JP3689181B2 - Photothermographic material - Google Patents
Photothermographic material Download PDFInfo
- Publication number
- JP3689181B2 JP3689181B2 JP16367096A JP16367096A JP3689181B2 JP 3689181 B2 JP3689181 B2 JP 3689181B2 JP 16367096 A JP16367096 A JP 16367096A JP 16367096 A JP16367096 A JP 16367096A JP 3689181 B2 JP3689181 B2 JP 3689181B2
- Authority
- JP
- Japan
- Prior art keywords
- group
- coupler
- light
- atom
- general formula
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Expired - Fee Related
Description
【0001】
【発明の属する技術分野】
本発明は熱現像カラー感光材料に関するものであり、特に画像のディスクリミネーション、ならびに色再現性に優れた熱現像カラー感光材料に関するものである。
【0002】
【従来の技術】
ハロゲン化銀を用いた写真法は、他の写真法、たとえば電子写真やジアゾ写真に比べて感度や階調調節などの写真特性に優れているため、従来から最も広範に用いられてきた。特にカラーハードコピーとしては最高の画質が得られるため、昨今より精力的に研究されている。
【0003】
近年になって、ハロゲン化銀を用いた感光材料の画像形成処理法を従来の湿式処理から、現像液を内蔵するインスタント写真システム、さらには加熱等による乾式熱現像処理などにより、簡易迅速に画像を得ることの出来るシステムが開発されてきた。熱現像感光材料については、「写真工学の基礎(非銀塩写真編)コロナ社刊 1982年」p.242 〜にその内容の記載があるが、その内容としてはドライシルバーを代表とした、白黒画像形成法にとどまっている。最近、熱現像カラー感光材料としては、富士写真フイルム(株)社からピクトログラフィー、ピクトロスタットといった商品が発売されている。上記の簡易迅速処理法では、プレフォームドダイを連結したレドックス性色材を用いたカラー画像形成を行っている。写真感光材料のカラー画像形成法としては、カプラーと発色現像主薬酸化体のカップリング反応を利用する方法が最も一般的であり、この方法を採用した熱現像カラー感光材料についても、米国特許第3,761,270号、同第4,021,240号、特開昭59−231539号等、多くのアイデアが出願されている。
【0004】
発明者らも上記のカップリング型熱現像カラー感光材料について検討を行ったが、現像主薬を内蔵する多層構成のカラー感光材料を作成する場合、現像主薬の酸化体が他の感光性層に移動するという問題が生じる。現像主薬の酸化体が、他の感光性層に移動し、そこでカップリング反応を行うと、本来発色するべきでない層で色素を生じてしまい、この色濁りによって画像の色再現性が損なわれることになる。従来の技術ではこれを回避するために、隣接する感光性層の間に、非感光性の中間層を設けて、現像主薬の酸化体を中間層で化学反応により失活させる方法が広く知られている。この具体的方法として、第1に中間層に別種の還元剤を含有させ、これとのクロス酸化反応により現像主薬酸化体を元の現像主薬に戻す方法が知られている。しかし、この方法では、現像主薬が再生され、再度銀現像を行うため、塩基の消費量が増大する。本発明で考えている処理の形態においては、塩基量は有限であるため、このようにクロストークによる塩基の消費が起こると、画像のDmax が低下してしまう。従ってこの方法は採用が困難であることがわかった。別の方法として、中間層に現像主薬の酸化体とカップリング反応して、実質的に無色の化合物を形成するカプラーを導入する技術が知られている。このような化合物としては、例えば通常のカプラーの離脱基の部位に、離脱不可能な置換基を導入する方法があり、このような置換基を導入したカプラーの例としては、例えば、特開昭49−84439号に記載されている。しかし、本発明の系でこのようなカプラーを使用した場合、十分な混色防止効果が得られないことがわかった。
【0005】
【発明が解決しようとする課題】
本発明の目的は、最高濃度が高く、ディスクリミネーション、ならびに色再現性に優れた熱現像カラー感光材料を与えることにある。
【0006】
【課題を解決するための手段】
本発明の目的は、下記の熱現像カラー感光材料によって達成された。
【0007】
1)支持体上に、少なくとも感光性ハロゲン化銀、バインダー、カプラーおよび現像主薬を含有する感光性乳剤層が、少なくとも2層以上塗設されており、それぞれが異なる波長領域に分光感度を有し、各々の感光性乳剤層の間に実質的に非感光性の中間層を少なくとも1層ずつ有する熱現像カラー感光材料において、該感光性乳剤層に含まれる該カプラーが4当量カプラーであって、かつ該現像主薬が下記一般式(1)、(2)又は(3)で表される化合物であり、該中間層の少なくとも1層に2当量カプラーを含有することを特徴とする熱現像カラー感光材料。
【0008】
一般式(1)
【0009】
【化6】
【0010】
一般式(2)
【0011】
【化7】
【0012】
一般式(3)
【0013】
【化8】
【0014】
式中、R1 〜R4 は水素原子、ハロゲン原子、アルキル基、アリール基、アルキルカルボンアミド基、アリールカルボンアミド基、アルキルスルホンアミド基、アリールスルホンアミド基、アルコキシ基、アリールオキシ基、アルキルチオ基、アリールチオ基、アルキルカルバモイル基、アリールカルバモイル基、カルバモイル基、アルキルスルファモイル基、アリールスルファモイル基、スルファモイル基、シアノ基、アルキルスルホニル基、アリールスルホニル基、アルコキシカルボニル基、アリールオキシカルボニル基、アルキルカルボニル基、アリールカルボニル基またはアシルオキシ基を表し、R5 はアルキル基、アリール基または複素環基を表す。Zは芳香環(複素芳香環も含む)を形成する原子群を表し、Zがベンゼン環である場合、その置換基のハメット定数(σ)の合計値は1以上である。R6 はアルキル基を表す。Xは酸素原子、硫黄原子、セレン原子または3級窒素原子(アルキル置換)を表す。R7 及びR8 はそれぞれ水素原子または置換基を表し、R7 とR8 が互いに結合して2重結合または環を形成してもよい。
【0015】
2)支持体上に、少なくとも感光性ハロゲン化銀、バインダー、カプラーおよび現像主薬を含有する感光性乳剤層が、少なくとも2層以上塗設されており、それぞれが異なる波長領域に分光感度を有し、各々の感光性乳剤層の間に実質的に非感光性の中間層を少なくとも1層ずつ有する熱現像カラー感光材料において、該感光性乳剤層に含まれる該カプラーが2当量カプラーであって、かつ該現像主薬が下記一般式(4)または(5)で表される化合物であり、該中間層の少なくとも1層に4当量カプラーを含有することを特徴とする熱現像カラー感光材料。
一般式(4)
【0016】
【化9】
【0017】
一般式(5)
【0018】
【化10】
【0019】
式中、R5 〜R8 ,X,Zは、一般式(2)又は(3)におけるそれぞれと同様である。
【0020】
【発明の実施の形態】
以下に本発明について詳細に述べる。
本発明の技術が目指す最終目的は、感光性乳剤層間で現像主薬の酸化体がお互いの層に拡散するのを防ぎ、混色反応が起きないようにすることにある。本発明においては、画像の階調の軟調化や粒状度を向上させる目的で、分光感度は同一で粒子サイズ等の異なるハロゲン化銀粒子等を含有する層を、何層かに分割して層状に塗り重ね、1つの感光性乳剤層とすることも可能である。本発明では、この感光性乳剤層の間に中間層を設け、ここに本発明に用いる現像主薬の酸化体とカップリング反応はするが発色しないカプラーを含有させる。
【0021】
本発明に好ましく用いられる現像主薬は、カップリング部位に離脱基を有しているという特徴を有する。このため、例えば一般式(1)〜(3)の現像主薬では、4当量カプラーとは色像を形成するが2当量カプラーとは色像を形成しない。この場合、一般式(1)〜(3)の現像主薬を用いた感材系において、2当量カプラーを中間層に添加すると、混色防止の目的が効率的に達成できる。逆に、一般式(4),(5)の現像主薬では、2当量カプラーとのみ色像を形成する。従って、一般式(4),(5)の現像主薬を用いた感材系では、中間層に4当量カプラーを使用することが有効である。
【0022】
一般式(1)で表される化合物はスルホンアミドフェノールと総称される化合物である。
【0023】
式中、R1 〜R4 は水素原子、ハロゲン原子(例えばクロル原子、ブロム原子)、置換又は無置換のアルキル基(例えばメチル基、エチル基、イソプロピル基、n−ブチル基、t−ブチル基)、置換又は無置換のアリール基(たとえばフェニル基、トリル基、キシリル基)、置換又は無置換のアルキルカルボンアミド基(例えばアセチルアミノ基、プロピオニルアミノ基、ブチロイルアミノ基)、置換又は無置換のアリールカルボンアミド基(例えばベンゾイルアミノ基)、置換又は無置換のアルキルスルホンアミド基(例えばメタンスルホニルアミノ基、エタンスルホニルアミノ基)、置換又は無置換のアリールスルホンアミド基(例えばベンゼンスルホニルアミノ基、トルエンスルホニルアミノ基)、置換又は無置換のアルコキシ基(例えばメトキシ基、エトキシ基、ブトキシ基)、置換又は無置換のアリールオキシ基(例えばフェノキシ基)、置換又は無置換のアルキルチオ基(例えばメチルチオ基、エチルチオ基、ブチルチオ基)、置換又は無置換のアリールチオ基(例えばフェニルチオ基、トリルチオ基)、置換又は無置換のアルキルカルバモイル基(例えばメチルカルバモイル基、ジメチルカルバモイル基、エチルカルバモイル基、ジエチルカルバモイル基、ジブチルカルバモイル基、ピペリジルカルバモイル基、モルホリルカルバモイル基)、置換又は無置換のアリールカルバモイル基(例えばフェニルカルバモイル基、メチルフェニルカルバモイル基、エチルフェニルカルバモイル基、ベンジルフェニルカルバモイル基)、カルバモイル基、置換又は無置換のアルキルスルファモイル基(例えばメチルスルファモイル基、ジメチルスルファモイル基、エチルスルファモイル基、ジエチルスルファモイル基、ジブチルスルファモイル基、ピペリジルスルファモイル基、モルホリルスルファモイル基)、置換又は無置換のアリールスルファモイル基(例えばフェニルスルファモイル基、メチルフェニルスルファモイル基、エチルフェニルスルファモイル基、ベンジルフェニルスルファモイル基)、スルファモイル基、シアノ基、置換又は無置換のアルキルスルホニル基(例えばメタンスルホニル基、エタンスルホニル基)、置換又は無置換のアリールスルホニル基(例えばフェニルスルホニル基、4−クロロフェニルスルホニル基、p−トルエンスルホニル基)、置換又は無置換のアルコキシカルボニル基(例えばメトキシカルボニル基、エトキシカルボニル基、ブトキシカルボニル基)、置換又は無置換のアリールオキシカルボニル基(例えばフェノキシカルボニル基)、置換又は無置換のアルキルカルボニル基(例えばアセチル基、プロピオニル基、ブチロイル基)、置換又は無置換のアリールカルボニル基(例えばベンゾイル基、アルキルベンゾイル基)、または置換又は無置換のアシルオキシ基(例えばアセチルオキシ基、プロピオニルオキシ基、ブチロイルオキシ基)を表す。R1 〜R4 の中で、R2 およびR4 は好ましくは水素原子である。また、R1 〜R4 のハメット置換基定数(σ値)の合計は、0以上となることが好ましい。R5 は置換又は無置換のアルキル基(例えばメチル基、エチル基、ブチル基、オクチル基、ラウリル基、セチル基、ステアリル基)、置換又は無置換のアリール基(例えばフェニル基、トリル基、キシリル基、4−メトキシフェニル基、ドデシルフェニル基、クロロフェニル基、トリクロロフェニル基、ニトロクロロフェニル基、トリイソプロピルフェニル基、4−ドデシルオキシフェニル基、3,5−ジ−(メトキシカルボニル)基)、または置換又は無置換の複素環基(例えばピリジル基)を表す。
【0024】
一般式(2)で表される化合物はスルホニルヒドラジンと総称される化合物である。また、一般式(4)で表される化合物はカルバモイルヒドラジンと総称される化合物である。
【0025】
式中、Zは芳香環を形成する原子群を表す。Zによって形成される芳香環は、本化合物に銀現像活性を付与するため、十分に電子吸引的であることが必要である。このため、含窒素芳香環を形成するか、或いはベンゼン環に電子吸引性基を導入したような芳香環が好ましく使用される。このような芳香環としては、ピリジン環、ピラジン環、ピリミジン環、キノリン環、キノキサリン環等が好ましい。ベンゼン環の場合、その置換基としては、アルキルスルホニル基(例えばメタンスルホニル基、エタンスルホニル基)、ハロゲン原子(例えばクロル基、ブロム基)、アルキルカルバモイル基(例えばメチルカルバモイル基、ジメチルカルバモイル基、エチルカルバモイル基、ジエチルカルバモイル基、ジブチルカルバモイル基、ピペリジルカルバモイル基、モルホリルカルバモイル基)、アリールカルバモイル基(例えばフェニルカルバモイル基、メチルフェニルカルバモイル基、エチルフェニルカルバモイル基、ベンジルフェニルカルバモイル基)、カルバモイル基、アルキルスルファモイル基(例えばメチルスルファモイル基、ジメチルスルファモイル基、エチルスルファモイル基、ジエチルスルファモイル基、ジブチルスルファモイル基、ピペリジルスルファモイル基、モルホリルスルファモイル基)、アリールスルファモイル基(例えばフェニルスルファモイル基、メチルフェニルスルファモイル基、エチルフェニルスルファモイル基、ベンジルフェニルスルファモイル基)、スルファモイル基、シアノ基、アルキルスルホニル基(例えばメタンスルホニル基、エタンスルホニル基)、アリールスルホニル基(例えばフェニルスルホニル基、4−クロロフェニルスルホニル基、p−トルエンスルホニル基)、アルコキシカルボニル基(例えばメトキシカルボニル基、エトキシカルボニル基、ブトキシカルボニル基)、アリールオキシカルボニル基(例えばフェノキシカルボニル基)、アルキルカルボニル基(例えばアセチル基、プロピオニル基、ブチロイル基)、またはアリールカルボニル基(例えばベンゾイル基、アルキルベンゾイル基)等が挙げられるが、上記置換基のハメット置換基定数(σ値)の合計は、1以上となることが好ましい。
【0026】
一般式(3)で表される化合物はスルホニルヒドラゾンと総称される化合物である。また、一般式(5)で表される化合物はカルバモイルヒドラゾンと総称される化合物である。
【0027】
式中、R6 は置換あるいは無置換のアルキル基(例えばメチル基、エチル基)を表す。Xは酸素原子、硫黄原子、セレン原子または3級窒素原子(アルキル置換)を表すが、アルキル置換の3級窒素原子が好ましい。R7 及びR8 はそれぞれ水素原子または置換基を表し、R7 とR8 が互いに結合して2重結合または環(例えば、ベンゼン環、ピリジン環)を形成してもよい。R7 、R8 の置換基としては、R1 〜R4 での水素原子以外の基を好ましく挙げることができる。
【0028】
以下に、一般式(1)〜(5)で表される化合物の具体例を示すが、本発明の化合物はもちろんこれによって限定されるものではない。
【0029】
【化11】
【0030】
【化12】
【0031】
【化13】
【0032】
【化14】
【0033】
【化15】
【0034】
【化16】
【0035】
【化17】
【0036】
【化18】
【0037】
【化19】
【0038】
【化20】
【0039】
【化21】
【0040】
【化22】
【0041】
上記の化合物は、一般的に公知の方法で合成することが可能である。以下に簡単な合成ルートを列挙する。
【0042】
【化23】
【0043】
【化24】
【0044】
【化25】
【0045】
本発明において、色素供与性化合物は、酸化カップリング反応によって色素を形成する化合物(カプラー)を使用する。このカプラーとして、本発明では4当量カプラーと2当量カプラーを主薬の種類によって使い分ける。まず、一般式(1)〜(3)の現像主薬に対しては4当量カプラーを使用する。一般式(1)〜(3)の現像主薬は、カップリング部位がスルホニル基によって置換されており、カップリング時に、このスルホニル基がスルフィン酸して離脱するため、カプラー側の離脱基はカチオンとして離脱しなければならないからである。このため、カップリング時にプロトンを離脱基として放出可能な4当量カプラーとは反応して発色するが、離脱基がアニオンである2当量カプラーの場合、反応はするが発色しない。逆に、一般式(4),(5)の現像主薬に対しては2等量カプラーを使用する。一般式(4),(5)の現像主薬は、カップリング部位がカルバモイル基によって置換されており、カップリング時に窒素原子上の水素原子がプロトンとして離脱するため、カプラー側の離脱基はアニオンとして離脱しなければならないからである。このため、カップリング時にアニオンを離脱基として放出可能な2当量カプラーとは反応して発色するが、離脱基がプロトンである4当量カプラーの場合、反応はするが発色しない。カプラーの具体例は、4当量、2当量の両者ともセオリー・オブ・ザ・フォトグラフィック・プロセス(4th.Ed.T.H.James編集 Macmillan,1977)291頁〜334頁、および354頁〜361頁、特開昭58─12353号、同58─149046号、同58─149047号、同59─11114号、同59─124399号、同59─174835号、同59─231539号、同59─231540号、同60─2951号、同60─14242号、同60─23474号、同60─66249号などに詳しく記載されている。
【0046】
本発明に好ましく使用されるカプラーの例を以下に列挙する。
【0047】
本発明に好ましく使用されるカプラーとしては、以下の一般式(6)〜(17)に記載するような構造の化合物がある。これらはそれぞれ当該分野で公知の化合物である。
【0048】
【化26】
【0049】
【化27】
【0050】
【化28】
【0051】
一般式(6)〜(9)は活性メチレン系カプラーと称されるカプラーを表し、式中、R24は置換又は無置換のアシル基、シアノ基、ニトロ基、置換又は無置換のアリール基、置換又は無置換のヘテロ環基、置換又は無置換のアルコキシカルボニル基、置換又は無置換のアリールオキシカルボニル基、カルバモイル基、スルファモイル基、置換又は無置換のアルキルスルホニル基、置換又は無置換のアリールスルホニル基である。
【0052】
一般式(6)〜(9)において、R25は置換又は無置換のアルキル基、置換又は無置換のアリール基または置換又は無置換のヘテロ環基である。一般式(9)において、R26は置換又は無置換のアリール基または置換又は無置換のヘテロ環基である。R24、R25、R26が有してもよい置換基としては、例えばアルキル基、アルケニル基、アルキニル基、アリール基、ヘテロ環基、アルコキシ基、アリールオキシ基、シアノ基、ハロゲン原子、アシルアミノ基、スルホンアミド基、カルバモイル基、スルファモイル基、アルコキシカルボニル基、アリールオキシカルボニル基、アルキルアミノ基、アリールアミノ基、水酸基、スルホ基等、種々の置換基を挙げることができる。R24の好ましい例としては置換又は無置換のアシル基、シアノ基、カルバモイル基、置換又は無置換のアルコキシカルボニル基が挙げられる。
【0053】
一般式(6)〜(9)において、Yは水素原子または現像主薬の酸化体とのカップリング反応により脱離可能な基である。Yの例として、2当量カプラーのアニオン性離脱基として作用する基としては、ハロゲン原子(例えばクロル、ブロム)、アルコキシ基(例えばメトキシ基、エトキシ基)、アリールオキシ基(例えばフェノキシ基、4−シアノフェノキシ基、4−アルコキシカルボニルフェニル基)、アルキルチオ基(例えばメチルチオ基、エチルチオ基、ブチルチオ基)、アリールチオ基(例えばフェニルチオ基、トリルチオ基)、アルキルカルバモイル基(例えばメチルカルバモイル基、ジメチルカルバモイル基、エチルカルバモイル基、ジエチルカルバモイル基、ジブチルカルバモイル基、ピペリジルカルバモイル基、モルホリルカルバモイル基)、アリールカルバモイル基(例えばフェニルカルバモイル基、メチルフェニルカルバモイル基、エチルフェニルカルバモイル基、ベンジルフェニルカルバモイル基)、カルバモイル基、アルキルスルファモイル基(例えばメチルスルファモイル基、ジメチルスルファモイル基、エチルスルファモイル基、ジエチルスルファモイル基、ジブチルスルファモイル基、ピペリジルスルファモイル基、モルホリルスルファモイル基)、アリールスルファモイル基(例えばフェニルスルファモイル基、メチルフェニルスルファモイル基、エチルフェニルスルファモイル基、ベンジルフェニルスルファモイル基)、スルファモイル基、シアノ基、アルキルスルホニル基(例えばメタンスルホニル基、エタンスルホニル基)、アリールスルホニル基(例えばフェニルスルホニル基、4−クロロフェニルスルホニル基、p−トルエンスルホニル基)、アルキルカルボニルオキシ基(例えばアセチルオキシ基、プロピオニルオキシ基、ブチロイルオキシ基)、アリールカルボニルオキシ基(例えばベンゾイルオキシ基、トルイルオキシ基、アニシルオキシ基)、含窒素複素環基(例えばイミダゾリル基、ベンゾトリアゾリル基)等が挙げられる。
【0054】
また、4当量カプラーのカチオン性離脱基として作用する基としては、水素原子、ホルミル基、、カルバモイル基、置換基を有するメチレン基(置換基としては、アリール基、スルファモイル基、カルバモイル基、アルコキシ基、アミノ基、水酸基等)、アシル基、スルホニル基等が挙げられる。
【0055】
一般式(6)〜(9)において、R24とR25、R24とR26は互いに結合して環を形成してもよい。
【0056】
一般式(10)は5−ピラゾロン系マゼンタカプラーと称されるカプラーを表し、式中、R27はそれぞれ置換又は無置換のアルキル基、アリール基、アシル基またはカルバモイル基を表す。R28はフェニル基、または1個以上のハロゲン原子、アルキル基、シアノ基、アルコキシ基、アルコキシカルボニル基もしくはアシルアミノ基が置換したフェニル基を表す。Yについては一般式(6)〜(9)と同様である。
【0057】
一般式(10)で表される5−ピラゾロン系マゼンタカプラーの中でも、R27がアリール基またはアシル基、R28が1個以上のハロゲン原子が置換したフェニル基のものが好ましい。
【0058】
これら好ましい基について詳しく述べると、R27はフェニル、2−クロロフェニル、2−メトキシフェニル、2−クロロ−5−テトラデカンアミドフェニル、2−クロロ−5−(3−オクタデセニル−1−スクシンイミド)フェニル、2−クロロ−5−オクタデシルスルホンアミドフェニルまたは2−クロロ−5−〔2−(4−ヒドロキシ−3−t−ブチルフェノキシ)テトラデカンアミド〕フェニル等のアリール基、またはアセチル、ピバロイル、テトラデカノイル、2−(2,4−ジ−t−ペンチルフェノキシ)アセチル、2−(2,4−ジ−t−ペンチルフェノキシ)ブタノイル、ベンゾイル、3−(2,4−ジ−t−アミルフェノキシアセトアジド)ベンゾイル等のアシル基であり、これらの基はさらに置換基を有してもよく、それらは炭素原子、酸素原子、窒素原子、またはイオウ原子で連結する有機置換基またはハロゲン原子である。
【0059】
R28は2,4,6−トリクロロフェニル、2,5−ジクロロフェニル、2−クロロフェニル基等の置換フェニル基が好ましい。
【0060】
一般式(11)はピラゾロアゾール系カプラーと称されるカプラーを表し、式中、R29は水素原子または置換基を表す。Zは窒素原子を2〜4個含む5員のアゾール環を形成するのに必要な非金属原子群を表し、該アゾール環は置換基(縮合環を含む)を有してもよい。Yについては、一般式(6)〜(9)と同様である。
【0061】
一般式(11)で表されるピラゾロアゾール系カプラーの中でも、発色色素の吸収特性の点で、米国特許第4500630号に記載のイミダゾ〔1,2−b〕ピラゾール類、米国特許第450654号に記載のピラゾロ〔1,5−b〕〔1,2,4〕トリアゾール類、米国特許第3725067号に記載のピラゾロ〔5,1−c〕〔1,2,4〕トリアゾール類が好ましく、光堅牢性の点で、これらのうちピラゾロ〔1,5−b〕〔1,2,4〕トリアゾール類が好ましい。
【0062】
置換基R29、YおよびZで表されるアゾール環の置換基の詳細については、例えば米国特許第4540654号明細書の第2カラム第41行〜第8カラム第27行に記載されている。好ましくは特開昭61−65245号に記載されているような分岐アルキル基がピラゾロトリアゾール基の2,3または6位に直結したピラゾロアゾールカプラー、特開昭61−65245号に記載されている分子内にスルホンアミド基を含んだピラゾロアゾールカプラー、特開昭61−147254号に記載されるアルコキシフェニルスルホンアミドバラスト基をもつピラゾロアゾールカプラー、特開昭62−209457号もしくは同63−307453号に記載されている6位にアルコキシ基やアリールオキシ基をもつピラゾロトリアゾールカプラー、および特願平1−22279号に記載される分子内にカルボンアミド基をもつピラゾロトリアゾールカプラーである。
【0063】
一般式(12),(13)はそれぞれフェノール系カプラー、ナフトール系カプラーと称されるカプラーであり、式中、R30は水素原子または−NHCOR32,−SO2 NR32R33,−NHSO2 R32, −NHCOR32, −NHCONR32R33,−NHSO2 NR32R33から選ばれる基を表す。R32、R33は水素原子または置換基を表す。一般式(12),(13)において、R31は置換基を表し、lは0〜2から選ばれる整数、mは0〜4から選ばれる整数を表す。Yについては一般式(6)〜(9)と同様である。R31〜R33としては前記R24〜R26の置換基として述べたものが挙げられる。
【0064】
一般式(12)で表されるフェノール系カプラーの好ましい例としては、米国特許第2369929号、同第2801171号、同第2772162号、同第2895826号、同第3772002号、等に記載の2−アルキルアミノ−5−アルキルフェノール系、米国特許第2772162号、同第3758308号、同第4126396号、同第4334011号、同第4327173号、西独特許公開第3329729号、特開昭59−166956号等に記載の2,5−ジアシルアミノフェノール系、米国特許第3446622号、同第4333999号、同第4451559号、同第4427767号等に記載の2−フェニルウレイド−5−アシルアミノフェノール系等を挙げることができる。
【0065】
一般式(13)で表されるナフトールカプラーの好ましい例としては、米国特許第2474293号、同第4052212号、同第4146396号、同大4228233号、同第4296200号等に記載の2−カルバモイル−1−ナフトール系および米国特許4690889号等に記載の2−カルバモイル−5−アミド−1−ナフトール系等を挙げることができる。
【0066】
一般式(14)〜(17)はピロロトリアゾールと称されるカプラーであり、R42,R43, R44は水素原子または置換基を表す。Yについては一般式(6)〜(9)と同様である。R42,R43, R44の置換基としては、前記R24〜R26の置換基として述べたものが挙げられる。一般式(14)〜(17)で表されるピロロトリアゾール系カプラーの好ましい例としては、欧州特許第488248A1号、同第491197A1号、同第545300号に記載の、R42,R43の少なくとも一方が電子吸引基であるカプラーが挙げられる。
【0067】
その他、縮環フェノール、イミダゾール、ピロール、3−ヒドロキシピリジン、活性メチン、5,5−縮環複素環、5,6−縮環複素環といった構造を有するカプラーが使用できる。
【0068】
縮環フェノール系カプラーとしては、米国特許第4327173号、同第4564586号、同第4904575号等に記載のカプラーが使用できる。
【0069】
イミダゾール系カプラーとしては、米国特許第4818672号、同第5051347号等に記載のカプラーが使用できる。
【0070】
ピロール系カプラーとしては特開平4−188137号、同4−190347号等に記載のカプラーが使用できる。
【0071】
3−ヒドロキシピリジン系カプラーとしては特開平1−315736号等に記載のカプラーが使用できる。
【0072】
活性メチン系カプラーとしては米国特許第5104783号、同第5162196号等に記載のカプラーが使用できる。
【0073】
5,5−縮環複素環系カプラーとしては、米国特許第5164289号に記載のピロロピラゾール系カプラー、特開平4−174429号に記載のピロロイミダゾール系カプラー等が使用できる。
【0074】
5,6−縮環複素環系カプラーとしては、米国特許第4950585号に記載のピラゾロピリミジン系カプラー、特開平4−204730号に記載のピロロトリアジン系カプラー、欧州特許第556700号に記載のカプラー等が使用できる。
【0075】
本発明には前述のカプラー以外に、西独特許第3819051A号、同第3823049号、米国特許第4840883号、同第5024930号、同第5051347号、同第4481268号、欧州特許第304856A2号、同第329036号、同第354549A2号、同第374781A2号、同第379110A2号、同第386930A1号、特開昭63−141055号、同64−32260号、同32261号、特開平2−297547号、同2−44340号、同2−110555号、同3−7938号、同3−160440号、同3−172839号、同4−172447号、同4−179949号、同4−182645号、同4−184437号、同4−188138号、同4−188139号、同4−194847号、同4−204532号、同4−204731号、同4−204732号等に記載されているカプラーも使用できる。
【0076】
本発明に使用できるカプラーの具体例を以下に示す。前述のとおり、4当量カプラーは、現像主薬として一般式(1)〜(3)の化合物との組み合わせで画像形成用に使用する。逆に現像主薬として一般式(4),(5)の化合物を用いた場合には、混色防止剤として使用可能である。また、2当量カプラーは、現像主薬として一般式(4),(5)の化合物との組み合わせで画像形成用に使用する。逆に現像主薬として一般式(1)〜(3)の化合物を用いた場合には、混色防止剤として使用可能である。本発明はもちろん、以下の化合物例によって限定されるわけではない。
【0077】
【化29】
【0078】
【化30】
【0079】
【化31】
【0080】
【化32】
【0081】
【化33】
【0082】
【化34】
【0083】
【化35】
【0084】
【化36】
【0085】
【化37】
【0086】
【化38】
【0087】
【化39】
【0088】
【化40】
【0089】
【化41】
【0090】
【化42】
【0091】
【化43】
【0092】
【化44】
【0093】
【化45】
【0094】
【化46】
【0095】
【化47】
【0096】
【化48】
【0097】
【化49】
【0098】
【化50】
【0099】
【化51】
【0100】
【化52】
【0101】
【化53】
【0102】
【化54】
【0103】
【化55】
【0104】
【化56】
【0105】
【化57】
【0106】
【化58】
【0107】
【化59】
【0108】
【化60】
【0109】
【化61】
【0110】
【化62】
【0111】
【化63】
【0112】
【化64】
【0113】
【化65】
【0114】
【化66】
【0115】
【化67】
【0116】
【化68】
【0117】
【化69】
【0118】
【化70】
【0119】
現像主薬およびカプラーの添加方法としては、まず、カプラー、現像主薬および高沸点有機溶媒(例えばリン酸アルキルエステル、フタル酸アルキルエステル等)を混合して低沸点有機溶媒(例えば酢酸エチル、メチルエチルケトン等)に溶解し、当該分野で公知の乳化分散法を用いて水に分散の後、添加することができる。また、特開昭63−271339号に記載の固体分散法による添加も可能である。
【0120】
乳剤層のカプラーの添加量は、そのモル吸光係数(ε)にもよるが、反射濃度で1.0以上の画像濃度を得るためには、カップリングにより生成する色素のεが5000〜500000程度のカプラーの場合、塗布量として0.001〜100ミリモル/m2程度、好ましくは0.01〜10ミリモル/m2、さらに好ましくは0.05〜5ミリモル/m2程度が適当である。
【0121】
現像主薬の添加量は広い範囲を持つが、好ましくはカプラーに対して0.01〜100モル倍、さらに好ましくは0.1〜10モル倍が適当である。
【0122】
混色防止用に使用する中間層のカプラーの添加量は、全現像主薬に対して0.001〜100モル倍、さらに好ましくは0.05〜50モル倍が適当である。
【0123】
本発明のカラー感光材料は、基本的には支持体上に感光性ハロゲン化銀、色素供与性化合物としてカプラー、還元剤、バインダーを有するものであり、さらに必要に応じて有機金属塩酸化剤などを含有させることができる。これらの成分は同一の層に添加することが多いが、反応可能な状態であれば別層に分割して添加することができる。
【0124】
本発明では感光性乳剤層は少なくとも2層以上、支持体上に塗設されており、各々の乳剤層の間には実質的に非感光性中間層を有しており、乳剤層はそれぞれ異なる波長域に分光感度を有している。
イエロー、マゼンタ、シアンの3原色を用いて色度図上の広範囲の色を得るためには、少なくとも3層のそれぞれ異なるスペクトル領域に感光性を持つハロゲン化銀乳剤層を組み合わせて用いる。たとえば青感層、緑感層、赤感層の3層、緑感層、赤感層、赤外感層の組み合わせなどがある。各感光層は通常のカラー感光材料で知られている種々の配列順序を採ることができる。また、これらの各感光層は必要に応じて2層以上に分割してもよい。
【0125】
感光材料には、感光層及び中間層以外に保護層、下塗り層、アンチハレーション層、バック層等の種々の補助層を設けることができる。さらに色分離性を改良するために種々のフィルター染料を添加することもできる。
【0126】
一般に写真感材の処理においては塩基を必要とするが、本発明の感材においては、さまざまな塩基供給方法が採用できる。例えば、感材側に塩基発生機能を与える場合、塩基プレカーサーとして感光材料中に導入することが可能である。このような塩基プレカーサーとしては、例えば熱により脱炭酸する有機酸と塩基の塩、分子内求核置換反応、ロッセン転位またはベックマン転位によりアミン類を放出する化合物などがある。この例については、米国特許第4514493号、同4657848号等に記載されている。
【0127】
また、感材と処理シートを重ね合わせて処理する形態を用いる場合、処理シート中に塩基または塩基プレカーサーを導入する方法も使用することができる。この場合の塩基としては、無機塩基のほかにアミン誘導体のような有機塩基を使用することもできる。
【0128】
さらに感材側と処理シート側それぞれに塩基プレカーサーを含有させ、2者の反応によって塩基を発生させる反応も利用可能である。このような2剤反応型の塩基発生方法の例としては、例えば難溶性塩基性金属塩とキレート剤の反応によるものや、求核剤とエポキシ化合物の反応によるもの等が利用可能である。この例については、特開昭63−198050号等に記載がある。
この場合、感材と処理シートの間に少量の溶媒(水など)を含ませた状態で加熱しても良い。この溶媒の付与方法は後述する。また、この溶媒としては極性の液体、特に水が好ましい。
【0129】
本発明の感光材料の支持体としては、当該分野、特に熱現像感光材料の支持体として公知のものを使用することができる。このような支持体としては、例えばポリエチレンでラミネートした紙支持体、ポリエチレンテレフタレート、ポリエチレンナフタレートに代表されるポリエステル支持体等を挙げることができる。このような支持体の例としては、特開昭63−189860号にその詳細な記載がある。
【0130】
本発明の感光材料の支持体には、上記に挙げたもののほかに、シンジオタクチック構造を有するスチレン系重合体ポリマーを延伸した支持体も好ましく使用できる。このポリマー支持体は、既述のものと同様、単独重合体でも、共重合体でもよい。このようなポリマー支持体については、特願平7−45079号にその詳細な記載がある。
【0131】
本発明で使用するハロゲン化銀乳剤は、表面潜像型乳剤であっても、内部潜像型乳剤であってもよい。内部潜像型乳剤は造核剤や光カブラセとを組合わせて直接反転乳剤として使用される。また、粒子内部と粒子表層が異なる相を持ったいわゆるコアシェル乳剤であってもよく、またエピタキシャル接合によって組成の異なるハロゲン化銀が接合されていても良い。ハロゲン化銀乳剤は単分散でも多分散でもよく、特開平1−167,743号、同4−223,463号記載のように単分散乳剤を混合し、階調を調節する方法が好ましく用いられる。粒子サイズは0.1〜2μm、特に0.2〜1.5μmが好ましい。ハロゲン化銀粒子の晶癖は立方体、8面体、14面体のような規則的な結晶を有するもの、球状、高アスペクト比の平板状のような変則的な結晶系を有するもの、双晶面のような結晶欠陥を有するもの、あるいはそれらの複合系その他のいずれでもよい。
具体的には、米国特許第4,500,626号第50欄、同4,628,021号、リサーチ・ディスクロージャー誌(以下RDと略記する)No. 17,029(1978年)、同No. 17,643(1978年12月)22〜23頁、同No. 18,716(1979年11月)648頁、同No. 307,105(1989年11月)863〜865頁、特開昭62−253,159号、同64−13,546号、特開平2−236,546号、同3−110,555号、およびグラフキデ著「写真の物理と化学」、ポールモンテル社刊(F. Glafkides, Chemie et Phisique Photographique, Paul Montel, 1967) 、ダフィン著「写真乳剤化学」、フォーカルプレス社刊(G. F. Duffin, Photographic Emulsion Chemistry, Focal Press, 1966)、ゼリクマンら著「写真乳剤の製造と塗布」、フォーカルプレス社刊(V. L. Zelikman et al., Making and Coating Photographic Emulsion, Focal Press, 1964)等に記載されている方法を用いて調製したハロゲン化銀乳剤のいずれもが使用できる。
【0132】
本発明の感光性ハロゲン化銀乳剤を調製する過程で、過剰の塩を除去するいわゆる脱塩を行うことが好ましい。このための手段として、ゼラチンをゲル化させて行うヌーデル水洗法を用いても良く、また多価アニオンより成る無機塩類(例えば硫酸ナトリウム)、アニオン性界面活性剤、アニオン性ポリマー(例えばポリスチレンスルホン酸ナトリウム)、あるいはゼラチン誘導体(例えば脂肪族アシル化ゼラチン、芳香族アシル化ゼラチン、芳香族カルバモイル化ゼラチンなど)を利用した沈降法を用いても良い。沈降法が好ましく用いられる。
【0133】
本発明で使用する感光性ハロゲン化銀乳剤は、種々の目的でイリジウム、ロジウム、白金、カドミウム、亜鉛、タリウム、鉛、鉄、オスミウムなどの重金属を含有させても良い。これらの化合物は、単独で用いても良いしまた2種以上組み合わせて用いても良い。添加量は、使用する目的によるが一般的には、ハロゲン化銀1モルあたり10-9〜10-3モル程度である。また含有させる時には、粒子に均一に入れてもよいし、また粒子の内部や表面に局在させてもよい。具体的には、特開平2−236,542号、同1−116,637号、同5−181246号等に記載の乳剤が好ましく用いられる。
【0134】
本発明の感光性ハロゲン化銀乳剤の粒子形成段階において、ハロゲン化銀溶剤としてロダン塩、アンモニア、4置換チオエーテル化合物や特公昭47−11,386号記載の有機チオエーテル誘導体または特開昭53−144,319号に記載されている含硫黄化合物等を用いることができる。
【0135】
その他の条件については、前記のグラフキデ著「写真の物理と化学」、ポールモンテル社刊(F. Glafkides, Chemie et Phisique photographique, Paul Montel, 1967)、ダフィン著「写真乳剤化学」、フォーカルプレス社刊(G. F. Duffin, Photographic Emulsion Chemistry, Focal Press, 1966)、ゼリクマンら著「写真乳剤の製造と塗布」、フォーカルプレス社刊(V. L. Zelikman et al., Making and Coating Photographic Emulsion, Focal Press, 1964)等の記載を参照すれば良い。すなわち酸性法、中性法、アンモニア法のいずれでもよく、また可溶性銀塩と可溶性ハロゲン塩を反応させる形式としては片側混合法、同時混合法、それらの組み合わせのいずれを用いてもよい。単分散乳剤を得るためには、同時混合法が好ましく用いられる。
粒子を銀イオン過剰の下において形成させる逆混合法も用いることができる。同時混合法の一つの形式としてハロゲン化銀の生成される液相中のpAgを一定に保つ、いわゆるコントロールドダブルジェット法も用いることができる。
【0136】
また、粒子成長を早めるために、添加する銀塩およびハロゲン塩の添加濃度、添加量、添加速度を上昇させてもよい(特開昭55−142,329号、同55−158,124号、米国特許第3650757号等)。
さらに反応液の攪拌方法は、公知のいずれの攪拌方法でもよい。またハロゲン化銀粒子形成中の反応液の温度、pHは、目的に応じてどのように設定してもよい。好ましいpH範囲は2.2〜8.5、より好ましくは2.5〜7.5である。
【0137】
感光性ハロゲン化銀乳剤は通常は化学増感されたハロゲン化銀乳剤である。本発明の感光性ハロゲン化銀乳剤の化学増感には、通常型感光材料用乳剤で公知の硫黄増感法、セレン増感法、テルル増感法などのカルコゲン増感法、金、白金、パラジウムなどを用いる貴金属増感法および還元増感法などを単独または組合わせて用いることができる(例えば特開平3−110,555号、同5−241267号など)。これらの化学増感を含窒素複素環化合物の存在下で行うこともできる(特開昭62−253,159号)。また後掲するかぶり防止剤を化学増感終了後に添加することができる。具体的には、特開平5−45,833号、特開昭62−40,446号記載の方法も用いることができる。
化学増感時のpHは好ましくは5.3〜10.5、より好ましくは5.5〜8.5であり、pAgは好ましくは6.0〜10.5、より好ましくは6.8〜9.0である。
本発明において使用される感光性ハロゲン化銀乳剤の塗設量は、銀換算1mgないし10g/m2の範囲である。
【0138】
本発明に用いられる感光性ハロゲン化銀に緑感性、赤感性、赤外感性の感色性を持たせるためには、感光性ハロゲン化銀乳剤をメチン色素類その他によって分光増感する。また、必要に応じて青感性乳剤に青色領域の分光増感を施してもよい。
用いられる色素には、シアニン色素、メロシアニン色素、複合シアニン色素、複合メロシアニン色素、ホロポーラーシアニン色素、ヘミシアニン色素、スチリル色素およびヘミオキソノール色素が包含される。
具体的には、米国特許第4,617,257号、特開昭59−180,550号、同64−13,546号、特開平5−45,828号、同5−45,834号などに記載の増感色素が挙げられる。
これらの増感色素は単独に用いてもよいが、それらの組合わせを用いてもよく、増感色素の組合わせは特に、強色増感や分光感度の波長調節の目的でしばしば用いられる。
増感色素とともに、それ自身分光増感作用を持たない色素あるいは可視光を実質的に吸収しない化合物であって、強色増感を示す化合物を乳剤中に含んでもよい(例えば米国特許第3,615,641号、特開昭63−23,145号等に記載のもの)。
これらの増感色素を乳剤中に添加する時期は化学熟成時もしくはその前後でもよいし、米国特許第4,183,756号、同4,225,666号に従ってハロゲン化銀粒子の核形成前後でもよい。またこれらの増感色素や強色増感剤は、メタノールなどの有機溶媒の溶液、ゼラチンなどの分散物あるいは界面活性剤の溶液で添加すればよい。添加量は一般にハロゲン化銀1モル当り10-8ないし10-2モル程度である。
【0139】
このような工程で使用される添加剤および本発明の感光材料や処理シートに使用できる公知の写真用添加剤は、前記のRDNo. 17,643、同No. 18,715および同No. 307,105に記載されており、その該当箇所を下記の表にまとめる。
【0140】
【0141】
感光材料の構成層のバインダーには親水性のものが好ましく用いられる。その例としては前記のリサーチ・ディスクロージャーおよび特開昭64−13,546号の(71)頁〜(75)頁に記載されたものが挙げられる。具体的には、透明か半透明の親水性バインダーが好ましく、例えばゼラチン、ゼラチン誘導体等の蛋白質またはセルロース誘導体、澱粉、アラビアゴム、デキストラン、プルラン等の多糖類のような天然化合物とポリビニールアルコール、ポリビニルピロリドン、アクリルアミド重合体等の合成高分子化合物が挙げられる。また、米国特許第4,960,681号、特開昭62−245,260号等に記載の高吸水性ポリマー、すなわち−COOMまたは−SO3 M(Mは水素原子またはアルカリ金属)を有するビニルモノマーの単独重合体またはこのビニルモノマーどうし、もしくは他のビニルモノマーとの共重合体(例えばメタクリル酸ナトリウム、メタクリル酸アンモニウム、住友化学(株)製のスミカゲルL−5H)も使用される。これらのバインダーは2種以上組み合わせて用いることもできる。特にゼラチンと上記バインダーの組み合わせが好ましい。またゼラチンは、種々の目的に応じて石灰処理ゼラチン、酸処理ゼラチン、カルシウムなどの含有量を減らしたいわゆる脱灰ゼラチンから選択すれば良く、組み合わせて用いることも好ましい。
【0142】
本発明においては、感光性ハロゲン化銀乳剤と共に、有機金属塩を酸化剤として併用することもできる。このような有機金属塩の中で、有機銀塩は、特に好ましく用いられる。
上記の有機銀塩酸化剤を形成するのに使用し得る有機化合物としては、米国特許第4,500,626号第52〜53欄等に記載のベンゾトリアゾール類、脂肪酸その他の化合物がある。また米国特許第4,775,613号記載のアセチレン銀も有用である。有機銀塩は、2種以上を併用してもよい。
以上の有機銀塩は、感光性ハロゲン化銀1モルあたり、0.01〜10モル、好ましくは0.01〜1モルを併用することができる。感光性ハロゲン化銀乳剤と有機銀塩の塗布量合計は銀換算で0.05〜10g/m2、好ましくは0.1〜4g/m2が適当である。
本発明の感光材料には、現像の活性化と同時に画像の安定化を図る化合物を用いることができる。好ましく用いられる具体的化合物については米国特許第4,500,626号の第51〜52欄に記載されている。また、特願平6−206331号に記載されているような、ハロゲン化銀を定着し得る化合物を使用することもできる。
【0143】
感光材料の構成層に用いる硬膜剤としては、前記リサーチ・ディスクロージャー、米国特許第4,678,739号第41欄、同4,791,042号、特開昭59−116,655号、同62−245,261号、同61−18,942号、特開平4−218,044号等に記載の硬膜剤が挙げられる。より具体的には、アルデヒド系硬膜剤(ホルムアルデヒドなど)、アジリジン系硬膜剤、エポキシ系硬膜剤、ビニルスルホン系硬膜剤(N,N′−エチレン−ビス(ビニルスルホニルアセタミド)エタンなど)、N−メチロール系硬膜剤(ジメチロール尿素など)、あるいは高分子硬膜剤(特開昭62−234,157号などに記載の化合物)が挙げられる。
これらの硬膜剤は、塗布されたゼラチン1gあたり0.001〜1g、好ましくは0.005〜0.5gが用いられる。また添加する層は、感光材料や色素固定材料の構成層のいずれの層でも良いし、2層以上に分割して添加しても良い。
【0144】
感光材料の構成層には、種々のカブリ防止剤または写真安定剤およびそれらのプレカーサーを使用することができる。その具体例としては、前記リサーチ・ディスクロージャー、米国特許第5,089,378号、同4,500,627号、同4,614,702号、特開昭64−13,546号(7)〜(9)頁、(57)〜(71)頁および(81)〜(97)頁、米国特許第4,775,610号、同4,626,500号、同4,983,494号、特開昭62−174,747号、同62−239,148号、同63−264,747号、特開平1−150,135号、同2−110,557号、同2−178,650号、RD17,643(1978年)(24)〜(25)頁等記載の化合物が挙げられる。
これらの化合物は、銀1モルあたり5×10-6〜1×10-1モルが好ましく、さらに1×10-5〜1×10-2モルが好ましく用いられる。
【0145】
感光材料の構成層には、塗布助剤、剥離性改良、スベリ性改良、帯電防止、現像促進等の目的で種々の界面活性剤を使用することができる。界面活性剤の具体例は前記リサーチ・ディスクロージャー、特開昭62−173,463号、同62−183,457号等に記載されている。
熱現像感光材料の構成層には、スベリ性改良、帯電防止、剥離性改良等の目的で有機フルオロ化合物を含ませてもよい。有機フルオロ化合物の代表例としては、特公昭57−9053号第8〜17欄、特開昭61−20944号、同62−135826号等に記載されているフッ素系界面活性剤、またはフッ素油などのオイル状フッ素系化合物もしくは四フッ化エチレン樹脂などの固体状フッ素化合物樹脂などの疎水性フッ素化合物が挙げられる。
【0146】
感光材料には、接着防止、スベリ性改良、非光沢面化などの目的でマット剤を用いることができる。マット剤としては二酸化ケイ素、ポリオレフィンまたはポリメタクリレートなどの特開昭61−88256号(29)頁記載の化合物の他に、ベンゾグアナミン樹脂ビーズ、ポリカーボネート樹脂ビーズ、AS樹脂ビーズなどの特開昭63−274944号、同63−274952号記載の化合物がある。その他前記リサーチ・ディスクロージャー記載の化合物が使用できる。これらのマット剤は、最上層(保護層)のみならず必要に応じて下層に添加することもできる。
その他、感光材料の構成層には、熱溶剤、消泡剤、防菌防バイ剤、コロイダルシリカ等を含ませてもよい。これらの添加剤の具体例は特開昭61−88256号第(26)〜(32)頁、特開平3−11,338号、特公平2−51,496号等に記載されている。
【0147】
本発明において感光材料には画像形成促進剤を用いることができる。画像形成促進剤には銀塩酸化剤と還元剤との酸化還元反応の促進、色素生成反応の促進等の機能があり、物理化学的な機能からは塩基または塩基プレカーサー、求核性化合物、高沸点有機溶媒(オイル)、熱溶剤、界面活性剤、銀または銀イオンと相互作用を持つ化合物等に分類される。ただし、これらの物質群は一般に複合機能を有しており、上記の促進効果のいくつかを合せ持つのが常である。これらの詳細については米国特許4,678,739号第38〜40欄に記載されている。
【0148】
本発明において熱現像感光材料には、現像時の処理温度および処理時間の変動に対し、常に一定の画像を得る目的で種々の現像停止剤を用いることができる。ここでいう現像停止剤とは、適正現像後、速やかに塩基を中和または塩基と反応して膜中の塩基濃度を下げ現像を停止する化合物または銀および銀塩と相互作用して現像を抑制する化合物である。具体的には、加熱により酸を放出する酸プレカーサー、加熱により共存する塩基と置換反応を起す親電子化合物、または含窒素ヘテロ環化合物、メルカプト化合物及びその前駆体等が挙げられる。更に詳しくは特開昭62−253,159号(31)〜(32)頁に記載されている。
【0149】
感光材料に画像を露光し記録する方法としては、例えばカメラなどを用いて風景や人物などを直接撮影する方法、プリンターや引伸機などを用いてリバーサルフィルムやネガフィルムを通して露光する方法、複写機の露光装置などを用いて、原画をスリットなどを通して走査露光する方法、画像情報を電気信号を経由して発光ダイオード、各種レーザー(レーザーダイオード、ガスレーザーなど)などを発光させ走査露光する方法(特開平2−129,625号、同5−176144号、同5−199372号、同6−127021号、等に記載の方法)、画像情報をCRT、液晶ディスプレイ、エレクトロルミネッセンスディスプレイ、プラズマディスプレイなどの画像表示装置に出力し、直接または光学系を介して露光する方法などがある。
【0150】
感光材料へ画像を記録する光源としては、上記のように、自然光、タングステンランプ、発光ダイオード、レーザー光源、CRT光源などの米国特許第4,500,626号第56欄、特開平2−53,378号、同2−54,672号記載の光源や露光方法を用いることができる。
また、非線形光学材料とレーザー光等のコヒーレントな光源を組み合わせた波長変換素子を用いて画像露光することもできる。ここで非線形光学材料とは、レーザー光のような強い光電界をあたえたときに現れる分極と電界との間の非線形性を発現可能な材料であり、ニオブ酸リチウム、リン酸二水素カリウム(KDP)、沃素酸リチウム、BaB2 O4 などに代表される無機化合物や、尿素誘導体、ニトロアニリン誘導体、例えば3−メチル−4−ニトロピリジン−N−オキシド(POM)のようなニトロピリジン−N−オキシド誘導体、特開昭61−53462号、同62−210432号に記載の化合物が好ましく用いられる。波長変換素子の形態としては、単結晶光導波路型、ファイバー型等が知られておりそのいずれもが有用である。
また、前記の画像情報は、ビデオカメラ、電子スチルカメラ等から得られる画像信号、日本テレビジョン信号規格(NTSC)に代表されるテレビ信号、原画をスキャナーなど多数の画素に分割して得た画像信号、CG、CADで代表されるコンピューターを用いて作成された画像信号を利用できる。
【0151】
本発明の感光材料を加熱現像で処理する場合、加熱現像のための加熱手段として導電性の発熱体層を有する形態であっても良い。この場合の発熱要素には、特開昭61−145,544号等に記載のものを利用できる。
熱現像工程での加熱温度は、約80℃〜180℃であり、加熱時間は0.1秒〜60秒である。
【0152】
現像工程における加熱方法としては、加熱されたブロックやプレートに接触させたり、熱板、ホットプレッサー、熱ローラー、熱ドラム、ハロゲンランプヒーター、赤外および遠赤外ランプヒーターなどに接触させたり、高温の雰囲気中を通過させる方法などがある。
感光材料と処理シートを重ね合わせる方法は特開昭62−253,159号、特開昭61−147,244号(27)頁記載の方法が適用できる。
【0153】
以下、実施例によって本発明を詳しく説明する。
【0154】
【実施例】
実施例1
<感光性ハロゲン化銀乳剤の調製方法>
良く攪拌しているゼラチン水溶液(水1000ml中に不活性ゼラチン30g、臭化カリウム2g)に、溶剤としてアンモニア・硝酸アンモニウムを溶剤として加えて75℃に保温し、ここに硝酸銀1モルを含む水溶液1000mlと、臭化カリウム1モルと沃化カリウム0.03モルを含む水溶液1000mlを78分かけて同時に添加した。水洗、脱塩の後、不活性ゼラチンを加えて再分散し、球相当径0.76μのヨード含有率3モル%の沃臭化銀乳剤を調製した。球相当径は、コールターカウンター社のモデルTA−IIで測定した。
上記乳剤に、56℃でチオシアン酸カリウム、塩化金酸、チオ硫酸ナトリウムを添加し、最適に化学増感した。この乳剤に各分光感度に相当する増感色素を、塗布液調液時に添加して感色性を与えた。
【0155】
<水酸化亜鉛分散物の調製方法>
一次粒子の粒子サイズが0.2μmの水酸化亜鉛の粉末31g、分散剤としてカルボキシメチルセルロース1.6gおよびポリアクリル酸ソーダ0.4g、石灰処理オセインゼラチン8.5g、水158.5mlを混合し、この混合物をガラスビーズを用いたミルで1時間分散した。分散後、ガラスビーズを濾別し、水酸化亜鉛の分散物188gを得た。
【0156】
<カプラーの乳化分散物の調製方法>
表1に示す組成の油相成分、水相成分をそれぞれ溶解し、60℃の均一な溶液とする。油相成分と水相成分を合わせ、1リットルのステンレス容器中で、直径5cmのディスパーサーのついたディゾルバーにより、10000 rpmで20分間分散した。これに、後加水として、表1に示す量の温水を加え、2000 rpmで10分間混合した。このようにして、シアン、マゼンタ、イエロー3色のカプラーの乳化分散物を調製した。
【0157】
【表1】
【0158】
【化71】
【0159】
【化72】
【0160】
このようにして得られた素材を用いて、表2、3に示す多層構成の熱現像カラー感光材料101を作製した。
【0161】
【表2】
【0162】
【表3】
【0163】
【化73】
【0164】
【化74】
【0165】
【化75】
【0166】
さらに、表4、5に示す内容の処理材料R−1を作製した。
【0167】
【表4】
【0168】
【表5】
【0169】
【表6】
【0170】
【化76】
【0171】
【化77】
【0172】
次に、表7に示すとおりに、各層のカプラーおよび現像主薬を101に対して等モル置き換えるように変更し、中間層に素材を添加した以外は、101と全く同じ組成の感光材料102〜120をそれぞれ作製した。このようにしてできた感光材料101〜120に連続的に濃度の変化したB、G、R、グレーのフィルターを通して2500 luxで0.01秒露光した。この露光済の感材面に40℃の温水を15ml/m2付与し、処理シートと互いの膜面同志を重ね合わせた後、ヒートドラムを用いて83℃で30秒間熱現像した。処理後受像材料を剥離すると、感材側に露光したフィルターに対応して、シアン、マゼンタ、イエロー、グレーのカラー画像が鮮明に得られた。処理直後にこのサンプルの各単色露光部のDmax ならびに白地部のDmin の濃度をX−rite濃測機で測定した結果を表8に示す。
【0173】
【表7】
【0174】
【化78】
【0175】
【化79】
【0176】
【表8】
【0177】
表8の結果をまとめると、まず、比較例サンプル101〜108では、画像に混色による色濁りが認められる。また、中間層に還元剤を添加したサンプル(109〜112)では、混色は軽減されるがDmax の低下が認められる。これに対して本発明のサンプル(113〜120)ではDmax が保たれたまま混色も軽減される。以上により本発明の効果は明らかである。
【0178】
実施例2
次に表9、10に示す多層構成の熱現像カラー感光材料201を作製した。
【0179】
【表9】
【0180】
【表10】
【0181】
【化80】
【0182】
【化81】
【0183】
次に、表11に示すとおりに、各層のカプラーおよび現像主薬を201に対して等モル置き換えるように変更し、中間層に素材を添加した以外は、201と全く同じ組成の感光材料202〜220をそれぞれ作製した。このようにしてできた感光材料201〜220に連続的に濃度の変化したB、G、R、グレーのフィルターを通して2500 luxで0.01秒露光した。この露光済の感材面に40℃の温水を15ml/m2付与し、処理シートと互いの膜面同志を重ね合わせた後、ヒートドラムを用いて83℃で30秒間熱現像した。処理後受像材料を剥離すると、感材側に露光したフィルターに対応して、シアン、マゼンタ、イエロー、グレーのカラー画像が鮮明に得られた。処理直後にこのサンプルの各単色露光部のDmax ならびに白地部のDmin の濃度をX−rite濃測機で測定した結果を表12に示す。
【0184】
【表11】
【0185】
【化82】
【0186】
【化83】
【0187】
【表12】
【0188】
表12の結果をまとめると、まず、比較例サンプル201〜208では、101の時と同様、画像に混色による色濁りが認められる。また、中間層に還元剤を添加したサンプル(209〜212)では、混色は軽減されるがDmax の低下が認められる。これに対して本発明のサンプル(213〜220)ではDmax が保たれたまま混色も軽減される。本実施例からも、本発明の効果は明らかである。
【0189】
【発明の効果】
最大発色濃度を高いまま、混色を低減することができる。[0001]
BACKGROUND OF THE INVENTION
The present invention relates to a heat-developable color light-sensitive material, and more particularly to a heat-developable color light-sensitive material excellent in image discrimination and color reproducibility.
[0002]
[Prior art]
A photographic method using silver halide has been used most widely in the past because it is superior in photographic characteristics such as sensitivity and gradation adjustment compared to other photographic methods such as electrophotography and diazo photography. In particular, since it is possible to obtain the best image quality as a color hard copy, it has been energetically studied more recently.
[0003]
In recent years, image formation processing methods for photosensitive materials using silver halide have been changed from conventional wet processing to instant photo systems with a built-in developer, and further to dry thermal development processing by heating, etc. Systems have been developed that can obtain The details of the photothermographic materials are described in “Basics of Photographic Engineering (Non-Silver Photo Edition) Corona Publishing, 1982” p.242. It remains in the image forming method. Recently, as photothermographic materials, Fuji Photo Film Co., Ltd. has released products such as pictography and pictrostat. In the above simple and rapid processing method, color image formation is performed using a redox color material connected with a preformed die. As a method for forming a color image of a photographic light-sensitive material, a method utilizing a coupling reaction between a coupler and an oxidized color developing agent is the most general. A heat-developable color light-sensitive material employing this method is also disclosed in US Pat. , 761,270, 4,021,240, and Japanese Patent Application Laid-Open No. 59-231539.
[0004]
The inventors have also studied the above-mentioned coupling-type heat-developable color photosensitive material. However, when creating a multi-layered color photosensitive material containing a developing agent, an oxidized form of the developing agent moves to another photosensitive layer. Problem arises. When the oxidized oxidant of the developing agent moves to another photosensitive layer and undergoes a coupling reaction there, a dye is produced in a layer that should not develop color, and this color turbidity impairs the color reproducibility of the image. become. In order to avoid this in the prior art, a method is known in which a non-photosensitive intermediate layer is provided between adjacent photosensitive layers, and the oxidized oxidized developer is deactivated by a chemical reaction in the intermediate layer. ing. As a specific method, firstly, a method is known in which another kind of reducing agent is contained in the intermediate layer, and the oxidized developer is returned to the original developing agent by a cross-oxidation reaction therewith. However, in this method, since the developing agent is regenerated and silver development is performed again, the consumption of base increases. In the processing mode considered in the present invention, since the amount of base is finite, when the consumption of the base due to crosstalk occurs in this way, the Dmax of the image decreases. Therefore, it was found that this method is difficult to adopt. As another method, a technique is known in which a coupler which forms a substantially colorless compound by coupling reaction with an oxidized form of a developing agent in an intermediate layer is known. As such a compound, for example, there is a method of introducing a non-leaving substituent into the site of a usual coupler leaving group. Examples of couplers into which such a substituent is introduced include, for example, 49-84439. However, it has been found that when such a coupler is used in the system of the present invention, a sufficient color mixing prevention effect cannot be obtained.
[0005]
[Problems to be solved by the invention]
An object of the present invention is to provide a heat-developable color photographic material having a high maximum density, excellent discrimination, and color reproducibility.
[0006]
[Means for Solving the Problems]
The object of the present invention has been achieved by the following heat developable color light-sensitive material.
[0007]
1) At least two or more photosensitive emulsion layers containing at least photosensitive silver halide, a binder, a coupler and a developing agent are coated on a support, each having spectral sensitivity in different wavelength regions. In a heat-developable color light-sensitive material having at least one substantially non-light-sensitive intermediate layer between each light-sensitive emulsion layer,The coupler contained in the photosensitive emulsion layer is a 4-equivalent coupler, and the developing agent is a compound represented by the following general formula (1), (2) or (3), and at least the intermediate layer A heat-developable color light-sensitive material comprising a 2-equivalent coupler in one layer.
[0008]
oneGeneral formula (1)
[0009]
[Chemical 6]
[0010]
General formula (2)
[0011]
[Chemical 7]
[0012]
General formula (3)
[0013]
[Chemical 8]
[0014]
Where R1~ RFourIs a hydrogen atom, halogen atom, alkyl group, aryl group, alkylcarbonamide group, arylcarbonamide group, alkylsulfonamide group, arylsulfonamide group, alkoxy group, aryloxy group, alkylthio group, arylthio group, alkylcarbamoyl group, Arylcarbamoyl group, carbamoyl group, alkylsulfamoyl group, arylsulfamoyl group, sulfamoyl group, cyano group, alkylsulfonyl group, arylsulfonyl group, alkoxycarbonyl group, aryloxycarbonyl group, alkylcarbonyl group, arylcarbonyl group or Represents an acyloxy group, RFiveRepresents an alkyl group, an aryl group or a heterocyclic group. Z represents an atomic group forming an aromatic ring (including a heteroaromatic ring). When Z is a benzene ring, the total value of Hammett constants (σ) of the substituents is 1 or more. R6Represents an alkyl group. X represents an oxygen atom, a sulfur atom, a selenium atom or a tertiary nitrogen atom (alkyl-substituted). R7And R8Each represents a hydrogen atom or a substituent, and R7And R8May be bonded to each other to form a double bond or a ring.
[0015]
2) At least two or more photosensitive emulsion layers containing at least photosensitive silver halide, a binder, a coupler and a developing agent are coated on the support, each having spectral sensitivity in a different wavelength region, In a heat developable color light-sensitive material having at least one substantially non-light-sensitive intermediate layer between each light-sensitive emulsion layer, the coupler contained in the light-sensitive emulsion layer is a 2-equivalent coupler, and A photothermographic material, wherein the developing agent is a compound represented by the following general formula (4) or (5), and at least one of the intermediate layers contains a 4-equivalent coupler.
General formula (4)
[0016]
[Chemical 9]
[0017]
General formula (5)
[0018]
[Chemical Formula 10]
[0019]
Where RFive~ R8, X, Z are the same as those in general formula (2) or (3).
[0020]
DETAILED DESCRIPTION OF THE INVENTION
The present invention is described in detail below.
The final goal of the technique of the present invention is to prevent the oxidant of the developing agent from diffusing into each other between the layers of the photosensitive emulsion, so that no color mixing reaction occurs. In the present invention, for the purpose of improving gradation and granularity of gradation of an image, a layer containing silver halide grains having the same spectral sensitivity and different grain sizes is divided into several layers. It is possible to form a single photosensitive emulsion layer. In the present invention, an intermediate layer is provided between the light-sensitive emulsion layers, and a coupler that does not develop color but undergoes a coupling reaction with an oxidized form of the developing agent used in the present invention.
[0021]
The developing agent preferably used in the present invention is characterized by having a leaving group at the coupling site. For this reason, for example, in the developing agents of the general formulas (1) to (3), a color image is formed with a 4-equivalent coupler, but a color image is not formed with a 2-equivalent coupler. In this case, when a 2-equivalent coupler is added to the intermediate layer in the light-sensitive material system using the developing agents of the general formulas (1) to (3), the purpose of preventing color mixing can be efficiently achieved. Conversely, the developing agents of general formulas (4) and (5) form a color image only with a 2-equivalent coupler. Accordingly, it is effective to use a 4-equivalent coupler in the intermediate layer in the light-sensitive material system using the developing agents of the general formulas (4) and (5).
[0022]
The compound represented by the general formula (1) is a compound generically called sulfonamidophenol.
[0023]
Where R1~ RFourIs a hydrogen atom, a halogen atom (for example, chloro atom, bromine atom), a substituted or unsubstituted alkyl group (for example, methyl group, ethyl group, isopropyl group, n-butyl group, t-butyl group), substituted or unsubstituted aryl group Groups (eg phenyl, tolyl, xylyl), substituted or unsubstituted alkylcarbonamide groups (eg acetylamino, propionylamino, butyroylamino), substituted or unsubstituted arylcarbonamide groups (eg benzoyl) Amino group), substituted or unsubstituted alkylsulfonamide group (for example, methanesulfonylamino group, ethanesulfonylamino group), substituted or unsubstituted arylsulfonamide group (for example, benzenesulfonylamino group, toluenesulfonylamino group), substituted or Unsubstituted alkoxy group (for example, methoxy group, Toxyl group, butoxy group), substituted or unsubstituted aryloxy group (for example, phenoxy group), substituted or unsubstituted alkylthio group (for example, methylthio group, ethylthio group, butylthio group), substituted or unsubstituted arylthio group (for example, phenylthio group) Group, tolylthio group), substituted or unsubstituted alkylcarbamoyl group (for example, methylcarbamoyl group, dimethylcarbamoyl group, ethylcarbamoyl group, diethylcarbamoyl group, dibutylcarbamoyl group, piperidylcarbamoyl group, morpholylcarbamoyl group), substituted or unsubstituted Arylcarbamoyl group (for example, phenylcarbamoyl group, methylphenylcarbamoyl group, ethylphenylcarbamoyl group, benzylphenylcarbamoyl group), carbamoyl group, substituted or unsubstituted alkylsulfamoy Group (for example, methylsulfamoyl group, dimethylsulfamoyl group, ethylsulfamoyl group, diethylsulfamoyl group, dibutylsulfamoyl group, piperidylsulfamoyl group, morpholylsulfamoyl group), substituted or non-substituted Substituted arylsulfamoyl group (eg phenylsulfamoyl group, methylphenylsulfamoyl group, ethylphenylsulfamoyl group, benzylphenylsulfamoyl group), sulfamoyl group, cyano group, substituted or unsubstituted alkylsulfonyl Group (for example, methanesulfonyl group, ethanesulfonyl group), substituted or unsubstituted arylsulfonyl group (for example, phenylsulfonyl group, 4-chlorophenylsulfonyl group, p-toluenesulfonyl group), substituted or unsubstituted alkoxycarbonyl group (for example, methoxycarbyl group) Bonyl group, ethoxycarbonyl group, butoxycarbonyl group), substituted or unsubstituted aryloxycarbonyl group (for example, phenoxycarbonyl group), substituted or unsubstituted alkylcarbonyl group (for example, acetyl group, propionyl group, butyroyl group), substituted or It represents an unsubstituted arylcarbonyl group (for example, benzoyl group, alkylbenzoyl group) or a substituted or unsubstituted acyloxy group (for example, acetyloxy group, propionyloxy group, butyroyloxy group). R1~ RFourIn R2And RFourIs preferably a hydrogen atom. R1~ RFourThe total Hammett substituent constant (σ value) is preferably 0 or more. RFiveIs a substituted or unsubstituted alkyl group (for example, methyl group, ethyl group, butyl group, octyl group, lauryl group, cetyl group, stearyl group), substituted or unsubstituted aryl group (for example, phenyl group, tolyl group, xylyl group, 4-methoxyphenyl group, dodecylphenyl group, chlorophenyl group, trichlorophenyl group, nitrochlorophenyl group, triisopropylphenyl group, 4-dodecyloxyphenyl group, 3,5-di- (methoxycarbonyl) group), or substituted or non-substituted Represents a substituted heterocyclic group (for example, a pyridyl group).
[0024]
The compound represented by the general formula (2) is a compound generically called sulfonyl hydrazine. Further, the compound represented by the general formula (4) is a compound generically called carbamoylhydrazine.
[0025]
In formula, Z represents the atomic group which forms an aromatic ring. The aromatic ring formed by Z needs to be sufficiently electron withdrawing in order to impart silver developing activity to the present compound. For this reason, an aromatic ring in which a nitrogen-containing aromatic ring is formed or an electron-withdrawing group is introduced into a benzene ring is preferably used. As such an aromatic ring, a pyridine ring, a pyrazine ring, a pyrimidine ring, a quinoline ring, a quinoxaline ring and the like are preferable. In the case of a benzene ring, examples of the substituent include alkylsulfonyl groups (for example, methanesulfonyl group and ethanesulfonyl group), halogen atoms (for example, chloro group and bromo group), alkylcarbamoyl groups (for example, methylcarbamoyl group, dimethylcarbamoyl group, ethyl). Carbamoyl group, diethylcarbamoyl group, dibutylcarbamoyl group, piperidylcarbamoyl group, morpholylcarbamoyl group), arylcarbamoyl group (eg phenylcarbamoyl group, methylphenylcarbamoyl group, ethylphenylcarbamoyl group, benzylphenylcarbamoyl group), carbamoyl group, alkyl Sulfamoyl group (for example, methylsulfamoyl group, dimethylsulfamoyl group, ethylsulfamoyl group, diethylsulfamoyl group, dibutylsulfamoyl group) Group, piperidylsulfamoyl group, morpholylsulfamoyl group), arylsulfamoyl group (for example, phenylsulfamoyl group, methylphenylsulfamoyl group, ethylphenylsulfamoyl group, benzylphenylsulfamoyl group) , Sulfamoyl group, cyano group, alkylsulfonyl group (for example, methanesulfonyl group, ethanesulfonyl group), arylsulfonyl group (for example, phenylsulfonyl group, 4-chlorophenylsulfonyl group, p-toluenesulfonyl group), alkoxycarbonyl group (for example, methoxycarbonyl) Group, ethoxycarbonyl group, butoxycarbonyl group), aryloxycarbonyl group (for example, phenoxycarbonyl group), alkylcarbonyl group (for example, acetyl group, propionyl group, butyroyl group), or Reel carbonyl group (e.g. a benzoyl group, an alkyl benzoyl group), but like, Hammett total substituent constant (sigma value) of the substituent is preferably made 1 or more.
[0026]
The compound represented by the general formula (3) is a compound generically called sulfonyl hydrazone. Further, the compound represented by the general formula (5) is a compound generically called carbamoylhydrazone.
[0027]
Where R6Represents a substituted or unsubstituted alkyl group (for example, a methyl group or an ethyl group). X represents an oxygen atom, a sulfur atom, a selenium atom or a tertiary nitrogen atom (alkyl-substituted), and an alkyl-substituted tertiary nitrogen atom is preferred. R7And R8Each represents a hydrogen atom or a substituent, and R7And R8May bond to each other to form a double bond or a ring (for example, a benzene ring or a pyridine ring). R7, R8As a substituent of R,1~ RFourA group other than a hydrogen atom in can be preferably mentioned.
[0028]
Specific examples of the compounds represented by the general formulas (1) to (5) are shown below, but the compounds of the present invention are not limited thereto.
[0029]
Embedded image
[0030]
Embedded image
[0031]
Embedded image
[0032]
Embedded image
[0033]
Embedded image
[0034]
Embedded image
[0035]
Embedded image
[0036]
Embedded image
[0037]
Embedded image
[0038]
Embedded image
[0039]
Embedded image
[0040]
Embedded image
[0041]
The above compounds can be synthesized by generally known methods. The following is a list of simple synthesis routes.
[0042]
Embedded image
[0043]
Embedded image
[0044]
Embedded image
[0045]
In the present invention, a compound (coupler) that forms a dye by an oxidative coupling reaction is used as the dye-donating compound. As this coupler, in the present invention, a 4-equivalent coupler and a 2-equivalent coupler are selectively used depending on the kind of the main agent. First, a 4-equivalent coupler is used for the developing agents of the general formulas (1) to (3). In the developing agents represented by the general formulas (1) to (3), the coupling site is substituted with a sulfonyl group, and at the time of coupling, the sulfonyl group is released by sulfinic acid. Because we have to leave. For this reason, it reacts with a 4-equivalent coupler capable of releasing a proton as a leaving group during coupling, and develops color. However, a 2-equivalent coupler whose leaving group is an anion reacts but does not develop color. On the contrary, 2 equivalent couplers are used for the developing agents of the general formulas (4) and (5). In the developing agents of the general formulas (4) and (5), the coupling site is substituted with a carbamoyl group, and the hydrogen atom on the nitrogen atom is released as a proton during coupling, so the leaving group on the coupler side is an anion. Because we have to leave. For this reason, it reacts with a 2-equivalent coupler capable of releasing an anion as a leaving group at the time of coupling, but develops color, but a 4-equivalent coupler whose leaving group is a proton reacts but does not develop color. Specific examples of couplers include both 4-equivalent and 2-equivalent theories of the photographic process (4th. Ed. TH James Edited by McMillan, 1977) pages 291-334, and pages 354-361. Pages, JP-A-58-12353, 58-149046, 58-149047, 59-11114, 59-124399, 59-174835, 59-231539, 59-231540. No. 60-2951, No. 60-14242, No. 60-23474, No. 60-66249, and the like.
[0046]
Examples of couplers preferably used in the present invention are listed below.
[0047]
Couplers preferably used in the present invention include compounds having structures as described in the following general formulas (6) to (17). Each of these is a compound known in the art.
[0048]
Embedded image
[0049]
Embedded image
[0050]
Embedded image
[0051]
General formulas (6) to (9) represent couplers called active methylene couplers, in which Rtwenty fourIs a substituted or unsubstituted acyl group, cyano group, nitro group, substituted or unsubstituted aryl group, substituted or unsubstituted heterocyclic group, substituted or unsubstituted alkoxycarbonyl group, substituted or unsubstituted aryloxycarbonyl group Carbamoyl group, sulfamoyl group, substituted or unsubstituted alkylsulfonyl group, substituted or unsubstituted arylsulfonyl group.
[0052]
In the general formulas (6) to (9), Rtwenty fiveIs a substituted or unsubstituted alkyl group, a substituted or unsubstituted aryl group or a substituted or unsubstituted heterocyclic group. In the general formula (9), R26Is a substituted or unsubstituted aryl group or a substituted or unsubstituted heterocyclic group. Rtwenty four, Rtwenty five, R26Examples of the substituent which may have include an alkyl group, an alkenyl group, an alkynyl group, an aryl group, a heterocyclic group, an alkoxy group, an aryloxy group, a cyano group, a halogen atom, an acylamino group, a sulfonamide group, and a carbamoyl group. And various substituents such as a sulfamoyl group, an alkoxycarbonyl group, an aryloxycarbonyl group, an alkylamino group, an arylamino group, a hydroxyl group, and a sulfo group. Rtwenty fourPreferred examples of these include a substituted or unsubstituted acyl group, a cyano group, a carbamoyl group, and a substituted or unsubstituted alkoxycarbonyl group.
[0053]
In the general formulas (6) to (9), Y is a group capable of leaving by a coupling reaction with a hydrogen atom or an oxidized form of a developing agent. Examples of Y include a group that acts as an anionic leaving group of a 2-equivalent coupler, such as a halogen atom (for example, chloro, bromo), an alkoxy group (for example, methoxy group, ethoxy group), an aryloxy group (for example, phenoxy group, 4- Cyanophenoxy group, 4-alkoxycarbonylphenyl group), alkylthio group (for example, methylthio group, ethylthio group, butylthio group), arylthio group (for example, phenylthio group, tolylthio group), alkylcarbamoyl group (for example, methylcarbamoyl group, dimethylcarbamoyl group), Ethylcarbamoyl group, diethylcarbamoyl group, dibutylcarbamoyl group, piperidylcarbamoyl group, morpholylcarbamoyl group), arylcarbamoyl group (eg phenylcarbamoyl group, methylphenylcarbamoyl group, ethyl Phenylcarbamoyl group, benzylphenylcarbamoyl group), carbamoyl group, alkylsulfamoyl group (for example, methylsulfamoyl group, dimethylsulfamoyl group, ethylsulfamoyl group, diethylsulfamoyl group, dibutylsulfamoyl group, Piperidylsulfamoyl group, morpholylsulfamoyl group), arylsulfamoyl group (eg phenylsulfamoyl group, methylphenylsulfamoyl group, ethylphenylsulfamoyl group, benzylphenylsulfamoyl group), sulfamoyl Group, cyano group, alkylsulfonyl group (for example, methanesulfonyl group, ethanesulfonyl group), arylsulfonyl group (for example, phenylsulfonyl group, 4-chlorophenylsulfonyl group, p-toluenesulfonyl group), alkyl group Bonyloxy group (for example, acetyloxy group, propionyloxy group, butyroyloxy group), arylcarbonyloxy group (for example, benzoyloxy group, toluyloxy group, anisyloxy group), nitrogen-containing heterocyclic group (for example, imidazolyl group, benzotriazolyl group) Etc.
[0054]
Further, as a group that acts as a cationic leaving group of the 4-equivalent coupler, a hydrogen atom, a formyl group, a carbamoyl group, a methylene group having a substituent (substituents include an aryl group, a sulfamoyl group, a carbamoyl group, an alkoxy group Amino group, hydroxyl group and the like), acyl group, sulfonyl group and the like.
[0055]
In the general formulas (6) to (9), Rtwenty fourAnd Rtwenty five, Rtwenty fourAnd R26May combine with each other to form a ring.
[0056]
The general formula (10) represents a coupler called a 5-pyrazolone-based magenta coupler, in which R27Each represents a substituted or unsubstituted alkyl group, aryl group, acyl group or carbamoyl group. R28Represents a phenyl group or a phenyl group substituted by one or more halogen atoms, alkyl groups, cyano groups, alkoxy groups, alkoxycarbonyl groups or acylamino groups. Y is the same as in the general formulas (6) to (9).
[0057]
Among the 5-pyrazolone-based magenta couplers represented by the general formula (10), R27Is an aryl group or an acyl group, R28Is preferably a phenyl group substituted with one or more halogen atoms.
[0058]
These preferred groups will be described in detail.27Is phenyl, 2-chlorophenyl, 2-methoxyphenyl, 2-chloro-5-tetradecanamidophenyl, 2-chloro-5- (3-octadecenyl-1-succinimide) phenyl, 2-chloro-5-octadecylsulfonamidophenyl or An aryl group such as 2-chloro-5- [2- (4-hydroxy-3-t-butylphenoxy) tetradecanamido] phenyl, or acetyl, pivaloyl, tetradecanoyl, 2- (2,4-di-t- Pentylphenoxy) acetyl, 2- (2,4-di-t-pentylphenoxy) butanoyl, benzoyl, 3- (2,4-di-t-amylphenoxyacetazido) benzoyl and the like, and these groups May further have a substituent, which may be a carbon atom, an oxygen atom, a nitrogen atom, or an ion. It is an organic substituent or a halogen atom which is linked with atoms.
[0059]
R28Is preferably a substituted phenyl group such as 2,4,6-trichlorophenyl, 2,5-dichlorophenyl or 2-chlorophenyl group.
[0060]
The general formula (11) represents a coupler called a pyrazoloazole coupler, in which R29Represents a hydrogen atom or a substituent. Z represents a group of nonmetallic atoms necessary for forming a 5-membered azole ring containing 2 to 4 nitrogen atoms, and the azole ring may have a substituent (including a condensed ring). Y is the same as in the general formulas (6) to (9).
[0061]
Among the pyrazoloazole couplers represented by the general formula (11), imidazo [1,2-b] pyrazoles described in U.S. Pat. No. 4,500,560 and U.S. Pat. Pyrazolo [1,5-b] [1,2,4] triazoles described in US Pat. No. 3,725,067 and pyrazolo [5,1-c] [1,2,4] triazoles described in US Pat. Of these, pyrazolo [1,5-b] [1,2,4] triazoles are preferable in terms of fastness.
[0062]
Substituent R29Details of the substituents of the azole ring represented by Y, Z and Z are described, for example, in US Pat. No. 4,540,654, column 2, line 41 to column 8, line 27. Preferably, a pyrazoloazole coupler in which a branched alkyl group as described in JP-A-61-65245 is directly linked to the 2,3 or 6-position of the pyrazolotriazole group, described in JP-A-61-65245 A pyrazoloazole coupler having a sulfonamide group in the molecule, a pyrazoloazole coupler having an alkoxyphenylsulfonamide ballast group described in JP-A No. 61-147254, JP-A No. 62-209457 or 63- These are pyrazolotriazole couplers having an alkoxy group or aryloxy group at the 6-position described in No. 307453, and pyrazolotriazole couplers having a carbonamide group in the molecule described in Japanese Patent Application No. 1-2279.
[0063]
General formulas (12) and (13) are couplers called phenol couplers and naphthol couplers, respectively.30Is a hydrogen atom or -NHCOR32, -SO2NR32R33, -NHSO2R32,-NHCOR32,-NHCONR32R33, -NHSO2NR32R33Represents a group selected from: R32, R33Represents a hydrogen atom or a substituent. In the general formulas (12) and (13), R31Represents a substituent, l represents an integer selected from 0 to 2, and m represents an integer selected from 0 to 4. Y is the same as in the general formulas (6) to (9). R31~ R33As said Rtwenty four~ R26And those mentioned as the substituents of.
[0064]
Preferable examples of the phenolic coupler represented by the general formula (12) include those described in U.S. Pat. Nos. 2,369,929, 2,801,171, 2,772,162, 2,895,826, and 3,777,2002. Alkylamino-5-alkylphenol series, U.S. Pat. Nos. 2,772,162, 3,758,308, 4,126,396, 4,334,411, 4,327,173, West German Patent Publication 3,329,729, Japanese Patent Laid-Open No. Sho 59-166756, etc. 2,5-diacylaminophenol-based compounds described in U.S. Pat. Nos. 3,446,622, 4,333,999, 4,451,559, 4,427,767, etc. Can do.
[0065]
Preferred examples of the naphthol coupler represented by the general formula (13) include 2-carbamoyl- described in US Pat. Nos. 2,474,293, 4,522,212, 4,146,396, 4,228,233, 4,296,200, Examples thereof include 1-naphthol series and 2-carbamoyl-5-amido-1-naphthol series described in US Pat. No. 4,690,889.
[0066]
Formulas (14) to (17) are couplers called pyrrolotriazole, and R42, R43,R44Represents a hydrogen atom or a substituent. Y is the same as in the general formulas (6) to (9). R42, R43,R44As the substituent of R,twenty four~ R26And those mentioned as the substituents of. Preferable examples of the pyrrolotriazole couplers represented by the general formulas (14) to (17) include R described in European Patent Nos. 488248A1, 491197A1, and 545300.42, R43And couplers in which at least one of them is an electron withdrawing group.
[0067]
In addition, couplers having a structure such as condensed phenol, imidazole, pyrrole, 3-hydroxypyridine, active methine, 5,5-condensed heterocyclic ring, and 5,6-condensed heterocyclic ring can be used.
[0068]
As the condensed phenol-based couplers, couplers described in U.S. Pat. Nos. 4,327,173, 4,564,586 and 4,904,575 can be used.
[0069]
As the imidazole couplers, couplers described in U.S. Pat. Nos. 4,818,672 and 5,051,347 can be used.
[0070]
As pyrrole couplers, couplers described in JP-A-4-188137, JP-A-4-190347 and the like can be used.
[0071]
As the 3-hydroxypyridine couplers, those described in JP-A-1-315736 can be used.
[0072]
As active methine couplers, couplers described in US Pat. Nos. 5,104,783 and 5,162,196 can be used.
[0073]
As 5,5-condensed heterocyclic couplers, pyrrolopyrazole couplers described in US Pat. No. 5,164,289, pyrroloimidazole couplers described in JP-A-4-174429, and the like can be used.
[0074]
Examples of the 5,6-condensed heterocyclic coupler include pyrazolopyrimidine couplers described in US Pat. No. 4,950,585, pyrrolotriazine couplers described in JP-A-4-204730, and couplers described in EP 556700. Etc. can be used.
[0075]
In addition to the couplers described above, the present invention includes West German Patent Nos. 3819051A, 3823049, U.S. Pat. Nos. 4,840,883, 5024930, 5051347, 4481268, European Patent No. 308856A2, No. 329036, No. 354549A2, No. 374781A2, No. 379110A2, No. 386930A1, JP-A-63-141055, No. 64-32260, No. 32261, JP-A-2-297547, No. 2 -44340, 2-110555, 3-7938, 3-160440, 3-17239, 4-172447, 4-179949, 4-182645, 4-184437 No., 4-188138, 4-188139, 4-1948 No. 7, the same 4-204532 Patent, the 4-204731 Patent, couplers as described in the 4-204732 Patent like can be used.
[0076]
Specific examples of couplers that can be used in the present invention are shown below. As described above, the 4-equivalent coupler is used for image formation in combination with the compounds of the general formulas (1) to (3) as a developing agent. Conversely, when the compounds of general formulas (4) and (5) are used as the developing agent, they can be used as color mixing inhibitors. The 2-equivalent coupler is used for image formation in combination with the compounds of the general formulas (4) and (5) as a developing agent. Conversely, when the compounds of general formulas (1) to (3) are used as developing agents, they can be used as color mixing inhibitors. Of course, the present invention is not limited by the following compound examples.
[0077]
Embedded image
[0078]
Embedded image
[0079]
Embedded image
[0080]
Embedded image
[0081]
Embedded image
[0082]
Embedded image
[0083]
Embedded image
[0084]
Embedded image
[0085]
Embedded image
[0086]
Embedded image
[0087]
Embedded image
[0088]
Embedded image
[0089]
Embedded image
[0090]
Embedded image
[0091]
Embedded image
[0092]
Embedded image
[0093]
Embedded image
[0094]
Embedded image
[0095]
Embedded image
[0096]
Embedded image
[0097]
Embedded image
[0098]
Embedded image
[0099]
Embedded image
[0100]
Embedded image
[0101]
Embedded image
[0102]
Embedded image
[0103]
Embedded image
[0104]
Embedded image
[0105]
Embedded image
[0106]
Embedded image
[0107]
Embedded image
[0108]
Embedded image
[0109]
Embedded image
[0110]
Embedded image
[0111]
Embedded image
[0112]
Embedded image
[0113]
Embedded image
[0114]
Embedded image
[0115]
Embedded image
[0116]
Embedded image
[0117]
Embedded image
[0118]
Embedded image
[0119]
As a method of adding a developing agent and a coupler, first, a coupler, a developing agent, and a high boiling point organic solvent (for example, phosphoric acid alkyl ester, phthalic acid alkyl ester, etc.) are mixed and a low boiling point organic solvent (for example, ethyl acetate, methyl ethyl ketone, etc.) And can be added after being dispersed in water using an emulsification dispersion method known in the art. Further, addition by a solid dispersion method described in JP-A-63-271339 is also possible.
[0120]
The amount of coupler added to the emulsion layer depends on its molar extinction coefficient (ε), but in order to obtain an image density of 1.0 or more in reflection density, the dye produced by coupling has an ε of about 5000 to 500,000. In the case of a coupler of 0.001 to 100 mmol / m as a coating amount2Degree, preferably 0.01 to 10 mmol / m2More preferably 0.05 to 5 mmol / m2The degree is appropriate.
[0121]
The addition amount of the developing agent has a wide range, but is preferably 0.01 to 100 moles, more preferably 0.1 to 10 moles, with respect to the coupler.
[0122]
The addition amount of the intermediate layer coupler used for preventing color mixing is suitably 0.001 to 100 mol times, more preferably 0.05 to 50 mol times with respect to the total developing agent.
[0123]
The color light-sensitive material of the present invention basically has a light-sensitive silver halide on the support, a coupler, a reducing agent, and a binder as a dye-donating compound. Can be contained. These components are often added to the same layer, but can be added separately in separate layers as long as they can react.
[0124]
In the present invention, at least two photosensitive emulsion layers are coated on the support, and each emulsion layer has a substantially non-photosensitive intermediate layer, and each emulsion layer is different. Has spectral sensitivity in the wavelength range.
In order to obtain a wide range of colors on the chromaticity diagram using the three primary colors of yellow, magenta, and cyan, at least three silver halide emulsion layers having sensitivity in different spectral regions are used in combination. For example, there are a blue-sensitive layer, a green-sensitive layer, and a red-sensitive layer, a green-sensitive layer, a red-sensitive layer, and an infrared-sensitive layer. Each photosensitive layer can take various arrangement sequences known in ordinary color photosensitive materials. Each of these photosensitive layers may be divided into two or more layers as necessary.
[0125]
The photosensitive material can be provided with various auxiliary layers such as a protective layer, an undercoat layer, an antihalation layer, and a back layer in addition to the photosensitive layer and the intermediate layer. Further, various filter dyes can be added to improve color separation.
[0126]
In general, a base is required in the processing of a photographic material, but various base supply methods can be employed in the photosensitive material of the present invention. For example, when a base generating function is given to the photosensitive material side, it can be introduced into the photosensitive material as a base precursor. Examples of such base precursors include salts of organic acids and bases that are decarboxylated by heat, compounds that release amines by intramolecular nucleophilic substitution reaction, Rossen rearrangement or Beckmann rearrangement, and the like. This example is described in US Pat. Nos. 4,514,493 and 4,657,848.
[0127]
Moreover, when using the form which superimposes and processes a photosensitive material and a processing sheet, the method of introduce | transducing a base or a base precursor into a processing sheet can also be used. As the base in this case, an organic base such as an amine derivative can be used in addition to the inorganic base.
[0128]
Furthermore, it is also possible to use a reaction in which a base precursor is contained on each of the light-sensitive material side and the treatment sheet side and a base is generated by a two-way reaction. As an example of such a two-agent reaction type base generation method, for example, a method by reaction of a hardly soluble basic metal salt and a chelating agent, a method by reaction of a nucleophile and an epoxy compound, or the like can be used. This example is described in JP-A No. 63-198050.
In this case, heating may be performed in a state where a small amount of solvent (water or the like) is included between the photosensitive material and the treatment sheet. A method for applying this solvent will be described later. The solvent is preferably a polar liquid, particularly water.
[0129]
As the support for the photosensitive material of the present invention, those known in the art, particularly as a support for the photothermographic material, can be used. Examples of such a support include a paper support laminated with polyethylene, a polyethylene support represented by polyethylene terephthalate, and polyethylene naphthalate. Examples of such a support are described in detail in JP-A No. 63-189860.
[0130]
In addition to the materials listed above, a support obtained by stretching a styrene polymer polymer having a syndiotactic structure can also be preferably used as the support for the photosensitive material of the present invention. This polymer support may be a homopolymer or a copolymer as described above. Such a polymer support is described in detail in Japanese Patent Application No. 7-45079.
[0131]
The silver halide emulsion used in the present invention may be a surface latent image type emulsion or an internal latent image type emulsion. The internal latent image type emulsion is used as a direct reversal emulsion in combination with a nucleating agent and optical fogging. Further, it may be a so-called core-shell emulsion in which the inside of the grain and the grain surface layer have different phases, and silver halides having different compositions may be joined by epitaxial joining. The silver halide emulsion may be monodispersed or polydispersed, and a method of adjusting the gradation by mixing monodispersed emulsions as described in JP-A-1-167,743 and 4-223,463 is preferably used. . The particle size is preferably 0.1 to 2 μm, particularly preferably 0.2 to 1.5 μm. The crystal habits of silver halide grains are those having regular crystals such as cubes, octahedrons, and tetrahedrons, those having irregular crystal systems such as spherical and high aspect ratio flat plate shapes, and those having twin planes. Any of those having such crystal defects or a composite system thereof may be used.
Specifically, U.S. Pat. No. 4,500,626, column 50, 4,628,021, Research Disclosure (hereinafter abbreviated as RD) No. 17,029 (1978), ibid. 17, 643 (December 1978) 22-23, No. 18,716 (November 1979) 648, No. 307,105 (November 1989) 863-865, JP-A-62. -253,159, 64-133,546, JP-A-2-236,546, 3-110,555, and Grafkide's "Physics and Chemistry of Photography", published by Paul Monter (F. Glafkides) , Chemie et Phisique Photographique, Paul Montel, 1967), “Photographic Emulsion Chemistry” by Duffin, published by Focal Press (GF Duffin, Photographic Emulsion Chemistry, Focal Press, 1966). Cloth ", Focal Press, published (V. L. Zelikman et al., Making and Coating Photographic Emulsion, Focal Press, 1964) none of the silver halide emulsion prepared using methods described in the like can be used.
[0132]
In the process of preparing the photosensitive silver halide emulsion of the present invention, it is preferable to carry out so-called desalting to remove excess salt. As a means for this, a Nudell water washing method in which gelatin is gelled may be used, and inorganic salts (for example, sodium sulfate) composed of polyvalent anions, anionic surfactants, anionic polymers (for example, polystyrene sulfonic acid) Sodium), or a precipitation method using gelatin derivatives (eg, aliphatic acylated gelatin, aromatic acylated gelatin, aromatic carbamoylated gelatin, etc.) may be used. A sedimentation method is preferably used.
[0133]
The photosensitive silver halide emulsion used in the present invention may contain heavy metals such as iridium, rhodium, platinum, cadmium, zinc, thallium, lead, iron and osmium for various purposes. These compounds may be used alone or in combination of two or more. The amount added depends on the intended use, but is generally 10 per mole of silver halide.-9-10-3It is about a mole. Moreover, when making it contain, you may put in a particle | grain uniformly and you may make it local in the inside and surface of particle | grains. Specifically, emulsions described in JP-A Nos. 2-236542, 1-116,637, and 5-181246 are preferably used.
[0134]
In the grain formation stage of the photosensitive silver halide emulsion of the present invention, a rhodan salt, ammonia, a tetrasubstituted thioether compound, an organic thioether derivative described in JP-B-47-11386, or JP-A-53-144 is used as a silver halide solvent. , 319, and the like can be used.
[0135]
For other conditions, Grafkide, "Physics and Chemistry of Photography", published by Paul Monter (F. Glafkides, Chemie et Phisique photographique, Paul Montel, 1967), Duffin's "Photoemulsion Chemistry", published by Focal Press (GF Duffin, Photographic Emulsion Chemistry, Focal Press, 1966), “Production and coating of photographic emulsion” by Zerikman et al., Published by Focal Press (VL Zelikman et al., Making and Coating Photographic Emulsion, Focal Press, 1964), etc. Refer to the description. That is, any of an acidic method, a neutral method, and an ammonia method may be used, and any one of a one-side mixing method, a simultaneous mixing method, and a combination thereof may be used as a form for reacting a soluble silver salt and a soluble halogen salt. In order to obtain a monodisperse emulsion, a simultaneous mixing method is preferably used.
A backmixing method in which grains are formed in the presence of excess silver ions can also be used. As one type of the simultaneous mixing method, a so-called controlled double jet method in which pAg in a liquid phase in which silver halide is generated is kept constant can be used.
[0136]
Further, in order to accelerate grain growth, the addition concentration, addition amount, and addition rate of silver salt and halogen salt to be added may be increased (Japanese Patent Laid-Open Nos. 55-142,329 and 55-158,124, U.S. Pat. No. 3,650,757).
Furthermore, the stirring method of the reaction solution may be any known stirring method. Further, the temperature and pH of the reaction solution during the formation of silver halide grains may be set in any manner according to the purpose. The preferred pH range is 2.2 to 8.5, more preferably 2.5 to 7.5.
[0137]
The photosensitive silver halide emulsion is usually a chemically sensitized silver halide emulsion. For the chemical sensitization of the photosensitive silver halide emulsion of the present invention, known chalcogen sensitizing methods such as sulfur sensitizing method, selenium sensitizing method, tellurium sensitizing method, gold, platinum, A noble metal sensitization method using palladium or the like, a reduction sensitization method, or the like can be used alone or in combination (for example, JP-A-3-110,555 and JP-A-5-241267). These chemical sensitizations can also be performed in the presence of a nitrogen-containing heterocyclic compound (Japanese Patent Laid-Open No. 62-253,159). Further, the antifoggant described later can be added after the chemical sensitization is completed. Specifically, methods described in JP-A Nos. 5-45,833 and 62-40,446 can also be used.
The pH during chemical sensitization is preferably 5.3 to 10.5, more preferably 5.5 to 8.5, and the pAg is preferably 6.0 to 10.5, more preferably 6.8 to 9 .0.
The coating amount of the photosensitive silver halide emulsion used in the present invention is 1 mg to 10 g / m in terms of silver.2Range.
[0138]
In order to give the photosensitive silver halide used in the present invention green sensitivity, red sensitivity, and infrared sensitivity, the photosensitive silver halide emulsion is spectrally sensitized with methine dyes and the like. If necessary, the blue-sensitive emulsion may be spectrally sensitized in the blue region.
The dyes used include cyanine dyes, merocyanine dyes, complex cyanine dyes, complex merocyanine dyes, holopolar cyanine dyes, hemicyanine dyes, styryl dyes and hemioxonol dyes.
Specifically, US Pat. No. 4,617,257, JP-A-59-180,550, JP-A-64-13,546, JP-A-5-45,828, JP-A-5-45,834, etc. And sensitizing dyes described in the above.
These sensitizing dyes may be used alone, or a combination thereof may be used, and the combination of sensitizing dyes is often used for the purpose of supersensitization or wavelength adjustment of spectral sensitivity.
In addition to the sensitizing dye, a dye that does not itself have spectral sensitizing action or a compound that does not substantially absorb visible light and exhibits supersensitization may be contained in the emulsion (for example, US Pat. 615,641, JP-A-63-23,145, etc.).
These sensitizing dyes may be added to the emulsion during or after chemical ripening, or before or after nucleation of silver halide grains according to US Pat. Nos. 4,183,756 and 4,225,666. Good. These sensitizing dyes and supersensitizers may be added in a solution of an organic solvent such as methanol, a dispersion such as gelatin, or a surfactant solution. The amount added is generally 10 per mole of silver halide.-810-2It is about a mole.
[0139]
Additives used in such a process and known photographic additives that can be used in the light-sensitive material and processing sheet of the present invention are RD No. 17,643, No. 18,715, and No. 307, respectively. 105, and the corresponding parts are summarized in the following table.
[0140]
[0141]
A hydrophilic material is preferably used for the binder of the constituent layer of the photosensitive material. Examples thereof include those described in Research Disclosure and pages (71) to (75) of JP-A-64-13546. Specifically, transparent or translucent hydrophilic binders are preferable, for example, proteins such as gelatin and gelatin derivatives or cellulose derivatives, natural compounds such as polysaccharides such as starch, gum arabic, dextran and pullulan, and polyvinyl alcohol, Examples thereof include synthetic polymer compounds such as polyvinyl pyrrolidone and acrylamide polymers. Also, superabsorbent polymers described in US Pat. No. 4,960,681, JP-A-62-245260, etc., that is, —COOM or —SO.ThreeHomopolymers of vinyl monomers having M (M is a hydrogen atom or an alkali metal), copolymers of these vinyl monomers, or copolymers with other vinyl monomers (for example, sodium methacrylate, ammonium methacrylate, manufactured by Sumitomo Chemical Co., Ltd.) Sumikagel L-5H) is also used. Two or more of these binders can be used in combination. In particular, a combination of gelatin and the above binder is preferable. The gelatin may be selected from so-called demineralized gelatin in which the content of lime-processed gelatin, acid-processed gelatin, calcium, etc. is reduced according to various purposes, and is preferably used in combination.
[0142]
In the present invention, an organic metal salt can be used as an oxidizing agent in combination with the photosensitive silver halide emulsion. Among such organometallic salts, organic silver salts are particularly preferably used.
Organic compounds that can be used to form the organic silver salt oxidizing agent include benzotriazoles, fatty acids and other compounds described in US Pat. No. 4,500,626, columns 52-53. Acetylene silver described in US Pat. No. 4,775,613 is also useful. Two or more organic silver salts may be used in combination.
The above organic silver salt can be used in an amount of 0.01 to 10 mol, preferably 0.01 to 1 mol, per mol of photosensitive silver halide. The total coating amount of photosensitive silver halide emulsion and organic silver salt is 0.05 to 10 g / m in terms of silver.2, Preferably 0.1 to 4 g / m2Is appropriate.
In the light-sensitive material of the present invention, a compound capable of stabilizing the image simultaneously with activation of development can be used. Specific compounds preferably used are described in columns 51 to 52 of US Pat. No. 4,500,626. A compound capable of fixing silver halide as described in Japanese Patent Application No. 6-206331 can also be used.
[0143]
As the hardener used for the constituent layer of the photosensitive material, the above-mentioned Research Disclosure, US Pat. No. 4,678,739, column 41, 4,791,042, JP-A-59-116,655, Examples thereof include hardeners described in 62-245,261, 61-18,942, and JP-A-4-218044. More specifically, aldehyde hardeners (formaldehyde, etc.), aziridine hardeners, epoxy hardeners, vinyl sulfone hardeners (N, N'-ethylene-bis (vinylsulfonylacetamide) Ethane, etc.), N-methylol hardeners (dimethylolurea, etc.), or polymer hardeners (compounds described in JP-A-62-234157, etc.).
These hardeners are used in an amount of 0.001 to 1 g, preferably 0.005 to 0.5 g, per 1 g of coated gelatin. Further, the layer to be added may be any of the constituent layers of the photosensitive material and the dye fixing material, or may be added in two or more layers.
[0144]
Various anti-fogging agents or photographic stabilizers and their precursors can be used in the constituent layers of the light-sensitive material. Specific examples thereof include the Research Disclosure, U.S. Pat. Nos. 5,089,378, 4,500,627, 4,614,702, and JP-A-64-13546 (7)- (9), (57) to (71) and (81) to (97), U.S. Pat. Nos. 4,775,610, 4,626,500, 4,983,494, Kaisho 62-174,747, 62-239,148, 63-264,747, JP-A-1-150,135, 2-110,557, 2-178,650, RD17,643 (1978) (24)-(25) pages etc. are mentioned.
These compounds are 5 × 10 5 per mole of silver.-6~ 1x10-1Moles are preferred, further 1 × 10-Five~ 1x10-2Mole is preferably used.
[0145]
In the constituent layers of the photosensitive material, various surfactants can be used for the purposes of coating aid, improvement of peelability, improvement of slipping property, antistatic, development promotion and the like. Specific examples of the surfactant are described in Research Disclosure, JP-A Nos. 62-173,463 and 62-183,457.
The constituent layer of the photothermographic material may contain an organic fluoro compound for the purpose of improving slipperiness, preventing static charge, and improving peelability. Representative examples of organic fluoro compounds include fluorine surfactants described in JP-B-57-9053, columns 8 to 17, JP-A-61-20944, 62-135826, and fluorine oil. And hydrophobic fluorine compounds such as oily fluorine compounds or solid fluorine compound resins such as tetrafluoroethylene resin.
[0146]
A matting agent can be used for the photosensitive material for the purpose of preventing adhesion, improving slipperiness, and making it non-glossy. As the matting agent, in addition to the compounds described on page 29 of JP-A-61-88256 such as silicon dioxide, polyolefin or polymethacrylate, JP-A-63-274944 such as benzoguanamine resin beads, polycarbonate resin beads and AS resin beads. No. 63-274922. In addition, the compounds described in Research Disclosure can be used. These matting agents can be added not only to the uppermost layer (protective layer) but also to the lower layer as necessary.
In addition, the constituent layer of the light-sensitive material may contain a thermal solvent, an antifoaming agent, an antibacterial and antibacterial agent, colloidal silica, and the like. Specific examples of these additives are described in JP-A-61-88256, pages (26) to (32), JP-A-3-11,338, JP-B-2-51,496, and the like.
[0147]
In the present invention, an image formation accelerator can be used in the photosensitive material. The image formation accelerator has functions such as the promotion of the oxidation-reduction reaction between the silver salt oxidizing agent and the reducing agent, and the promotion of the dye formation reaction. From the physicochemical function, a base or a base precursor, a nucleophilic compound, a high It is classified into a boiling point organic solvent (oil), a thermal solvent, a surfactant, a compound having an interaction with silver or silver ions, and the like. However, these substance groups generally have a composite function, and usually have some of the above-mentioned promoting effects. Details of these are described in U.S. Pat. No. 4,678,739, columns 38-40.
[0148]
In the present invention, various development stoppers can be used in the photothermographic material for the purpose of always obtaining a constant image with respect to variations in processing temperature and processing time during development. A development terminator here means that after proper development, the base is quickly neutralized or reacted with the base to lower the base concentration in the film and to interact with a compound that stops development, or silver and silver salts to suppress development. It is a compound. Specific examples include an acid precursor that releases an acid upon heating, an electrophilic compound that causes a substitution reaction with a base that coexists upon heating, a nitrogen-containing heterocyclic compound, a mercapto compound, and a precursor thereof. Further details are described in JP-A-62-253159, pages (31) to (32).
[0149]
Examples of methods for exposing and recording an image on a photosensitive material include a method of directly photographing a landscape or a person using a camera, a method of exposing through a reversal film or a negative film using a printer or an enlarger, and a copying machine. A method of scanning exposure of an original image through a slit or the like using an exposure apparatus or the like, and a method of scanning exposure by emitting light from a light emitting diode, various lasers (laser diode, gas laser, etc.) via an electrical signal as image information 2-129,625, 5-176144, 5-199372, 6-127021, etc.), image information such as CRT, liquid crystal display, electroluminescence display, plasma display, etc. Output to the device and expose directly or via an optical system. .
[0150]
As a light source for recording an image on a photosensitive material, as described above, natural light, tungsten lamp, light emitting diode, laser light source, CRT light source, etc., US Pat. No. 4,500,626, column 56, JP-A-2-53, The light sources and exposure methods described in Nos. 378 and 2-54,672 can be used.
In addition, image exposure can be performed using a wavelength conversion element that combines a nonlinear optical material and a coherent light source such as a laser beam. Here, the non-linear optical material is a material capable of expressing non-linearity between polarization and electric field that appears when a strong optical electric field such as laser light is applied, such as lithium niobate, potassium dihydrogen phosphate (KDP). ), Lithium iodate, BaB2OFourInorganic compounds represented by the above, urea derivatives, nitroaniline derivatives, for example, nitropyridine-N-oxide derivatives such as 3-methyl-4-nitropyridine-N-oxide (POM), JP-A-61-53462 The compounds described in JP-A-62-210432 are preferably used. As a form of the wavelength conversion element, a single crystal optical waveguide type, a fiber type and the like are known, and any of them is useful.
The image information includes an image signal obtained from a video camera, an electronic still camera, a television signal typified by the Nippon Television Signal Standard (NTSC), and an image obtained by dividing an original image into a number of pixels such as a scanner. Signals, image signals created using a computer represented by CG and CAD can be used.
[0151]
When the light-sensitive material of the present invention is processed by heat development, a form having a conductive heating element layer as a heating means for heat development may be used. As the heat generating element in this case, those described in JP-A No. 61-145,544 can be used.
The heating temperature in the heat development step is about 80 ° C. to 180 ° C., and the heating time is 0.1 second to 60 seconds.
[0152]
Heating methods in the development process include contact with heated blocks and plates, contact with hot plates, hot presses, heat rollers, heat drums, halogen lamp heaters, infrared and far infrared lamp heaters, etc. There is a method of passing through the atmosphere.
The method described in JP-A-62-253,159 and JP-A-61-147,244 (27) can be applied as a method for superimposing the photosensitive material and the processing sheet.
[0153]
Hereinafter, the present invention will be described in detail by way of examples.
[0154]
【Example】
Example 1
<Preparation method of photosensitive silver halide emulsion>
To a well-stirred aqueous gelatin solution (30 g of inert gelatin in 1000 ml of water and 2 g of potassium bromide), ammonia and ammonium nitrate are added as solvents and kept at 75 ° C., and 1000 ml of an aqueous solution containing 1 mol of silver nitrate Then, 1000 ml of an aqueous solution containing 1 mol of potassium bromide and 0.03 mol of potassium iodide was added simultaneously over 78 minutes. After washing with water and desalting, inert gelatin was added and redispersed to prepare a silver iodobromide emulsion having an equivalent sphere diameter of 0.76 μm and an iodine content of 3 mol%. The equivalent sphere diameter was measured with Coulter Counter Model TA-II.
To the above emulsion, potassium thiocyanate, chloroauric acid, and sodium thiosulfate were added at 56 ° C. for optimum chemical sensitization. To this emulsion, a sensitizing dye corresponding to each spectral sensitivity was added during preparation of the coating solution to give color sensitivity.
[0155]
<Method for preparing zinc hydroxide dispersion>
Mix 31 g of zinc hydroxide powder with a primary particle size of 0.2 μm, 1.6 g of carboxymethylcellulose and 0.4 g of sodium polyacrylate as a dispersant, 8.5 g of lime-processed ossein gelatin, and 158.5 ml of water. This mixture was dispersed for 1 hour in a mill using glass beads. After the dispersion, the glass beads were separated by filtration to obtain 188 g of a dispersion of zinc hydroxide.
[0156]
<Method for preparing emulsified dispersion of coupler>
The oil phase component and the aqueous phase component having the composition shown in Table 1 are dissolved to form a uniform solution at 60 ° C. The oil phase component and the aqueous phase component were combined and dispersed in a 1 liter stainless steel container at 10,000 rpm for 20 minutes by a dissolver with a 5 cm diameter disperser. To this, hot water in the amount shown in Table 1 was added as post-hydration and mixed at 2000 rpm for 10 minutes. Thus, an emulsified dispersion of couplers of three colors, cyan, magenta and yellow, was prepared.
[0157]
[Table 1]
[0158]
Embedded image
[0159]
Embedded image
[0160]
Using the material thus obtained, a heat-developable color photosensitive material 101 having a multilayer structure shown in Tables 2 and 3 was produced.
[0161]
[Table 2]
[0162]
[Table 3]
[0163]
Embedded image
[0164]
Embedded image
[0165]
Embedded image
[0166]
Furthermore, treatment materials R-1 having the contents shown in Tables 4 and 5 were produced.
[0167]
[Table 4]
[0168]
[Table 5]
[0169]
[Table 6]
[0170]
Embedded image
[0171]
Embedded image
[0172]
Next, as shown in Table 7, the photosensitive materials 102 to 120 having the same composition as 101 were used except that the coupler and developing agent in each layer were changed so as to replace equimolar amounts with respect to 101, and the material was added to the intermediate layer. Were prepared respectively. The light-sensitive materials 101 to 120 thus obtained were exposed for 0.01 second at 2500 lux through B, G, R, and gray filters having continuously changed densities. 15 ml / m of 40 ° C. hot water is applied to the exposed photosensitive material surface.2After applying and superimposing the processing sheets and the film surfaces of each other, heat development was performed at 83 ° C. for 30 seconds using a heat drum. When the image-receiving material was peeled off after processing, cyan, magenta, yellow and gray color images were clearly obtained corresponding to the filter exposed on the light-sensitive material side. Table 8 shows the results of measuring the Dmax density of each monochromatic exposure portion and the Dmin density of the white background portion of this sample with an X-rite densitometer immediately after the processing.
[0173]
[Table 7]
[0174]
Embedded image
[0175]
Embedded image
[0176]
[Table 8]
[0177]
When the results of Table 8 are summarized, first, in Comparative Samples 101 to 108, color turbidity due to color mixture is recognized in the image. In the samples (109 to 112) in which a reducing agent is added to the intermediate layer, the color mixing is reduced, but a decrease in Dmax is observed. On the other hand, in the samples (113 to 120) of the present invention, color mixing is reduced while Dmax is maintained. From the above, the effect of the present invention is clear.
[0178]
Example 2
Next, a heat-developable color photosensitive material 201 having a multilayer structure shown in Tables 9 and 10 was produced.
[0179]
[Table 9]
[0180]
[Table 10]
[0181]
Embedded image
[0182]
Embedded image
[0183]
Next, as shown in Table 11, the photosensitive materials 202 to 220 having exactly the same composition as 201 except that the couplers and developing agents in each layer were changed so as to replace equimolar amounts with respect to 201 and the material was added to the intermediate layer. Were prepared respectively. The light-sensitive materials 201 to 220 thus prepared were exposed for 0.01 second at 2500 lux through B, G, R, and gray filters having continuously changed densities. 15 ml / m of 40 ° C. hot water is applied to the exposed photosensitive material surface.2After applying and superimposing the processing sheets and the film surfaces of each other, heat development was performed at 83 ° C. for 30 seconds using a heat drum. When the image-receiving material was peeled off after processing, cyan, magenta, yellow and gray color images were clearly obtained corresponding to the filter exposed on the light-sensitive material side. Table 12 shows the results obtained by measuring the Dmax density of each monochromatic exposure portion and the Dmin density of the white background portion of this sample with an X-rite densitometer immediately after the processing.
[0184]
[Table 11]
[0185]
Embedded image
[0186]
Embedded image
[0187]
[Table 12]
[0188]
To summarize the results in Table 12, first, in Comparative Samples 201 to 208, as in the case of 101, color turbidity due to color mixing is recognized in the image. Further, in the samples (209 to 212) in which the reducing agent is added to the intermediate layer, the color mixing is reduced, but a decrease in Dmax is observed. On the other hand, in the samples (213 to 220) of the present invention, color mixing is reduced while Dmax is maintained. The effect of this invention is clear also from a present Example.
[0189]
【The invention's effect】
Color mixing can be reduced while the maximum color density is kept high.
Claims (2)
一般式(1)
General formula (1)
一般式(4)
General formula (4)