JP3832970B2 - Temperature-responsive biodegradable polymer - Google Patents
Temperature-responsive biodegradable polymer Download PDFInfo
- Publication number
- JP3832970B2 JP3832970B2 JP12797998A JP12797998A JP3832970B2 JP 3832970 B2 JP3832970 B2 JP 3832970B2 JP 12797998 A JP12797998 A JP 12797998A JP 12797998 A JP12797998 A JP 12797998A JP 3832970 B2 JP3832970 B2 JP 3832970B2
- Authority
- JP
- Japan
- Prior art keywords
- temperature
- polymer
- responsive
- biodegradable
- biodegradable polymer
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
【0001】
【発明の属する技術分野】
この出願の発明は、温度応答型生体内分解性高分子に関するものである。さらに詳しくは、この出願の発明は、薬物送達システム(DDS)のための新しい薬剤構成を可能とする、温度応答型生体内分解性高分子に関するものである。
【0002】
【従来の技術と発明が解決しようとする課題】
これまでの薬物送達システムを目的とした生体内分解性高分子材料の多くは、材料中に溶解あるいは分散した薬物を材料の生体内分解により徐放する疎水性高分子材料に限定されていた。それと言うのも、材料の分解に律速な薬物放出を実現するには、材料中の薬物拡散を制御して非分解時の薬物漏出を回避するとともに、材料の不安定性(生体内分解性)を向上させて、材料の加水分解を表面近傍に限定することが不可欠であったが、通常、材料の生体内分解は酵素的あるいは非酵素的加水分解によっているので、従来では、材料中への侵入速度と加水分解速度とを制御する立場から、結果として材料自身を疎水性にして水の侵入速度を制限するとともに、高分子鎖の不安定性を増して分解速度を上げざるをえなかったからである。しかしながら、このことは、製剤としての保存安定性の低下や材料の埋植時の生体適合性の低下をもたらし、製品化や適用部位に制限を生じることとなっていた。
【0003】
また近年では、生体の恒常性を考慮して、疾患時など生体が必要とする時のみに薬物を放出するインテリジェント製剤の設計が、刺激応答性高分子を用いて可能になってきている。主には、刺激に対する高分子材料の膨潤−収縮挙動によって薬物の拡散を制御することが検討されている。だがこの場合には、材料の生体内分解挙動によって薬物放出をON−OFFと制御することは困難であった。そこで最近になって、活性酵素や一部の酵素反応を利用して、材料の刺激応答型分解性が検討されてきており、疾患に応答して薬物を送達するシステムが可能となりつつある。
【0004】
しかしながら実際の疾患では、多種多様な生体変動が相互に関連して生起しているので、単一の生体変動によって疾患の特定やその程度を判断して薬物放出量を規定することは危険性が高い。実際の医療においても、疾患を特定するためには複数の検査項目によって総合的な診断が行なわれているように、薬物放出を制御する高分子材料の生体内分解機構にも、このような複合刺激に基づいた総合的な診断機能が必要とされている。
【0005】
つまり、より高度な薬物療法を実現するためには、複合的な診断機能を有する埋植可能な薬物担体の実現が不可欠であり、そのための有力な方法論として、複数の刺激に応答して生体内で分解する高分子材料が求められているのである。
【0006】
【課題を解決するための手段】
この出願の発明は、以上のとおりの、従来からの薬物担体としての生体内分解性高分子材料の問題点に鑑み、複合的な診断機能を有する刺激応答型高分子材料が求められているとの観点から、複数の生体変動(温度と酵素)に応答して生体内で分解する親水性高分子材料(高分子ヒドロゲル)を提供する。
【0007】
すなわち、この出願の発明は、第1には、水溶性高分子であって、3次元網目構造を持ち、生体内分解性高分子あるいは分子中に生体内分解性部位を有する高分子に温度応答性高分子がグラフト鎖として導入されており、温度応答性高分子のグラフト鎖と生体内分解性高分子網目が体温以下では相溶しており、この状態では生体内分解性高分子を分解可能な酵素によってゲル分解は進行しないが、疾患による温度上昇によって両者が相分離してゲル表面からの酵素分解が進行する温度応答型生体内分解性高分子であって、前記温度応答性高分子がポリ(N−イソプロピルアクリルアミド)、ポリジメチルアクリルアミド、これら共重合体、あるいはポリエチレングリコールとポリプロピレングリコールとのブロック共重合体であり、前記3次元網目を構成する生体内分解性高分子が、構成アミノ酸がアラニン、バリン、ロイシン、イソロイシン、メチオニン、プロリン、フェニルアラニン、トリプトファン、アスパラギン酸、グルタミン酸、グリシン、セリン、スレオニン、チロシン、システイン、リシン、アルギニン、ヒスチジンのいずれか単独もしくは複数からなるオリゴペプチド鎖、あるいは構成多糖としてデキストラン、ヒアルロン酸、キチン、キトサン、アルギン酸、コンドロイチン硫酸、でんぷん、プルランからなるオリゴ糖鎖であり、3次元網目構造の形成前のそれぞれの分子量が500−1000000であることを特徴とする温度応答型生体内分解性高分子を提供する。
【0008】
また、この出願の発明は、第2には、生体内非分解性の水溶性高分子をその構成の一部としている上記の温度応答型生体内分解性高分子であって、前記生体内非分解性の水溶性高分子は、ポリエーテルまたはポリエーテルエステルである温度応答型生体内分解性高分子を、第3には、非分解性の水溶性高分子は、その分子量が500−10000であり、その分子鎖中に含まれる生体内分解性部位としては、繰り返し単位が1−5であり、構成アミノ酸としてアラニン、バリン、ロイシン、イソロイシン、メチオニン、プロリン、フェニルアラニン、トリプトファン、アスパラギン酸、グルタミン酸、グリシン、セリン、スレオニン、チロシン、システイン、リシン、アルギニン、ヒスチジンのいずれか単独もしくは複数からなるオリゴペプチド鎖、あるいは繰り返し単位が1−5であり、構成多糖としてデキストラン、ヒアルロン酸、キチン、キトサン、アルギン酸、コンドロイチン硫酸、でんぷん、プルランからなるオリゴ糖鎖を有する温度応答型生体内分解性高分子を提供する。
【0009】
【発明の実施の形態】
この出願の発明の温度応答型生体内分解性高分子は、まずなによりも、従来の生体内分解性高分子ヒドロゲルのように単一の高分子鎖が架橋されているのではなく、温度応答性高分子がグラフト鎖として導入された3次元網目構造を形成していることが特徴である。このことは、単に生体内分解速度の制御ではなく、生体内分解の質的制御を可能にしている。すなわち、高分子網目を分解する疾患由来の酵素が存在するだけでは、グラフト鎖に基づく立体傷害によって酵素の接近が妨げられ、結果として分解が進行しない。これに対して、酵素の存在とともに疾患によって温度が上昇すると、たとえば、グラフト鎖が収縮して3次元網目と相分離し、酵素の網目に対する接近が容易となって加水分解がゲル表面より順次進行する。このように、刺激としての分解酵素と温度上昇が単独に存在する場合には分解せず、2つ同時に存在する場合のみ分解する。従って、この発明の温度応答型生体内分解性高分子は、従来の単独刺激により分解する高分子ゲルに比べ、より総合的な生体変動を認識することができ、生体内分解性を質的に制御できる利点を有している。
【0010】
このように本温度応答型生体内分解性高分子では、温度応答性高分子がグラフト鎖として導入された構造により、酵素分解性の質的変化を可能にしている。これにより、複合的な診断機能を有するインテリジェント製剤や医療用マイクロマシンへの応用が期待される。とりわけこの発明によって、静注、経口、皮下埋植など広範囲な投与経路において、疾患の種類や程度など総合的な診断に基づいた薬物送達を実現する製剤の設計が可能になる。
【0011】
より詳しくこの発明の温度応答型生体内分解性高分子の構成について説明すると、まず、3次元網目を構成している高分子全体、あるいは高分子の両末端など一部が、オリゴペプチド類あるいはオリゴ糖類などの生体内分解性高分子であり、疾患特異的な酵素によって分解されるものとするのが適当である。このような3次元網目を構成する生体内分解性高分子としては、前記のとおり構成アミノ酸がアラニン、バリン、ロイシン、イソロイシン、メチオニン、プロリン、フェニルアラニン、トリプトファン、アスパラギン酸、グルタミン酸、グリシン、セリン、スレオニン、チロシン、システイン、リシン、アルギニン、ヒスチジンのいずれか単独もしくは複数からなるオリゴペプチド鎖、あるいは構成多糖としてデキストラン、ヒアルロン酸、キチン、キトサン、アルギン酸、コンドロイチン硫酸、でんぷん、プルランからなるオリゴ糖鎖であり、3次元網目構造の形成前のそれぞれの分子量が500−1000000、望ましくは5000−100000であることが好適なものとして例示される。
【0012】
この発明の高分子には、非分解性の高分子、たとえばポリエーテルやポリエーテルエステルなどがその一部として含有されていてもよい。
たとえばポリエチレングリコールなどの非分解性の水溶性高分子を用いる場合、その分子量は、500−10000、望ましくは1000−5000であり、両末端などその分子鎖中に含まれる生体内分解性部位としては、繰り返し単位が1−5であり、構成アミノ酸としてアラニン、バリン、ロイシン、イソロイシン、メチオニン、プロリン、フェニルアラニン、トリプトファン、アスパラギン酸、グルタミン酸、グリシン、セリン、スレオニン、チロシン、システイン、リシン、アルギニン、ヒスチジンのいずれか単独もしくは複数からなるオリゴペプチド鎖、あるいは繰り返し単位が1−5であり、構成多糖としてデキストラン、ヒアルロン酸、キチン、キトサン、アルギン酸、コンドロイチン硫酸、でんぷん、プルランからなるオリゴ糖鎖を有するものとすることが好ましい。
【0013】
また、温度応答性高分子としては、ポリ(N−イソプロピルアクリルアミド)、ポリジメチルアクリルアミド、これら共重合体、あるいはポリエチレングリコールとポリプロピレングリコールとのブロック共重合体が適当なものとして挙げられる。
これらの温度応答性高分子はグラフト鎖として導入されるものであるが、そのグラフト鎖長については、分子量として1000−100000、望ましくは2000−10000の範囲となるものが考慮される。
【0014】
なかでも、温度応答性高分子グラフト鎖と生体内分解性高分子網目が体温以下で相溶しており、この状態では生体内分解性高分子を分解可能な酵素によってゲル分解は進行しないが、疾患による温度上昇によって両者が相分離し、結果としてゲル表面からの酵素分解が進行するように、このグラフト鎖と分解性高分子とが構成されるのが望ましい。
【0015】
以上のような、この発明の温度応答型生体内分解性高分子は、従来より知られている各種の重合方法やその条件を勘案して製造することができる。前記グラフト鎖の導入についても同様である。
たとえば3次元網目構造を成形する架橋方法については一般的に知られている多糖類の架橋方法が全て適用される。後述の実施例もその一つの方法を示しており、メタクリル基のような二重結合を導入してラジカル反応によって架橋する方法や、多糖類に存在する水酸基と反応するジイソシアネート化合物との付加反応による架橋方法等が適宜に採用される。
【0016】
そこで以下に実施例を示し、さらに詳しくこの発明について説明する。
【0017】
【実施例】
(実施例1)
<A>片末端にアミノ基を有するN−イソプロピルアクリルアミド(IPAAm)−N,N−ジメチルアクリルアミド(DMAAm)共重合体(1)の合成
所定量の連鎖移動剤であるアミノエタンチオール、ラジカル開始剤であるアゾビスイソブチロアクリロニトリル(AIBN)およびIPAAm(8.2g、72mmol)、DMAAm(1.8g、18mmol)をDMFに溶解し、均一溶液とした。この溶液を75℃で15時間窒素雰囲気でラジカル重合した後、溶液をジエチルエーテルに投じ、共重合体を単離した。その数平均分子量は、クリスタルヴァイオレットを指示薬として用い、過塩素酸−酢酸標準溶液による滴定により算出した(表1)。下限臨界溶液温度(LCST)は、500nmの可視光の透過度変化を観察することによって行った。図1はその結果を示したものである。
【0018】
連鎖移動剤とモノマー濃度比を変化させて合成した1の分子量は、それぞれ2600、4200、8800であった。 1H−NMR測定より、すべての共重合体のIPAAm含率は0.7であった。図1の温度変化による500nmにおけるリン酸緩衝溶液(PBS)中での透過度変化に見られるように、全てのIPAAm共重合体のLCSTは分子量が異なるにも依らず、35℃付近であった。
【0019】
【表1】
【0020】
<B>片末端にメタクリル基を有するIPAAm−DMAAm共重合体(2)の 合成
<A>の共重合体(1)(5g)とメタクリル酸クロリド(2ml)および酸受容剤として過剰量のトリエチルアミンをDMFに溶解し、4℃で24時間攪拌した。反応終了後、溶液をジエチルエーテルに投じ、2を単離した。
<C>IPAAm−DMAAm共重合体をグラフト鎖として有するデキストランヒドロゲル(3)の合成
<B>の共重合体(2)(0.3g)、メタクリル化デキストラン(Ma−Dex)(0.7g)、過硫酸アンモニウム(APS)(50mg)をDMSO3mlに溶解し、均一溶液を調製した。この溶液を両面がガラスで覆われているゲル作製用スペーサーに投入した後、高圧水銀灯を用いて室温で4時間光照射した。反応終了後、ヒドロゲルを蒸留水に投じ、室温で10日間平衡膨潤させた。
【0021】
分子量が2600、4200、8800のIPAAm共重合体をグラフト鎖として有するデキストランヒドロゲルをそれぞれ3a、3b、3cとして、PBS中での温度変化に伴うヒドロゲルの膨潤度変化を図2に示した。全てのヒドロゲルの膨潤度は10−45℃の範囲で一定であった。また、ヒドロゲル中のグラフト鎖の分子量が低いほど、ヒドロゲルの膨潤度は大きかった。図3に膨潤状態におけるヒドロゲルの透過度の温度依存性を示す。全てのヒドロゲルの透過度は温度上昇と共に低下し、温度を低下させることによって増大した。
(実施例2)
IPAAm−DMAAm共重合体をグラフト鎖として有するデキストランヒドロゲルの分解挙動の解析
平板状(20×20×2mm)に裁断した実施例1により得られたヒドロゲル(20×20×2mm)を、所定温度のデキストラナーゼ含有リン酸緩衝溶液(pH7.4)に浸漬し、その重量変化を経時的に測定した。異なる温度におけるデキストラナーゼの酵素活性は、各温度におけるデキストランの酵素分解速度より求め、ヒドロゲルの分解実験は、それぞれの温度で酵素活性が同一になるように調製した。
【0022】
前記3aは30−40℃のいずれの温度範囲においても完全に分解したが、酵素分解性の温度依存性は認められなかった(図4)。3bは35℃以上において完全に分解したが、30℃においては4時間30分後に分解が停止した(図5)。3cの分解は、いずれの温度においても完全に進行しなかったが、その酵素分解性の温度依存性は認められた(図6)。ヒドロゲルの酵素分解性を次式の分解指数を用いて評価した。
【0023】
分解指数(%)=A/Ao×100
(Ao:分解の標準累積量、A:実験から得られる分解の累積量)
図7は、分解指数の計算の特徴を図示したものであり、また図8は、計算された分解指数と温度との関係を示したものである。
3aの分解指数は、いずれの温度においても一定であった。3bおよび3cの分解指数は温度上昇とともに増大した。
【0024】
【発明の効果】
以上詳しく説明したとおり、この出願の発明の温度応答型生体内分解性高分子においては、複数の刺激(酵素と温度)に応じて生体内で分解することから、ゲル中に含有した薬物が複合刺激に応答してのみ放出される。すなわち、疾患の種類や程度など生体の情報を総合的に診断した上で、必要とされる薬物放出量を規定する、いわゆる複合診断による薬物投与が、生体内分解性ヒドロゲル自身の機能によって可能となる。このことにより、疾患の高度診断に基づいた治療、あるいは種々の合併症を伴うような複合的疾患の治療など、各種の疾患に対する有効性の高い薬物療法が可能となるものと期待される。また、複合的な刺激が存在する部位特異的な生体内分解性も実現可能であることから、生体内の特定な部位で医療行為を実施する医療用マイクロマシンとしての応用も期待される。
【図面の簡単な説明】
【図1】実施例としての片末端アミノ基を有するIPAAm−DMAAm共重合体の透過度の温度依存性を示した図である。
【図2】IPAAm−DMAAm共重合体をグラフト鎖とするDexヒドロゲルの膨潤度の温度依存性を示した図である。
【図3】図2に関連してDexヒドロゲルの透過度の温度依存性を示した図である。
【図4】実施例としてのDexヒドロゲル(3a)の酵素分解挙動を示した図である。
【図5】Dexヒドロゲル(3b)の酵素分解挙動を示した図である。
【図6】Dexヒドロゲル(3c)の酵素分解挙動を示した図である。
【図7】分解指数の計算を示した図である。
【図8】Dexヒドロゲル(3a、3b、3c)の分解指数と温度との関係を示した図である。[0001]
BACKGROUND OF THE INVENTION
The invention of this application relates to a temperature-responsive biodegradable polymer. More specifically, the invention of this application relates to a temperature-responsive biodegradable polymer that enables a new drug configuration for a drug delivery system (DDS).
[0002]
[Prior art and problems to be solved by the invention]
Many biodegradable polymer materials aimed at drug delivery systems so far have been limited to hydrophobic polymer materials that slowly release drugs dissolved or dispersed in the material by biodegradation of the material. That said, in order to achieve rate-determining drug release for material degradation, drug diffusion in the material is controlled to avoid drug leakage during non-degradation, and material instability (biodegradability) is reduced. It was indispensable to improve and limit the hydrolysis of the material to the vicinity of the surface, but since the biodegradation of the material is usually by enzymatic or non-enzymatic hydrolysis, it has traditionally penetrated into the material. This is because, from the standpoint of controlling the rate and hydrolysis rate, as a result, the material itself was made hydrophobic to limit the water penetration rate, and the instability of the polymer chain was increased to increase the degradation rate. . However, this has resulted in a decrease in storage stability as a preparation and a decrease in biocompatibility at the time of implantation of the material, resulting in limitations on the product and application site.
[0003]
In recent years, in consideration of homeostasis, it has become possible to design an intelligent preparation that releases a drug only when a living body needs it, such as a disease, using a stimulus-responsive polymer. Mainly, it has been studied to control the diffusion of a drug by the swelling-contraction behavior of a polymer material in response to a stimulus. However, in this case, it has been difficult to control drug release ON-OFF by the biodegradation behavior of the material. Therefore, recently, stimulation-responsive degradability of materials has been studied using active enzymes and some enzyme reactions, and a system for delivering drugs in response to diseases is becoming possible.
[0004]
However, in actual diseases, a wide variety of biological fluctuations occur in relation to each other, so it is dangerous to determine the amount of drug release by determining the degree of disease and its degree by a single biological fluctuation. high. In actual medical treatment, in order to identify a disease, a comprehensive diagnosis is performed by using a plurality of test items, and the biodegradation mechanism of a polymer material that controls drug release is also included in such a complex. There is a need for a comprehensive diagnostic function based on stimuli.
[0005]
In other words, in order to realize more advanced drug therapy, it is indispensable to realize an implantable drug carrier having a complex diagnostic function, and as a powerful methodology for that purpose, in vivo in response to multiple stimuli There is a need for a polymer material that decomposes in
[0006]
[Means for Solving the Problems]
In view of the problems of biodegradable polymer materials as conventional drug carriers as described above, the invention of this application is required to be a stimulus-responsive polymer material having a composite diagnostic function. In view of the above, a hydrophilic polymer material (polymer hydrogel) that decomposes in vivo in response to a plurality of biological fluctuations (temperature and enzyme) is provided.
[0007]
That is, the invention of this application is primarily a water-soluble polymer having a three-dimensional network structure, and having a temperature response to a biodegradable polymer or a polymer having a biodegradable site in the molecule. The polymer is introduced as a graft chain, and the temperature-responsive polymer graft chain and the biodegradable polymer network are compatible at or below body temperature. In this state, the biodegradable polymer can be degraded. Is a temperature-responsive biodegradable polymer in which gel degradation does not proceed by a temperature-enhanced enzyme but phase separation occurs due to a temperature rise due to a disease, and enzymatic degradation proceeds from the gel surface. Poly (N-isopropylacrylamide), polydimethylacrylamide, copolymers thereof, or block copolymers of polyethylene glycol and polypropylene glycol, The biodegradable polymer constituting the network is composed of alanine, valine, leucine, isoleucine, methionine, proline, phenylalanine, tryptophan, aspartic acid, glutamic acid, glycine, serine, threonine, tyrosine, cysteine, lysine, arginine, Oligopeptide chain consisting of one or more histidines, or an oligosaccharide chain consisting of dextran, hyaluronic acid, chitin, chitosan, alginic acid, chondroitin sulfate, starch, and pullulan as a constituent polysaccharide, before the formation of the three-dimensional network structure A temperature-responsive biodegradable polymer having a molecular weight of 500 to 1,000,000 is provided.
[0008]
In addition, the invention of this application is, secondly, the above-described temperature-responsive biodegradable polymer comprising a non-biodegradable water-soluble polymer as a part of its configuration, The degradable water-soluble polymer is a temperature-responsive biodegradable polymer that is a polyether or a polyether ester. Third, a non-degradable water-soluble polymer has a molecular weight of 500 to 10,000. The biodegradable site contained in the molecular chain has a repeating unit of 1-5, and the constituent amino acids are alanine, valine, leucine, isoleucine, methionine, proline, phenylalanine, tryptophan, aspartic acid, glutamic acid, Oligope consisting of one or more of glycine, serine, threonine, tyrosine, cysteine, lysine, arginine, and histidine A temperature-responsive biodegradable polymer having an oligosaccharide chain consisting of dextran, hyaluronic acid, chitin, chitosan, alginic acid, chondroitin sulfate, starch, and pullulan as a constituent polysaccharide. provide.
[0009]
DETAILED DESCRIPTION OF THE INVENTION
First of all, the temperature-responsive biodegradable polymer of the invention of this application is not a single polymer chain cross-linked unlike the conventional biodegradable polymer hydrogel, but the temperature response. It is characterized by forming a three-dimensional network structure in which a conductive polymer is introduced as a graft chain. This allows qualitative control of biodegradation, not just biodegradation rate control. That is, if there is only a disease-derived enzyme that degrades the polymer network, the steric hindrance based on the graft chain prevents the enzyme from approaching, and as a result, degradation does not proceed. On the other hand, when the temperature rises due to a disease due to the presence of the enzyme, for example, the graft chain contracts and phase separates from the three-dimensional network, and the enzyme is easily accessible to the network and hydrolysis proceeds sequentially from the gel surface. To do. Thus, it does not decompose when a decomposing enzyme as a stimulus and a temperature increase are present alone, but only when two are present simultaneously. Therefore, the temperature-responsive biodegradable polymer of the present invention can recognize more comprehensive biological fluctuations than the conventional polymer gel that is degraded by single stimulation, and qualitatively improves biodegradability. It has the advantage of being controllable.
[0010]
As described above, in the present thermoresponsive biodegradable polymer, the qualitative change of the enzyme decomposability is enabled by the structure in which the thermoresponsive polymer is introduced as a graft chain. This is expected to be applied to intelligent preparations and medical micromachines that have multiple diagnostic functions. In particular, the present invention makes it possible to design a formulation that realizes drug delivery based on a comprehensive diagnosis such as the type and degree of disease in a wide range of administration routes such as intravenous injection, oral administration, and subcutaneous implantation.
[0011]
The structure of the temperature-responsive biodegradable polymer of the present invention will be described in more detail. First, the entire polymer constituting the three-dimensional network, or both ends of the polymer, such as oligopeptides or oligopeptides It is suitable for biodegradable polymers such as saccharides, which are degraded by disease-specific enzymes. As the biodegradable polymer constituting such a three-dimensional network, as described above, the constituent amino acids are alanine, valine, leucine, isoleucine, methionine, proline, phenylalanine, tryptophan, aspartic acid, glutamic acid, glycine, serine, threonine. , Tyrosine, cysteine, lysine, arginine, histidine alone or in multiple oligopeptide chains, or constituent polysaccharides such as dextran, hyaluronic acid, chitin, chitosan, alginic acid, chondroitin sulfate, starch, pullulan A suitable example is that each molecular weight before the formation of the three-dimensional network structure is 500 to 1,000,000, desirably 5000 to 100,000.
[0012]
The polymer of the present invention may contain a non-degradable polymer such as polyether or polyether ester as a part thereof.
For example, when using a non-degradable water-soluble polymer such as polyethylene glycol, the molecular weight is 500-10000, preferably 1000-5000, and the biodegradable sites contained in the molecular chain such as both ends are as follows. The repeating unit is 1-5, and the constituent amino acids are alanine, valine, leucine, isoleucine, methionine, proline, phenylalanine, tryptophan, aspartic acid, glutamic acid, glycine, serine, threonine, tyrosine, cysteine, lysine, arginine, histidine An oligopeptide chain consisting of any one or a plurality, or a repeating unit of 1-5, and a constituent polysaccharide comprising dextran, hyaluronic acid, chitin, chitosan, alginic acid, chondroitin sulfate, starch, and pullulan. It is preferable that those having a sugar chain.
[0013]
Examples of suitable temperature-responsive polymers include poly (N-isopropylacrylamide), polydimethylacrylamide, copolymers thereof, and block copolymers of polyethylene glycol and polypropylene glycol.
These temperature-responsive polymers are introduced as graft chains, and the graft chain length is considered to have a molecular weight in the range of 1000-100000, preferably 2000-10000.
[0014]
Among them, the temperature-responsive polymer graft chain and the biodegradable polymer network are compatible at body temperature or lower, and in this state, gel degradation does not proceed with an enzyme capable of degrading the biodegradable polymer, It is desirable that the graft chain and the degradable polymer are configured so that both of them are phase-separated by a temperature increase due to a disease, and as a result, enzymatic degradation from the gel surface proceeds.
[0015]
The temperature-responsive biodegradable polymer of the present invention as described above can be produced in consideration of various conventionally known polymerization methods and conditions. The same applies to the introduction of the graft chain.
For example, as a crosslinking method for forming a three-dimensional network structure, all generally known polysaccharide crosslinking methods are applied. Examples to be described later also show one method, such as a method of introducing a double bond such as a methacryl group and crosslinking by a radical reaction, or an addition reaction with a diisocyanate compound that reacts with a hydroxyl group present in a polysaccharide. A crosslinking method or the like is appropriately employed.
[0016]
Therefore, the present invention will be described in more detail with reference to the following examples.
[0017]
【Example】
Example 1
<A> Synthesis of N-isopropylacrylamide (IPAAm) -N, N-dimethylacrylamide (DMAAm) copolymer (1) having an amino group at one end Aminoethanethiol which is a predetermined amount of chain transfer agent Azobisisobutyroacrylonitrile (AIBN), IPAAm (8.2 g, 72 mmol) and DMAAm (1.8 g, 18 mmol) as radical initiators were dissolved in DMF to obtain a homogeneous solution. After radically polymerizing this solution at 75 ° C. for 15 hours in a nitrogen atmosphere, the solution was poured into diethyl ether to isolate a copolymer. The number average molecular weight was calculated by titration with a perchloric acid-acetic acid standard solution using crystal violet as an indicator (Table 1). The lower critical solution temperature (LCST) was determined by observing a change in visible light transmittance at 500 nm. FIG. 1 shows the result.
[0018]
The molecular weights of 1 synthesized by changing the chain transfer agent and monomer concentration ratio were 2600, 4200, and 8800, respectively. From the 1 H-NMR measurement, the IPAAm content of all the copolymers was 0.7. As can be seen from the change in permeability in a phosphate buffer solution (PBS) at 500 nm due to the temperature change in FIG. 1, the LCST of all IPAAm copolymers was around 35 ° C. regardless of the difference in molecular weight. .
[0019]
[Table 1]
[0020]
<B> excess of triethylamine as a copolymer (1) (5 g) and methacrylic acid chloride (2 ml) and the acid acceptor Synthesis <A> of IPAAm-DMAAm copolymer having methacryl group at one terminal (2) Was dissolved in DMF and stirred at 4 ° C. for 24 hours. After completion of the reaction, the solution was poured into diethyl ether and 2 was isolated.
<C> Synthesis of Dextran Hydrogel (3) Having IPAAm-DMAAm Copolymer as Graft Chain Copolymer (2) (0.3 g) of <B>, Methacrylated Dextran (Ma-Dex) (0.7 g) Ammonium persulfate (APS) (50 mg) was dissolved in 3 ml of DMSO to prepare a homogeneous solution. This solution was put into a gel preparation spacer whose both surfaces were covered with glass, and then irradiated with light at room temperature for 4 hours using a high pressure mercury lamp. After completion of the reaction, the hydrogel was poured into distilled water and allowed to swell at room temperature for 10 days.
[0021]
The dextran hydrogels having IPAAm copolymers having molecular weights of 2600, 4200, and 8800 as graft chains are designated as 3a, 3b, and 3c, respectively, and the change in the degree of swelling of the hydrogel with temperature change in PBS is shown in FIG. The swelling degree of all hydrogels was constant in the range of 10-45 ° C. Further, the lower the molecular weight of the graft chain in the hydrogel, the greater the degree of swelling of the hydrogel. FIG. 3 shows the temperature dependence of the permeability of the hydrogel in the swollen state. The permeability of all hydrogels decreased with increasing temperature and increased with decreasing temperature.
(Example 2)
Analysis of degradation behavior of dextran hydrogel having IPAAm-DMAAm copolymer as graft chain Hydrogel (20 × 20 × 2 mm) obtained in Example 1 cut into a plate (20 × 20 × 2 mm) was obtained. The sample was immersed in a dextranase-containing phosphate buffer solution (pH 7.4) at a predetermined temperature, and the weight change was measured over time. The enzymatic activity of dextranase at different temperatures was determined from the enzymatic degradation rate of dextran at each temperature, and hydrogel degradation experiments were prepared such that the enzymatic activity was the same at each temperature.
[0022]
Although 3a was completely decomposed in any temperature range of 30 to 40 ° C., the temperature dependency of the enzymatic degradability was not recognized (FIG. 4). 3b completely decomposed at 35 ° C. or higher, but the decomposition stopped after 4
[0023]
Degradation index (%) = A / Ao × 100
(Ao: standard cumulative amount of degradation, A: cumulative amount of degradation obtained from experiments)
FIG. 7 illustrates the characteristics of the calculation of the decomposition index, and FIG. 8 illustrates the relationship between the calculated decomposition index and temperature.
The decomposition index of 3a was constant at any temperature. The decomposition indices of 3b and 3c increased with increasing temperature.
[0024]
【The invention's effect】
As explained in detail above, the temperature-responsive biodegradable polymer of the invention of this application is decomposed in vivo in response to a plurality of stimuli (enzyme and temperature), so that the drug contained in the gel is complex. Only released in response to a stimulus. In other words, after comprehensively diagnosing biological information such as the type and degree of disease, drug administration by so-called combined diagnosis that regulates the required amount of drug release is possible by the function of the biodegradable hydrogel itself. Become. This is expected to enable highly effective pharmacotherapy for various diseases such as treatment based on advanced diagnosis of diseases or treatment of complex diseases accompanied by various complications. In addition, since site-specific biodegradability in the presence of complex stimuli can also be realized, application as a medical micromachine for performing a medical practice at a specific site in the living body is also expected.
[Brief description of the drawings]
FIG. 1 is a graph showing the temperature dependence of the permeability of an IPAAm-DMAAm copolymer having one terminal amino group as an example.
FIG. 2 is a graph showing the temperature dependence of the degree of swelling of a Dex hydrogel having an IPAAm-DMAAm copolymer as a graft chain.
FIG. 3 shows the temperature dependence of the permeability of the Dex hydrogel in relation to FIG.
FIG. 4 is a diagram showing the enzymatic degradation behavior of Dex hydrogel (3a) as an example.
FIG. 5 shows the enzymatic degradation behavior of Dex hydrogel (3b).
FIG. 6 shows the enzymatic degradation behavior of Dex hydrogel (3c).
FIG. 7 is a diagram showing calculation of a decomposition index.
FIG. 8 is a graph showing the relationship between the decomposition index of Dex hydrogel (3a, 3b, 3c) and temperature.
Claims (3)