[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP3053231B2 - Inkjet recording sheet - Google Patents

Inkjet recording sheet

Info

Publication number
JP3053231B2
JP3053231B2 JP3047661A JP4766191A JP3053231B2 JP 3053231 B2 JP3053231 B2 JP 3053231B2 JP 3047661 A JP3047661 A JP 3047661A JP 4766191 A JP4766191 A JP 4766191A JP 3053231 B2 JP3053231 B2 JP 3053231B2
Authority
JP
Japan
Prior art keywords
group
recording sheet
parts
support substrate
amino group
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
JP3047661A
Other languages
Japanese (ja)
Other versions
JPH04263984A (en
Inventor
弘年 宮崎
和俊 寺田
真明 衣川
均 丸山
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kuraray Co Ltd
Original Assignee
Kuraray Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kuraray Co Ltd filed Critical Kuraray Co Ltd
Priority to JP3047661A priority Critical patent/JP3053231B2/en
Publication of JPH04263984A publication Critical patent/JPH04263984A/en
Application granted granted Critical
Publication of JP3053231B2 publication Critical patent/JP3053231B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【産業上の利用分野】本発明は、インク吸収性にすぐ
れ、かつ著しく耐水性に優れたインクジェット用記録シ
ートに関する。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to an ink jet recording sheet having excellent ink absorbency and remarkably excellent water resistance.

【0002】[0002]

【従来の技術】インクジェット記録方式は、騒音が少な
いこと、カラー化が容易であること、高速記録が可能で
あること等の理由から、ファクシミリ、オーバーヘッド
プロジェクター(以下、OHPと略記する)用シート、
各種プリンター等への応用が進められている。インクジ
ェット記録方式に使用される被記録材料としては通常紙
が使用されてきたが、記録の高速化あるいは多色化など
記録用シートの性能向上に伴い、インクジェット用記録
シートに対してもより高度な特性が要求されてきてい
る。すなわち、第1にインクの吸収速度が大きいこと、
第2にインクジェットの液滴を吸収した後のインク径が
必要以上に大きくならないこと、第3にインクジェット
用記録シート自身の耐水性が高いことである。従来、こ
れらの要求を満たすため水溶性のインクジェット用イン
クの吸収材として、紙あるいは水溶性樹脂を用いる等の
種々の検討がなされている。しかし、インクの吸収速度
を大きくするとインクドット径が必要以上に大きくなっ
たり、耐水性が著しく低下するなど実用レベルの要求に
は遠く及ばないというのが現状である。
2. Description of the Related Art Ink jet recording systems are known as facsimile and overhead projector (hereinafter abbreviated as OHP) sheets because of their low noise, easy colorization, and high-speed recording.
Applications to various printers and the like are being promoted. Normally, paper has been used as a recording material used in the ink jet recording method.However, with the performance improvement of the recording sheet such as faster recording or multi-color recording, a more advanced paper than the ink jet recording sheet has been used. Characteristics are being demanded. That is, first, the ink absorption speed is high,
Secondly, the ink diameter after absorbing the ink-jet droplets does not become larger than necessary, and thirdly, the water resistance of the ink-jet recording sheet itself is high. In order to satisfy these requirements, various studies have been made to use paper or a water-soluble resin as an absorbent for a water-soluble inkjet ink. However, at present, when the ink absorption speed is increased, the ink dot diameter becomes larger than necessary and the water resistance is remarkably reduced.

【0003】[0003]

【発明が解決しようとする課題】本発明の目的は、前記
のような要求性能を満足させ、特にインク吸収性と耐水
性に優れたインクジェット用記録シートを提供すること
にある。本発明のさらにもう一つの目的は、スライドや
OPHなどの光学機器により記録画像をスクリーン等へ
投影することにより観察に用いるもの、あるいはカラー
ディスプレイ等の透過光観察用に用いることのできる透
明性に優れたインクジェット用記録シートを提供するこ
とにある。
SUMMARY OF THE INVENTION It is an object of the present invention to provide an ink jet recording sheet which satisfies the above-mentioned required performance and is particularly excellent in ink absorbency and water resistance. Still another object of the present invention is to provide a transparency that can be used for observation by projecting a recorded image on a screen or the like by an optical device such as a slide or OPH, or that can be used for transmitted light observation such as a color display. An object of the present invention is to provide an excellent ink jet recording sheet.

【0004】[0004]

【課題を解決するための手段】本発明者等は、上記の問
題点を解決すべく鋭意検討した結果、下記式(I)、(I
I)および(III)から選ばれる少なくとも一種の単量体
とビニルエステルとの共重合体をけん化または加水分解
して得られる分子内に一級アミノ基、一級アンモニウム
塩基、二級アミノ基および二級アンモニウム塩基から選
ばれた少なくとも1種の官能基を有するポリビニルアル
コール(PVA)(A)と多価ジアルデヒド化合物(B)
からなり、成分(A)100重量部に対して成分(B)
1〜50重量部である組成物を支持基体中または支持基
体表面に有するインクジェット用記録シートは、インク
吸収性に優れ、かつ著しく耐水性に優れたインクジェッ
ト用記録シートであることを見出だし、本発明を完成す
るに到ったものである。。
The present inventors have conducted intensive studies to solve the above problems, and as a result, the following formulas (I) and (I)
At least one monomer selected from I) and (III)
Or hydrolysis of copolymers of vinyl and vinyl esters
Polyvinyl alcohol (PVA) (A) having at least one functional group selected from a primary amino group, a primary ammonium group, a secondary amino group and a secondary ammonium group in a molecule obtained by the method and a polyhydric dialdehyde compound (B)
Consisting of 100 parts by weight of component (A) and component (B)
It has been found that an ink jet recording sheet having a composition in an amount of 1 to 50 parts by weight in a support substrate or on the surface of a support substrate is an ink jet recording sheet having excellent ink absorbency and extremely excellent water resistance. The invention has been completed. .

【0005】[0005]

【化4】 Embedded image

【0006】[0006]

【化5】 Embedded image

【0007】[0007]

【化6】 Embedded image

【0008】(ここで、R1は水素原子またはメチル
基、R2は水素原子または低級アルキル基、R3は水素原
子、低級アルキル基、メチロール基またはエチロール
基、nは0〜4の整数、mは2〜4の整数をそれぞれ示
す。)
(Where R 1 is a hydrogen atom or a methyl group, R 2 is a hydrogen atom or a lower alkyl group, R 3 is a hydrogen atom, a lower alkyl group, a methylol group or an ethylol group, n is an integer of 0-4, m shows the integer of 2-4, respectively.)

【0009】以下、本発明について詳細に説明する。本
発明に用いられる分子内に一級アミノ基、一級アンモニ
ウム塩基、二級アミノ基および二級アンモニウム塩基か
ら選ばれた少なくとも1種の官能基を有するPVA
(A)は、上記式(I)、(II)または(III)で表され
単量体とビニルエステルとの共重合体をけん化または
加水分解することにより得られる。PVA(A)の平均
重合度は通常100〜5000、好ましくは200〜2
500から選ばれる。PVA(A)の平均重合度が10
0未満では、バインダーとしての性能、特にフィルム物
性が不足し、5000を越えると溶液粘度が高くなりす
ぎ、作業性の点で好ましくない。PVA(A)の平均け
ん化度は60〜100モル%が好ましい。PVA(A)
の平均けん化度が60モル%未満だと水に溶けにくくな
るため好ましくない。上記のPVA(A)中の一級アミ
ノ基、一級アンモニウム塩基、二級アミノ基または二級
アンモニウム塩基の含有量は、0.05モル%以上であ
れば特に制限はないが、通常0.1〜30モル%の範囲
から選ばれ、好ましくは0.5〜10モル%である。該
アミノ基または該アンモニウム塩基の含有量が0.05
モル%未満の場合には、本発明のインクジェット用記録
シートのインク吸収性の向上および耐水性の向上が得が
たく、また30モル%をこえて更に多い場合にはインク
の吸収速度が低下するので好ましくない。
Hereinafter, the present invention will be described in detail. PVA having at least one functional group selected from a primary amino group, a primary ammonium base, a secondary amino group and a secondary ammonium group in the molecule used in the present invention
(A) is represented by the above formula (I), (II) or (III)
That it is obtained by saponifying or hydrolyzing a copolymer of a monomer with a vinyl ester. The average degree of polymerization of PVA (A) is usually 100 to 5,000, preferably 200 to 2,000.
Selected from 500. The average degree of polymerization of PVA (A) is 10
If it is less than 0, the performance as a binder, particularly the physical properties of the film, is insufficient. If it exceeds 5,000, the solution viscosity becomes too high, which is not preferable in view of workability. The average degree of saponification of PVA (A) is preferably from 60 to 100 mol%. PVA (A)
If the average degree of saponification is less than 60 mol%, it is not preferable because it becomes difficult to dissolve in water. The content of the primary amino group, primary ammonium group, secondary amino group or secondary ammonium group in the PVA (A) is not particularly limited as long as it is 0.05 mol% or more, but is usually 0.1 to 0.1 mol%. It is selected from the range of 30 mol%, and preferably 0.5 to 10 mol%. When the content of the amino group or the ammonium base is 0.05
When the amount is less than mol%, it is difficult to improve the ink absorbency and the water resistance of the ink jet recording sheet of the present invention, and when the amount exceeds 30 mol%, the ink absorption speed decreases. It is not preferable.

【0010】上記の式(I)で表される単量体として
は、ビニルアミンまたはその有機酸あるいは無機酸の
塩、式(II)で表される単量体としては、N−ビニルア
ミド、式(III)で表される単量体としては、N−ビニ
ルイミドなどが挙げられる。
As the monomer represented by the above formula (I),
Is a salt of vinylamine or an organic or inorganic acid thereof, a monomer represented by the formula (II) is N-vinylamide, and a monomer represented by the formula (III) is N-vinylimide. No.

【0011】上記の共重合体を加水分解する触媒として
は酸あるいはアルカリが使用できる。酸触媒を使用する
場合、上記の式(II)あるいは(III)で表される単量
体からなる単位中のアミド基の加水分解によって生成す
るアミノ基は、引き続き酸触媒と反応せしめることによ
りアンモニウム塩基にすることができる。またアルカリ
触媒を使用する場合、上記のアミド基の加水分解によっ
てアミノ基を生成することができ、さらにこれを酸と反
応せしめることによりアンモニウム塩基にすることがで
きる。また該アミノ基または該アンモニウムを含有する
PVA(A)の中でも一級アミノ基または一級アンモニ
ウム塩基を分子内に有するPVAが、インク吸収性およ
び耐水性の点で好ましい。
As a catalyst for hydrolyzing the above copolymer, an acid or an alkali can be used. When an acid catalyst is used, the amino group formed by hydrolysis of the amide group in the unit composed of the monomer represented by the above formula (II) or (III) is reacted with the acid catalyst to form an ammonium group. It can be a base. When an alkali catalyst is used, an amino group can be generated by hydrolysis of the amide group, and the amino group can be converted to an ammonium base by reacting the amino group with an acid. In addition, among PVAs (A) containing the amino group or the ammonium, PVA having a primary amino group or a primary ammonium group in the molecule is preferable in terms of ink absorption and water resistance.

【0012】本発明で用いられる多価ジアルデヒド化合
(B)としては、グリオキザール、グルタルアルデヒ
ド、ジアルデヒドでんぷん等の多価アルデヒド化合物が
挙げられる。なかでもジアルデヒド化合物が該アミノ基
または該アンモニウム基を有するPVAを含む塗工液へ
耐水化剤として添加した時の経時増粘が非常に小さく、
水との副反応による耐水化剤の劣化が小さい点で特に好
ましく用いられる。
Polyhydric dialdehyde compound used in the present invention
Examples of the product (B) include polyhydric aldehyde compounds such as glyoxal, glutaraldehyde, and dialdehyde starch. Above all, when the dialdehyde compound is added as a waterproofing agent to a coating solution containing PVA having the amino group or the ammonium group as a water-resistant agent, the viscosity over time is extremely small,
It is particularly preferably used because deterioration of the water-resistant agent due to a side reaction with water is small.

【0013】本発明のPVA(A)と多価ジアルデヒド
化合物(B)の配合割合は、成分(A)100重量部
(以下、重量部を部と略記する)に対して成分(B)1
〜50部であり、好ましくは成分(A)100部に対し
て成分(B)2〜20部である。成分(A)が1部未満
の場合には耐水性付与の効果の発現がなく、また50部
を越えるとインク吸収速度の低下や塗工液の粘度安定性
が悪くなり好ましくない。本発明において用いられる該
アミノ基または該アンモニウム塩基を有するPVA
(A)と多価ジアルデヒド化合物(B)は、それらのみ
で使用することもできるが、他の水溶性樹脂、水分散性
樹脂、水溶性無機化合物あるいは無機充填剤などを併用
することもできる。
The PVA (A) of the present invention and a polyvalent dialdehyde
The compounding ratio of the compound (B) is such that 100 parts by weight of the component (A) (hereinafter, part by weight is abbreviated as “parts”) and 1 part of the component (B)
To 50 parts, preferably 2 to 20 parts of component (B) based on 100 parts of component (A). When the amount of the component (A) is less than 1 part, the effect of imparting water resistance is not exhibited, and when the amount exceeds 50 parts, the ink absorption rate is lowered and the viscosity stability of the coating liquid is unfavorably deteriorated. PVA having the amino group or the ammonium base used in the present invention
(A) and polyhydric dialdehyde compound (B) is used in combination it can also be used in their only, other water-soluble resins, water dispersible resins, and water-soluble inorganic compound or inorganic filler
It is also possible to.

【0014】併用できる他の水溶性あるいは水分散性樹
脂としては、アルブミン、ゼラチン、カゼイン、でん
粉、アラビアゴム、メチルセルロース、ヒドロキシエチ
ルセルロースなどのセルロース誘導体、ポリアミド樹
脂、メラミン樹脂、通常の無変性PVA、ポリ(メタ)
アクリルアミド、ポリビニルピロリドン等のノニオン性
水溶性樹脂、CMC、ポリ(メタ)アクリル酸ナトリウ
ム、アニオン変性PVA、アルギン酸ナトリウム、水溶
性ポリエステルなどのアニオン性水溶性樹脂、カチオン
化でん粉、カチオン化ポリ(メタ)アクリルアミド、カ
チオン変性PVA、カチオン化ポリアミド樹脂等のカチ
オン性水溶性樹脂、SBRラテックス、NBRラテック
ス、酢酸ビニル系エマルジョン、エチレン−酢酸ビニル
共重合体エマルジョン、(メタ)アクリル酸エステル系
エマルジョン、塩化ビニル系エマルジョン等の水分散性
樹脂があげられる。これらの水溶性あるいは水分散性樹
脂を本発明において用いられるPVA(A)と多価ジア
ルデヒド化合物(B)に併用する場合の併用割合として
は、本発明のPVA(A)100重量部に対して100
部以下、好ましくは50部以下で使用される。
Other water-soluble or water-dispersible resins that can be used in combination include albumin, gelatin, casein, starch, gum arabic, cellulose derivatives such as methylcellulose, hydroxyethylcellulose, polyamide resins, melamine resins, ordinary unmodified PVA, (Meta)
Nonionic water-soluble resins such as acrylamide and polyvinylpyrrolidone, CMC, anionic water-soluble resins such as sodium poly (meth) acrylate, anion-modified PVA, sodium alginate, water-soluble polyester, cationized starch, cationized poly (meth) Cationic water-soluble resin such as acrylamide, cation-modified PVA, cationized polyamide resin, SBR latex, NBR latex, vinyl acetate emulsion, ethylene-vinyl acetate copolymer emulsion, (meth) acrylate emulsion, vinyl chloride Water-dispersible resins such as emulsions can be used. These water-soluble or water-dispersible resins are used in combination with the PVA (A) used in the present invention and the polyvalent dial.
When used in combination with the aldehyde compound (B), the combination ratio is 100 parts by weight with respect to 100 parts by weight of the PVA (A) of the present invention.
Parts or less, preferably 50 parts or less.

【0015】本発明において併用できる水溶性の無機化
合物としては、硫酸アルミニウム、カリ明バン、アンモ
ニウム明バン、塩化マグネシウム、塩化亜鉛、塩化第2
鉄、塩化アルミニウム等が挙げられる。これらの水溶性
無機化合物を併用する場合には、上記のPVA(A)1
00部に対して0.5〜10部の範囲で用いることが好
ましい。また本発明において併用できる無機充填剤とし
ては、シリカ、クレー、タルク、ケイソウ土、ゼオライ
ト、炭酸カルシウム、アルミナ、酸化亜鉛、サチンホワ
イトなどが挙げられる。この場合の併用割合としては、
透明性を必要とするインクジェット用記録シートとそれ
以外の場合とで異なるが、通常本発明で用いられるPV
A(A)100重量部に対して0.1〜10000部、
好ましくは5〜2000部の範囲から選ばれる。
The water-soluble inorganic compounds which can be used in combination in the present invention include aluminum sulfate, potassium ash, ammonium ash, magnesium chloride, zinc chloride, and secondary chloride.
Iron, aluminum chloride and the like. When these water-soluble inorganic compounds are used in combination, the above-mentioned PVA (A) 1
It is preferable to use 0.5 to 10 parts with respect to 00 parts. Examples of the inorganic filler that can be used in the present invention include silica, clay, talc, diatomaceous earth, zeolite, calcium carbonate, alumina, zinc oxide, and satin white. In this case,
The recording sheet for inkjet which requires transparency is different from the other cases, but the PV sheet usually used in the present invention is
0.1 to 10,000 parts per 100 parts by weight of A (A),
Preferably it is selected from the range of 5 to 2000 parts.

【0016】本発明において用いられる一級アミノ基、
一級アンモニウム塩基、二級アミノ基および二級アンモ
ニウム塩基から選ばれた少なくとも1種の官能基を有す
るPVA(A)と多価ジアルデヒド化合物(B)からな
る組成物は、それ自身でインク吸収性にすぐれているた
め、支持基体表面に組成物層を形成させインク吸収層と
しても使用できるが、他のインク吸収性材料よりなるイ
ンク吸収層の上に本発明の組成物よりなる層を形成せし
め耐水性層として使用することもできる。また発明の組
成物は支持基体中に含浸されたものも使用できる。
A primary amino group used in the present invention,
A composition comprising PVA (A) having at least one functional group selected from a primary ammonium base, a secondary amino group and a secondary ammonium base and a polyvalent dialdehyde compound (B) has an ink absorbing property by itself. Because of its excellent properties, it can be used as an ink-absorbing layer by forming a composition layer on the surface of a supporting substrate.However, a layer made of the composition of the present invention is formed on an ink-absorbing layer made of another ink-absorbing material. It can also be used as a water-resistant layer. Further, the composition of the present invention may be used by impregnating it in a supporting substrate.

【0017】本発明で用いられる支持基体としては、透
明性または不透明性の従来公知の支持基体がいずれも使
用できる。透明性支持基体としては、たとえばポリエス
テル、ポリアミド、ポリスチレン、ポリ塩化ビニル、ポ
リメチルメタアクリレート、酢酸セルロース、ポリカー
ボネート、ポリイミド、セロハン、セルロイド等のフィ
ルム、シートあるいは透明性の高い紙などが挙げられ
る。不透明性支持体としては、たとえば一般の紙、コー
ト紙、布、木材、金属板、合成紙、不透明処理した合成
樹脂系フィルムあるいはシート等が挙げられる。本発明
の目的の1つである透明性に優れたインクジェット用記
録シートの場合には、透明性支持基体が用いられる。本
発明において、支持基体に上記の一級アミノ基、一級ア
ンモニウム塩基、二級アミノ基および二級アンモニウム
塩基から選ばれた少なくとも1種の官能基を有するPV
A(A)と多価ジアルデヒド化合物(B)からなる組成
物を付与せしめる方法としては、この組成物の水溶液単
独、または組成物と他の水溶性樹脂、水分散性樹脂、水
溶性無機化合物あるいは充填剤との混合物水溶液あるい
は水分散液をサイズプレス、エアーナイフコーター、ロ
ールコーター、バーコーター、ブレードコーター等の通
常のコーティング方法によって、支持基体中に含浸せし
めるか、支持基体の上表面あるいは上表面と下表面の両
表面上にコート層を形成せしめる等の方法が使用でき
る。また、支持基体が紙である場合には抄紙時に上記の
水溶液あるいは水分散液を内添する方法も使用できる。
本発明のインクジェット用記録シート中の該PVA
(A)と多価ジアルデヒド化合物(B)からなる組成物
の含有量としては特に制限はないが、通常0.1〜20
0g/m2、好ましくは1〜100g/m2である。
As the support substrate used in the present invention, any of transparent or opaque conventionally known support substrates can be used. Examples of the transparent support substrate include films, sheets, and highly transparent papers such as polyester, polyamide, polystyrene, polyvinyl chloride, polymethyl methacrylate, cellulose acetate, polycarbonate, polyimide, cellophane, and celluloid. Examples of the opaque support include general paper, coated paper, cloth, wood, metal plate, synthetic paper, opaque-treated synthetic resin film or sheet, and the like. In the case of an ink jet recording sheet having excellent transparency, which is one of the objects of the present invention, a transparent support substrate is used. In the present invention, a PV having at least one functional group selected from the above-mentioned primary amino group, primary ammonium group, secondary amino group and secondary ammonium group on the supporting substrate
As a method for giving a composition comprising A (A) and a polyvalent dialdehyde compound (B), an aqueous solution of the composition alone, or a composition and another water-soluble resin, a water-dispersible resin, a water-soluble inorganic compound, Alternatively, an aqueous solution or aqueous dispersion of a mixture with a filler is impregnated into a support substrate by a usual coating method such as a size press, an air knife coater, a roll coater, a bar coater, a blade coater, or the like, or the upper surface of the support substrate A method of forming a coat layer on both the surface and the lower surface can be used. When the supporting substrate is paper, a method of internally adding the above aqueous solution or aqueous dispersion during papermaking can also be used.
The PVA in the ink jet recording sheet of the present invention
The content of the composition comprising (A) and the polyvalent dialdehyde compound (B) is not particularly limited, but is usually 0.1 to 20.
0 g / m 2 , preferably 1 to 100 g / m 2 .

【0018】[0018]

【実施例】以下に実施例をあげて本発明をさらに詳しく
説明するが、本発明はこれによって限定されるものでは
ない。なお実施例中、特にことわりのないかぎり「%」
および「部」は重量基準を表す。実施例中の諸物性の測
定方法を以下に示す。 (1)インクジェット記録方法 吐出オリフィス径60μmのオンディマンド型インクジ
ェット記録ヘッドを有する記録装置を用い、イェロー、
マジェンダ、シアン、ブラックの4色水性インクを用い
て、カラーインクジェット記録を行ない、記録特性の評
価を行なった。 (2)インク吸収速度 インクジェット記録後、一定時間ごとに、記録シート上
の印字を指でこすり、印字部分が変化しなくなるまでの
時間を測定した。時間が短いほどインク吸収速度は大で
ある。 (3)にじみ度 印字ドットの直系を実体顕微鏡で測定し、インク滴の何
倍になったかを示した。 (4)透明度 インクジェット用記録シートの非印字部分の可視光線透
過率(%)を波長500nmの可視光線を用いて分光光
度計で測定した。この透過率をもって透明度とする。透
過率が大であるほど透明性が高いことを示す。 (5)耐水性 インクジェット記録後のシートの印字部に水を付け指で
こすったとき、印字部が溶解したり、にじんだりするか
どうかを5段階で判定した。 5 :変化無し。 1 :にじみ、または溶解がある。 4〜2:5〜1の中間(数字が大きい方がにじみまたは
変化が少ない)。
EXAMPLES The present invention will be described in more detail with reference to the following Examples, but it should not be construed that the present invention is limited thereto. In the examples, unless otherwise specified, "%"
And "part" represents a basis of weight. The methods for measuring various physical properties in the examples are shown below. (1) Inkjet recording method Using a recording apparatus having an on-demand type inkjet recording head having a discharge orifice diameter of 60 μm, yellow,
Color ink jet recording was performed using four-color aqueous inks of magenta, cyan, and black, and recording characteristics were evaluated. (2) Ink absorption speed After ink jet recording, the print on the recording sheet was rubbed with a finger at regular intervals, and the time until the printed portion did not change was measured. The shorter the time, the higher the ink absorption speed. (3) Bleeding degree The direct line of the printing dot was measured by a stereoscopic microscope, and the number of times the ink droplet became larger was shown. (4) Transparency The visible light transmittance (%) of the non-printed portion of the inkjet recording sheet was measured with a spectrophotometer using visible light having a wavelength of 500 nm. The transmittance is defined as the transparency. The higher the transmittance, the higher the transparency. (5) Water Resistance When water was applied to the printed portion of the sheet after inkjet recording and the finger was rubbed with the finger, it was determined in five stages whether the printed portion was dissolved or bleed. 5: No change. 1: There is bleeding or dissolution. 4-2: Middle of 5-1 (larger numbers have less bleeding or change).

【0019】実施例1 N−ビニルアセトアミドと酢酸ビニルとの共重合体をア
ルカリけん化して一級アミノ基を5モル%含有し、酢酸
ビニル単位のけん化度92.5モル%、重合度1100
の分子内に一級アミノ基を有する変性PVAを得た。厚
さ50μm、透明度95%のポリエステルシート上に、
上記の一級アミノ基変性PVA100部と耐水化剤とし
てグリオキザール5部とを含む10%水溶液を、乾燥後
の塗布量が15g/m2になるよう塗布し、乾燥して、
インクジェット用記録シートを得た。このシートのイン
ク吸収速度、にじみ度、透明度、耐水性を評価し、その
結果を表1に示す。
EXAMPLE 1 A copolymer of N-vinylacetamide and vinyl acetate was alkali-saponified to contain 5 mol% of primary amino groups, a degree of saponification of vinyl acetate units of 92.5 mol%, and a degree of polymerization of 1100
A modified PVA having a primary amino group in the molecule was obtained. On a 50 μm thick, 95% transparent polyester sheet,
A 10% aqueous solution containing 100 parts of the primary amino group-modified PVA and 5 parts of glyoxal as a water-proofing agent is applied so that the coating amount after drying is 15 g / m 2 , and dried,
An ink jet recording sheet was obtained. The ink absorption rate, bleeding degree, transparency, and water resistance of this sheet were evaluated, and the results are shown in Table 1.

【0020】実施例2 実施例1で用いたN−ビニルアセトアミドの代わりにN
−ビニルコハク酸イミドを用い、酢酸ビニルと共重合
し、アルカリけん化して一級アミノ基変性PVAを作成
した。この変性PVAは一級アミノ基を7モル%含有
し、酢酸ビニル単位のけん化度88.2モル%、重合度
1050であった。実施例1で用いた変性PVAの代わ
りに上記の変性PVAを用い、さらにグリオキザールの
代わりにグルタルアルデヒドを用いたほかは、実施例1
と同様にして、インクジェット用記録シートを作成し
た。評価結果を表1に併せて示す。
Example 2 N-vinylacetamide used in Example 1 was replaced by N
-Using vinyl succinimide, copolymerized with vinyl acetate, and saponified with alkali to prepare a primary amino group-modified PVA. This modified PVA contained 7 mol% of primary amino groups, had a saponification degree of vinyl acetate units of 88.2 mol% and a polymerization degree of 1050. Example 1 was repeated except that the above-mentioned modified PVA was used in place of the modified PVA used in Example 1 and glutaraldehyde was used instead of glyoxal.
In the same manner as in the above, an ink jet recording sheet was prepared. The evaluation results are also shown in Table 1.

【0021】比較例1〜3 実施例1で用いた組成物に代えて、以下の樹脂および耐
水化剤を用いる以外は、実施例1と同様に行った。結果
を表1に併せて示す。 比較例1で用いた樹脂および耐水化剤:重合度100
0、けん化度88モル%の無変性PVA100部とグオ
キザール5部。 比較例2で用いた樹脂(耐水化剤は使用しない):ポリ
ビニルピロリドン(PVP)。比較例3で用いた樹脂およ
び耐水化剤:第四級アンモニウム塩基を2モル%含有
し、重合度1750、けん化度88モル%のカチオン変
性PVA100部とグリオキザール5部。
Comparative Examples 1 to 3 The same procedures as in Example 1 were carried out except that the following resin and water-proofing agent were used instead of the composition used in Example 1. The results are shown in Table 1. Resin and waterproofing agent used in Comparative Example 1: degree of polymerization 100
0, 100 parts of unmodified PVA having a saponification degree of 88 mol% and 5 parts of guoxal. Resin used in Comparative Example 2 (waterproofing agent was not used): polyvinylpyrrolidone (PVP). Resin and water-proofing agent used in Comparative Example 3: 100 parts of cation-modified PVA containing 2 mol% of a quaternary ammonium base, having a polymerization degree of 1750 and a saponification degree of 88 mol%, and 5 parts of glyoxal.

【0022】実施例 比較例3で得られたインクジェット用記録シートについ
て、第四級アンモニウム塩基変性PVAとグリオキザー
ルからなる組成物を含有する層の上に実施例1で用いら
れた配合物を乾燥固形分が3g/m2となるよう塗布
し、乾燥して、インクジェット用記録シートを得た。結
果を表1に併せて示す。
Example 3 With respect to the ink jet recording sheet obtained in Comparative Example 3, the composition used in Example 1 was dried on a layer containing a composition comprising quaternary ammonium base-modified PVA and glyoxal. The composition was applied so that the solid content was 3 g / m 2, and dried to obtain an ink jet recording sheet. The results are shown in Table 1.

【0023】実施例 実施例1で用いられた組成物25部、非膠質シリカ粉末
100部、水500部からなる塗工液を、上質紙に乾燥
固形分が17g/m2になるようバーコーターで塗布し
乾燥して記録用シートを得た。結果を併せて表1に示
す。
Example 4 A coating liquid consisting of 25 parts of the composition used in Example 1, 100 parts of non-colloidal silica powder and 500 parts of water was applied to a high quality paper so that the dry solid content was 17 g / m 2. It was applied with a coater and dried to obtain a recording sheet. The results are shown in Table 1.

【0024】[0024]

【表1】 [Table 1]

【0025】[0025]

【発明の効果】本発明のインクジェット用記録シート
は、インク吸収性に優れ、耐水性が著しく優れた物性を
与える。この理由については十分解明されていないが、
次のように推定される。本発明において用いられる分子
内に一級アミノ基、一級アンモニウム塩基、二級アミノ
基および二級アンモニウム塩基から選ばれた少なくとも
1種の官能基を有するPVA(A)はインクジェット等
に使用される水性インクとの親和性が大きいために、
価ジアルデヒド化合物(B)との架橋反応が行われた後
の被膜も優れたインク吸収性能を示し、また多価ジアル
デヒド化合物との反応性も高いため優れた耐水性を与え
ると推定される。これらの効果は無変性のPVAや従来
のカチオン変性PVAである第四級アンモニウム塩基を
含有変性したPVAでは得られないものである。また表
1から明らかなように、インクのにじみが小さく、さら
に透明性基体を使用し、その表面に上記(A)および
(B)の組成物をコーテイングした場合には、透明性が
損なわれずに、優れた透明性を有するインクジェット用
記録シートが得られる。
The ink jet recording sheet of the present invention has excellent ink absorbency and excellent physical properties such as remarkably excellent water resistance. The reason for this is not fully understood,
It is estimated as follows. PVA (A) having at least one functional group selected from a primary amino group, a primary ammonium group, a secondary amino group, and a secondary ammonium group in the molecule used in the present invention is an aqueous ink used for ink jet or the like. because of the greater affinity with a multi
Shows the valence dialdehyde compound (B) and the ink absorption performance of the coating also excellent after the crosslinking reaction has been performed, also polyhydric dialkyl
It is presumed that it has excellent water resistance because of its high reactivity with the aldehyde compound . These effects cannot be obtained with unmodified PVA or modified PVA containing a quaternary ammonium base, which is a conventional cation-modified PVA. Table
As is clear from FIG. 1, the ink bleeding was small and
A transparent substrate is used, and the above (A) and
When the composition of (B) is coated, the transparency is
Inkjet with excellent transparency without loss
A recording sheet is obtained.

フロントページの続き (51)Int.Cl.7 識別記号 FI C09D 129/04 C09D 129/04 (56)参考文献 特開 平1−159286(JP,A) 特開 昭63−315283(JP,A) 特開 平1−157884(JP,A) (58)調査した分野(Int.Cl.7,DB名) B41M 5/00 C08F 8/12 C08F 8/30 C08L 29/04 C09D 129/04 Continuation of the front page (51) Int.Cl. 7 Identification symbol FI C09D 129/04 C09D 129/04 (56) References JP-A-1-159286 (JP, A) JP-A-63-315283 (JP, A) JP-A-1-15784 (JP, A) (58) Fields investigated (Int. Cl. 7 , DB name) B41M 5/00 C08F 8/12 C08F 8/30 C08L 29/04 C09D 129/04

Claims (3)

(57)【特許請求の範囲】(57) [Claims] 【請求項1】 下記式(I)、(II)および(III)から
選ばれる少なくとも一種の単量体とビニルエステルとの
共重合体をけん化または加水分解して得られる分子内に
一級アミノ基、一級アンモニウム塩基、二級アミノ基お
よび二級アンモニウム塩基から選ばれた少なくとも1種
の官能基を有するポリビニルアルコール(A)と多価ジ
アルデヒド化合物(B)からなり、成分(A)100重
量部に対して成分(B)1〜50重量部である組成物を
支持基体中または支持基体表面に有するインクジェット
用記録シート。【化1】 【化2】 【化3】 (ここで、R 1 は水素原子またはメチル基、R 2 は水素原
子または低級アルキル基、R 3 は水素原子、低級アルキ
ル基、メチロール基またはエチロール基、nは0 〜4の
整数、mは2〜4の整数をそれぞれ示す。)
(1) From the following formulas (I), (II) and (III)
Of at least one selected monomer and vinyl ester
A polyvinyl alcohol (A) having at least one functional group selected from a primary amino group, a primary ammonium group, a secondary amino group and a secondary ammonium group in a molecule obtained by saponifying or hydrolyzing the copolymer; Multivalent
An ink jet recording sheet comprising a composition comprising the aldehyde compound (B) and 1 to 50 parts by weight of the component (B) based on 100 parts by weight of the component (A) in the support substrate or on the surface of the support substrate. Embedded image Embedded image Embedded image (Where R 1 is a hydrogen atom or a methyl group, R 2 is a hydrogen atom
R 3 is a hydrogen atom, lower alkyl,
Group, a methylol group or ethylol group, n represents 0-4 of
Integer and m each represent an integer of 2 to 4. )
【請求項2】 官能基が一級アミノ基または一級アンモ
ニウム塩基である請求項1記載のインクジェット用記録
シート。
2. The ink jet recording sheet according to claim 1, wherein the functional group is a primary amino group or a primary ammonium base.
【請求項3】 支持基体が透明性支持基体である請求項3. The support substrate according to claim 1, wherein the support substrate is a transparent support substrate.
1または2記載のインクジェット用記録シート。3. The recording sheet for inkjet according to 1 or 2.
JP3047661A 1991-02-19 1991-02-19 Inkjet recording sheet Expired - Fee Related JP3053231B2 (en)