してもよく、該有機アルミニウム化合物としては、トリイソブチルアルミニウム、トリノルマルオクチルアルミニウム等をあげることができる。   In the polymerization catalyst comprising the above-described solid particulate promoter component and the metallocene complex, an organoaluminum compound may be used in combination as a catalyst component as appropriate. Examples of the organoaluminum compound include triisobutylaluminum, trinormal Examples include octyl aluminum.

上記メタロセン錯体の使用量は、上記固体粒子状の助触媒成分1gあたり、好ましくは5×10-6〜5×10-4molである。また有機アルミニウム化合物の使用量として、好ましくは、上記メタロセン錯体の金属原子1モルあたり、有機アルミニウム化合物のアルミニウム原子が1〜2000モルとなる量である。 The amount of the metallocene complex used is preferably 5 × 10 −6 to 5 × 10 −4 mol per 1 g of the solid particulate promoter component. The amount of the organoaluminum compound used is preferably such that the aluminum atom of the organoaluminum compound is 1 to 2000 mol per mol of the metal atom of the metallocene complex.

また、上記の固体粒子状の助触媒成分とメタロセン錯体とを用いてなる重合触媒においては、適宜、電子供与性化合物を触媒成分として併用してもよく、該電子供与性化合物としては、トリエチルアミン、トリノルマルオクチルアミン等をあげることができる。   In addition, in the polymerization catalyst using the solid particulate promoter component and the metallocene complex, an electron donating compound may be used as a catalyst component as appropriate. Examples of the electron donating compound include triethylamine, Examples thereof include tri-normal octylamine.

上記成分(b)のフッ素化フェノールとしてフッ素数の異なる2種類のフッ素化フェノールを用いる場合は、電子供与性化合物を用いることが好ましい。   When two types of fluorinated phenols having different numbers of fluorine are used as the component (b) fluorinated phenol, it is preferable to use an electron donating compound.

電子供与性化合物の使用量としては、上記の触媒成分として用いられる有機アルミニウム化合物のアルミニウム原子のモル数に対して、通常0.1〜10mol%であり、成分(A)の分子量分布(Mw/Mn)を高める観点から、該使用量は高い方が好ましい。   The amount of the electron-donating compound used is usually 0.1 to 10 mol% with respect to the number of moles of aluminum atoms in the organoaluminum compound used as the catalyst component, and the molecular weight distribution (Mw / From the viewpoint of increasing Mn), the amount used is preferably higher.

成分(A)のエチレン−α−オレフィン共重合体の製造方法としては、より具体的には、上記助触媒担体(イ)、架橋型ビスインデニルジルコニウム錯体および有機アルミニウム化合物を接触させてなる触媒の存在下、エチレンと炭素原子数3〜20のα−オレフィンとを共重合する方法があげられる。   More specifically, as a method for producing the ethylene-α-olefin copolymer of component (A), a catalyst obtained by contacting the promoter support (a), the crosslinked bisindenylzirconium complex and the organoaluminum compound. In the presence of, there is a method of copolymerizing ethylene and an α-olefin having 3 to 20 carbon atoms.

重合方法として、好ましくは、エチレン−α−オレフィン共重合体の粒子の形成を伴う連続重合方法であり、例えば、連続気相重合、連続スラリー重合、連続バルク重合であり、好ましくは、連続気相重合である。気相重合反応装置としては、通常、流動層型反応槽を有する装置であり、好ましくは、拡大部を有する流動層型反応槽を有する装置である。反応槽内に攪拌翼が設置されていてもよい。   The polymerization method is preferably a continuous polymerization method involving the formation of ethylene-α-olefin copolymer particles, for example, continuous gas phase polymerization, continuous slurry polymerization, continuous bulk polymerization, preferably continuous gas phase Polymerization. The gas phase polymerization reaction apparatus is usually an apparatus having a fluidized bed type reaction tank, and preferably an apparatus having a fluidized bed type reaction tank having an enlarged portion. A stirring blade may be installed in the reaction vessel.

成分(A)のエチレン−α−オレフィン共重合体の製造に用いられる重合触媒の各成分を反応槽に供給する方法としては、通常、窒素、アルゴン等の不活性ガス、水素、エチレン等を用いて、水分のない状態で供給する方法、各成分を溶媒に溶解または稀釈して、溶液またはスラリー状態で供給する方法が用いられる。重合触媒の各成分は個別に供給してもよく、任意の成分を任意の順序にあらかじめ接触させて供給してもよい。   As a method for supplying each component of the polymerization catalyst used for the production of the component (A) ethylene-α-olefin copolymer to the reaction vessel, usually, an inert gas such as nitrogen or argon, hydrogen, ethylene or the like is used. Then, a method of supplying in a state free from moisture, or a method of supplying each component in a solution or slurry after dissolving or diluting each component in a solvent is used. Each component of the polymerization catalyst may be supplied individually, or arbitrary components may be supplied in contact in advance in any order.

また、本重合を実施する前に、予備重合を実施し、予備重合された予備重合触媒成分を本重合の触媒成分または触媒として使用することが好ましい。本重合と予備重合では異なるα−オレフィンを用いてもよく、炭素原子数が4〜12のα−オレフィンとエチレンとを予備重合することが好ましく、炭素原子数が6〜8のα−オレフィンとエチレンとを予備重合することがより好ましい。   Moreover, it is preferable to carry out prepolymerization before carrying out the main polymerization and to use the prepolymerized prepolymerized catalyst component as a catalyst component or catalyst for the main polymerization. Different α-olefins may be used in the main polymerization and the prepolymerization, and it is preferable to prepolymerize an α-olefin having 4 to 12 carbon atoms with ethylene, and an α-olefin having 6 to 8 carbon atoms. It is more preferable to prepolymerize with ethylene.

重合温度としては、通常、エチレン−α−オレフィン共重合体が溶融する温度よりも低く、好ましくは0〜150℃であり、より好ましくは30〜100℃であり、さらに好ましくは50〜90℃である。また、エチレン−α−オレフィン共重合体の分子量分布(Mw/Mn)を広げる観点からは、重合温度は高い方が好ましい。   The polymerization temperature is usually lower than the temperature at which the ethylene-α-olefin copolymer melts, preferably 0 to 150 ° C, more preferably 30 to 100 ° C, and even more preferably 50 to 90 ° C. is there. From the viewpoint of expanding the molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, a higher polymerization temperature is preferable.

重合時間としては(連続重合反応である場合は平均滞留時間として)、通常1〜20時間である。エチレン−α−オレフィン共重合体の分子量分布(Mw/Mn)を広げる観点からは、重合時間(平均滞留時間)は長い方が好ましい。   The polymerization time is usually 1 to 20 hours (as an average residence time in the case of a continuous polymerization reaction). From the viewpoint of expanding the molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, it is preferable that the polymerization time (average residence time) is long.

また、共重合体の溶融流動性を調節する目的で、重合反応ガスに水素を分子量調節剤として添加してもよく、重合反応ガス中に不活性ガスを共存させてもよい。重合反応ガス中のエチレンのモル濃度に対する重合反応ガス中の水素のモル濃度は、重合反応ガス中のエチレンのモル濃度100モル%として、通常、0.1〜3mol%である。また、また、エチレン−α−オレフィン共重合体の分子量分布(Mw/Mn)を広げる観点からは、該重合反応ガス中の水素のモル濃度は、高い方が好ましい。   Further, for the purpose of adjusting the melt fluidity of the copolymer, hydrogen may be added to the polymerization reaction gas as a molecular weight regulator, and an inert gas may be allowed to coexist in the polymerization reaction gas. The molar concentration of hydrogen in the polymerization reaction gas with respect to the molar concentration of ethylene in the polymerization reaction gas is usually 0.1 to 3 mol% as the molar concentration of ethylene in the polymerization reaction gas is 100 mol%. Moreover, from the viewpoint of widening the molecular weight distribution (Mw / Mn) of the ethylene-α-olefin copolymer, it is preferable that the molar concentration of hydrogen in the polymerization reaction gas is high.

本発明の中空成形容器の中空成形においては、成分(A)に、必要に応じて、酸化防止剤、抗ブロッキング剤、滑剤、帯電防止剤、耐候安定剤、顔料、加工性改良剤等の添加剤;成分(A)以外の重合体成分等を添加してもよく、該添加剤および該重合体成分は2種以上を併用されてもよい。   In the hollow molding of the hollow molding container of the present invention, an antioxidant, an antiblocking agent, a lubricant, an antistatic agent, a weathering stabilizer, a pigment, a processability improving agent, etc. are added to the component (A) as necessary. Agent; Polymer components other than component (A) may be added, and two or more of these additives and polymer components may be used in combination.

成分(A)以外の重合体成分(以下、成分(B)と称する。)としては、エチレンに基づく単量体単位の含有量が50重量%以上であるエチレン系重合体(ただし、該重合体の全重量を100重量%とする。)が好適であり、高圧法低密度ポリエチレン、エチレン−酢酸ビニル共重合体、エチレン−メタアクリル酸エステル共重合体、エチレン−アクリル酸共重合体、エチレン−アクリル酸エステル共重合体、流動の活性化エネルギー(Ea)が40kJ/mol未満であるエチレン−α−オレフィン共重合体などがあげられる。これらは、1種でも2種以上を組み合わせて用いてもよい。   As the polymer component other than the component (A) (hereinafter referred to as the component (B)), an ethylene polymer in which the content of monomer units based on ethylene is 50% by weight or more (however, the polymer) Is preferably 100% by weight, and high pressure method low density polyethylene, ethylene-vinyl acetate copolymer, ethylene-methacrylic acid ester copolymer, ethylene-acrylic acid copolymer, ethylene- Examples thereof include acrylic acid ester copolymers and ethylene-α-olefin copolymers having a flow activation energy (Ea) of less than 40 kJ / mol. These may be used alone or in combination of two or more.

成分(B)のエチレン系重合体としては、高圧法低密度ポリエチレンおよび流動の活性化エネルギー(Ea)が40kJ/mol未満であるエチレン−α−オレフィン共重合体からなるエチレン系重合体群から選ばれた少なくとも1種のエチレン系重合体であることが好ましい。   The ethylene polymer of component (B) is selected from the group of ethylene polymers consisting of high pressure process low density polyethylene and ethylene-α-olefin copolymers having a flow activation energy (Ea) of less than 40 kJ / mol. The at least one ethylene polymer is preferably used.

成分(B)に用いられるエチレン−α−オレフィン共重合体は、エチレンと炭素原子数3〜20のα−オレフィンを共重合して得られるエチレン−α−オレフィン共重合体である。炭素原子数3〜20のα−オレフィンとしては、例えば、プロピレン、1−ブテン、1−ペンテン、1−ヘキセン、1−ヘプテン、1−オクテン、1−ノネン、1−デセン、1−ドデセン、4−メチル−1−ペンテン、4−メチル−1−ヘキセン等があげられ、好ましくは1−ブテン、1−ヘキセン、1−オクテンである。また、上記の炭素原子数3〜20のα−オレフィンは単独で用いてもよく、2種以上を併用してもよい。   The ethylene-α-olefin copolymer used for the component (B) is an ethylene-α-olefin copolymer obtained by copolymerizing ethylene and an α-olefin having 3 to 20 carbon atoms. Examples of the α-olefin having 3 to 20 carbon atoms include propylene, 1-butene, 1-pentene, 1-hexene, 1-heptene, 1-octene, 1-nonene, 1-decene, 1-dodecene, 4 -Methyl-1-pentene, 4-methyl-1-hexene and the like can be mentioned, and 1-butene, 1-hexene and 1-octene are preferable. Moreover, said C3-C20 alpha olefin may be used independently and may use 2 or more types together.

成分(B)に用いられるエチレン−α−オレフィン共重合体は、例えば、エチレン−プロピレン共重合体、エチレン−1−ブテン共重合体、エチレン−1−ヘキセン共重合体、エチレン−1−オクテン共重合体等があげられ、好ましくはエチレン−1−ブテン共重合体、エチレン−1−ヘキセン共重合体、エチレン−1−ブテン−1−ヘキセン共重合体、エチレン−1−ブテン−1−オクテン共重合体である。   Examples of the ethylene-α-olefin copolymer used in the component (B) include an ethylene-propylene copolymer, an ethylene-1-butene copolymer, an ethylene-1-hexene copolymer, and an ethylene-1-octene copolymer. Examples thereof include ethylene-1-butene copolymer, ethylene-1-hexene copolymer, ethylene-1-butene-1-hexene copolymer, and ethylene-1-butene-1-octene copolymer. It is a polymer.

成分(B)に用いられるエチレン−α−オレフィン共重合体の製造方法としては、チーグラー・ナッタ系触媒、クロム系触媒、メタロセン系触媒等の公知の重合触媒を用いて、液相重合法、スラリー重合法、気相重合法、高圧イオン重合法等の公知の重合方法によって製造する方法があげられる。また、該重合法は、回分重合法、連続重合法のいずれでもよく、2段階以上の多段重合法でもよい。   As a method for producing an ethylene-α-olefin copolymer used for the component (B), a known polymerization catalyst such as a Ziegler-Natta catalyst, a chromium catalyst, a metallocene catalyst or the like is used. Examples thereof include a production method by a known polymerization method such as a polymerization method, a gas phase polymerization method, and a high-pressure ion polymerization method. The polymerization method may be either a batch polymerization method or a continuous polymerization method, and may be a multistage polymerization method having two or more stages.

上記のチーグラー・ナッタ系触媒としては、例えば、次の(1)または(2)の触媒があげられる。
(1)三塩化チタン、三塩化バナジウム、四塩化チタンおよびチタンのハロアルコラートからなる群から選ばれる少なくとも1種をマグネシウム化合物系担体に担持した成分と、共触媒である有機金属化合物からなる触媒
(2)マグネシウム化合物とチタン化合物の共沈物または共晶体と共触媒である有機金属化合物からなる触媒
Examples of the Ziegler-Natta catalyst include the following catalysts (1) or (2).
(1) A catalyst comprising a component in which at least one selected from the group consisting of titanium trichloride, vanadium trichloride, titanium tetrachloride and titanium haloalcolate is supported on a magnesium compound carrier, and an organometallic compound as a cocatalyst ( 2) A catalyst comprising an organometallic compound which is a coprecipitate of a magnesium compound and a titanium compound or a eutectic and a cocatalyst.

上記のクロム系触媒としては、例えば、シリカまたはシリカ−アルミナにクロム化合物を担持した成分と、共触媒である有機金属化合物からなる触媒があげられる。   Examples of the chromium-based catalyst include a catalyst comprising a component in which a chromium compound is supported on silica or silica-alumina, and an organometallic compound as a cocatalyst.

メタロセン系触媒としては、例えば、次の(1)〜(4)の触媒があげられる。
(1)シクロペンタジエニル型アニオン骨格を1つ持つ配位子を1つ有する遷移金属化合物あるいはシクロペンタジエニル型アニオン骨格を1つ持つ配位子を2つ有する(2つの該配位子は架橋基等で結合していない)遷移金属化合物を含む成分と、アルモキサン化合物を含む成分からなる触媒
(2)前記遷移金属化合物を含む成分と、トリチルボレート、アニリニウムボレート等のイオン性化合物を含む成分からなる触媒
(3)前記遷移金属化合物を含む成分と、前記イオン性化合物を含む成分と、有機アルミニウム化合物を含む成分からなる触媒
(4)前記の各成分をSiO2、Al23等の無機粒子状担体や、エチレン、スチレン等のオレフィン重合体等の粒子状ポリマー担体に担持または含浸させて得られる触媒
Examples of the metallocene catalyst include the following catalysts (1) to (4).
(1) a transition metal compound having one ligand having one cyclopentadienyl type anion skeleton or two ligands having one cyclopentadienyl type anion skeleton (two such ligands) A catalyst comprising a component containing a transition metal compound (not bonded by a bridging group or the like), a component containing an alumoxane compound, and (2) a component containing the transition metal compound and an ionic compound such as trityl borate or anilinium borate. A catalyst comprising a component comprising (3) a component comprising the transition metal compound, a component comprising the ionic compound, and a catalyst comprising a component comprising an organoaluminum compound. (4) Each of the above components can be converted into SiO 2 , Al 2 O 3. Catalysts obtained by supporting or impregnating inorganic particulate carriers such as ethylene and particulate polymer carriers such as olefin polymers such as ethylene and styrene

成分(B)に用いられる高圧法低密度ポリエチレン、エチレン−酢酸ビニル共重合体、エチレン−メタアクリル酸エステル共重合体、エチレン−アクリル酸共重合体、エチレン−アクリル酸エステル共重合体の製造方法としては、公知の重合方法があげられ、例えば、エチレン単独あるいはエチレンと共重合単量体とを、高温高圧下でラジカル重合する方法があげられる。   Method for producing high-pressure low-density polyethylene, ethylene-vinyl acetate copolymer, ethylene-methacrylic acid ester copolymer, ethylene-acrylic acid copolymer, ethylene-acrylic acid ester copolymer used for component (B) Examples of the polymerization method include known polymerization methods, for example, a method of radical polymerization of ethylene alone or ethylene and a comonomer at high temperature and high pressure.

成分(B)のエチレン系重合体のJIS K7210−1995に規定された温度190℃、荷重21.18Nの条件で測定されるメルトフローレート(MFR)は、中空成形性を高める観点から、好ましくは0.1g/10分以上であり、より好ましくは0.5g/10分以上であり、更に好ましくは0.8g/10分以上である。また、中空成形体の落下強度を高める観点から、該MFRは、好ましくは100g/10分以下であり、より好ましくは10g/10分以下であり、更に好ましくは4g/10分以下である。   The melt flow rate (MFR) measured under conditions of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210-1995 of the ethylene-based polymer of the component (B) is preferably from the viewpoint of improving the hollow moldability. It is 0.1 g / 10 min or more, more preferably 0.5 g / 10 min or more, still more preferably 0.8 g / 10 min or more. Further, from the viewpoint of increasing the drop strength of the hollow molded body, the MFR is preferably 100 g / 10 min or less, more preferably 10 g / 10 min or less, and further preferably 4 g / 10 min or less.

成分(B)に用いられるエチレン系重合体の密度は、通常、880〜960kg/m3である。該密度は、中空成形体の落下強度を高める観点から、好ましくは940kg/m3以下であり、より好ましくは930kg/m3以下であり、さらに好ましくは925kg/m3以下である。また、中空成形容器の剛性を高める観点から、890kg/m3以上であり、より好ましくは895kg/m3以上であり、さらに好ましくは900kg/m3以上である。なお、該密度は、JIS K6760−1995に記載のアニーリングを行い、JIS K7112−1980に規定された方法に従って測定される。 The density of the ethylene polymer used for the component (B) is usually 880 to 960 kg / m 3 . The density is preferably 940 kg / m 3 or less, more preferably 930 kg / m 3 or less, and further preferably 925 kg / m 3 or less, from the viewpoint of increasing the drop strength of the hollow molded body. Further, from the viewpoint of enhancing the rigidity of the hollow molded container, it is 890 kg / m 3 or more, more preferably 895kg / m 3 or more, more preferably 900 kg / m 3 or more. The density is measured according to the method defined in JIS K7112-1980 after annealing described in JIS K6760-1995.

成分(B)に用いられるエチレン−α−オレフィン共重合体のメルトフローレート比(MFRR)は、通常10〜200である。該MFRRは、中空成形容器の外観を高める観点から、好ましくは12以上であり、より好ましくは15以上である。また、該MFRは、中空成形体の落下強度を高める観点から、好ましくは100以下であり、より好ましくは50以下であり、最も好ましくは35以下である。なお、MFRRは、JIS K7210−1995に規定された温度190℃および荷重211.8Nの条件で測定されるメルトフローレートを、JIS K7210−1995に規定された温度190℃および荷重21.18Nの条件で測定されるメルトフローレートで除した値である。   The melt flow rate ratio (MFRR) of the ethylene-α-olefin copolymer used for the component (B) is usually 10 to 200. The MFRR is preferably 12 or more, more preferably 15 or more, from the viewpoint of enhancing the appearance of the hollow molded container. The MFR is preferably 100 or less, more preferably 50 or less, and most preferably 35 or less, from the viewpoint of increasing the drop strength of the hollow molded body. The MFRR is a melt flow rate measured under the conditions of a temperature of 190 ° C. and a load of 211.8 N specified in JIS K7210-1995, and a condition of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210-1995. It is the value divided by the melt flow rate measured in

成分(A)と成分(B)とを含有する中空成形体とする場合、成分(A)と成分(B)の含有量としては、成分(A)と成分(B)の合計を100重量%として、中空成形体の透明性、光沢、外観を高める観点から、成分(A)の含有量が50重量%以上(成分(B)の含有量が50重量%以下)であり、成分(A)の含有量が60重量%以上(成分(B)の含有量が40重量%以下)であることが好ましく、成分(A)の含有量が70重量%以上(成分(B)の含有量が30重量%以下)であることがより好ましい。また、中空成形体の落下強度を高める観点からは、成分(A)の含有量が95重量%以下(成分(B)の含有量が5重量%以上)であり、成分(A)の含有量が90重量%以下(成分(B)の含有量が10重量%以上)であることが好ましく、成分(A)の含有量が85重量%以下(成分(B)の含有量が15重量%以上)であることがより好ましい。   When it is set as the hollow molded object containing a component (A) and a component (B), as content of a component (A) and a component (B), the sum total of a component (A) and a component (B) is 100 weight%. From the viewpoint of enhancing the transparency, gloss and appearance of the hollow molded article, the content of the component (A) is 50% by weight or more (the content of the component (B) is 50% by weight or less), and the component (A) Is preferably 60% by weight or more (component (B) content is 40% by weight or less), and component (A) content is 70% by weight or more (component (B) content is 30%). More preferably, it is not more than% by weight. From the viewpoint of increasing the drop strength of the hollow molded body, the content of the component (A) is 95% by weight or less (the content of the component (B) is 5% by weight or more), and the content of the component (A) Is 90% by weight or less (component (B) content is 10% by weight or more), component (A) content is 85% by weight or less (component (B) content is 15% by weight or more) ) Is more preferable.

上述した必要に応じて添加される添加剤、成分(B)等は、成分(A)にあらかじめ溶融混練してもよく、成分(A)にドライブレンドして中空成形に用いてもよく、また、一種以上のマスターバッチを用意して成分(A)にドライブレンドして中空成形に用いてもよい。   The additive, component (B), etc. added as necessary may be previously melt-kneaded with component (A), dry blended with component (A) and used for hollow molding, Alternatively, one or more master batches may be prepared and dry blended with the component (A) for use in hollow molding.

中空成形方法としては、公知の方法が用いられ、押出式、アキュムレーター式、ホットパリソン式、コールドパリソン式、射出式等があげられる。例えば、本発明の中空成形容器は、押出機から押し出して溶融パリソンを得、該パリソンを中空成形機の所望の容器形状を有する金型内にセットした後、これに圧縮ガスを吹き込んで金型内面壁まで膨らませ、しかる後、冷却させることにより得られる。また、連続成形機構としては、シャトル型、ロータリー型、サテライト型など形式があげられ、型締め方法としては、油圧式、電動式、トグル式などがあげられ、成形時に延伸を行ってもよい。   As the hollow molding method, a known method is used, and examples thereof include an extrusion method, an accumulator method, a hot parison method, a cold parison method, and an injection method. For example, the hollow molding container of the present invention is extruded from an extruder to obtain a molten parison, and the parison is set in a mold having a desired container shape of the hollow molding machine, and then compressed gas is blown into the mold. It is obtained by inflating to the inner wall and then cooling. Further, examples of the continuous molding mechanism include a shuttle type, a rotary type, and a satellite type, and examples of the mold clamping method include a hydraulic type, an electric type, a toggle type, and the like, and stretching may be performed at the time of molding.

本発明の中空成形容器には、必要に応じて多層構成とし、本発明の効果を損なわない範囲において、滑り性を付与した層や、酸素などの気体や水蒸気のバリア層、遮光層、酸素吸収層、接着層、着色層、導電性層、再生樹脂含有層などを設けてもよい。   The hollow molded container of the present invention has a multilayer structure as necessary, and within a range that does not impair the effects of the present invention, a layer provided with slipperiness, a barrier layer of gas such as oxygen or water vapor, a light shielding layer, oxygen absorption A layer, an adhesive layer, a colored layer, a conductive layer, a recycled resin-containing layer, or the like may be provided.

本発明の中空成形容器の内容物としては、例えば、しょうゆ、ソース、味噌、マヨネーズ、ケチャップ、焼肉のたれ、練りからし、練りわさび、擂ったにんにく、ミネラルウォーター、清涼飲料水、お茶、食用油、流動食、スープなどの食品;シャンプー、リンス、ハンドソープ、ボディソープ、洗濯洗剤、柔軟剤、台所洗剤などの界面活性剤類;内服薬、点眼薬、点滴薬、浣腸薬などの医薬品;機械の作動油、潤滑油などの油類;写真現像液、洗浄液、クーラント、殺菌剤、漂白剤などの化学薬品類;農薬;飼料などがあげられる。   The contents of the hollow molded container of the present invention include, for example, soy sauce, sauce, miso, mayonnaise, ketchup, grilled meat sauce, knead, kneaded wasabi, garlic garlic, mineral water, soft drink, tea, edible Oils, liquid foods, soups and other foods; shampoos, rinses, hand soaps, body soaps, laundry detergents, softeners, kitchen detergents, and other surfactants; internal medicines, eye drops, drops, enemas, etc .; machinery Oils such as hydraulic oils, lubricating oils, etc .; chemicals such as photographic developers, cleaning liquids, coolants, bactericides, bleaching agents; agricultural chemicals; feeds.

本発明の中空成形容器は、例えば、ボトル、取手付ボトル、スクイズボトル、プラスチックタンク、バッグインボックス、洗瓶、ドラム缶内容器、IBC、コンテナ、ガソリンタンク、チューブ状容器、点眼容器、浣腸容器、折りたたみ容器などとして用いられる。   The hollow molded container of the present invention is, for example, a bottle, a bottle with a handle, a squeeze bottle, a plastic tank, a bag-in-box, a washing bottle, a container in a drum, an IBC, a container, a gasoline tank, a tubular container, an eye drop container, an enema container, Used as a folding container.

本発明の中空成形容器は、透明性、光沢および落下強度に優れる。また、外観にも優れうるため、食品用容器に好適に用いられる。   The hollow molded container of the present invention is excellent in transparency, gloss and drop strength. Moreover, since it may be excellent in appearance, it is suitably used for food containers.

以下、実施例および比較例により本発明を説明する。
実施例および比較例での物性は、次の方法に従って測定した。
Hereinafter, the present invention will be described with reference to examples and comparative examples.
The physical properties in Examples and Comparative Examples were measured according to the following methods.

(1)メルトフローレート(MFR、単位:g/10分)
JIS K7210−1995に規定された方法に従い、荷重21.18N、温度190℃の条件で測定した。
(1) Melt flow rate (MFR, unit: g / 10 minutes)
According to the method defined in JIS K7210-1995, the measurement was performed under the conditions of a load of 21.18 N and a temperature of 190 ° C.

(2)メルトフローレート比(MFRR)
JIS K7210−1995に従って測定した。試験荷重211.83N、測定温度190℃の条件で測定した値を、試験荷重21.18N、測定温度190℃の条件で測定した値で、除した値をMFRRとした。
(2) Melt flow rate ratio (MFRR)
It measured according to JIS K7210-1995. The value measured under the conditions of a test load of 21.83 N and a measurement temperature of 190 ° C. and the value measured under the conditions of a test load of 21.18 N and a measurement temperature of 190 ° C. was taken as MFRR.

(3)密度(単位:kg/m3)
JIS K7112−1980のうち、A法に規定された方法に従って測定した。なお、測定試料片は、JIS K6760−1995に記載のアニーリングを行い測定に用いた。
(3) Density (Unit: kg / m 3 )
It measured according to the method prescribed | regulated to A method among JISK7112-1980. The measurement sample piece was annealed according to JIS K6760-1995 and used for measurement.

(4)分子量分布(Mw/Mn)
ゲル・パーミエイション・クロマトグラフ(GPC)法を用いて、下記の条件(1)〜(7)により測定を行った。予め分子量分布が単分散とみなせる分子量分布の狭い標準ポリスチレン(東ソー製TSK STANDARD POLYSTYRNE)を用いて作成しておいた検量線を用いて、ポリスチレン換算の重量平均分子量(Mw)とポリスチレン換算の数平均分子量(Mn)をもとめ、それらより分子量分布(Mw/Mn)を求めた。
(1)装置:Water製Waters150C
(2)分離カラム:TOSOH TSKgelGMH−HT
(3)測定温度:145℃
(4)キャリア:オルトジクロロベンゼン
(5)流量:1.0mL/分
(6)注入量:500μL
(7)検出器:示差屈折
(4) Molecular weight distribution (Mw / Mn)
The measurement was performed under the following conditions (1) to (7) using a gel permeation chromatograph (GPC) method. The weight average molecular weight (Mw) in terms of polystyrene and the number average in terms of polystyrene using a calibration curve prepared in advance using a standard polystyrene (TSK STANDARD POLYSTYRNE manufactured by Tosoh Corporation) with a narrow molecular weight distribution that can be regarded as monodisperse. The molecular weight (Mn) was determined, and the molecular weight distribution (Mw / Mn) was determined from them.
(1) Equipment: Waters 150C manufactured by Water
(2) Separation column: TOSOH TSKgelGMH-HT
(3) Measurement temperature: 145 ° C
(4) Carrier: Orthodichlorobenzene
(5) Flow rate: 1.0 mL / min
(6) Injection volume: 500 μL
(7) Detector: Differential refraction

(5)流動の活性化エネルギー(Ea、単位:kJ/mol)
粘弾性測定装置(Rheometrics社製Rheometrics Mechanical Spectrometer RMS−800)を用いて、下記測定条件で130℃、150℃、170℃および190℃での溶融複素粘度−角周波数曲線を測定し、次に、得られた溶融複素粘度−角周波数曲線から、Rheometrics社製計算ソフトウェア Rhios V.4.4.4を用いて、活性化エネルギー(Ea)を求めた。
<測定条件>
ジオメトリー:パラレルプレート
プレート直径:25mm
プレート間隔:1.2〜2mm
ストレイン :5%
角周波数 :0.1〜100rad/秒
測定雰囲気 :窒素下
(5) Flow activation energy (Ea, unit: kJ / mol)
Using a viscoelasticity measuring device (Rheometrics Mechanical Spectrometer RMS-800 manufactured by Rheometrics), a melt complex viscosity-angular frequency curve at 130 ° C., 150 ° C., 170 ° C. and 190 ° C. was measured under the following measurement conditions. From the obtained melt complex viscosity-angular frequency curve, calculation software Rhios V. The activation energy (Ea) was determined using 4.4.4.
<Measurement conditions>
Geometry: Parallel plate Plate diameter: 25mm
Plate spacing: 1.2-2mm
Strain: 5%
Angular frequency: 0.1 to 100 rad / sec Measurement atmosphere: Under nitrogen

(6)溶融複素粘度(η*(100)、単位:Pa・sec)
上記の(5)流動の活性化エネルギーを測定した際に得られた190℃での溶融複素粘度−角周波数の測定結果から、角速度が100rad/secにおける190℃の溶融複素粘度を求めた。
(6) Melt complex viscosity (η * (100), unit: Pa · sec)
The melt complex viscosity at 190 ° C. at an angular velocity of 100 rad / sec was determined from the measurement result of the melt complex viscosity at 190 ° C.-angular frequency obtained when the above (5) flow activation energy was measured.

(7)溶融張力(MT、単位:cN)
東洋精機製作所製 メルトテンションテスターを用いて、温度が190℃の条件で、9.5mmφのバレルに充填した溶融樹脂を、ピストン降下速度5.5mm/分で、径が2.09mmφ、長さ8mmのオリフィスから押出し、該押し出された溶融樹脂を、径が150mmφの巻き取りロールを用い、40rpm/分の巻き取り上昇速度で巻き取り、溶融樹脂が破断する直前における張力値を測定した。この値が大きいほど溶融張力が大きいことを示す。
(7) Melt tension (MT, unit: cN)
Using a melt tension tester manufactured by Toyo Seiki Seisakusho, a molten resin filled in a 9.5 mmφ barrel at a temperature of 190 ° C., a piston descending speed of 5.5 mm / min, a diameter of 2.09 mmφ, and a length of 8 mm The melted resin extruded from the orifice was wound up at a winding speed of 40 rpm / min using a winding roll having a diameter of 150 mmφ, and the tension value immediately before the molten resin broke was measured. It shows that melt tension is so large that this value is large.

(8)極限粘度([η]、単位:dl/g)
2,6−ジ−t−ブチル−p−クレゾール(BHT)を5重量%溶解したテトラリン溶液(以下、ブランク溶液と称する。)と、該ブランク溶液に対して、エチレン重合体樹脂の濃度が1mg/mlとなる135℃のテトラリン溶液(以下、サンプル溶液と称する。)とを調整し、ウベローデ型粘度計により、該ブランク溶液と該サンプル溶液の135℃での降下時間を測定し、該降下時間から135℃での相対粘度(ηrel)を求めた後、下記式より算出した。
[η]=23.3×log(ηrel
(8) Intrinsic viscosity ([η], unit: dl / g)
A tetralin solution (hereinafter referred to as a blank solution) in which 5% by weight of 2,6-di-t-butyl-p-cresol (BHT) is dissolved, and the concentration of the ethylene polymer resin with respect to the blank solution is 1 mg. A 135 ° C. tetralin solution (hereinafter referred to as a sample solution) is prepared, and the falling time of the blank solution and the sample solution at 135 ° C. is measured by an Ubbelohde viscometer. From the following formula, the relative viscosity (η rel ) at 135 ° C. was calculated and calculated from the following formula.
[Η] = 23.3 × log (η rel )

(9)透明性(Haze、単位:%)
容器の胴部の平坦な部分から試験片を採取し、該試験片のHazeをASTM D1003に従って測定した。この値が小さいほど透明性が良いことを示す。
(9) Transparency (Haze, unit:%)
A test piece was taken from the flat part of the body of the container, and the haze of the test piece was measured according to ASTM D1003. It shows that transparency is so good that this value is small.

(10)光沢(Gloss、単位:%)
容器の胴部の平坦な部分から試験片を採取し、該試験片の45度鏡面光沢度をJIS K7105−1981に従って測定した。この値が大きいほど光沢が優れることを示す。
(10) Gloss (Gloss, unit:%)
A test piece was collected from the flat portion of the body of the container, and the 45-degree specular gloss of the test piece was measured according to JIS K7105-1981. The larger this value, the better the gloss.

(11)外観
中空成形容器の表面について、メルトフラクチャーによる縞状の外観荒れが認められるものを「×」、メルトフラクチャーによる縞状の外観荒れが認められないものを「○」と判定した。
(11) Appearance With respect to the surface of the hollow molded container, “X” indicates that striped appearance roughness due to melt fracture is observed, and “◯” indicates that no stripe appearance roughness due to melt fracture is observed.

(12)落下強度
中空成形容器に飲料水500gを充填し、該容器をゴム製パッキング付キャップにより密閉した。次に、該容器を5℃の恒温槽に12時間以上入れて状態調整した。状態調整後、落下試験として、室温雰囲気にて、高さ1.5mから容器を縦方向(容器の口が上)にした落下(縦落下)と、高さ1.5mから容器を横向(容器の口が横)にした落下(横落下)とを、縦落下から交互に最大で各10回(縦落下と横落下の合計で20回)行った。上記落下試験により、中空成形容器にピンホールや割れが発生するまでの落下回数、すなわち、n回目で中空成形容器にピンホールや割れが発生した場合はn−1(ただし、20回の落下でも中空成形容器にピンホールや割れが発生しない場合は20とする。)を、5本の中空成形容器について求め、該5本の中空成形容器の落下回数の総数を落下強度指数として求めた。5本全てが20回の落下で割れなければ、(落下強度指数)=100であり、5本全てが1回目の落下で割れれば、(落下強度指数)=0となる。
落下強度指数が、0以上33未満の場合を「落下強度:×」、33以上66未満の場合を「落下強度:△」、66以上100以下の場合を「落下強度:○」と判定した。
(12) Drop strength A hollow molded container was filled with 500 g of drinking water, and the container was sealed with a cap with rubber packing. Next, the container was placed in a thermostatic bath at 5 ° C. for 12 hours or longer for condition adjustment. After the condition adjustment, as a drop test, in a room temperature atmosphere, the container was dropped in the vertical direction from the height of 1.5 m (the container mouth was up) (vertical drop), and the container was turned sideways from the height of 1.5 m (container The fall (lateral drop) was performed 10 times each alternately from the vertical drop (a total of 20 times of the vertical drop and the horizontal drop). According to the above drop test, the number of drops until a pinhole or crack occurs in the hollow molded container, that is, n-1 when a pinhole or crack occurs in the hollow molded container at the nth time (however, even when dropped 20 times) When no pinholes or cracks occur in the hollow molded container, it is set to 20.) was determined for five hollow molded containers, and the total number of drops of the five hollow molded containers was determined as a drop strength index. If all 5 pieces are not broken by 20 drops, (drop strength index) = 100, and if all 5 pieces are broken by the first drop, (drop strength index) = 0.
The case where the drop strength index was 0 or more and less than 33 was determined as “drop strength: x”, the case where it was 33 or more and less than 66 was determined as “drop strength: Δ”, and the case where it was 66 or more and 100 or less was determined as “drop strength: ○”.

実施例1
(1)助触媒担体の調製
窒素置換した撹拌機を備えた反応器に、窒素流通下で300℃において加熱処理したシリカ(デビソン社製 Sylopol948;平均粒子径=55μm;細孔容量=1.67ml/g;比表面積=325m2/g)2.8kgとトルエン24kgとを入れて、撹拌した。5℃に冷却した後、1,1,1,3,3,3−ヘキサメチルジシラザン0.91kgとトルエン1.43kgと混合溶液を反応器内の温度を5℃に保ちながら33分間で滴下した。滴下終了後、5℃で1時間、95℃で3時間攪拌し、ろ過した。得られた固体成分をトルエン21kgで6回、洗浄を行った。その後、トルエンを6.9kg加えてスラリーとし、一晩静置した。
Example 1
(1) Preparation of cocatalyst carrier Silica (Sypolol 948 manufactured by Devison, average particle size = 55 μm; pore volume = 1.67 ml) heat-treated at 300 ° C. under nitrogen flow in a reactor equipped with a nitrogen-substituted stirrer / G; specific surface area = 325 m 2 / g) 2.8 kg and 24 kg of toluene were added and stirred. After cooling to 5 ° C., 0.91 kg of 1,1,1,3,3,3-hexamethyldisilazane and 1.43 kg of toluene were added dropwise over 33 minutes while keeping the temperature inside the reactor at 5 ° C. did. After completion of the dropping, the mixture was stirred at 5 ° C. for 1 hour and then at 95 ° C. for 3 hours and filtered. The obtained solid component was washed 6 times with 21 kg of toluene. Thereafter, 6.9 kg of toluene was added to form a slurry, which was allowed to stand overnight.

上記で得られたスラリーに、ジエチル亜鉛のヘキサン溶液(ジエチル亜鉛濃度:50wt%)2.05kgとヘキサン1.3kgとを投入し、攪拌した。その後、5℃に冷却した後、ペンタフルオロフェノール0.77kgとトルエン1.17kgとの混合溶液を、反応器内の温度を5℃に保ちながら61分間で滴下した。滴下終了後、5℃で1時間、40℃で1時間攪拌した。その後、H2O0.11kgを反応器内の温度を5℃に保ちながら1.5時間で滴下した。滴下終了後、5℃で1.5時間、55℃で2時間攪拌した。その後、室温にてジエチル亜鉛のヘキサン溶液(ジエチル亜鉛濃度:50wt%)1.4kgとヘキサン0.8kgとを投入した。5℃に冷却した後、3,4,5−トリフルオロフェノール0.42kgとトルエン0.77kgとの混合溶液を、反応器内の温度を5℃に保ちながら60分間で滴下した。滴下終了後、5℃で1時間、40℃で1時間攪拌した。その後、H2O0.077kgを反応器内の温度を5℃に保ちながら1.5時間で滴下した。滴下終了後、5℃で1.5時間、40℃で2時間、更に、80℃で2時間攪拌した。攪拌を停止し残量16Lまで上澄み液を抜き出し、トルエン11.6kgを投入し、攪拌した。95℃に昇温し、4時間攪拌した。静置し、固体成分を沈降させ、沈降した固体成分の層と上層のスラリー部分との界面が見えた時点で上層のスラリー部分を取り除き、次いで残りの液成分をフィルターにてろ過した。得られた固体成分をトルエン20.8kgで4回、ヘキサン24リットルで3回、洗浄を行った。その後、乾燥することにより、固体成分(以下、助触媒担体(a−1)と称する。)を得た。 To the slurry obtained above, 2.05 kg of diethyl zinc in hexane (diethyl zinc concentration: 50 wt%) and 1.3 kg of hexane were added and stirred. Then, after cooling to 5 ° C., a mixed solution of 0.77 kg of pentafluorophenol and 1.17 kg of toluene was added dropwise over 61 minutes while maintaining the temperature in the reactor at 5 ° C. After completion of dropping, the mixture was stirred at 5 ° C. for 1 hour and at 40 ° C. for 1 hour. Thereafter, 0.11 kg of H 2 O was added dropwise over 1.5 hours while maintaining the temperature in the reactor at 5 ° C. After completion of dropping, the mixture was stirred at 5 ° C. for 1.5 hours and at 55 ° C. for 2 hours. Thereafter, 1.4 kg of diethylzinc in hexane (diethylzinc concentration: 50 wt%) and 0.8 kg of hexane were added at room temperature. After cooling to 5 ° C., a mixed solution of 3,4,5-trifluorophenol 0.42 kg and toluene 0.77 kg was added dropwise over 60 minutes while maintaining the temperature in the reactor at 5 ° C. After completion of dropping, the mixture was stirred at 5 ° C. for 1 hour and at 40 ° C. for 1 hour. Thereafter, 0.077 kg of H 2 O was added dropwise over 1.5 hours while maintaining the temperature in the reactor at 5 ° C. After completion of dropping, the mixture was stirred at 5 ° C for 1.5 hours, at 40 ° C for 2 hours, and further at 80 ° C for 2 hours. Stirring was stopped, the supernatant liquid was extracted to a remaining amount of 16 L, 11.6 kg of toluene was added, and the mixture was stirred. The temperature was raised to 95 ° C. and stirred for 4 hours. The solid component was allowed to settle, and when the interface between the precipitated solid component layer and the upper slurry portion was seen, the upper slurry portion was removed, and then the remaining liquid component was filtered through a filter. The obtained solid component was washed 4 times with 20.8 kg of toluene and 3 times with 24 liters of hexane. Thereafter, by drying, a solid component (hereinafter referred to as promoter support (a-1)) was obtained.

(2)予備重合
予め窒素置換した内容積210リットルの撹拌機付きオートクレーブに、助触媒担体(a−1)0.71kgと、ブタン80リットル、1−ブテン0.02kg、常温常圧の水素として3リットルを仕込んだ後、オートクレーブを30℃まで上昇した。さらにエチレンをオーツクレーブ内のガス相圧力で0.03MPa分仕込み、系内が安定した後、トリイソブチルアルミニウム208mmol、ラセミ−エチレンビス(1−インデニル)ジルコニウムジフェノキシド70mmolを投入して重合を開始した。50℃へ昇温するとともに、エチレンと水素を連続で供給しながら、50℃で合計4時間の予備重合を実施した。重合終了後、エチレン、ブタン、水素ガスなどをパージして残った固体を室温にて真空乾燥し、上記助触媒担体(a−1)1g当り11.9gのエチレン−1−ブテン共重合体が予備重合された予備重合触媒成分を得た。
(2) Prepolymerization In an autoclave with a stirrer having an internal volume of 210 liters that had been previously purged with nitrogen, 0.71 kg of the promoter support (a-1), 80 liters of butane, 0.02 kg of 1-butene, and hydrogen at normal temperature and pressure After charging 3 liters, the autoclave was raised to 30 ° C. Further, ethylene was charged in an amount of 0.03 MPa at the gas phase pressure in the oat clave, and after the system was stabilized, 208 mmol of triisobutylaluminum and 70 mmol of racemic-ethylenebis (1-indenyl) zirconium diphenoxide were added to initiate polymerization. . While raising the temperature to 50 ° C. and supplying ethylene and hydrogen continuously, prepolymerization was carried out at 50 ° C. for a total of 4 hours. After completion of the polymerization, purging ethylene, butane, hydrogen gas, etc., the remaining solid was vacuum-dried at room temperature, and 11.9 g of ethylene-1-butene copolymer per 1 g of the promoter support (a-1) was obtained. A prepolymerized prepolymerized catalyst component was obtained.

(3)連続気相重合
上記の予備重合触媒成分を用い、連続式流動床気相重合装置でエチレンと1−ヘキセンの共重合を実施した。重合条件は、温度84.9℃、全圧2MPa、ガス線速度0.25m/s、エチレンに対する水素モル比は0.220%、エチレンに対する1−ヘキセンモル比は1.14%とし、重合中はガス組成を一定に維持するためにエチレン、1−ヘキセン、水素を連続的に供給した。さらに、流動床の総パウダー重量を80kgに維持し、平均重合時間3.5hrとなるように、上記予備重合触媒成分と、トリイソブチルアルミニウムとを一定の割合で連続的に供給した。重合により、22.7kg/hrの重合効率でエチレン−1−ヘキセン共重合体(以下、PE−1と称する。)のパウダーを得た。
(3) Continuous gas phase polymerization Using the above prepolymerization catalyst component, ethylene and 1-hexene were copolymerized in a continuous fluidized bed gas phase polymerization apparatus. The polymerization conditions were a temperature of 84.9 ° C., a total pressure of 2 MPa, a gas linear velocity of 0.25 m / s, a hydrogen molar ratio to ethylene of 0.220%, and a 1-hexene molar ratio to ethylene of 1.14%. In order to keep the gas composition constant, ethylene, 1-hexene and hydrogen were continuously supplied. Further, the pre-polymerization catalyst component and triisobutylaluminum were continuously supplied at a constant ratio so that the total powder weight of the fluidized bed was maintained at 80 kg and the average polymerization time was 3.5 hr. By polymerization, a powder of an ethylene-1-hexene copolymer (hereinafter referred to as PE-1) was obtained with a polymerization efficiency of 22.7 kg / hr.

(4)エチレン−1−ヘキセン共重合体パウダーの造粒
上記で得たPE−1のパウダーを、神戸製鋼所社製LCM50押出機により、フィード速度50kg/hr、スクリュー回転数450rpm、ゲート開度4.2mm、サクション圧力0.2MPa、樹脂温度200〜230℃条件で造粒することにより、PE−1のペレットを得た。PE−1のペレットの評価結果を表1に示す。
(4) Granulation of ethylene-1-hexene copolymer powder The PE-1 powder obtained above was fed with an LCM50 extruder manufactured by Kobe Steel, Ltd., at a feed rate of 50 kg / hr, a screw rotation speed of 450 rpm, and a gate opening degree. PE-1 pellets were obtained by granulation under conditions of 4.2 mm, a suction pressure of 0.2 MPa, and a resin temperature of 200 to 230 ° C. The evaluation results of PE-1 pellets are shown in Table 1.

(5)中空成形
PE−1のペレットを用いて、50mmφの押出機の日本製鋼所製NB−3B中空成形機により、500ml用円筒瓶の中空成形を行った。ダイ内径17mmφ、コア15mmφの円形のダイとコアを用いて、押出機のクロスヘッド温度:210℃、ダイ温度:210℃、金型温度:30℃、吐出量:8kg/hrの成形条件で、パリソンコントロールを用いて目付量20gの中空成形容器を得た。また、二つに分かれた金型のそれぞれについて、円筒瓶の胴に当たる部分に100μm厚みで7×5cmのラベルを予め貼り、成形品に2箇所の凹状のくぼみができるようにして成形を行った。得られた中空成形容器の評価結果を表3に示す。
(5) Hollow molding Using a pellet of PE-1, hollow molding of a cylindrical bottle for 500 ml was performed by an NB-3B hollow molding machine manufactured by Nippon Steel Works of a 50 mmφ extruder. Using a circular die and a core with a die inner diameter of 17 mmφ and a core of 15 mmφ, the extruder crosshead temperature: 210 ° C., die temperature: 210 ° C., mold temperature: 30 ° C., discharge amount: 8 kg / hr, Using a parison control, a hollow molded container having a basis weight of 20 g was obtained. In addition, for each of the two divided molds, a 7 × 5 cm label having a thickness of 100 μm was previously attached to a portion corresponding to the barrel of the cylindrical bottle, and molding was performed so that two concave depressions were formed on the molded product. . Table 3 shows the evaluation results of the obtained hollow molded container.

比較例1
市販の直鎖状低密度ポリエチレン(住友化学社製 スミカセン−L HR150;以下、PE−2と称する。)を用いて、実施例1の(5)中空成形と同様にして中空成形を行い、中空成形容器を得た。PE−2のペレットの物性を表1に、得られた中空成形容器の評価結果を表3に示す。
Comparative Example 1
Using a commercially available linear low density polyethylene (Sumikasen-L HR150 manufactured by Sumitomo Chemical Co., Ltd .; hereinafter referred to as PE-2), hollow molding is performed in the same manner as (5) hollow molding in Example 1, and hollow A molded container was obtained. Table 1 shows the physical properties of the PE-2 pellets, and Table 3 shows the evaluation results of the obtained hollow molded containers.

比較例2
市販の直鎖状低密度ポリエチレン(住友化学社製 スミカセン−E FV102;以下、PE−3と称する。)を用いて、実施例1の(5)中空成形と同様にして中空成形を行い、中空成形容器を得た。PE−3のペレットの物性を表1に、得られた中空成形容器の評価結果を表3に示す。
Comparative Example 2
Using a commercially available linear low-density polyethylene (Sumikasen-E FV102 manufactured by Sumitomo Chemical Co., Ltd .; hereinafter referred to as PE-3), hollow molding is carried out in the same manner as (5) hollow molding in Example 1, and hollow A molded container was obtained. Table 1 shows the physical properties of the PE-3 pellets, and Table 3 shows the evaluation results of the obtained hollow molded containers.

比較例3
市販の高密度低密度ポリエチレン(三井化学社製 ハイゼックス 3000B;以下、PE−4と称する。)を用いて、実施例1の(5)中空成形と同様にして中空成形を行い、中空成形容器を得た。PE−4のペレットの物性を表1に、得られた中空成形容器の評価結果を表3に示す。
Comparative Example 3
Using a commercially available high-density and low-density polyethylene (Hi-Zex 3000B manufactured by Mitsui Chemicals; hereinafter referred to as PE-4), hollow molding is performed in the same manner as (5) hollow molding in Example 1 to obtain a hollow molded container. Obtained. Table 1 shows the physical properties of the PE-4 pellets, and Table 3 shows the evaluation results of the obtained hollow molded containers.

実施例2
(1)助触媒担体の調製
特開2003−171415号公報の実施例10(1)および(2)の成分(A)と同様な方法で、固体成分(以下、助触媒担体(a−2)と称する。)を得た。
Example 2
(1) Preparation of promoter support In the same manner as component (A) in Example 10 (1) and (2) of JP-A No. 2003-171415, a solid component (hereinafter referred to as promoter support (a-2)) is prepared. Obtained.).

(2)予備重合
予め窒素置換した内容積210リットルの撹拌機付きオートクレーブに、助触媒担体(a−2)0.70kgと、ブタン80リットル、1−ブテン0.13kg、常温常圧の水素として3リットルを仕込んだ後、オートクレーブを22℃まで上昇した。さらにエチレンをオーツクレーブ内のガス相圧力で0.07MPa分仕込み、系内が安定した後、トリイソブチルアルミニウム736mmol、ラセミ−エチレンビス(1−インデニル)ジルコニウムジフェノキシド105mmolを投入して重合を開始した。30℃へ昇温するとともに、エチレンと水素を連続で供給しながら、30℃で合計2時間の予備重合を実施した。重合終了後、エチレン、ブタン、水素ガスなどをパージして残った固体を室温にて真空乾燥し、上記助触媒担体(a−2)1g当り10.0gのエチレン−1−ブテン共重合体が予備重合された予備重合触媒成分を得た。
(2) Prepolymerization In an autoclave with a stirrer with an internal volume of 210 liters that had been previously purged with nitrogen, 0.70 kg of the promoter support (a-2), 80 liters of butane, 0.13 kg of 1-butene, and hydrogen at normal temperature and pressure After charging 3 liters, the autoclave was raised to 22 ° C. Further, ethylene was charged at a gas phase pressure of 0.07 MPa in the autoclave, and after the system was stabilized, 736 mmol of triisobutylaluminum and 105 mmol of racemic-ethylenebis (1-indenyl) zirconium diphenoxide were added to initiate polymerization. . While raising the temperature to 30 ° C. and continuously supplying ethylene and hydrogen, preliminary polymerization was carried out at 30 ° C. for a total of 2 hours. After completion of the polymerization, the remaining solids purged with ethylene, butane, hydrogen gas and the like are vacuum-dried at room temperature, and 10.0 g of ethylene-1-butene copolymer per 1 g of the promoter support (a-2) is obtained. A prepolymerized prepolymerized catalyst component was obtained.

(3)連続気相重合
上記の予備重合触媒成分を用い、連続式流動床気相重合装置でエチレンと1−ヘキセンの共重合を実施した。重合条件は、温度73.9℃、全圧2MPa、ガス線速度0.24m/s、エチレンに対する水素モル比は0.145%、エチレンに対する1−ヘキセンモル比は0.88%とし、重合中はガス組成を一定に維持するためにエチレン、1−ヘキセン、水素を連続的に供給した。さらに、流動床の総パウダー重量を80kgに維持し、平均重合時間3.3hrとなるように、上記予備重合触媒成分と、トリイソブチルアルミニウムとを一定の割合で連続的に供給した。重合により、24.0kg/hrの重合効率でエチレン−1−ヘキセン共重合体(以下、PE−5と称する。)のパウダーを得た。
(3) Continuous gas phase polymerization Using the above prepolymerization catalyst component, ethylene and 1-hexene were copolymerized in a continuous fluidized bed gas phase polymerization apparatus. The polymerization conditions were a temperature of 73.9 ° C., a total pressure of 2 MPa, a gas linear velocity of 0.24 m / s, a hydrogen molar ratio to ethylene of 0.145%, and a 1-hexene molar ratio to ethylene of 0.88%. In order to keep the gas composition constant, ethylene, 1-hexene and hydrogen were continuously supplied. Further, the pre-polymerization catalyst component and triisobutylaluminum were continuously supplied at a constant ratio so that the total powder weight of the fluidized bed was maintained at 80 kg and the average polymerization time was 3.3 hr. By polymerization, a powder of an ethylene-1-hexene copolymer (hereinafter referred to as PE-5) was obtained with a polymerization efficiency of 24.0 kg / hr.

(4)エチレン−1−ヘキセン共重合体パウダーの造粒
上記で得たPE−5のパウダーを、実施例1の(4)エチレン−1−ヘキセン共重合体パウダーの造粒と同様にして造粒することにより、PE−5のペレットを得た。PE−5のペレットの物性を表2に示す。
(4) Granulation of ethylene-1-hexene copolymer powder The PE-5 powder obtained above was granulated in the same manner as the granulation of (4) ethylene-1-hexene copolymer powder in Example 1. By pelletizing, pellets of PE-5 were obtained. Table 2 shows the physical properties of the PE-5 pellets.

(5)中空成形
上記で得たPE−5のペレットを用いて、実施例1の(5)中空成形と同様にして中空成形を行い、中空成形容器を得た。得られた中空成形容器の評価結果を表4に示す。
(5) Hollow molding Using the PE-5 pellets obtained above, hollow molding was performed in the same manner as (5) hollow molding in Example 1 to obtain a hollow molded container. Table 4 shows the evaluation results of the obtained hollow molded container.

実施例3
成分(A)として上記のPE−5のパウダーと、成分(B)として市販の直鎖状低密度ポリエチレン(住友化学社製 スミカセン−E FV203(メタロセン触媒を用いて製造;エチレン−1−ヘキセン共重合体);以下、PE−6と称する。)とを、PE−5の重量とPE−6の重量の比が85/15になるようにブレンドし、実施例1の(4)エチレン−1−ヘキセン共重合体パウダーの造粒と同様に造粒してペレットを得た。次に、該ペレットを用いて実施例1の(5)中空成形と同様にして中空成形を行い、中空成形容器を得た。PE−6の物性を表2に、得られた中空成形容器の評価結果を表4に示す。
Example 3
PE-5 powder as component (A) and commercially available linear low density polyethylene as component (B) (Sumikasen-E FV203 (manufactured using metallocene catalyst; manufactured by Sumitomo Chemical Co .; ethylene-1-hexene) Polymer); hereinafter referred to as PE-6) was blended so that the ratio of the weight of PE-5 to the weight of PE-6 was 85/15, and (4) ethylene-1 of Example 1 was blended. -Pellet was obtained by granulation in the same manner as granulation of hexene copolymer powder. Next, hollow molding was performed using the pellets in the same manner as (5) hollow molding in Example 1 to obtain a hollow molded container. Table 2 shows the physical properties of PE-6, and Table 4 shows the evaluation results of the obtained hollow molded container.

Figure 0004650060
Figure 0004650060

Figure 0004650060
Figure 0004650060

Figure 0004650060
Figure 0004650060

Figure 0004650060
Figure 0004650060

Claims (1)

下記成分(A)と成分(B)とを含有し、成分(A)と成分(B)との合計を100重量%として、成分(A)の含有量が95〜50重量%であり、成分(B)の含有量が5〜50重量%であるエチレン系樹脂組成物を中空成形してなる中空成形容器。
成分(A):流動の活性化エネルギー(Ea)が40kJ/mol以上であり、JIS K7210に規定された温度190℃、荷重21.18Nの条件で測定されるメルトフローレート(MFR)が0.1〜100g/10分であり、分子量分布(Mw/Mn)が6〜25であるエチレン−α−オレフィン共重合体
成分(B):高圧法低密度ポリエチレンおよび流動の活性化エネルギー(Ea)が40kJ/mol未満であるエチレン−α−オレフィン共重合体からなるエチレン系重合体群から選ばれた少なくとも1種のエチレン系重合体
The following component (A) and component (B) are contained, the sum of component (A) and component (B) is 100% by weight, the content of component (A) is 95 to 50% by weight, A hollow molded container formed by hollow molding an ethylene-based resin composition having a content of (B) of 5 to 50% by weight .
Component (A): The flow activation energy (Ea) is 40 kJ / mol or more, the melt flow rate (MFR) measured under the conditions of a temperature of 190 ° C. and a load of 21.18 N specified in JIS K7210 is 0.1. An ethylene-α-olefin copolymer having a molecular weight distribution (Mw / Mn) of 6 to 25 and 1 to 100 g / 10 minutes
Component (B): at least one ethylene selected from the group of ethylene polymers consisting of a high-pressure low-density polyethylene and an ethylene-α-olefin copolymer having a flow activation energy (Ea) of less than 40 kJ / mol Polymer
JP2005098193A 2005-03-30 2005-03-30 Hollow molded container Active JP4650060B2 (en)