[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP2015171811A - decorative sheet - Google Patents

decorative sheet Download PDF

Info

Publication number
JP2015171811A
JP2015171811A JP2014191386A JP2014191386A JP2015171811A JP 2015171811 A JP2015171811 A JP 2015171811A JP 2014191386 A JP2014191386 A JP 2014191386A JP 2014191386 A JP2014191386 A JP 2014191386A JP 2015171811 A JP2015171811 A JP 2015171811A
Authority
JP
Japan
Prior art keywords
layer
decorative sheet
resin
meth
acrylate
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2014191386A
Other languages
Japanese (ja)
Other versions
JP6582380B2 (en
Inventor
雄一 伊勢森
Yuichi Isemori
雄一 伊勢森
一輝 北島
Kazuki Kitajima
一輝 北島
康介 中井
Kosuke Nakai
康介 中井
須賀 和宏
Kazuhiro Suga
和宏 須賀
和保 河野
Kazuyasu Kono
和保 河野
啓史 川崎
Hiroshi Kawasaki
啓史 川崎
陽子 鷹野
Yoko Takano
陽子 鷹野
千草 栗山
Chigusa Kuriyama
千草 栗山
古田 哲
Satoru Furuta
哲 古田
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Dai Nippon Printing Co Ltd
Original Assignee
Dai Nippon Printing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Dai Nippon Printing Co Ltd filed Critical Dai Nippon Printing Co Ltd
Priority to JP2014191386A priority Critical patent/JP6582380B2/en
Publication of JP2015171811A publication Critical patent/JP2015171811A/en
Application granted granted Critical
Publication of JP6582380B2 publication Critical patent/JP6582380B2/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

PROBLEM TO BE SOLVED: To provide a decorative sheet that gives a realistic feeling, for example, a decorative sheet with a woodgrain pattern that gives a tactile feeling and gloss similar to those of real wood and that can impart a high-class impression to a decorative material.SOLUTION: The decorative sheet includes : a raised layer at least partially disposed on a substrate; and a surface protective layer covering an entire surface including an area where the raised layer is formed and an area where no raised layer is formed. The surface protective layer is a crosslinked and cured product of an ionization radiation-curable resin composition and has a ten-point average roughness of 5 to 35 μm on a surface thereof. An occupation area ratio of the raised layer is 2 to 25%.

Description

本発明は、建築物の内装、外装、家具、建具等の表面化粧、車両の内装等に用いられる化粧シートに関する。   The present invention relates to a decorative sheet used for surface decoration of buildings, interiors, exteriors, furniture, joinery and the like, interiors of vehicles, and the like.

建築物の内装,外装、家具、建具、車両の内装等の表面化粧板としては、例えば木目調柄などを印刷した化粧シートを接着剤で貼り合わせた構造のものが用いられている。
このような表面化粧板に使用される化粧シートには、触感、マット感、光沢感、耐汚染性に加え、意匠性に優れることなど、種々の特性が要求されている。
これらのうち、特に、触感、マット感、光沢感、意匠性を得るために、化粧シートの表面に盛上部を設けることが提案されている。
このような化粧シートとして、例えば、特許文献1には、化粧シートの表面に多角形や円形の規則的もしくは定形な盛上部を設けた化粧シート、特許文献2には、盛上部の凹凸の高低差及び凸部の表面積割合を限定した化粧シート、特許文献3には、表面の電離放射線硬化性樹脂のインキからなる凹凸部を設けた化粧シートが開示されている。
しかしながら、これらの化粧シートは、シートとしての、耐傷性、耐汚染性、触感、マット感及び光沢感が十分ではなく、意匠性についてもさらなる向上が求められていた。
As surface decorative boards for interiors, exteriors, furniture, joinery, and vehicle interiors of buildings, for example, those having a structure in which a decorative sheet printed with a wood grain pattern or the like is bonded with an adhesive are used.
The decorative sheet used for such a decorative sheet is required to have various characteristics such as excellent design as well as touch, matte, gloss and stain resistance.
Among these, it has been proposed to provide a raised portion on the surface of the decorative sheet, in particular, in order to obtain a tactile sensation, matte sensation, glossiness, and design.
As such a decorative sheet, for example, Patent Document 1 discloses a decorative sheet in which a polygonal or circular regular or regular raised portion is provided on the surface of the decorative sheet, and Patent Document 2 describes the unevenness of the raised portion. A decorative sheet, in which the surface area ratio of the difference and the convex portion is limited, Patent Document 3 discloses a decorative sheet provided with a concavo-convex portion made of an ionizing radiation curable resin ink on the surface.
However, these decorative sheets do not have sufficient scratch resistance, stain resistance, tactile sensation, matte feeling and glossiness as sheets, and further improvements in design properties have been demanded.

特開2003−94592号JP 2003-94592 A 特許第3334365号Japanese Patent No. 3334365 特開2004−249586号JP 2004-249586

本発明の課題は、上記のような状況下で、触感、マット感及び光沢感に優れ、かつ耐傷性、耐汚染性、及び意匠性に優れる化粧シートを提供することにある。   The subject of this invention is providing the decorative sheet which is excellent in tactile sensation, a mat | matte feeling, and a glossy feeling in the above situations, and is excellent in a flaw resistance, stain resistance, and designability.

本発明者らは、前記目的を達成するために鋭意研究を重ねた結果、基材上に、盛上層及び表面保護層を有する化粧シートであって、表面の十点平均粗さが特定の範囲であり、かつ盛上層の占有面積比を特定の範囲とすることで、前記課題を解決し得ることを見出した。本発明は、かかる知見に基づいて完成したものである。   As a result of intensive studies to achieve the above object, the inventors of the present invention are decorative sheets having a raised layer and a surface protective layer on a substrate, and the surface 10-point average roughness is in a specific range. And it discovered that the said subject could be solved by making the occupation area ratio of a raised layer into a specific range. The present invention has been completed based on such findings.

すなわち、本発明は、基材上に少なくとも、部分的に設けられた盛上層と、該盛上層が形成された領域及び該盛上層が形成されていない領域とを含む全面にわたって被覆する表面保護層を有する化粧シートであって、該表面保護層が電離放射線硬化性樹脂組成物の架橋硬化したものであり、表面の十点平均粗さが5〜35μmであり、かつ前記盛上層の占有面積比が2〜25%である化粧シートを提供するものである。   That is, the present invention provides a surface protective layer that covers the entire surface including a raised layer provided at least partially on a substrate, a region where the raised layer is formed, and a region where the raised layer is not formed. The surface protective layer is obtained by crosslinking and curing the ionizing radiation curable resin composition, the surface has a ten-point average roughness of 5 to 35 μm, and the occupied area ratio of the raised layer Is a decorative sheet having a content of 2 to 25%.

本発明の化粧シートは、触感、マット感及び光沢感に優れ、かつ耐傷性、耐汚染性、及び意匠性に優れる。   The decorative sheet of the present invention is excellent in tactile sensation, matte sensation, and glossiness, and is excellent in scratch resistance, stain resistance, and design.

本発明の化粧シートの断面を示す模式図である。It is a schematic diagram which shows the cross section of the decorative sheet of this invention.

本発明の化粧シートは、基材上に少なくとも、部分的に設けられた盛上層と、該盛上層が形成された領域及び該盛上層が形成されていない領域とを含む全面にわたって被覆する表面保護層を有する。
以下、本発明の化粧シートについて、好適な態様を示す図1を用いて詳細に説明する。
The decorative sheet of the present invention has a surface protection covering the entire surface including at least a raised layer provided on a substrate, a region where the raised layer is formed, and a region where the raised layer is not formed. Having a layer.
Hereinafter, the decorative sheet of the present invention will be described in detail with reference to FIG.

図1に示される本発明の化粧シート10は、基材20上に必要に応じて設けられる、例えばベタ印刷層31及び絵柄層32からなる装飾層30を有し、その上に必要に応じて形成されるプライマー層40を有し、その上に部分的に設けられた盛上層50を有し、該盛上層上に表面保護層60を有する。   The decorative sheet 10 of the present invention shown in FIG. 1 has a decoration layer 30 that is provided on a base material 20 as necessary, for example, a solid print layer 31 and a pattern layer 32, and on that, as necessary. It has the primer layer 40 to be formed, has a raised layer 50 partially provided thereon, and has a surface protective layer 60 on the raised layer.

<基材>
本発明の化粧シート10における基材20としては、通常化粧シートの基材として用いられるものであれば、特に限定されず、各種の紙類、プラスチックフィルム、プラスチックシート等を用途に応じて適宜選択することができる。これらの材料はそれぞれ単独で使用してもよいが、紙同士の複合体や紙とプラスチックフィルムの複合体等、任意の組み合わせによる積層体であってもよい。
これらの基材、特にプラスチックフィルムやプラスチックシートを基材として用いる場合には、その上に設けられる層との密着性を向上させるために、所望により、片面または両面に酸化法や凹凸化法などの物理的または化学的表面処理を施すことができる。
<Base material>
The base material 20 in the decorative sheet 10 of the present invention is not particularly limited as long as it is normally used as a base material of a decorative sheet, and various papers, plastic films, plastic sheets, and the like are appropriately selected depending on applications. can do. Each of these materials may be used alone, but may be a laminate of any combination such as a composite of paper or a composite of paper and a plastic film.
When using these substrates, particularly plastic films or plastic sheets, as a substrate, an oxidation method or a concavo-convex method may be applied to one or both sides as desired in order to improve the adhesion to the layer provided thereon. Physical or chemical surface treatment can be applied.

上記酸化法としては、例えばコロナ放電処理法、クロム酸化処理法、火炎処理法、熱風処理法、オゾン及び紫外線処理法などが挙げられ、凹凸化法としては、例えばサンドブラスト法、溶剤処理法などが挙げられる。これらの表面処理は、基材の種類に応じて適宜選択されるが、一般にはコロナ放電処理法が効果及び操作性などの面から好ましく用いられる。
また該基材はプライマー層を形成する等の処理を施してもよいし、色彩を整えるための塗装や、デザイン的な観点での模様があらかじめ形成されていてもよい。
Examples of the oxidation method include a corona discharge treatment method, a chromium oxidation treatment method, a flame treatment method, a hot air treatment method, ozone and an ultraviolet treatment method, and examples of the unevenness method include a sand blast method and a solvent treatment method. Can be mentioned. These surface treatments are appropriately selected depending on the type of substrate, but generally, a corona discharge treatment method is preferably used from the viewpoints of effects and operability.
Further, the substrate may be subjected to a treatment such as forming a primer layer, or a coating for adjusting the color or a pattern from a design viewpoint may be formed in advance.

基材として用いられる各種の紙類としては、薄葉紙、クラフト紙、チタン紙などが使用できる。これらの紙基材は、紙基材の繊維間ないしは他層と紙基材との層間強度を強化したり、ケバ立ち防止のため、これら紙基材に、更に、アクリル樹脂、スチレンブタジエンゴム、メラミン樹脂、ウレタン樹脂等の樹脂を添加(抄造後樹脂含浸、又は抄造時に内填)させたものでもよい。例えば、紙間強化紙、樹脂含浸紙等である。
これらの他、リンター紙、板紙、石膏ボード用原紙、又は紙の表面に塩化ビニル樹脂層を設けたビニル壁紙原反等、建材分野で使われることの多い各種紙が挙げられる。さらには、事務分野や通常の印刷、包装などに用いられるコート紙、アート紙、硫酸紙、グラシン紙、パーチメント紙、パラフィン紙、又は和紙等を用いることもできる。また、これらの紙とは区別されるが、紙に似た外観と性状を持つ各種繊維の織布や不織布も基材として使用することができる。各種繊維としてはガラス繊維、石綿繊維、チタン酸カリウム繊維、アルミナ繊維、シリカ繊維、若しくは炭素繊維等の無機質繊維、又はポリエステル繊維、アクリル繊維、若しくはビニロン繊維などの合成樹脂繊維が挙げられる。
As various papers used as the substrate, thin paper, kraft paper, titanium paper and the like can be used. These paper base materials are used to reinforce the interlaminar strength between the fibers of the paper base material or between the other layers and the paper base material, and to prevent the occurrence of scuffing, in addition to these paper base materials, acrylic resin, styrene butadiene rubber, A resin such as a melamine resin or a urethane resin may be added (resin impregnation after paper making or embedded during paper making). For example, inter-paper reinforced paper, resin-impregnated paper, and the like.
In addition to these, various papers often used in the field of building materials such as linter paper, paperboard, base paper for gypsum board, or a vinyl wallpaper raw material in which a vinyl chloride resin layer is provided on the surface of the paper can be mentioned. Furthermore, coated paper, art paper, sulfate paper, glassine paper, parchment paper, paraffin paper, Japanese paper, or the like used in the office field or normal printing and packaging can also be used. Moreover, although distinguished from these papers, woven fabrics and non-woven fabrics of various fibers having an appearance and properties similar to paper can be used as the base material. Examples of various fibers include inorganic fibers such as glass fibers, asbestos fibers, potassium titanate fibers, alumina fibers, silica fibers, and carbon fibers, or synthetic resin fibers such as polyester fibers, acrylic fibers, and vinylon fibers.

プラスチックフィルム又はプラスチックシートとしては、各種の合成樹脂からなるものが挙げられる。合成樹脂としては、ポリエチレン樹脂、ポリプロピレン樹脂、ポリメチルペンテン樹脂、ポリ塩化ビニル樹脂、ポリ塩化ビニリデン樹脂、ポリビニルアルコール樹脂、塩化ビニル−酢酸ビニル共重合樹脂、エチレン−酢酸ビニル共重合樹脂、エチレン−ビニルアルコール共重合樹脂、ポリエチレンテレフタレート樹脂、ポリブチレンテレフタレート樹脂、ポリエチレンナフタレート−イソフタレート共重合樹脂、ポリメタクリル酸メチル樹脂、ポリメタクリル酸エチル樹脂、ポリアクリル酸ブチル樹脂、ナイロン6又はナイロン66等で代表されるポリアミド樹脂、三酢酸セルロース樹脂、セロファン、ポリスチレン樹脂、ポリカーボネート樹脂、ポリアリレート樹脂、又はポリイミド樹脂等が挙げられる。   As a plastic film or a plastic sheet, what consists of various synthetic resins is mentioned. Synthetic resins include polyethylene resin, polypropylene resin, polymethylpentene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl alcohol resin, vinyl chloride-vinyl acetate copolymer resin, ethylene-vinyl acetate copolymer resin, ethylene-vinyl. Representative examples include alcohol copolymer resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene naphthalate-isophthalate copolymer resin, polymethyl methacrylate resin, polyethyl methacrylate resin, polybutyl acrylate resin, nylon 6 or nylon 66 And polyamide resin, cellulose triacetate resin, cellophane, polystyrene resin, polycarbonate resin, polyarylate resin, polyimide resin, and the like.

基材の厚さについては特に制限はないが、プラスチックを素材とするフィルム又はシートを用いる場合には、厚さは、通常20〜150μm程度、好ましくは30〜100μmの範囲であり、紙基材を用いる場合には、坪量として、通常20〜150g/m2程度、好ましくは30〜100g/m2の範囲である。 The thickness of the substrate is not particularly limited, but when a film or sheet made of plastic is used, the thickness is usually in the range of about 20 to 150 μm, preferably 30 to 100 μm. Is used, the basis weight is usually about 20 to 150 g / m 2 , preferably 30 to 100 g / m 2 .

本発明の化粧シート10は、基材20上に、少なくとも、部分的に設けられた盛上層50を有することを特徴とする。
<盛上層>
本発明の化粧シートにおける盛上層50は、基材20と表面保護層60の間に位置し、化粧シートに触感を付与し、意匠性を高める機能を有するものである。
本発明において、盛上層の高さは、表面保護層を設けた後の化粧シートの表面の十点平均粗さ(Rz)が5〜35μmの範囲となる高さであることを必須とする。化粧シート表面の十点平均粗さ(Rz)が5μm未満であると、化粧シートの表面に十分な触感を付与することができない。一方、当該十点平均粗さ(Rz)が35μmを超えると、曲げ加工性に劣る。以上の観点から、本願発明の化粧シート表面の十点平均粗さ(Rz)は10〜25μmの範囲であることが好ましい。
また、盛上層の占有面積比は化粧シートの平面の面積に対して2〜25%の範囲である。当該占有面積比が2%以下であると、化粧シートの表面に十分な触感を付与することができない。一方、占有面積比が25%を超えると、曲げ加工性に劣る。その上、化粧シートの表面の触感も悪化するとともに、汚染性も低下する。以上の観点から、占有面積比は5〜25%の範囲であることが好ましい。
このような盛上層の厚さ及び占有面積比の範囲を選択することにより、化粧シートに、特に好適な触感を付与することができる。
なお、盛上層の占有面積比とは、盛上部の底面の面積の化粧シートの平面の面積に対する比率をいう。
The decorative sheet 10 of the present invention is characterized in that it has a raised layer 50 provided at least partially on the base material 20.
<Heisei layer>
The raised layer 50 in the decorative sheet of the present invention is located between the base material 20 and the surface protective layer 60 and has a function of imparting touch to the decorative sheet and enhancing the design.
In the present invention, it is essential that the height of the raised layer is such that the ten-point average roughness (Rz) of the surface of the decorative sheet after providing the surface protective layer is in the range of 5 to 35 μm. When the ten-point average roughness (Rz) of the decorative sheet surface is less than 5 μm, sufficient tactile sensation cannot be imparted to the decorative sheet surface. On the other hand, when the ten-point average roughness (Rz) exceeds 35 μm, the bending workability is inferior. From the above viewpoint, the ten-point average roughness (Rz) of the decorative sheet surface of the present invention is preferably in the range of 10 to 25 μm.
Moreover, the occupation area ratio of the raised layer is in the range of 2 to 25% with respect to the area of the flat surface of the decorative sheet. If the occupied area ratio is 2% or less, sufficient tactile sensation cannot be imparted to the surface of the decorative sheet. On the other hand, if the occupation area ratio exceeds 25%, the bending workability is inferior. In addition, the tactile sensation on the surface of the decorative sheet is deteriorated and the contamination is also reduced. From the above viewpoint, the occupation area ratio is preferably in the range of 5 to 25%.
By selecting the range of the thickness of the raised layer and the occupied area ratio, a particularly suitable tactile sensation can be imparted to the decorative sheet.
The occupied area ratio of the raised layer refers to the ratio of the area of the bottom surface of the raised portion to the area of the flat surface of the decorative sheet.

本発明における盛上層を構成する各盛上部の形状は、特に限定されず、丸、4角形、6角形の規則的に並んだような定形の形状でも、不定型な絵柄であってもよいが、不定型な絵柄であると触感、マット感、光沢感及び意匠性に優れることから好ましい。
また、盛上層の材料としては、特に限定されず、熱硬化性樹脂組成物、電離放射線硬化性樹脂組成物等を用いることができる。これらのうち、特に、ベヒクル成分として、アクリル系、ポリエステル系、アクリルウレタン系、ウレタン系の樹脂で水酸基、カルボキシル基、アミノ基等の官能基を有する樹脂に、硬化剤としてポリイソシアネートを添加した2液硬化型樹脂が表面性能維持及びコストの点から望ましい。
The shape of each raised portion constituting the raised layer in the present invention is not particularly limited, and may be a regular shape such as a regular arrangement of circles, squares, hexagons, or an irregular pattern. An irregular pattern is preferable because it is excellent in touch, matte, gloss and design.
Moreover, it does not specifically limit as a material of a raised layer, A thermosetting resin composition, an ionizing radiation curable resin composition, etc. can be used. Among these, in particular, as a vehicle component, polyisocyanate is added as a curing agent to a resin having a functional group such as a hydroxyl group, a carboxyl group, or an amino group as an acrylic, polyester, acrylic urethane, or urethane resin. A liquid curable resin is desirable from the viewpoint of maintaining surface performance and cost.

<表面保護層>
本発明の化粧シート10における表面保護層60は、前記盛上層50上に存在し、部分的に設けられた盛上層と、該盛上層が形成された領域及び該盛上層が形成されていない領域とを含む全面にわたって被覆するもので、電離放射線硬化性樹脂組成物が架橋硬化したもので構成される。ここで、電離放射線硬化性樹脂組成物とは、電磁波または荷電粒子線の中で分子を架橋、重合させ得るエネルギー量子を有するもの、すなわち、紫外線または電子線などを照射することにより、架橋、硬化する樹脂組成物を指す。電離放射線硬化性樹脂組成物中の電離放射線硬化性樹脂は、具体的には、従来電離放射線硬化性樹脂組成物として慣用されている重合性モノマー及び重合性オリゴマーないしはプレポリマーの中から適宜選択して用いることができる。
代表的には、重合性モノマーとして、分子中にラジカル重合性不飽和基を持つ(メタ)アクリレート単量体が好適である。
<Surface protective layer>
The surface protective layer 60 in the decorative sheet 10 of the present invention is present on the raised layer 50, a partially provided raised layer, a region where the raised layer is formed, and a region where the raised layer is not formed. The ionizing radiation curable resin composition is formed by crosslinking and curing. Here, the ionizing radiation curable resin composition is one having an energy quantum capable of crosslinking and polymerizing molecules in an electromagnetic wave or a charged particle beam, that is, crosslinking or curing by irradiating ultraviolet rays or electron beams. Refers to a resin composition. Specifically, the ionizing radiation curable resin in the ionizing radiation curable resin composition is appropriately selected from polymerizable monomers and polymerizable oligomers or prepolymers conventionally used as ionizing radiation curable resin compositions. Can be used.
Typically, a (meth) acrylate monomer having a radical polymerizable unsaturated group in the molecule is suitable as the polymerizable monomer.

(メタ)アクリレート単量体としては、多官能性(メタ)アクリレートが好ましい。なお、ここで「(メタ)アクリレート」とは「アクリレート又はメタクリレート」を意味する。多官能性(メタ)アクリレートとしては、分子内にエチレン性不飽和結合を2個以上有する(メタ)アクリレートであればよく、特に制限はない。具体的にはエチレングリコールジ(メタ)アクリレート、プロピレングリコールジ(メタ)アクリレート、1,4−ブタンジオールジ(メタ)アクリレート、1,6−ヘキサンジオールジ(メタ)アクリレート、ネオペンチルグリコールジ(メタ)アクリレート、ポリエチレングリコールジ(メタ)アクリレート、ヒドロキシピバリン酸ネオペンチルグリコールジ(メタ)アクリレート、ジシクロペンタニルジ(メタ)アクリレート、カプロラクトン変性ジシクロペンテニルジ(メタ)アクリレート、エチレンオキシド変性リン酸ジ(メタ)アクリレート、アリル化シクロヘキシルジ(メタ)アクリレート、イソシアヌレートジ(メタ)アクリレート、トリメチロールプロパントリ(メタ)アクリレート、エチレンオキシド変性トリメチロールプロパントリ(メタ)アクリレート、ジペンタエリスリトールトリ(メタ)アクリレート、プロピオン酸変性ジペンタエリスリトールトリ(メタ)アクリレート、ペンタエリスリトールトリ(メタ)アクリレート、プロピレンオキシド変性トリメチロールプロパントリ(メタ)アクリレート、トリス(アクリロキシエチル)イソシアヌレート、プロピオン酸変性ジペンタエリスリトールペンタ(メタ)アクリレート、ジペンタエリスリトールヘキサ(メタ)アクリレート、エチレンオキシド変性ジペンタエリスリトールヘキサ(メタ)アクリレート、カプロラクトン変性ジペンタエリスリトールヘキサ(メタ)アクリレートなどが挙げられる。これらの多官能性(メタ)アクリレートは1種を単独で用いてもよいし、2種以上を組み合わせて用いてもよい。   As the (meth) acrylate monomer, a polyfunctional (meth) acrylate is preferable. Here, “(meth) acrylate” means “acrylate or methacrylate”. The polyfunctional (meth) acrylate is not particularly limited as long as it is a (meth) acrylate having two or more ethylenically unsaturated bonds in the molecule. Specifically, ethylene glycol di (meth) acrylate, propylene glycol di (meth) acrylate, 1,4-butanediol di (meth) acrylate, 1,6-hexanediol di (meth) acrylate, neopentyl glycol di (meth) ) Acrylate, polyethylene glycol di (meth) acrylate, hydroxypivalate neopentyl glycol di (meth) acrylate, dicyclopentanyl di (meth) acrylate, caprolactone modified dicyclopentenyl di (meth) acrylate, ethylene oxide modified diphosphate ( (Meth) acrylate, allylated cyclohexyl di (meth) acrylate, isocyanurate di (meth) acrylate, trimethylolpropane tri (meth) acrylate, ethylene oxide modified trimethylo Propane tri (meth) acrylate, dipentaerythritol tri (meth) acrylate, propionic acid modified dipentaerythritol tri (meth) acrylate, pentaerythritol tri (meth) acrylate, propylene oxide modified trimethylolpropane tri (meth) acrylate, tris ( Acryloxyethyl) isocyanurate, propionic acid modified dipentaerythritol penta (meth) acrylate, dipentaerythritol hexa (meth) acrylate, ethylene oxide modified dipentaerythritol hexa (meth) acrylate, caprolactone modified dipentaerythritol hexa (meth) acrylate, etc. Is mentioned. These polyfunctional (meth) acrylates may be used singly or in combination of two or more.

本発明においては、前記多官能性(メタ)アクリレートとともに、その粘度を低下させるなどの目的で、単官能性(メタ)アクリレートを、本発明の目的を損なわない範囲で適宜併用することができる。単官能性(メタ)アクリレートとしては、例えば、メチル(メタ)アクリレート、エチル(メタ)アクリレート、プロピル(メタ)アクリレート、ブチル(メタ)アクリレート、ペンチル(メタ)アクリレート、ヘキシル(メタ)アクリレート、シクロヘキシル(メタ)アクリレート、2−エチルヘキシル(メタ)アクリレート、ラウリル(メタ)アクリレート、ステアリル(メタ)アクリレート、イソボルニル(メタ)アクリレートなどが挙げられる。これらの単官能性(メタ)アクリレートは1種を単独で用いてもよいし、2種以上を組み合わせて用いてもよい。   In the present invention, a monofunctional (meth) acrylate can be used in combination with the polyfunctional (meth) acrylate as long as the object of the present invention is not impaired, for the purpose of lowering the viscosity. Examples of monofunctional (meth) acrylates include methyl (meth) acrylate, ethyl (meth) acrylate, propyl (meth) acrylate, butyl (meth) acrylate, pentyl (meth) acrylate, hexyl (meth) acrylate, cyclohexyl ( Examples include meth) acrylate, 2-ethylhexyl (meth) acrylate, lauryl (meth) acrylate, stearyl (meth) acrylate, and isobornyl (meth) acrylate. These monofunctional (meth) acrylates may be used alone or in combination of two or more.

次に、重合性オリゴマーとしては、分子中にラジカル重合性不飽和基を持つオリゴマー、例えばエポキシ(メタ)アクリレート系、ウレタン(メタ)アクリレート系、ポリエステル(メタ)アクリレート系、ポリエーテル(メタ)アクリレート系のオリゴマーなどが挙げられる。ここで、エポキシ(メタ)アクリレート系オリゴマーは、例えば、比較的低分子量のビスフェノール型エポキシ樹脂やノボラック型エポキシ樹脂のオキシラン環に、(メタ)アクリル酸を反応しエステル化することにより得ることができる。また、このエポキシ(メタ)アクリレート系オリゴマーを部分的に二塩基性カルボン酸無水物で変性したカルボキシル変性型のエポキシ(メタ)アクリレートオリゴマーも用いることができる。ウレタン(メタ)アクリレート系オリゴマーは、例えば、ポリエーテルポリオールやポリエステルポリオールとポリイソシアネートの反応によって得られるポリウレタンオリゴマーを、(メタ)アクリル酸でエステル化することにより得ることができる。ポリエステル(メタ)アクリレート系オリゴマーとしては、例えば多価カルボン酸と多価アルコールの縮合によって得られる両末端に水酸基を有するポリエステルオリゴマーの水酸基を(メタ)アクリル酸でエステル化することにより、あるいは、多価カルボン酸にアルキレンオキシドを付加して得られるオリゴマーの末端の水酸基を(メタ)アクリル酸でエステル化することにより得ることができる。ポリエーテル(メタ)アクリレート系オリゴマーは、ポリエーテルポリオールの水酸基を(メタ)アクリル酸でエステル化することにより得ることができる。   Next, as the polymerizable oligomer, an oligomer having a radical polymerizable unsaturated group in the molecule, for example, epoxy (meth) acrylate, urethane (meth) acrylate, polyester (meth) acrylate, polyether (meth) acrylate System oligomers and the like. Here, the epoxy (meth) acrylate oligomer can be obtained, for example, by reacting (meth) acrylic acid with an oxirane ring of a relatively low molecular weight bisphenol type epoxy resin or novolak type epoxy resin and esterifying it. . Further, a carboxyl-modified epoxy (meth) acrylate oligomer obtained by partially modifying this epoxy (meth) acrylate oligomer with a dibasic carboxylic acid anhydride can also be used. The urethane (meth) acrylate oligomer can be obtained, for example, by esterifying a polyurethane oligomer obtained by reaction of polyether polyol or polyester polyol and polyisocyanate with (meth) acrylic acid. Examples of polyester (meth) acrylate oligomers include esterification of hydroxyl groups of polyester oligomers having hydroxyl groups at both ends obtained by condensation of polycarboxylic acid and polyhydric alcohol with (meth) acrylic acid, It can be obtained by esterifying the terminal hydroxyl group of an oligomer obtained by adding an alkylene oxide to a carboxylic acid with (meth) acrylic acid. The polyether (meth) acrylate oligomer can be obtained by esterifying the hydroxyl group of the polyether polyol with (meth) acrylic acid.

さらに、重合性オリゴマーとしては、他にポリブタジエンオリゴマーの側鎖に(メタ)アクリレート基をもつ疎水性の高いポリブタジエン(メタ)アクリレート系オリゴマー、主鎖にポリシロキサン結合をもつシリコーン(メタ)アクリレート系オリゴマー、小さな分子内に多くの反応性基をもつアミノプラスト樹脂を変性したアミノプラスト樹脂(メタ)アクリレート系オリゴマー、あるいはノボラック型エポキシ樹脂、ビスフェノール型エポキシ樹脂、脂肪族ビニルエーテル、芳香族ビニルエーテル等の分子中にカチオン重合性官能基を有するオリゴマーなどがある。   Furthermore, other polymerizable oligomers include polybutadiene (meth) acrylate oligomers with high hydrophobicity that have (meth) acrylate groups in the side chain of polybutadiene oligomers, and silicone (meth) acrylate oligomers that have polysiloxane bonds in the main chain. In a molecule such as an aminoplast resin (meth) acrylate oligomer modified with an aminoplast resin having many reactive groups in a small molecule, or a novolak epoxy resin, bisphenol epoxy resin, aliphatic vinyl ether, aromatic vinyl ether, etc. There are oligomers having a cationic polymerizable functional group.

電離放射線硬化性樹脂組成物として紫外線硬化性樹脂組成物を用いる場合には、光重合用開始剤を樹脂組成物100質量部に対して、0.1〜5質量部程度添加することが望ましい。光重合用開始剤としては、従来慣用されているものから適宜選択することができ、特に限定されず、例えば、分子中にラジカル重合性不飽和基を有する重合性モノマーや重合性オリゴマーに対しては、ベンゾイン、ベンゾインメチルエーテル、ベンゾインエチルエーテル、ベンゾインイソプロピルエーテル、ベンゾイン−n−ブチルエーテル、ベンゾインイソブチルエーテル、アセトフェノン、ジメチルアミノアセトフェノン、2,2−ジメトキシ−2−フェニルアセトフェノン、2,2−ジエトキシ−2−フェニルアセトフェノン、2−ヒドロキシ−2−メチル−1−フェニルプロパン−1−オン、1−ヒドロキシシクロヘキシルフェニルケトン、2−メチル−1−[4−(メチルチオ)フェニル]−2−モルフォリノ−プロパン−1−オン、4−(2−ヒドロキシエトキシ)フェニル−2(ヒドロキシ−2−プロピル)ケトン、ベンゾフェノン、p−フェニルベンゾフェノン、4,4’−ジエチルアミノベンゾフェノン、ジクロロベンゾフェノン、2−メチルアントラキノン、2−エチルアントラキノン、2−ターシャリーブチルアントラキノン、2−アミノアントラキノン、2−メチルチオキサントン、2−エチルチオキサントン、2−クロロチオキサントン、2,4−ジメチルチオキサントン、2,4−ジエチルチオキサントン、ベンジルジメチルケタール、アセトフェノンジメチルケタールなどが挙げられる。
また、分子中にカチオン重合性官能基を有する重合性オリゴマー等に対しては、芳香族スルホニウム塩、芳香族ジアゾニウム塩、芳香族ヨードニウム塩、メタロセン化合物、ベンゾインスルホン酸エステル等が挙げられる。
また、光増感剤としては、例えばp−ジメチル安息香酸エステル、第三級アミン類、チオール系増感剤などを用いることができる。
When an ultraviolet curable resin composition is used as the ionizing radiation curable resin composition, it is desirable to add about 0.1 to 5 parts by mass of the photopolymerization initiator with respect to 100 parts by mass of the resin composition. The initiator for photopolymerization can be appropriately selected from those conventionally used and is not particularly limited. For example, for a polymerizable monomer or polymerizable oligomer having a radically polymerizable unsaturated group in the molecule. Benzoin, benzoin methyl ether, benzoin ethyl ether, benzoin isopropyl ether, benzoin-n-butyl ether, benzoin isobutyl ether, acetophenone, dimethylaminoacetophenone, 2,2-dimethoxy-2-phenylacetophenone, 2,2-diethoxy-2 -Phenylacetophenone, 2-hydroxy-2-methyl-1-phenylpropan-1-one, 1-hydroxycyclohexyl phenyl ketone, 2-methyl-1- [4- (methylthio) phenyl] -2-morpholino-propane-1 - 4- (2-hydroxyethoxy) phenyl-2 (hydroxy-2-propyl) ketone, benzophenone, p-phenylbenzophenone, 4,4′-diethylaminobenzophenone, dichlorobenzophenone, 2-methylanthraquinone, 2-ethylanthraquinone, 2 -Tertiary butylanthraquinone, 2-aminoanthraquinone, 2-methylthioxanthone, 2-ethylthioxanthone, 2-chlorothioxanthone, 2,4-dimethylthioxanthone, 2,4-diethylthioxanthone, benzyldimethyl ketal, acetophenone dimethyl ketal It is done.
Examples of the polymerizable oligomer having a cationic polymerizable functional group in the molecule include aromatic sulfonium salts, aromatic diazonium salts, aromatic iodonium salts, metallocene compounds, and benzoin sulfonic acid esters.
Moreover, as a photosensitizer, p-dimethylbenzoic acid ester, tertiary amines, a thiol type sensitizer, etc. can be used, for example.

本発明で用いられる化粧シート10においては、電離放射線硬化性樹脂として電子線硬化性樹脂を用いることが好ましい。電子線硬化性樹脂は無溶剤化が可能であって、環境や健康の観点からより好ましく、また光重合用開始剤を必要とせず、安定な硬化特性が得られるからである。   In the decorative sheet 10 used in the present invention, it is preferable to use an electron beam curable resin as the ionizing radiation curable resin. This is because the electron beam curable resin can be made solvent-free, is more preferable from the viewpoint of environment and health, and does not require a photopolymerization initiator, and can provide stable curing characteristics.

また、電離放射線硬化性樹脂組成物には、得られる硬化樹脂層の所望物性に応じて、各種添加剤を配合することができる。この添加剤としては、例えば耐候性改善剤、耐摩耗性向上剤、重合禁止剤、架橋剤、赤外線吸収剤、帯電防止剤、接着性向上剤、酸化防止剤、レベリング剤、チクソ性付与剤、カップリング剤、可塑剤、消泡剤、充填剤、溶剤などが挙げられる。
ここで、耐候性改善剤としては、紫外線吸収剤や光安定剤を用いることができる。化粧シートの長期使用を図るために添加するものである。紫外線吸収剤は、無機系、有機系のいずれでもよく、無機系紫外線吸収剤としては、平均粒径が5〜120nm程度の二酸化チタン、酸化セリウム、酸化亜鉛などを好ましく用いることができる。また、有機系紫外線吸収剤としては、例えばベンゾトリアゾール系、具体的には、2−(2−ヒドロキシ−5−メチルフェニル)ベンゾトリアゾール、2−(2−ヒドロキシ−3,5−ジ−tert−アミルフェニル)ベンゾトリアゾール、ポリエチレングリコールの3−[3−(ベンゾトリアゾール−2−イル)−5−tert−ブチル−4−ヒドロキシフェニル]プロピオン酸エステルなどが挙げられる。一方、光安定剤としては、例えばヒンダードアミン系、具体的には2−(3,5−ジ−tert−ブチル−4−ヒドロキシベンジル)−2’−n−ブチルマロン酸ビス(1,2,2,6,6−ペンタメチル−4−ピペリジル)、ビス(1,2,2,6,6−ペンタメチル−4−ピペリジル)セバケート、テトラキス(2,2,6,6−テトラメチル−4−ピペリジル)−1,2,3,4−ブタンテトラカルボキシレートなどが挙げられる。また、紫外線吸収剤や光安定剤として、分子内に(メタ)アクリロイル基などの重合性基を有する反応性の紫外線吸収剤や光安定剤を用いることもできる。
Moreover, various additives can be mix | blended with an ionizing radiation curable resin composition according to the desired physical property of the cured resin layer obtained. Examples of the additive include a weather resistance improver, an abrasion resistance improver, a polymerization inhibitor, a crosslinking agent, an infrared absorber, an antistatic agent, an adhesion improver, an antioxidant, a leveling agent, a thixotropic agent, Examples include coupling agents, plasticizers, antifoaming agents, fillers, and solvents.
Here, as the weather resistance improving agent, an ultraviolet absorber or a light stabilizer can be used. It is added for long-term use of the decorative sheet. The ultraviolet absorber may be either inorganic or organic, and as the inorganic ultraviolet absorber, titanium dioxide, cerium oxide, zinc oxide or the like having an average particle diameter of about 5 to 120 nm can be preferably used. Examples of the organic ultraviolet absorber include benzotriazole-based compounds, specifically 2- (2-hydroxy-5-methylphenyl) benzotriazole, 2- (2-hydroxy-3,5-di-tert-). Amylphenyl) benzotriazole, 3- [3- (benzotriazol-2-yl) -5-tert-butyl-4-hydroxyphenyl] propionic acid ester of polyethylene glycol, and the like. On the other hand, examples of the light stabilizer include hindered amines, specifically 2- (3,5-di-tert-butyl-4-hydroxybenzyl) -2′-n-butylmalonate bis (1,2,2). , 6,6-pentamethyl-4-piperidyl), bis (1,2,2,6,6-pentamethyl-4-piperidyl) sebacate, tetrakis (2,2,6,6-tetramethyl-4-piperidyl)- 1,2,3,4-butanetetracarboxylate and the like. Further, as the ultraviolet absorber or light stabilizer, a reactive ultraviolet absorber or light stabilizer having a polymerizable group such as a (meth) acryloyl group in the molecule can be used.

耐摩耗性向上剤としては、例えば無機物ではα−アルミナ、シリカ、カオリナイト、酸化鉄、ダイヤモンド、炭化ケイ素等の球状粒子が挙げられる。粒子形状は、球、楕円体、多面体、鱗片形等が挙げられ、特に制限はないが、球状が好ましい。有機物では架橋アクリル樹脂、ポリカーボネート樹脂等の合成樹脂ビーズが挙げられる。粒径は、通常膜厚の30〜200%程度とする。これらの中でも球状のα−アルミナは、硬度が高く、耐摩耗性の向上に対する効果が大きいこと、また、球状の粒子を比較的得やすい点で特に好ましいものである。
重合禁止剤としては、例えばハイドロキノン、p−ベンゾキノン、ハイドロキノンモノメチルエーテル、ピロガロール、t−ブチルカテコールなどが、架橋剤としては、例えばポリイソシアネート化合物、エポキシ化合物、金属キレート化合物、アジリジン化合物、オキサゾリン化合物などが用いられる。
充填剤としては、例えば硫酸バリウム、タルク、クレー、炭酸カルシウム、水酸化アルミニウムなどが用いられる。
赤外線吸収剤としては、例えば、ジチオール系金属錯体、フタロシアニン系化合物、ジインモニウム化合物等が用いられる。
Examples of the wear resistance improver include, for inorganic substances, spherical particles such as α-alumina, silica, kaolinite, iron oxide, diamond, and silicon carbide. Examples of the particle shape include a sphere, an ellipsoid, a polyhedron, a scale shape, and the like. Although there is no particular limitation, a spherical shape is preferable. Organic materials include synthetic resin beads such as cross-linked acrylic resin and polycarbonate resin. The particle size is usually about 30 to 200% of the film thickness. Among these, spherical α-alumina is particularly preferable because it has high hardness and a large effect on improving wear resistance, and it is relatively easy to obtain spherical particles.
Examples of the polymerization inhibitor include hydroquinone, p-benzoquinone, hydroquinone monomethyl ether, pyrogallol, and t-butylcatechol. Examples of the crosslinking agent include a polyisocyanate compound, an epoxy compound, a metal chelate compound, an aziridine compound, and an oxazoline compound. Used.
As the filler, for example, barium sulfate, talc, clay, calcium carbonate, aluminum hydroxide and the like are used.
As the infrared absorber, for example, a dithiol metal complex, a phthalocyanine compound, a diimmonium compound, or the like is used.

また、表面保護層は、その他の成分として焼成カオリン粒子を含有することが好ましい。この表面保護層中に焼成カオリン粒子を含有させることで、耐マーリング(marring)性が向上する。ここでマーリングとは、シート表面が擦られた場合に、小さい擦り傷が発生することをいい、耐マーリング性が優れているとは、擦り傷ができにくいことをいう。   The surface protective layer preferably contains calcined kaolin particles as other components. By including the calcined kaolin particles in the surface protective layer, the marring resistance is improved. Here, the term “marling” means that small scratches are generated when the sheet surface is rubbed, and “excellent marring resistance” means that scratches are difficult to be made.

化粧シートの表面に耐マーリング性を付与するために使用する焼成カオリン粒子は、一般的な(含水)カオリン粒子を焼成して得られるカオリン粒子であるが、充填剤として焼成カオリン粒子を添加することで、シリカ粒子や焼成前の含水カオリン粒子では実現できなかった耐マーリング性の改善が実現する。なお、焼成カオリン粒子の粒径は、用途、要求物性等に応じて適宜選択すればよいが、例えば平均粒径で0.5〜2μm程度のものを使用する。また、焼成カオリン粒子の添加量も、用途、要求物性等に応じて適宜選択すれば良いが、例えば、電離放射線硬化性樹脂(ただし、表面保護層が、他の樹脂を含む場合には、電離放射線硬化性樹脂とその他の樹脂との合計)100質量部に対して5〜50質量部程度である。なお、焼成カオリン粒子は含水カオリン粒子よりも塗料安定性にも優れている。   The calcined kaolin particles used for imparting marring resistance to the surface of the decorative sheet are kaolin particles obtained by calcining general (hydrous) kaolin particles, but the calcined kaolin particles should be added as a filler. Thus, the improvement in marring resistance, which could not be realized with silica particles or hydrous kaolin particles before firing, is realized. The particle size of the calcined kaolin particles may be appropriately selected according to the application, required physical properties, etc. For example, those having an average particle size of about 0.5 to 2 μm are used. Also, the amount of calcined kaolin particles added may be appropriately selected according to the application, required physical properties, etc., for example, ionizing radiation curable resin (however, if the surface protective layer contains other resins, ionization The total of the radiation curable resin and other resin) is about 5 to 50 parts by mass with respect to 100 parts by mass. The calcined kaolin particles are superior in paint stability to the hydrous kaolin particles.

焼成カオリン粒子としては、さらにその表面を処理したものを用いても良い。この表面処理された焼成カオリン粒子を用いることで、耐マーリング性向上効果をさらに増すことができる。表面処理としては、シランカップリング剤による表面処理がある。該シランカップリング剤としては、アルコキシ基、アミノ基、ビニル基、エポキシ基、メルカプト基、クロル基等を有する公知のシランカップリング剤が挙げられる。例えば、γ―アミノプロピルトリエトキシシラン、γ―メタクリロキシプロピルトリメトキシシラン、γ―メタクリロキシプロピルメチルジメトキシシラン、γ―メタクリロキシプロピルジメチルメトキシシラン、γ―メタクリロキシプロピルトリエトキシシラン、γ―メタクリロキシプロピルジメチルエトキシシラン、γ―アクリロキシプロピルトリメトキシシラン、γ―アクリロキシプロピルメチルジメトキシシラン、γ―アクリロキシプロピルジメチルメトキシシラン、γ―アクリロキシプロピルトリエトキシシラン、γ―アクリロキシプロピルメチルジエトキシシラン、γ―アクリロキシプロピルジメチルエトキシシラン、ビニルトリエトキシシラン、γ―グリシドキシプロピルトリメトキシシラン、γ―メルカプトプロピルトリメトキシシランなどである。   As the calcined kaolin particles, those whose surfaces are further treated may be used. By using the surface-treated calcined kaolin particles, the effect of improving marring resistance can be further increased. As the surface treatment, there is a surface treatment with a silane coupling agent. Examples of the silane coupling agent include known silane coupling agents having an alkoxy group, amino group, vinyl group, epoxy group, mercapto group, chloro group and the like. For example, γ-aminopropyltriethoxysilane, γ-methacryloxypropyltrimethoxysilane, γ-methacryloxypropylmethyldimethoxysilane, γ-methacryloxypropyldimethylmethoxysilane, γ-methacryloxypropyltriethoxysilane, γ-methacryloxy Propyldimethylethoxysilane, γ-acryloxypropyltrimethoxysilane, γ-acryloxypropylmethyldimethoxysilane, γ-acryloxypropyldimethylmethoxysilane, γ-acryloxypropyltriethoxysilane, γ-acryloxypropylmethyldiethoxysilane , Γ-acryloxypropyldimethylethoxysilane, vinyltriethoxysilane, γ-glycidoxypropyltrimethoxysilane, γ-mercaptopropyltrimethoxysila Etc.

化粧シート10の表面保護層60は、例えば以下のように形成することができる。まず、前記の電離放射線硬化性樹脂、必要に応じて配合されるその他の成分及び各種添加剤を、それぞれ所定の割合で均質に混合し、電離放射線硬化性樹脂組成物からなる塗工液を調製する。この塗工液の粘度は、後述の塗工方式により、基材の表面に未硬化樹脂層を形成し得る粘度であればよく、特に制限はない。
このようにして調製された塗工液を、基材の表面に、硬化後の厚さが1〜20μmになるように、グラビアコート、バーコート、ロールコート、リバースロールコート、コンマコートなどの公知の方式、好ましくはグラビアコートにより塗工し、未硬化樹脂層を形成させる。
The surface protective layer 60 of the decorative sheet 10 can be formed as follows, for example. First, the above-mentioned ionizing radiation curable resin, other components to be blended as necessary, and various additives are homogeneously mixed at predetermined ratios to prepare a coating liquid comprising an ionizing radiation curable resin composition. To do. The viscosity of the coating solution is not particularly limited as long as it is a viscosity capable of forming an uncured resin layer on the surface of the substrate by a coating method described later.
Gravure coating, bar coating, roll coating, reverse roll coating, comma coating, etc., so that the coating liquid prepared in this manner is applied to the surface of the substrate so that the thickness after curing is 1 to 20 μm. This method is preferably applied by gravure coating to form an uncured resin layer.

このようにして形成された未硬化樹脂層に、電子線、紫外線等の電離放射線を照射して該未硬化樹脂層を硬化させると、硬化後の厚さが1μm以上であると所望の機能を有する硬化樹脂層が得られる。硬化後の表面保護層の厚さは、好ましくは2〜20μm程度である。
ここで、電離放射線として電子線を用いる場合、その加速電圧については、用いる樹脂や層の厚みに応じて適宜選定し得るが、通常加速電圧70〜300kV程度で未硬化樹脂層を硬化させることが好ましい。
なお、電子線の照射においては、加速電圧が高いほど透過能力が増加するため、基材として電子線により劣化する基材を使用する場合には、電子線の透過深さと樹脂層の厚みが実質的に等しくなるように、加速電圧を選定することにより、基材への余分の電子線の照射を抑制することができ、過剰電子線による基材の劣化を最小限にとどめることができる。
また、照射線量は、樹脂層の架橋密度が飽和する量が好ましく、通常5〜300kGy(0.5〜30Mrad)、好ましくは10〜50kGy(1〜5Mrad)の範囲で選定される。
さらに、電子線源としては、特に制限はなく、例えばコックロフトワルトン型、バンデグラフト型、共振変圧器型、絶縁コア変圧器型、あるいは直線型、ダイナミトロン型、高周波型などの各種電子線加速器を用いることができる。
電離放射線として紫外線を用いる場合には、波長190〜380nmの紫外線を含むものを放射する。紫外線源としては特に制限はなく、例えば高圧水銀燈、低圧水銀燈、メタルハライドランプ、カーボンアーク燈等が用いられる。
このようにして、形成された硬化樹脂層には、各種の添加剤を添加して各種の機能、例えば、高硬度で耐擦傷性を有する、いわゆるハードコート機能、防曇コート機能、防汚コート機能、防眩コート機能、反射防止コート機能、紫外線遮蔽コート機能、赤外線遮蔽コート機能などを付与することもできる。
When the uncured resin layer thus formed is irradiated with ionizing radiation such as an electron beam and ultraviolet rays to cure the uncured resin layer, the desired function is obtained when the thickness after curing is 1 μm or more. A cured resin layer is obtained. The thickness of the surface protective layer after curing is preferably about 2 to 20 μm.
Here, when an electron beam is used as the ionizing radiation, the acceleration voltage can be appropriately selected according to the resin used and the thickness of the layer, but the uncured resin layer is usually cured at an acceleration voltage of about 70 to 300 kV. preferable.
In electron beam irradiation, the transmission capability increases as the acceleration voltage increases. Therefore, when using a base material that deteriorates due to the electron beam as the base material, the transmission depth of the electron beam and the thickness of the resin layer are substantially equal. By selecting the accelerating voltage so as to be equal to each other, it is possible to suppress the irradiation of the electron beam to the base material, and to minimize the deterioration of the base material due to the excessive electron beam.
The irradiation dose is preferably such that the crosslink density of the resin layer is saturated, and is usually selected in the range of 5 to 300 kGy (0.5 to 30 Mrad), preferably 10 to 50 kGy (1 to 5 Mrad).
Further, the electron beam source is not particularly limited. For example, various electron beam accelerators such as a cockroft Walton type, a bandegraft type, a resonant transformer type, an insulated core transformer type, a linear type, a dynamitron type, and a high frequency type. Can be used.
When ultraviolet rays are used as the ionizing radiation, those containing ultraviolet rays having a wavelength of 190 to 380 nm are emitted. There is no restriction | limiting in particular as an ultraviolet-ray source, For example, a high pressure mercury lamp, a low pressure mercury lamp, a metal halide lamp, a carbon arc lamp, etc. are used.
The cured resin layer thus formed has various functions by adding various additives, for example, a so-called hard coat function, anti-fogging coat function, and anti-fouling coat having high hardness and scratch resistance. A function, an antiglare coating function, an antireflection coating function, an ultraviolet shielding coating function, an infrared shielding coating function, and the like can also be imparted.

<装飾層>
本発明の化粧シート10では、化粧シートに装飾性を付与するために、装飾層30を設けることができる。装飾層は基材20と盛上層50の間に設けることが好ましく、より具体的には、図1に好適な態様として示すように、基材20上に設けることが好ましい。装飾層はベタ印刷層31のみからなってもよく、ベタ印刷層31と絵柄層32により構成されてもよい。
本発明の化粧シートにおいて、基材上に設けられるベタ印刷層は、本発明の化粧シートの意匠性を高めるために所望により設けられる、隠蔽層とも称されるものである。ベタ印刷層は、基材の表面の色を整えることで、化粧シート自身が着色していたり、色ムラがあるときに形成して、化粧シートの表面に意図した色彩を与えるものである。通常不透明色で形成することが多いが、着色透明色で形成し、下地が持っている模様を活かす場合もある。基材が白色であることを活かす場合や、基材自身が適切に着色されている場合にはベタ印刷層の形成を行う必要はない。
ベタ印刷層の形成に用いられるインキとしては、バインダーに顔料、染料などの着色剤、体質顔料、溶剤、安定剤、可塑剤、触媒、硬化剤などを適宜混合したものが使用される。該バインダーとしては特に制限はなく、例えば、ポリウレタン系樹脂、塩化ビニル−酢酸ビニル系共重合体樹脂、塩化ビニル−酢酸ビニル−アクリル系共重合体樹脂、塩素化ポリプロピレン系樹脂、アクリル系樹脂、ポリエステル系樹脂、ポリアミド系樹脂、ブチラール系樹脂、ポリスチレン系樹脂、ニトロセルロース系樹脂、酢酸セルロース系樹脂などの中から任意のものが、1種単独で又は2種以上を混合して用いられる。
着色剤としては、カーボンブラック(墨)、鉄黒、チタン白、アンチモン白、黄鉛、チタン黄、弁柄、カドミウム赤、群青、コバルトブルー等の無機顔料、キナクリドンレッド、イソインドリノンイエロー、フタロシアニンブルー等の有機顔料又は染料、アルミニウム、真鍮等の鱗片状箔片からなる金属顔料、二酸化チタン被覆雲母、塩基性炭酸鉛等の鱗片状箔片からなる真珠光沢(パール)顔料等が用いられる。
このベタ印刷層の厚さは1〜20μm程度であることが好ましい。
<Decoration layer>
In the decorative sheet 10 of the present invention, a decorative layer 30 can be provided in order to impart decorativeness to the decorative sheet. The decoration layer is preferably provided between the base material 20 and the raised layer 50, and more specifically, it is preferably provided on the base material 20 as shown in a preferred embodiment in FIG. The decoration layer may consist of only the solid print layer 31 or may be constituted by the solid print layer 31 and the pattern layer 32.
In the decorative sheet of the present invention, the solid print layer provided on the substrate is also referred to as a concealing layer provided as desired in order to enhance the design of the decorative sheet of the present invention. The solid print layer is formed when the color of the surface of the base material is adjusted so that the decorative sheet itself is colored or uneven in color, and gives the intended color to the surface of the decorative sheet. Usually, it is formed with an opaque color, but it may be formed with a colored transparent color to make use of the pattern of the base. When taking advantage of the fact that the base material is white or when the base material itself is appropriately colored, there is no need to form a solid print layer.
As the ink used for forming the solid printing layer, an ink obtained by appropriately mixing a binder, a colorant such as a pigment or a dye, an extender pigment, a solvent, a stabilizer, a plasticizer, a catalyst, or a curing agent is used. The binder is not particularly limited, and examples thereof include polyurethane resins, vinyl chloride-vinyl acetate copolymer resins, vinyl chloride-vinyl acetate-acrylic copolymer resins, chlorinated polypropylene resins, acrylic resins, polyesters. Arbitrary resins, polyamide resins, butyral resins, polystyrene resins, nitrocellulose resins, cellulose acetate resins and the like may be used alone or in combination of two or more.
Colorants include carbon black (black), iron black, titanium white, antimony white, yellow lead, titanium yellow, petal, cadmium red, ultramarine, cobalt blue and other inorganic pigments, quinacridone red, isoindolinone yellow, phthalocyanine Organic pigments or dyes such as blue, metallic pigments composed of scaly foil pieces such as aluminum and brass, pearlescent pigments composed of scaly foil pieces such as titanium dioxide-coated mica and basic lead carbonate, and the like are used.
The thickness of the solid print layer is preferably about 1 to 20 μm.

絵柄層32は、化粧シートに装飾性を与えるものであり、基材20上に、又はベタ印刷層31上に、種々の模様をインキと印刷機を使用して印刷することにより形成される。模様としては、木目模様、大理石模様(例えばトラバーチン大理石模様)等の岩石の表面を模した石目模様、布目や布状の模様を模した布地模様、タイル貼模様、煉瓦積模様等があり、これらを複合した寄木、パッチワーク等の模様もある。これらの模様は通常の黄色、赤色、青色、および黒色のプロセスカラーによる多色印刷によって形成される他、模様を構成する個々の色の版を用意して行う特色による多色印刷等によっても形成される。
絵柄層32に用いる絵柄インキとしては、ベタ印刷層に用いるインキと同様のものを用いることができる。
The pattern layer 32 gives decorativeness to the decorative sheet, and is formed by printing various patterns on the base material 20 or the solid print layer 31 using ink and a printing machine. As patterns, there are stone patterns imitating the surface of rocks, such as wood grain patterns, marble patterns (for example, travertine marble patterns), fabric patterns imitating cloth or cloth-like patterns, tiled patterns, brickwork patterns, etc. There are also patterns such as marquetry and patchwork that combine these. These patterns are formed by multicolor printing with the usual yellow, red, blue and black process colors, as well as by multicolor printing with special colors prepared by preparing the individual color plates that make up the pattern. Is done.
As the pattern ink used for the pattern layer 32, the same ink as that used for the solid print layer can be used.

<プライマー層>
本発明の化粧シート10は、基材20上にプライマー層40を有し、該プライマー層上に盛上層50を有することが好ましい。該プライマー層には種々の機能を持たせることができる。
その機能の一つとして艶消し機能がある。すなわち、当該プライマー層に艶消剤を含有させ、化粧シート全体の艶を下げる機能である。
当該艶消剤としては、無機微粒子及び有機微粒子のいずれであってもよい。当該微粒子の例としては、無機微粒子として、シリカ、アルミナ、アルミノシリケート、カオリナイト、炭酸カルシウム、硫酸バリウム、ガラスなどの粒子を挙げることができ、有機微粒子として、アクリル系樹脂、ポリカーボネート樹脂、ウレタン系樹脂、尿素系樹脂、ベンゾグアナミン樹脂、ベンゾグアナミン−メラミン−ホルムアルデヒド縮合物などの粒子を挙げることができる。これらのうち、本発明の効果の点から、シリカ粒子が好適であり、効果及び取扱い性の観点から、その粒径は1〜10μmの範囲が好ましく、さらには2〜5μmの範囲が好ましい。
また、これらの微粒子は1種を単独で用いてもよく、2種以上を組み合わせて用いてもよい。
<Primer layer>
The decorative sheet 10 of the present invention preferably has the primer layer 40 on the substrate 20 and has the raised layer 50 on the primer layer. The primer layer can have various functions.
One of the functions is a matte function. That is, the primer layer contains a matting agent to lower the gloss of the entire decorative sheet.
The matting agent may be either inorganic fine particles or organic fine particles. Examples of the fine particles include inorganic fine particles such as silica, alumina, aluminosilicate, kaolinite, calcium carbonate, barium sulfate, and glass, and the organic fine particles include acrylic resin, polycarbonate resin, and urethane. Examples thereof include particles such as resin, urea resin, benzoguanamine resin, and benzoguanamine-melamine-formaldehyde condensate. Among these, silica particles are preferable from the viewpoint of the effects of the present invention, and the particle diameter is preferably in the range of 1 to 10 μm, and more preferably in the range of 2 to 5 μm, from the viewpoints of effects and handleability.
Moreover, these fine particles may be used individually by 1 type, and may be used in combination of 2 or more type.

また、プライマー層が有する他の機能として浸透防止機能がある。すなわち、盛上部を構成する樹脂組成物及び表面保護層を構成する電離放射線硬化性樹脂組成物が、基材中に浸透することを抑制する機能である。基材が紙や不織布などの浸透性基材である場合に特に効果を発揮する。
また、基材20又は装飾層30と盛上層50との接着性を高める機能をも併せて持たせることもできる。
Another function of the primer layer is a penetration preventing function. That is, it is a function which suppresses that the resin composition which comprises an elevated part, and the ionizing radiation-curable resin composition which comprises a surface protective layer penetrate | invade in a base material. This is particularly effective when the substrate is a permeable substrate such as paper or nonwoven fabric.
Moreover, the function which improves the adhesiveness of the base material 20 or the decoration layer 30, and the build-up layer 50 can also be given together.

<裏面プライマー層>
本発明の化粧シートにおいては、装飾層、盛上層、表面保護層等が形成される側の反対側、すなわち基材の裏面側に裏面プライマー層70を設けることができる。裏面プライマー層によって、後述する化粧板を作製するに際し、基板との密着性及び接着性を向上させることができる。
裏面プライマー層に用いる材料としては、基板との密着性及び接着性を向上させることができるものであれば特に制限はなく、具体的には、ウレタン樹脂、アクリル樹脂、ポリエステル樹脂、塩化ビニル−酢酸ビニル共重合体、塩素化ポリプロピレン樹脂、塩素化ポリエチレン樹脂などが好ましく挙げられ、なかでもウレタン樹脂が好ましい。なお、裏面プライマー層7用いられる材料は被着材によって、適宜選択される。
また、裏面プライマー層の厚さは、1〜5μm程度であることが好ましく、より好ましくは1〜3μmである。厚さが上記範囲内であると、効率よく、プライマー層としての優れた性能を得ることができる。
<Backside primer layer>
In the decorative sheet of the present invention, the back primer layer 70 can be provided on the side opposite to the side on which the decorative layer, the raised layer, the surface protective layer and the like are formed, that is, on the back side of the substrate. With the back primer layer, adhesion and adhesion to the substrate can be improved when producing a decorative board to be described later.
The material used for the back primer layer is not particularly limited as long as it can improve the adhesion and adhesion to the substrate. Specifically, urethane resin, acrylic resin, polyester resin, vinyl chloride-acetic acid Preferred examples include vinyl copolymers, chlorinated polypropylene resins, and chlorinated polyethylene resins. Among these, urethane resins are preferred. In addition, the material used for the back surface primer layer 7 is appropriately selected depending on the adherend.
Moreover, it is preferable that the thickness of a back surface primer layer is about 1-5 micrometers, More preferably, it is 1-3 micrometers. When the thickness is within the above range, excellent performance as a primer layer can be obtained efficiently.

<化粧板>
本発明の化粧シート10は、各種基板に貼着して化粧板として使用することができる。被着体となる基板は、特に限定されず、プラスチックシート、金属板、木材などの木質系の板、窯業系素材等を用途に応じて適宜選択することができる。これらの基板、特にプラスチックシートを基板として用いる場合には、化粧シートとの密着性を向上させるために、所望により、片面又は両面に酸化法や凹凸化法などの物理的又は化学的表面処理を施すことができる。
上記酸化法としては、例えばコロナ放電処理、クロム酸化処理、火炎処理、熱風処理、オゾン処理及び紫外線処理法などが挙げられ、凹凸化法としては、例えばサンドブラスト法、溶剤処理法などが挙げられる。これらの表面処理は、基材の種類に応じて適宜選択されるが、一般にはコロナ放電処理法が効果及び操作性などの面から好ましく用いられる。
<Decorative board>
The decorative sheet 10 of the present invention can be used as a decorative plate by sticking to various substrates. The board | substrate used as a to-be-adhered body is not specifically limited, A plastic board, a metal board, woody board | plates, such as a timber, a ceramic material, etc. can be selected suitably according to a use. When these substrates, particularly plastic sheets, are used as substrates, a physical or chemical surface treatment such as an oxidation method or a concavo-convex method is applied to one or both sides as desired in order to improve adhesion to the decorative sheet. Can be applied.
Examples of the oxidation method include corona discharge treatment, chromium oxidation treatment, flame treatment, hot air treatment, ozone treatment, and ultraviolet treatment method. Examples of the unevenness method include a sand blast method and a solvent treatment method. These surface treatments are appropriately selected depending on the type of substrate, but generally, a corona discharge treatment method is preferably used from the viewpoints of effects and operability.

プラスチックシートとしては、各種の合成樹脂からなるものが挙げられる。合成樹脂としては、ポリエチレン樹脂、ポリプロピレン樹脂、ポリメチルペンテン樹脂、ポリ塩化ビニル樹脂、ポリ塩化ビニリデン樹脂、ポリビニルアルコール樹脂、塩化ビニル−酢酸ビニル共重合樹脂、エチレン−酢酸ビニル共重合樹脂、エチレン−ビニルアルコール共重合樹脂、ポリエチレンテレフタレート樹脂、ポリブチレンテレフタレート樹脂、ポリエチレンナフタレート−イソフタレート共重合樹脂、ポリメタクリル酸メチル樹脂、ポリメタクリル酸エチル樹脂、ポリアクリル酸ブチル樹脂、ナイロン6又はナイロン66等で代表されるポリアミド樹脂、三酢酸セルロース樹脂、セロファン、ポリスチレン樹脂、ポリカーボネート樹脂、ポリアリレート樹脂、又はポリイミド樹脂等が挙げられる。   As a plastic sheet, what consists of various synthetic resins is mentioned. Synthetic resins include polyethylene resin, polypropylene resin, polymethylpentene resin, polyvinyl chloride resin, polyvinylidene chloride resin, polyvinyl alcohol resin, vinyl chloride-vinyl acetate copolymer resin, ethylene-vinyl acetate copolymer resin, ethylene-vinyl. Representative examples include alcohol copolymer resin, polyethylene terephthalate resin, polybutylene terephthalate resin, polyethylene naphthalate-isophthalate copolymer resin, polymethyl methacrylate resin, polyethyl methacrylate resin, polybutyl acrylate resin, nylon 6 or nylon 66 And polyamide resin, cellulose triacetate resin, cellophane, polystyrene resin, polycarbonate resin, polyarylate resin, polyimide resin, and the like.

金属板としては、例えばアルミニウム、鉄、ステンレス鋼、又は銅等からなるものを用いることができ、またこれらの金属をめっき等によって施したものを使用することもできる。
木質系の板としては、杉、檜、欅、松、ラワン、チーク、メラピー等各種素材の突板、木材単板、木材合板、パーチクルボード、中密度繊維板(MDF)等の木質材等が挙げられる。これらは単独で、又は積層して用いることもできる。なお、木質系の板には、木質板に限らず、紙粉入りのプラスチック板や、補強され強度を有する紙類も包含される。
窯業系素材としては、石膏板、珪酸カルシウム板、木片セメント板などの窯業系建材、陶磁器、ガラス、琺瑯、焼成タイル、火山灰を主原料とした板等が例示される。
これらの他、繊維強化プラスチック(FRP)の板、ペーパーハニカムの両面に鉄板を貼ったもの、2枚のアルミニウム板でポリエチレン樹脂を挟んだもの等、各種の素材の複合体も基材として使用できる。
As a metal plate, what consists of aluminum, iron, stainless steel, or copper can be used, for example, and what gave these metals by plating etc. can also be used.
Examples of wood-based boards include veneer of various materials such as cedar, firewood, firewood, pine, lawan, teak and melapie, and wood materials such as wood veneer, wood plywood, particle board, and medium density fiber board (MDF). . These can be used alone or in a stacked manner. The wooden board includes not only a wooden board but also a plastic board containing paper powder and reinforced paper having strength.
Examples of the ceramic material include ceramic building materials such as a gypsum plate, a calcium silicate plate, and a wood piece cement plate, ceramics, glass, firewood, fired tiles, plates made mainly of volcanic ash, and the like.
In addition to these, composites of various materials, such as fiber reinforced plastic (FRP) plates, paper honeycombs with iron plates pasted on both sides, and two aluminum plates sandwiched with polyethylene resin can also be used as the base material. .

また、前記基板はプライマー層を形成する等の処理を施してもよいし、色彩を整えるための塗装や、デザイン的な観点での模様があらかじめ形成されていてもよい。被着体となる基板としては各種素材の平板、曲面板等の板材、或いは上記素材が単体か或いは複合された立体形状物品(成形品)が対象となる。
化粧シートに、和紙、洋紙、合成紙、不織布、織布、寒冷紗、含浸紙、合成樹脂シート等の裏打ち材を貼着して用いてもよい。裏打ち材を貼着することにより、化粧シート自体の補強、化粧シートの割れや破け防止、接着剤の化粧シート表面への染み出し防止等の作用がなされ、不良品の発生が防止されると共に、取り扱いが容易となることとなり、生産性を向上することができる。
このようにして接着剤を介して毎葉ごとにあるいは連続して化粧シートが載置された基板を、コールドプレス、ホットプレス、ロールプレス、ラミネーター、ラッピング、縁貼り機,真空プレス等の貼着装置を用いて圧締して、化粧シートを基板表面に接着し、化粧板とする。
Further, the substrate may be subjected to a treatment such as forming a primer layer, or a coating for adjusting the color or a pattern from a design viewpoint may be formed in advance. As a substrate to be an adherend, plate materials such as flat plates and curved plates of various materials, or three-dimensional shaped articles (molded products) in which the above materials are used alone or in combination are targeted.
A backing material such as Japanese paper, Western paper, synthetic paper, non-woven fabric, woven fabric, cold paper, impregnated paper, synthetic resin sheet, or the like may be attached to the decorative sheet. By sticking the backing material, it acts to reinforce the decorative sheet itself, prevent cracking and tearing of the decorative sheet, prevent bleeding of the adhesive to the decorative sheet surface, and prevent the occurrence of defective products, Handling becomes easy and productivity can be improved.
Thus, a substrate on which a decorative sheet is placed every leaf or continuously via an adhesive is attached to a cold press, a hot press, a roll press, a laminator, a lapping, an edge pasting machine, a vacuum press, etc. The decorative sheet is bonded to the substrate surface by pressing with an apparatus to obtain a decorative plate.

接着剤はスプレー、スプレッダー、バーコーター等の塗布装置を用いて塗布する。この接着剤には、酢酸ビニル樹脂系、ユリア樹脂系、メラミン樹脂系、フェノール樹脂系、イソシアネート系等の接着剤を、単独であるいは任意混合した混合型接着剤として用いられる。接着剤には、必要に応じてタルク、炭酸カルシウム、クレー、チタン白等の無機質粉末、小麦粉、木粉、プラスチック粉、着色剤、防虫剤、防カビ剤等を添加混合して用いることができる。一般に、接着剤は固形分を35〜80質量%とし、塗布量50〜300g/m2の範囲で基板表面に塗布される。
化粧シートの基板上への貼着は、通常、本発明の化粧シートの裏面に接着剤層を形成し、基板を貼着するか基板の上に接着剤を塗布し、化粧シートを貼着する等の方法による。
The adhesive is applied using an application device such as a spray, spreader, or bar coater. As the adhesive, vinyl acetate resin-based, urea resin-based, melamine resin-based, phenol resin-based, isocyanate-based adhesives, etc., are used alone or as a mixed adhesive obtained by arbitrarily mixing them. As needed, talc, calcium carbonate, clay, titanium white and other inorganic powders, wheat flour, wood flour, plastic powder, coloring agents, insect repellents, fungicides and the like can be added and mixed in the adhesive. . In general, the adhesive is applied to the substrate surface with a solid content of 35 to 80% by mass and an application amount of 50 to 300 g / m 2 .
Adhesion of the decorative sheet on the substrate is usually performed by forming an adhesive layer on the back surface of the decorative sheet of the present invention and adhering the substrate or applying an adhesive on the substrate and adhering the decorative sheet. Etc.

以上のようにして製造される化粧板は、任意切断し、表面や木口部にルーター、カッター等の切削加工機を用いて溝加工、面取加工等の任意加飾を施すことができる。そして種々の用途、例えば、壁、天井、床等の建築物の内装又は外装材、窓枠、扉、手すり、幅木、廻り縁、モール等の建具の表面化粧板、キッチン、家具又は弱電、OA機器等のキャビネットの表面化粧板、車両の内装、外装等に用いることができる。   The decorative board manufactured as described above can be arbitrarily cut and subjected to optional decoration such as grooving and chamfering on the surface and the end of the cut using a cutting machine such as a router or a cutter. And various uses, for example, interior or exterior materials of buildings such as walls, ceilings, floors, window frames, doors, handrails, skirting boards, margins, surface decorative boards for fittings such as malls, kitchens, furniture or light electrical appliances, It can be used for surface decorative boards of cabinets such as OA equipment, interiors and exteriors of vehicles.

<化粧タックシート>
本発明の化粧シート10は、基材側に粘着剤層を設けて、化粧タックシートとして用いることができる。この化粧タックシートは、上記の基板に粘着剤層を介して貼着し、化粧板を製造することができる。
粘着剤層に用いられる粘着剤としては、アクリル系粘着剤、ウレタン系粘着剤、ゴム系粘着剤、シリコン系粘着剤等の粘着剤が好ましく挙げられ、耐久性及び粘着性能の点でアクリル系粘着剤がより好ましい。アクリル系粘着剤としては、例えば、炭素数2〜14(メタ)アルキルアクリレートが好ましく挙げられる。
<Makeup tack sheet>
The decorative sheet 10 of the present invention can be used as a decorative tack sheet by providing an adhesive layer on the substrate side. This decorative tack sheet can be attached to the substrate via an adhesive layer to produce a decorative board.
Preferable examples of the pressure-sensitive adhesive used in the pressure-sensitive adhesive layer include pressure-sensitive adhesives such as acrylic pressure-sensitive adhesives, urethane-based pressure-sensitive adhesives, rubber-based pressure-sensitive adhesives, and silicon-based pressure-sensitive adhesives. An agent is more preferable. As an acrylic adhesive, C2-C14 (meth) alkyl acrylate is mentioned preferably, for example.

化粧タックシートと基板とを積層して化粧板を製造する際、粘着剤層を介して直接積層してもよいが、これらの層のより強固な接着性を得るために、化粧タックシートと基板との間に粘着補強層を設けることも可能である。この粘着補強層は、化粧タックシートの基材の表面保護層を設ける面とは反対側の面(裏面プライマー層を設ける場合は裏面プライマー層の面)、基板のいずれに設けてもよい。粘着補強層を基板に設ける処理、及び基板と化粧タックシートとの接着処理は、通常現場にて施工し行う。   When producing a decorative board by laminating a decorative tack sheet and a substrate, the decorative tack sheet and the substrate may be laminated directly via an adhesive layer, in order to obtain stronger adhesion of these layers. It is also possible to provide an adhesive reinforcing layer between the two. This adhesion reinforcing layer may be provided on either the surface opposite to the surface on which the surface protective layer of the base material of the decorative tack sheet is provided (the surface of the back surface primer layer when the back surface primer layer is provided) or the substrate. The process of providing the adhesive reinforcing layer on the substrate and the adhesion process between the substrate and the decorative tack sheet are usually performed on site.

粘着補強層は、基板に設けることが好ましく、固形物換算での塗工量が3〜20g/m2となるように塗布することが好ましい。粘着補強層の材質としては、クロロプレンゴム、ニトリルゴム、スチレン−ブタジエンゴム、スチレン−イソプレンゴム等からなるゴム系接着剤が好ましく、不燃性確保の観点からクロロプレンゴム系接着剤であることが特に好ましい。
粘着補強層の厚さは、5〜200μmであることが好ましく、20〜100μmであることがより好ましい。5μm以上であると基材との良好な接着性が得られ、200μm以下であると良好な曲げ加工性が得られる。
The adhesive reinforcing layer is preferably provided on the substrate, and is preferably applied so that the coating amount in terms of solid matter is 3 to 20 g / m 2 . As the material of the adhesive reinforcing layer, a rubber adhesive made of chloroprene rubber, nitrile rubber, styrene-butadiene rubber, styrene-isoprene rubber or the like is preferable, and a chloroprene rubber adhesive is particularly preferable from the viewpoint of ensuring nonflammability. .
The thickness of the adhesive reinforcing layer is preferably 5 to 200 μm, and more preferably 20 to 100 μm. When it is 5 μm or more, good adhesion to the substrate is obtained, and when it is 200 μm or less, good bending workability is obtained.

次に、本発明を実施例により、さらに詳細に説明するが、本発明は、この例によってなんら限定されるものではない。
(評価方法)
各実施例で得られた化粧シートについて、以下の方法で評価した。
(1)盛上部の占有面積比
オリンパス(株)製、非接触表面粗さ計「3次元測定顕微鏡」STM6ZP(商品名)を用い、倍率50倍、測定ピッチ0.10mm、駆動スピードは高速の条件で盛上部の占有面積を測定した。該占有面積を化粧シートの平面の面積で除して盛上部の占有面積比を求めた。
(2)十点平均表面粗さ(Rz)
十点平均粗さRzを、JIS B 0601:2001に準拠して、測定長8mm、カットオフ値0.8mmで測定した
(3)表面の触感
人の手で接触した感触を以下の基準で評価した。
◎:大きな盛上感がある
○:盛上感がある
△:若干の盛上感がある
×:殆ど盛上感が無い
(4)耐汚染性
JIS K−6902に準拠して、汚染物を化粧シートの表面に塗布し、ふき取った後の汚染物の残存具合を目視にて観察した。判定基準を以下のようにして評価した。
◎;汚染物の残存は全くない
〇;汚染物の残存がかすかに見られる
△;汚染物の残存はあるものの軽微なもので実用上問題がない
△×;凹部に汚染物の残存が見られる
×;汚染物の残存が著しい
(5)化粧シートの曲げ加工性
Vカット加工を行ったのち、目視にてVカット部分の確認を行い、下記の判定基準で評価した。
◎;化粧シートの表面の割れはまったく確認されなかった。
〇;化粧シートの割れが軽微であり、実用上問題ない。
△;化粧シートの割れが若干確認された。
×;化粧シートの割れが著しかった。
EXAMPLES Next, although an Example demonstrates this invention further in detail, this invention is not limited at all by this example.
(Evaluation method)
The decorative sheet obtained in each example was evaluated by the following methods.
(1) Occupied area ratio of the upper part Using a non-contact surface roughness meter “three-dimensional measurement microscope” STM6ZP (trade name) manufactured by Olympus Corporation, magnification is 50 times, measurement pitch is 0.10 mm, and driving speed is high The occupied area of the upper part was measured under the conditions. The occupied area ratio was calculated by dividing the occupied area by the plane area of the decorative sheet.
(2) Ten-point average surface roughness (Rz)
Ten-point average roughness Rz was measured in accordance with JIS B 0601: 2001 with a measurement length of 8 mm and a cut-off value of 0.8 mm. (3) Surface tactile sensation Tactile sensation touched by human hands was evaluated according to the following criteria. did.
◎: There is a great feeling of sensation ○: There is a feeling of sensation △: There is a feeling of some sensation ×: There is almost no feeling of sensation (4) Contamination resistance Contaminant according to JIS K-6902 The remaining condition of the contaminants after applying and wiping off the surface of the decorative sheet was visually observed. Judgment criteria were evaluated as follows.
◎: No contamination remains ○: Contamination remains faint △: Contamination remains slight, but there is no problem in practical use △: Contamination remains in the recess ×: Contaminant remains remarkably (5) Bending processability of decorative sheet After V-cut processing, the V-cut portion was visually confirmed and evaluated according to the following criteria.
(Double-circle): The crack of the surface of a decorative sheet was not confirmed at all.
◯: Cracking of the decorative sheet is slight and there is no practical problem.
Δ: Some cracks on the decorative sheet were confirmed.
X: The crack of the decorative sheet was remarkable.

実施例1
易接着処理されたポリエチレンテレフタレート(PET)フィルム(東洋紡績(株)製「A4100(厚さ;50μm)」)の易接着処理面上の全面に、アクリル樹脂と硝化綿をバインダーとし、チタン白、弁柄、黄鉛を着色剤とするインキを用いて、塗工量5g/m2の層をグラビア印刷にて施してベタ印刷層とした。その上に硝化綿をバインダーとし、弁柄を主成分とする着色剤を含有するインキを用いて、木目模様の絵柄層をグラビア印刷にて形成し、装飾層を得た。
次いで、プライマーインキ((株)昭和インク工業所製アクリル系インキ「EBF同調プライマー」)に艶消剤としてシリカを加えたインキ組成物をグラビア印刷にて施して、浸透防止機能を有するプライマー層を形成した。
次に、アクリル樹脂を主成分とした盛り上げ用のインキ(大日精化工業(株)製、商品名:KKBキュアUセミマットメヂウム)を用いて、不定型な形状の絵柄の盛上部が形成できるような版型を用い、グラビア印刷にて複数の盛上部を形成して、盛上層を形成した。ここで、版型は、全平面に対する盛上部の占有面積比が2%となり、かつ盛上部の高さが5μmとなるような版深とした。
この盛上層上に電子線硬化性樹脂(大日精化工業(株)製「REB−GE」)に焼成カオリン粒子5質量%、珪フッ化マグネシウム0.5質量%を添加した電子線硬化性樹脂組成物を塗工量4g/m2でグラビアオフセットコータ法により塗工した。塗工後、加速電圧175kV、照射線量30kGy(3Mrad)の電子線を照射して、電子線硬化性樹脂組成物を硬化させて表面保護層とし、化粧シートを得た。
該化粧シートについて、上記評価を行った結果を第1表に示す。
Example 1
Easy-adhesive polyethylene terephthalate (PET) film (“A4100 (thickness: 50 μm)” manufactured by Toyobo Co., Ltd.) is coated on the entire surface of the easy-adhesion treated surface using acrylic resin and nitrified cotton as a binder, A layer having a coating amount of 5 g / m 2 was applied by gravure printing using an ink having a petal and chrome lead as a colorant to form a solid printing layer. On top of that, a woodgrain pattern layer was formed by gravure printing using an ink containing nitrified cotton as a binder and a colorant mainly composed of a petiole to obtain a decorative layer.
Next, an ink composition in which silica as a matting agent is added to primer ink (Showa Ink Co., Ltd. acrylic ink “EBF Tuning Primer”) is applied by gravure printing to form a primer layer having a penetration preventing function. Formed.
Next, a raised portion of an irregularly shaped pattern is formed using an ink for swelling mainly composed of acrylic resin (manufactured by Dainichi Seika Kogyo Co., Ltd., trade name: KKB Cure U Semi Matte Medium). Using such a plate, a plurality of raised portions were formed by gravure printing to form a raised layer. Here, the plate type was such that the ratio of the occupied area of the raised portion to the entire plane was 2% and the height of the raised portion was 5 μm.
An electron beam curable resin in which 5% by mass of calcined kaolin particles and 0.5% by mass of magnesium silicofluoride are added to an electron beam curable resin ("REB-GE" manufactured by Dainichi Seika Kogyo Co., Ltd.) on the top layer. The composition was applied at a coating amount of 4 g / m 2 by a gravure offset coater method. After coating, an electron beam with an acceleration voltage of 175 kV and an irradiation dose of 30 kGy (3 Mrad) was applied to cure the electron beam curable resin composition to form a surface protective layer, thereby obtaining a decorative sheet.
Table 1 shows the results of the above evaluations on the decorative sheet.

実施例2
実施例1における盛上部の作製過程において、盛上部の占有面積比が25%となるような版型を用いたこと以外は実施例1と同様にして化粧シートを作製した。該化粧シートについて、実施例1と同様にして評価を行った結果を第1表に示す。
Example 2
A decorative sheet was produced in the same manner as in Example 1 except that in the production process of the raised portion in Example 1, a plate mold having an occupied area ratio of 25% was used. The results of evaluating the decorative sheet in the same manner as in Example 1 are shown in Table 1.

実施例3
実施例1における盛上部の作製過程において、盛上部の高さが35μmとなり、かつ全平面に対する盛上部の占有面積比が2%となる版型を用いたこと以外は実施例1と同様にして化粧シートを作製した。該化粧シートについて、実施例1と同様にして評価を行った結果を第1表に示す。
Example 3
In the production process of the raised portion in Example 1, the height of the raised portion was 35 μm, and the same procedure as in Example 1 was used except that a plate mold having an occupied area ratio of 2% with respect to the entire plane was used. A decorative sheet was prepared. The results of evaluating the decorative sheet in the same manner as in Example 1 are shown in Table 1.

実施例4
実施例1における盛上部の作製過程において、盛上部の高さが35μmとなり、かつ全平面に対する盛上部の占有面積比が25%となる版型を用いたこと以外は実施例1と同様にして化粧シートを作製した。該化粧シートについて、実施例1と同様にして評価を行った結果を第1表に示す。
Example 4
In the production process of the raised portion in Example 1, the same procedure as in Example 1 was used except that a plate having a height of the raised portion of 35 μm and a ratio of the occupied area of the raised portion to the entire plane being 25% was used. A decorative sheet was prepared. The results of evaluating the decorative sheet in the same manner as in Example 1 are shown in Table 1.

比較例1
実施例1における盛上部の作製過程において、盛上層を設けないこと以外は実施例1と同様にして化粧シートを作製した。該化粧シートについて、実施例1と同様にして評価を行った結果を第1表に示す。
Comparative Example 1
A decorative sheet was produced in the same manner as in Example 1 except that in the process of producing the raised portion in Example 1, no raised layer was provided. The results of evaluating the decorative sheet in the same manner as in Example 1 are shown in Table 1.

比較例2
実施例1における盛上部の作製過程において、盛上部の高さが2μmとなり、かつ全面積に対する盛上げ部分の占有面積比が25%となる版型を用いたこと以外は実施例1と同様にして化粧シートを作製した。該化粧シートについて、実施例1と同様にして評価を行った結果を第1表に示す。
Comparative Example 2
In the manufacturing process of the raised portion in Example 1, the height of the raised portion was 2 μm, and the same procedure as in Example 1 was used except that a plate mold in which the occupied area ratio of the raised portion to the total area was 25% was used. A decorative sheet was prepared. The results of evaluating the decorative sheet in the same manner as in Example 1 are shown in Table 1.

比較例3
実施例1における盛上部の作製過程において、盛上部の高さが35μmとなり、且つ全面積に対する盛上げ部分の占有面積比が1%となる版型を用いたこと以外は実施例1と同様にして化粧シートを作製した。該化粧シートについて、実施例1と同様にして評価を行った結果を第1表に示す。
Comparative Example 3
In the production process of the raised portion in Example 1, the same procedure as in Example 1 was used except that the height of the raised portion was 35 μm and the ratio of the occupied area of the raised portion to the total area was 1%. A decorative sheet was prepared. The results of evaluating the decorative sheet in the same manner as in Example 1 are shown in Table 1.

比較例4
実施例1における盛上部の作製過程において、盛上部の高さが40μmとなり、且つ全面積に対する盛上げ部分の占有面積比が30%となる版型を用いたこと以外は実施例3と同様にして化粧シートを作製した。該化粧シートについて、実施例1と同様にして評価を行った結果を第1表に示す。
Comparative Example 4
In the production process of the raised portion in Example 1, the height of the raised portion was 40 μm, and the same procedure as in Example 3 was used except that a plate mold having an occupied area ratio of the raised portion with respect to the total area was 30%. A decorative sheet was prepared. The results of evaluating the decorative sheet in the same manner as in Example 1 are shown in Table 1.

本発明によれば、例えば、木目模様であれば実際の木の触感及び艶感に近い意匠を付与することができ、内装材等に高級感を与える化粧シートを提供することができる。本発明の化粧シートは、建築物の内装、外装、家具、建具等の表面化粧、車両の内装等に好適に用いられる。   According to the present invention, for example, if it is a wood grain pattern, it is possible to provide a design close to the feel and gloss of an actual tree, and it is possible to provide a decorative sheet that gives an interior material or the like a high-class feeling. The decorative sheet of the present invention is suitably used for interior decoration of buildings, exteriors, furniture for furniture, furniture for furniture, interiors of vehicles, and the like.

10.化粧シート
20.基材
30.装飾層
31.ベタ印刷層
32.絵柄層
40.プライマー層
50.盛上層
60.表面保護層
70.裏面プライマー層
10. Cosmetic sheet 20. Base material 30. Decoration layer 31. Solid print layer 32. Pattern layer 40. Primer layer 50. Top layer 60. Surface protective layer 70. Back primer layer

Claims (7)

基材上に少なくとも、部分的に設けられた盛上層と、該盛上層が形成された領域及び該盛上層が形成されていない領域とを含む全面にわたって被覆する表面保護層を有する化粧シートであって、該表面保護層が電離放射線硬化性樹脂組成物の架橋硬化したものであり、表面の十点平均粗さが5〜35μmであり、かつ前記盛上層の占有面積比が2〜25%である化粧シート。   A decorative sheet having a surface protective layer covering the entire surface including at least a partially formed overlay layer on a substrate, a region where the build-up layer is formed, and a region where the build-up layer is not formed. The surface protective layer is obtained by crosslinking and curing the ionizing radiation curable resin composition, the surface 10-point average roughness is 5 to 35 μm, and the occupying area ratio of the raised layer is 2 to 25%. A certain decorative sheet. 前記基材上にプライマー層を有し、該プライマー層上に前記盛上層を有する請求項1に記載の化粧シート。   The decorative sheet according to claim 1, comprising a primer layer on the substrate, and the raised layer on the primer layer. 前記プライマー層が艶消剤を含有する請求項2に記載の化粧シート。   The decorative sheet according to claim 2, wherein the primer layer contains a matting agent. 前記基材と前記盛上層の間に、さらに装飾層を有する請求項1〜3のいずれかに記載の化粧シート。   The decorative sheet according to any one of claims 1 to 3, further comprising a decorative layer between the base material and the raised layer. 前記装飾層がベタ印刷層又はベタ印刷層の上に絵柄層を有してなる請求項4に記載の化粧シート。   The decorative sheet according to claim 4, wherein the decorative layer has a solid print layer or a pattern layer on the solid print layer. 前記表面保護層の厚さが1〜20μmである請求項1〜5のいずれかに記載の化粧シート。   The decorative sheet according to any one of claims 1 to 5, wherein the surface protective layer has a thickness of 1 to 20 µm. 前記電離放射線硬化性樹脂組成物が電子線硬化性樹脂組成物である請求項1〜6のいずれかに記載の化粧シート。   The decorative sheet according to any one of claims 1 to 6, wherein the ionizing radiation curable resin composition is an electron beam curable resin composition.
JP2014191386A 2014-02-18 2014-09-19 Decorative sheet Active JP6582380B2 (en)