[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP4413237B2 - Manufacturing method of solar cell - Google Patents

Manufacturing method of solar cell Download PDF

Info

Publication number
JP4413237B2
JP4413237B2 JP2007044511A JP2007044511A JP4413237B2 JP 4413237 B2 JP4413237 B2 JP 4413237B2 JP 2007044511 A JP2007044511 A JP 2007044511A JP 2007044511 A JP2007044511 A JP 2007044511A JP 4413237 B2 JP4413237 B2 JP 4413237B2
Authority
JP
Japan
Prior art keywords
solar cell
silicon substrate
etching
manufacturing
unevenness
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP2007044511A
Other languages
Japanese (ja)
Other versions
JP2007221148A (en
Inventor
洋介 猪股
健次 福井
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kyocera Corp
Original Assignee
Kyocera Corp
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kyocera Corp filed Critical Kyocera Corp
Priority to JP2007044511A priority Critical patent/JP4413237B2/en
Publication of JP2007221148A publication Critical patent/JP2007221148A/en
Application granted granted Critical
Publication of JP4413237B2 publication Critical patent/JP4413237B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

本発明は太陽電池の製造方法に関する。   The present invention relates to a method for manufacturing a solar cell.

太陽電池は表面に入射した太陽光などの光エネルギーを電気エネルギーに変換するものである。この電気エネルギーへの変換効率を向上させるため、従来から様々な試みがなされてきた。そのひとつに基板の表面に入射した光の反射を少なくする技術があり、入射した光の反射を低減することで電気エネルギーヘの変換効率を高めることができる。   The solar cell converts light energy such as sunlight incident on the surface into electric energy. Various attempts have been made to improve the conversion efficiency into electric energy. One of them is a technique for reducing the reflection of light incident on the surface of the substrate. By reducing the reflection of incident light, the conversion efficiency to electric energy can be increased.

太陽電池のうち主要なものは使用材料の種類により結晶系、アモルファス系、化合物系などに分類される。このうち、現在市場で流通しているのはほとんどが結晶系シリコン太陽電池である。この結晶系シリコン太陽電池はさらに単結晶型、多結晶型に分類される。単結晶型シリコン太陽電池は基板の品質がよいため、高効率化が容易であるという長所を有する反面、基板の製造コストが大きいという短所を有する。それに対し、多結晶型シリコン太陽電池は基板品質が劣るために高効率化が難しいという弱点はあるものの、低コストで製造できるというメリットがある。また、最近では多結晶シリコン基板の品質の向上やセル化技術の進歩により、研究レベルでは18%程度の変換効率が達成されている。   Major solar cells are classified into crystalline, amorphous, and compound types depending on the type of materials used. Of these, most of the crystalline silicon solar cells currently on the market are in the market. This crystalline silicon solar cell is further classified into a single crystal type and a polycrystalline type. Single crystal silicon solar cells have the advantage that the substrate quality is good, and thus the efficiency is easy, while the substrate manufacturing cost is high. On the other hand, a polycrystalline silicon solar cell has the merit that it can be manufactured at a low cost although it has a weak point that it is difficult to achieve high efficiency due to poor substrate quality. In recent years, conversion efficiency of about 18% has been achieved at the research level due to the improvement of the quality of the polycrystalline silicon substrate and the advancement of cell technology.

一方、量産レベルの多結晶シリコン太陽電池は低コストであったため、従来から市場に流通してきたが、近年環境問題が取りざたされる中でさらに需要が増してきており、低コストで且つより高い変換効率が求められるようになった。   On the other hand, mass-produced polycrystalline silicon solar cells have been distributed in the market because of their low cost. However, in recent years, demand has increased further as environmental issues have been addressed, and low cost and higher conversion are required. Efficiency has been demanded.

シリコン基板を用いて太陽電池素子を形成する場合に、基板表面を水酸化ナトリウムなどのアルカリ水溶液でエッチングすると、表面に微細な凹凸が形成され、基板表面の反射をある程度低減させることができる。   When a solar cell element is formed using a silicon substrate, if the substrate surface is etched with an alkaline aqueous solution such as sodium hydroxide, fine irregularities are formed on the surface, and reflection on the substrate surface can be reduced to some extent.

面方位が(100)面の単結晶シリコン基板を用いた場合は、このような方法でテクスチャー構造と呼ばれるピラミッド構造を基板表面に均一に形成することができるものの、アルカリ水溶液によるエッチングは結晶の面方位に依存することから、多結晶シリコン基板で太陽電池素子を形成する場合、ピラミッド構造を均一には形成できず、そのため全体の反射率も効果的には低減できないという問題がある。   When a single crystal silicon substrate having a (100) plane orientation is used, a pyramid structure called a texture structure can be uniformly formed on the substrate surface by such a method. Since it depends on the orientation, when a solar cell element is formed from a polycrystalline silicon substrate, there is a problem that the pyramid structure cannot be formed uniformly, and therefore the overall reflectance cannot be reduced effectively.

このような問題を解決するために、太陽電池素子を多結晶シリコン基板で形成する場合に、基板表面に微細な突起を反応性イオンエッチング(Reactive Ion Etching)法で形成することが提案されている(たとえば特公昭60−27195号、特開平5−75152号、特開平9−102625号公報参照)。すなわち、微細な突起を多結晶シリコンにおける不規則な結晶の面方位に左右されずに均一に形成し、特に多結晶シリコンを用いた太陽電池素子においても、反射率をより効果的に低減しようとするものである。   In order to solve such problems, it has been proposed that when a solar cell element is formed of a polycrystalline silicon substrate, fine protrusions are formed on the substrate surface by a reactive ion etching method. (For example, see Japanese Patent Publication No. 60-27195, Japanese Patent Laid-Open No. 5-75152, Japanese Patent Laid-Open No. 9-102625). That is, fine protrusions are uniformly formed regardless of the plane orientation of the irregular crystal in the polycrystalline silicon, and the reflectance is more effectively reduced particularly in the solar cell element using the polycrystalline silicon. To do.

しかしながら、凹凸形成条件は非常に微妙であり、また、装置の構造によっても変化するため、条件の検討は非常に難しいことが多い。微細な突起を均一に形成できない場合は、太陽電池の光電変換効率が低下し、個々の太陽電池の価値はその発電効率で決まることから、そのコストを低減するためには、太陽電池の変換効率を向上させなければならない。   However, since the unevenness forming conditions are very delicate and change depending on the structure of the apparatus, it is often very difficult to examine the conditions. If the fine protrusions cannot be formed uniformly, the photoelectric conversion efficiency of the solar cell will decrease, and the value of each solar cell will be determined by its power generation efficiency, so in order to reduce its cost, the conversion efficiency of the solar cell Must be improved.

また、反応性イオンエッチング法で用いられる反応性イオンエッチング装置は一般に平行平板電極型をしており、基板を設置している電極の側にRF電圧を印加し、他の一方の側及び内部の側壁をアースに接続してある。この容器内部を真空ポンプで真空引きし、真空引き完了後、エッチングガスを導入し、圧力を一定に保持しながら内部の被エッチング基板をエッチングする。このような手順を踏むことから、反応性イオンエッチング装置では真空引き及び大気リークの待ち時間が多い。また、反応性イオンエッチング装置はLSIなどの精密な小型半導体素子に用いられる場合が多いが、太陽電池に用いる際には太陽電池自身の面積が大きいため、1回あたりの処理枚数が少なく、コストが高くなるという問題があった。そのため反応性イオンエッチング装置を太陽電池製造工程に用いる場合には、いかに高タクトで処理を行うかも重要なポイントである。   Moreover, the reactive ion etching apparatus used in the reactive ion etching method is generally a parallel plate electrode type, and an RF voltage is applied to the electrode side on which the substrate is installed, The side wall is connected to ground. The inside of the container is evacuated by a vacuum pump, and after the evacuation is completed, an etching gas is introduced, and the substrate to be etched is etched while keeping the pressure constant. Since such a procedure is followed, the reactive ion etching apparatus has a long waiting time for evacuation and air leakage. Reactive ion etching apparatuses are often used for precision small semiconductor elements such as LSIs, but when used for solar cells, the area of the solar cell itself is large, so the number of treatments per process is small and the cost is low. There was a problem that became high. Therefore, when a reactive ion etching apparatus is used in a solar cell manufacturing process, it is an important point how high-tact processing is performed.

本発明はこのような従来技術の問題点に鑑みてなされたものであり、半導体基板、特に太陽電池に用いられるシリコン基板表面の凹凸を効率よく均一に形成する方法を提供することを目的とする。   The present invention has been made in view of such problems of the prior art, and an object thereof is to provide a method for efficiently and uniformly forming irregularities on the surface of a semiconductor substrate, particularly a silicon substrate used in a solar cell. .

本発明の太陽電池の製造方法は、HOを含むエッチングガスを用いた反応性イオンエッチング法によって、多結晶シリコン基板の表面にマイクロマスクとなるエッチング生成物を付着させながら該表面に凹凸を形成する凹凸形成工程を備えてなるものである。 Producing a solar cell of the present invention, unevenness of H 2 O by a reactive ion etching method using the free non-image Tchingugasu, to the surface while the surface of the polycrystalline silicon substrate by adhering etching products of the micro-mask It is provided with the uneven | corrugated formation process which forms .

上記太陽電池の製造方法において、前記エッチングガスはSFを含み、該SFの量よりも前記HOの量が少ないことが好ましい。 In the method for manufacturing the solar cell, wherein the etching gas comprises SF 6, it is preferred that the amount of the H 2 O than the amount of the SF 6 is small.

上記太陽電池の製造方法において、前記凹凸形成工程によって、前記多結晶シリコン基板の表面に、幅と高さがそれぞれ1μm以下の凹凸を形成することが好ましい。   In the method for manufacturing a solar cell, it is preferable that the unevenness having a width and a height of 1 μm or less is formed on the surface of the polycrystalline silicon substrate by the unevenness forming step.

上記太陽電池の製造方法において、前記凹凸形成工程によって、前記多結晶シリコン基板の表面に、アスペクト比が2以下の凹凸を形成することが好ましい。   In the method for manufacturing a solar cell, it is preferable that unevenness having an aspect ratio of 2 or less is formed on the surface of the polycrystalline silicon substrate by the unevenness forming step.

つまり、シリコン基板の表面を反応性イオンエッチング法および類似のドライエッチング法で粗面化する際に、エッチングされたシリコンを主成分とするエッチング残渣をシリコン表面に再付着させて、これをエッチングのマイクロマスクとして利用することでシリコン基板表面に凹凸構造を形成するものである。   That is, when the surface of the silicon substrate is roughened by a reactive ion etching method or a similar dry etching method, an etching residue mainly composed of etched silicon is reattached to the silicon surface, and this is etched. By using it as a micromask, a concavo-convex structure is formed on the surface of the silicon substrate.

本発明の太陽電池の製造方法では、HOを含む第一のエッチングガスを用いた反応性イオンエッチング法によって、多結晶シリコン基板の表面に凹凸を形成する工程を備えてなることから、高効率の太陽電池などに必要なシリコン基板表面の凹凸構造(粗面)を高タクト・低コストで形成することが可能となる。 In the method for manufacturing a solar cell according to the present invention, the method includes a step of forming irregularities on the surface of a polycrystalline silicon substrate by a reactive ion etching method using a first etching gas containing H 2 O. It is possible to form a concavo-convex structure (rough surface) on the surface of a silicon substrate necessary for an efficient solar cell or the like with high tact and low cost.

以下、本発明の実施形態を添付図面に基づき詳細に説明する。図1は本発明に係る一実施形態を示す太陽電池セルの構造である。図1において1はシリコン基板、1aは表面凹凸構造、1bは受光面側不純物拡散層、1cは裏面側不純物拡散層(BSF)、1dは表面反射防止膜、1eは表面電極、1fは裏面電極を示している。   Embodiments of the present invention will be described below in detail with reference to the accompanying drawings. FIG. 1 shows the structure of a solar battery cell according to an embodiment of the present invention. In FIG. 1, 1 is a silicon substrate, 1a is a surface uneven structure, 1b is a light-receiving surface side impurity diffusion layer, 1c is a back surface side impurity diffusion layer (BSF), 1d is a surface antireflection film, 1e is a surface electrode, 1f is a back electrode Is shown.

前記シリコン基板1は単結晶もしくは多結晶のシリコン基板である。この基板はp型、n型いずれでもよい。単結晶シリコンの場合は引き上げ法などによって形成され、多結晶シリコンの場合は鋳造法などによって形成される。多結晶シリコンは、大量生産が可能で製造コスト面で単結晶シリコンよりもきわめて有利である。引き上げ法や鋳造法によって形成されたインゴットを300μm程度の厚みにスライスして、10cm×10cmもしくは15cm×15cm程度の大きさに切断してシリコン基板となる。   The silicon substrate 1 is a monocrystalline or polycrystalline silicon substrate. This substrate may be either p-type or n-type. In the case of monocrystalline silicon, it is formed by a pulling method or the like, and in the case of polycrystalline silicon, it is formed by a casting method or the like. Polycrystalline silicon can be mass-produced and is extremely advantageous over single-crystal silicon in terms of manufacturing cost. An ingot formed by a pulling method or a casting method is sliced to a thickness of about 300 μm and cut into a size of about 10 cm × 10 cm or 15 cm × 15 cm to form a silicon substrate.

シリコン基板1の表面側には、入射した光を反射させずに有効に取り込むために微細な凹凸1aを形成する。これは、真空引きされたチャンバー内にガスを導入し、一定圧力に保持して、チャンバー内に設けられた電極にRF電力を印加することでプラズマを発生させ、生じた活性種であるイオン・ラジカル等の作用により基板表面をエッチングするものである。反応性イオンエッチング(RIE)法と呼ばれるこの方法は図2及び図3のように示される。   On the surface side of the silicon substrate 1, fine irregularities 1a are formed in order to effectively capture incident light without reflecting it. This is because a gas is introduced into a vacuumed chamber, held at a constant pressure, and plasma is generated by applying RF power to an electrode provided in the chamber. The substrate surface is etched by the action of radicals or the like. This method, called the reactive ion etching (RIE) method, is shown in FIGS.

図2および図3において、2aはマスフローコントローラー、2bはシリコン基板、2cはRF電極、2dは圧力調整器、2eは真空ポンプ、2fはRF電源である。装置内にマスフローコントローラー2a部分からエッチングガスとエッチング残渣生成用ガスを導入するとともに、RF電極2cでプラズマを発生させてイオンやラジカルを励起活性化して、RF電極2cの上部に設置されたシリコン基板2bの表面に作用させてエッチングする。図2に示す装置では、RF電極2cを装置内に設置して1枚のシリコン基板2bの表面をエッチングするが、図3に示す装置では、RF電極2cを装置の外壁に設置して複数枚のシリコン基板2bの表面を同時にエッチングするようにしている。   2 and 3, 2a is a mass flow controller, 2b is a silicon substrate, 2c is an RF electrode, 2d is a pressure regulator, 2e is a vacuum pump, and 2f is an RF power source. An etching gas and an etching residue generation gas are introduced into the apparatus from the mass flow controller 2a portion, and plasma is generated by the RF electrode 2c to activate ions and radicals, and a silicon substrate placed above the RF electrode 2c. Etching by acting on the surface of 2b. In the apparatus shown in FIG. 2, the RF electrode 2c is installed in the apparatus to etch the surface of one silicon substrate 2b. In the apparatus shown in FIG. 3, a plurality of RF electrodes 2c are installed on the outer wall of the apparatus. The surface of the silicon substrate 2b is simultaneously etched.

発生した活性種のうち、イオンがエッチングに作用する効果を大きくした方法を一般に反応性イオンエッチング法と呼んでいる。類似する方法にプラズマエッチングなどがあるが、プラズマ発生の原理は基本的に同じであり、基板に作用する活性種の種類の分布をチャンバー構造あるいは電極構造により異なる分布に変化させているだけである。そのため、本発明は反応性イオンエッチング法だけに限らず、広くプラズマエッチング法全般に対して有効である。   Of the generated active species, a method that increases the effect of ions on etching is generally called a reactive ion etching method. Plasma etching is a similar method, but the principle of plasma generation is basically the same, and the distribution of the active species acting on the substrate is simply changed to a different distribution depending on the chamber structure or electrode structure. . Therefore, the present invention is effective not only for the reactive ion etching method but also for the plasma etching method in general.

本発明では、例えば三フッ化メタン(CHF3)を20sccm、塩素(Cl2)を50sccm、酸素(O2)を10sccm、SF6を80sccm、さらにこれらに加えてH2Oを1sccm流しながら、反応圧力7Pa、プラズマを発生させるRFパワー500Wで3分間程度エッチングする。これによりシリコン基板表面には凹凸構造が形成される。エッチング中はシリコンがエッチングされて基本的には気化するが、一部は気化しきれずに分子同士が吸着して基板表面に残渣として残る。 In the present invention, for example, methane trifluoride (CHF 3) 20 sccm, chlorine (Cl 2) of 50 sccm, oxygen (O 2) of 10 sccm, 80 sccm of SF 6, while passing further 1sccm of H 2 O in addition to these, Etching is performed at a reaction pressure of 7 Pa and RF power of 500 W for generating plasma for about 3 minutes. Thereby, an uneven structure is formed on the surface of the silicon substrate. During the etching, silicon is etched and basically vaporized, but a part of the silicon is not vaporized and molecules are adsorbed and remain on the substrate surface as a residue.

また、ガス条件、反応圧力、RFパワーなどを凹凸形成ガス条件のエッチング後に主成分がシリコンである残渣がシリコン基板表面に残るような条件に設定すると、確実に凹凸形成を行うことができる。ただし、その凹凸のアスペクト比に関しては、条件により最適化が必要である。逆に、凹凸形成用のエッチング後の表面に残渣が残らないような条件ではいかなる条件でも凹凸形成を行うことは不可能である。   In addition, if the gas conditions, reaction pressure, RF power, etc. are set such that a residue whose main component is silicon remains on the silicon substrate surface after etching under the concavo-convex forming gas conditions, the concavo-convex formation can be performed reliably. However, the aspect ratio of the irregularities needs to be optimized depending on conditions. On the other hand, it is impossible to form unevenness under any conditions so long as no residue remains on the surface after etching for forming unevenness.

図4に、H2Oを添加してエッチングした場合におけるエッチング時間とシリコン基板表面の反射率との関係を示す。図4は、三フッ化メタン(CHF3)を20sccm、塩素(Cl2)を50sccm、酸素(O2)を10sccm、SF6を80sccm、さらにこれらに加えてH2Oを1sccm流しながら、反応圧力7Pa、プラズマを発生させるRFパワー500Wでエッチングを行ったものである。これによりH2Oを添加しない従来条件(図4中の■印)では5分間必要なエッチング時間がH2Oを添加すると3分で行えるようになることがわかる(図4中の●印および▲印)。つまり、H2Oガスの添加によって、凹凸の形成・シリコン表面の粗面化は促進することができる。また、水分の量は、エッチングガスであるSF6と等量(sccm)を流すと凹凸の形成が遅くなることが示された。 FIG. 4 shows the relationship between the etching time and the reflectance of the silicon substrate surface when etching is performed with H 2 O added. 4, 20 sccm methane trifluoride (CHF 3), 50 sccm chlorine (Cl 2), oxygen (O 2) of 10 sccm, a SF 6 80 sccm, while passing further 1sccm of H 2 O In addition to these, the reaction Etching was performed at a pressure of 7 Pa and an RF power of 500 W for generating plasma. Thus, it can be seen that under the conventional conditions in which H 2 O is not added (■ mark in FIG. 4), an etching time required for 5 minutes can be achieved in 3 minutes if H 2 O is added (marked with ● in FIG. 4 and ▲). That is, the addition of H 2 O gas can promote the formation of irregularities and the roughening of the silicon surface. In addition, it was shown that the formation of the unevenness becomes slow when the amount of moisture is equal to the etching gas SF 6 (sccm).

このようにエッチングマスクを用いない場合のドライエッチングによる凹凸の形成過程は、主に、シリコンがエッチングされた際にエッチング生成物が基板上に再付着し、これがマイクロマスクとなって次のステップで下地のシリコンがエッチングされ、凹凸が形成されることになる。そのため、H2Oを導入すると凹凸形成が促進されるのは、主にH2Oがシリコン表面やエッチング生成物表面に吸着しやすく、この再付着が促進されるためである。この水分の最適値や上限・下限については、エッチング用の混合ガスの種類や比率、反応時の圧力、RFパワー、エッチングチャンバー形状などに左右される。 In this way, the unevenness formation process by dry etching without using an etching mask is mainly performed when the etching product is reattached on the substrate when silicon is etched, and this becomes a micromask in the next step. The underlying silicon is etched to form irregularities. Therefore, when H 2 O is introduced, the formation of irregularities is promoted mainly because H 2 O is easily adsorbed on the silicon surface or the etching product surface, and this reattachment is promoted. The optimum value and upper and lower limits of the moisture depend on the type and ratio of the mixed gas for etching, the pressure during the reaction, the RF power, the shape of the etching chamber, and the like.

また、エッチングガス条件にH2Oガスを添加する場合に限らず、元のガスに不純物を含んだものを用いる方法も有効である。一般に販売されている半導体エッチング用ガスは、99.999%程度の純度を有するのが普通である。しかし、例えばO2ガスに純度の低い液体酸素を用いると、H2Oガスを添加することと同様の効果を得ることができる。これは純度の低いO2ガスには水分が含まれているためである。市場にある液体酸素は通常99.5%程度であり、水分は数十〜数百ppmである。これを用いることで、低純度のためランニングコストを低く押さえることができ、また別途H2Oの供給を必要としないため、装置のコストを低減することができる。また、O2ガスに低純度のものを用いる代わりに他のガスに純度の低いものを用いることもできる。これは通常どのようなガスであっても不純物としては水分が非常に多く含まれているためである。 In addition to the case where H 2 O gas is added to the etching gas conditions, a method using an original gas containing impurities is also effective. Generally, the gas for semiconductor etching that is generally sold has a purity of about 99.999%. However, for example, when liquid oxygen having a low purity is used for the O 2 gas, the same effect as that obtained by adding the H 2 O gas can be obtained. This is because the low purity O 2 gas contains moisture. The liquid oxygen on the market is usually about 99.5%, and the water content is several tens to several hundred ppm. By using this, the running cost can be kept low because of its low purity, and the supply of H 2 O is not required separately, so that the cost of the apparatus can be reduced. Further, instead of using a low-purity O 2 gas, another gas having a low purity can be used. This is because, in any gas, water is very much contained as impurities.

この微細な凹凸1aは円錐形もしくはそれが連なったような形状を呈し、RIE法によりガス濃度もしくはエッチング時間を制御することにより、その大きさを変化させることができる。この微細な凹凸1aの幅と高さはそれぞれ2μm以下に形成される。この微細な凹凸1aをシリコン基板1の必要部分全面にわたって均一且つ正確に制御性を持たせて形成するためには、1μm以下が好適である。この微細な凹凸1aのアスペクト比(凹凸1aの幅/高さ)は、2以下であることが望ましい。このアスペクト比が2以上の場合、製造過程で微細な凹凸1aが破損し、太陽電池セルを形成した場合にリーク電流が大きくなって良好な出力特性が得られない。   The fine irregularities 1a have a conical shape or a continuous shape, and the size can be changed by controlling the gas concentration or etching time by the RIE method. The width and height of the fine irregularities 1a are each set to 2 μm or less. In order to form the fine irregularities 1a uniformly and accurately over the entire necessary portion of the silicon substrate 1, a thickness of 1 μm or less is preferable. The aspect ratio of the fine irregularities 1a (the width / height of the irregularities 1a) is desirably 2 or less. When this aspect ratio is 2 or more, fine irregularities 1a are damaged in the manufacturing process, and when a solar battery cell is formed, a leak current increases and good output characteristics cannot be obtained.

反応性イオンエッチング装置あるいは類似のプラズマエッチング装置で凹凸形成を行った後、シリコン基板表面に残ったエッチング残渣を除去する。これにより作製する太陽電池の特性を向上させることができる。この残渣を除去する方法の一つは、エッチングが可能なガスを導入してドライエッチングを行うことで除去する。エッチングが可能なガスとしては、たとえばSF6などがあるが、残渣が除去できる能力があれば、ガス種は選ばない。このように連続して残渣を除去することにより、別途残渣を除去する工程を設ける必要がなくなり、低コスト化が図れる。なお、このエッチング残渣を除去するためのエッチングは、凹凸を形成したのと同じチャンバー内で行ってもよいし、別に設けられたチャンバーで行ってもよい。ただしこの方法ではシリコン基板の表面もエッチングされるために凹凸の形状が崩れやすくなる傾向があり、エッチング条件の管理が必要である。 After forming irregularities with a reactive ion etching apparatus or a similar plasma etching apparatus, etching residues remaining on the surface of the silicon substrate are removed. Thereby, the characteristic of the solar cell produced can be improved. One method for removing the residue is to perform dry etching by introducing a gas that can be etched. Examples of gases that can be etched include SF 6 , but any gas type can be used as long as it has the ability to remove residues. By continuously removing the residue in this way, it is not necessary to provide a separate step for removing the residue, and the cost can be reduced. Note that the etching for removing the etching residue may be performed in the same chamber in which the unevenness is formed, or may be performed in a separate chamber. However, in this method, since the surface of the silicon substrate is also etched, the shape of the unevenness tends to collapse, and management of etching conditions is necessary.

エッチング残渣を除去する他の方法としては、反応性イオンエッチング装置あるいは類似のプラズマエッチング装置によって凹凸を形成して基板を取り出した後に水槽内で超音波をかける方法もある。この超音波を印加する装置の種類としては、通常市販されている主な洗浄用超音波装置の周波数は数十kHzから数百kHzで、印加する振動子も材質、形状、出力など様々なタイプがあるが、この装置のタイプは表面の残渣除去の容易さによって選択することができる。残渣除去の容易さは凹凸の形状・大きさ・残渣の残量・基板の厚みなどによっても変化し、さらに超音波の周波数によっても変化するが、比較的残渣除去が困難な条件であっても印加時間を長くすることで残渣除去することが可能であり、本発明としてはいずれでも使用可能である。   As another method for removing the etching residue, there is also a method in which an ultrasonic wave is applied in a water tank after the substrate is taken out by forming irregularities with a reactive ion etching apparatus or a similar plasma etching apparatus. As the types of devices that apply ultrasonic waves, the frequency of main commercially available ultrasonic cleaning devices is several tens of kHz to several hundreds of kHz, and the vibrator to be applied is of various types such as material, shape, and output. However, this type of device can be selected depending on the ease of removal of residue on the surface. The ease of residue removal varies depending on the shape and size of the unevenness, the remaining amount of residue, the thickness of the substrate, etc., and also varies depending on the frequency of the ultrasonic wave, but even under conditions where residue removal is relatively difficult It is possible to remove the residue by extending the application time, and any of them can be used as the present invention.

半導体基板1の表面側には、逆導電型半導体不純物が拡散された層1bが形成されている。この逆導電型半導体不純物が拡散された層1bは、シリコン基板1内に半導体接合部を形成するために設けるものであり、例えばn型の不純物を拡散させる場合、POCl3を用いた気相拡散法、P25を用いた塗布拡散法、及びP+イオンを直接拡散させるイオン打ち込み法などによって形成される。この逆導電型半導体不純物を含有する層1は0.3〜0.5μm程度の深さに形成される。 On the surface side of the semiconductor substrate 1, a layer 1b in which a reverse conductivity type semiconductor impurity is diffused is formed. The layer 1b in which the reverse conductivity type semiconductor impurity is diffused is provided to form a semiconductor junction in the silicon substrate 1. For example, when n-type impurity is diffused, vapor phase diffusion using POCl 3 is performed. And a coating diffusion method using P 2 O 5 and an ion implantation method for directly diffusing P + ions. The layer 1 containing the reverse conductivity type semiconductor impurity is formed to a depth of about 0.3 to 0.5 μm.

このシリコン基板1の表面側には、反射防止膜1dが形成されている。この反射防止膜1dは、シリコン基板1の表面で光が反射するのを防止して、シリコン基板1内に光を有効に取り込むために設ける。この反射防止膜は、シリコン基板1との屈折率差等を考慮して、屈折率が2程度の材料で構成され、厚み500〜2000Å程度の窒化シリコン膜や酸化シリコン(SiO2)膜などで構成される。 An antireflection film 1 d is formed on the surface side of the silicon substrate 1. The antireflection film 1 d is provided to prevent light from being reflected from the surface of the silicon substrate 1 and to effectively take light into the silicon substrate 1. This antireflection film is made of a material having a refractive index of about 2 in consideration of the difference in refractive index from the silicon substrate 1, and is made of a silicon nitride film or a silicon oxide (SiO 2 ) film having a thickness of about 500 to 2000 mm. Composed.

シリコン基板1の裏面側には、一導電型半導体不純物が高濃度に拡散された層1cを形成することが望ましい。この一導電型半導体不純物が高濃度に拡散された層1cは、シリコン基板1の裏面近くでキャリアの再結合による効率の低下を防ぐために、シリコン基板1の裏面側に内部電界を形成するものである。   On the back side of the silicon substrate 1, it is desirable to form a layer 1c in which one conductivity type semiconductor impurity is diffused at a high concentration. The layer 1c in which this one-conductivity-type semiconductor impurity is diffused at a high concentration forms an internal electric field on the back surface side of the silicon substrate 1 in order to prevent a decrease in efficiency due to carrier recombination near the back surface of the silicon substrate 1. is there.

つまり、シリコン基板1の裏面近くで発生したキャリアがこの電界によって加速される結果、電力が有効に取り出されることとなり、特に長波長の光感度が増大すると共に、高温における太陽電池特性の低下を軽減できる。このように一導電型半導体不純物が高濃度に拡散された層1cが形成されたシリコン基板1の裏面側のシート抵抗は、15Ω/□程度になる。   In other words, as a result of the carriers generated near the back surface of the silicon substrate 1 being accelerated by this electric field, the electric power is effectively extracted, and particularly the long wavelength photosensitivity increases and the deterioration of the solar cell characteristics at high temperatures is reduced. it can. Thus, the sheet resistance on the back surface side of the silicon substrate 1 on which the layer 1c in which one conductivity type semiconductor impurity is diffused at a high concentration is formed is about 15Ω / □.

シリコン基板1の表面側および裏面側には、表面電極1eおよび裏面電極1fが形成されている。この表面電極1e及び裏面電極1fは主にAg紛、バインダー、フリットなどからなるAgペーストをスクリーン印刷して焼成し、その上に半田層を形成する。表面電極1eは、例えば幅200μm程度に、またピッチ3mm程度に形成される多数のフィンガー電極(不図示)と、この多数のフィンガー電極を相互に接続する2本のバスバー電極(1e)で構成される。裏面電極1fは、例えば幅300μm程度に、またピッチ5mm程度に形成される多数のフィンガー電極(不図示)と、この多数のフィンガー電極を相互に接続する2本のバスバー電極(1f)で構成される。   A front surface electrode 1 e and a back surface electrode 1 f are formed on the front surface side and the back surface side of the silicon substrate 1. The front electrode 1e and the back electrode 1f are screen-printed and fired with an Ag paste mainly composed of Ag powder, binder, frit, etc., and a solder layer is formed thereon. The surface electrode 1e is composed of, for example, a large number of finger electrodes (not shown) formed with a width of about 200 μm and a pitch of about 3 mm, and two bus bar electrodes (1e) that connect the large number of finger electrodes to each other. The The back electrode 1f is composed of, for example, a large number of finger electrodes (not shown) formed with a width of about 300 μm and a pitch of about 5 mm, and two bus bar electrodes (1f) that connect the large number of finger electrodes to each other. The

本発明に係る太陽電池の製造方法により形成された太陽電池を示す図である。It is a figure which shows the solar cell formed by the manufacturing method of the solar cell which concerns on this invention. 本発明に係る太陽電池の製造方法に用いる反応性イオンエッチング装置の一例を示す図である。It is a figure which shows an example of the reactive ion etching apparatus used for the manufacturing method of the solar cell which concerns on this invention. 本発明に係る太陽電池の製造方法に用いる反応性イオンエッチング装置の他の例を示す図である。It is a figure which shows the other example of the reactive ion etching apparatus used for the manufacturing method of the solar cell which concerns on this invention. 本発明に係る太陽電池の製造方法の効果をシリコン基板の表面反射率で示す図である。It is a figure which shows the effect of the manufacturing method of the solar cell which concerns on this invention by the surface reflectance of a silicon substrate.

符号の説明Explanation of symbols

1:シリコン基板、1a:表面凹凸構造、1b:不純物拡散層、1c:裏面不純物拡散層、1d:反射防止膜、1e:表面電極、1f:裏面電極 1: silicon substrate, 1a: surface uneven structure, 1b: impurity diffusion layer, 1c: back surface impurity diffusion layer, 1d: antireflection film, 1e: surface electrode, 1f: back surface electrode

Claims (5)

Oを含むエッチングガスを用いた反応性イオンエッチング法によって、多結晶シリコン基板の表面にマイクロマスクとなるエッチング生成物を付着させながら該表面に凹凸を形成する凹凸形成工程を備えてなる太陽電池の製造方法。 By H 2 O reactive ion etching using the free non-image Tchingugasu becomes comprise irregularities forming step of forming irregularities on said surface while the surface of the polycrystalline silicon substrate by adhering etching products of the micro-mask A method for manufacturing a solar cell. 記エッチングガスはSFを含み、該SFの量よりも前記HOの量が少ないことを特徴とする請求項1に記載の太陽電池の製造方法。 Before disappeared Tchingugasu comprises SF 6, for producing a solar cell according to claim 1 wherein the amount of said H 2 O than the amount of the SF 6 is small. 前記凹凸形成工程によって、前記多結晶シリコン基板の表面に、幅と高さがそれぞれ1μm以下の凹凸を形成することを特徴とする請求項1又は2に記載の太陽電池の製造方法。   3. The method for manufacturing a solar cell according to claim 1, wherein the unevenness having a width and a height of 1 μm or less is formed on the surface of the polycrystalline silicon substrate by the unevenness forming step. 前記凹凸形成工程によって、前記多結晶シリコン基板の表面に、アスペクト比が2以下の凹凸を形成することを特徴とする請求項1乃至3のいずれかに記載の太陽電池の製造方法。   The method for manufacturing a solar cell according to claim 1, wherein the unevenness having an aspect ratio of 2 or less is formed on the surface of the polycrystalline silicon substrate by the unevenness forming step. 前記エッチングガスはO ガスを含むことを特徴とする請求項1乃至4のいずれかに記載の太陽電池の製造方法。 The method for manufacturing a solar cell according to claim 1, wherein the etching gas contains O 2 gas .
JP2007044511A 2007-02-23 2007-02-23 Manufacturing method of solar cell Expired - Fee Related JP4413237B2 (en)