JP2011185973A - Toner for developing electrostatic charge image, image forming apparatus, process cartridge, and developer - Google Patents

Toner for developing electrostatic charge image, image forming apparatus, process cartridge, and developer Download PDF

Info

Publication number
JP2011185973A
JP2011185973A JP2010047847A JP2010047847A JP2011185973A JP 2011185973 A JP2011185973 A JP 2011185973A JP 2010047847 A JP2010047847 A JP 2010047847A JP 2010047847 A JP2010047847 A JP 2010047847A JP 2011185973 A JP2011185973 A JP 2011185973A
Authority
JP
Japan
Prior art keywords
toner
resin
acid
polyester resin
core
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP2010047847A
Other languages
Japanese (ja)
Inventor
Hideki Sugiura
英樹 杉浦
Yuka Mizoguchi
由花 溝口
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Ricoh Co Ltd
Original Assignee
Ricoh Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ricoh Co Ltd filed Critical Ricoh Co Ltd
Priority to JP2010047847A priority Critical patent/JP2011185973A/en
Publication of JP2011185973A publication Critical patent/JP2011185973A/en
Pending legal-status Critical Current

Abstract

<P>PROBLEM TO BE SOLVED: To provide a toner which secures advanced low-temperature fixability, high-temperature storage stability, low staining properties of a photoreceptor, and high-speed printing adaptability, and to provide an image forming apparatus. <P>SOLUTION: The toner contains at least a binder resin, a colorant, a release agent and has a core-shell structure which has a core therein and a shell on a surface of the core. A core portion contains at least a crystalline polyester resin, an amorphous polyester resin, the colorant, and the release agent. A softening temperature ST (°C) of a shell layer, which is measured by an SPM probe incorporating a heater, and a softening temperature CT (°C) of an inner core portion have a relationship 1.1≤ST/CT≤2.5. <P>COPYRIGHT: (C)2011,JPO&INPIT

Description

本発明は、画像形成装置、プロセスカートリッジ、静電荷像現像用トナー、現像剤に関する。   The present invention relates to an image forming apparatus, a process cartridge, an electrostatic charge image developing toner, and a developer.

電子写真装置や静電記録装置等においては、感光体上に形成された静電潜像にトナーを付着させ、それを転写材に転写し、次いで熱により紙等の転写材に定着させ、トナー画像を形成している。また、フルカラー画像形成は一般に黒、イエロー、マゼンタ、シアンの4色のトナーを用いて色の再現を行うものであり、各色について現像を行い、各トナー層を転写材上に重ね合わせたトナー像に加熱し、同時に定着することによって、フルカラー画像を得ている。   In an electrophotographic apparatus, an electrostatic recording apparatus, etc., toner is attached to an electrostatic latent image formed on a photoreceptor, transferred to a transfer material, and then fixed to a transfer material such as paper by heat. An image is formed. Also, full-color image formation is generally performed by using four color toners of black, yellow, magenta, and cyan. Each toner is developed, and each toner layer is superimposed on a transfer material. To obtain a full-color image.

ところが、一般に印刷、銀塩写真に見慣れたユーザーからすると、フルカラー複写機における画像は未だ満足できるレベルではなく、写真、印刷に迫る高精細性、高解像度を満足するさらなる高画質化が求められている。特に厚紙を使用した場合や高速印字する場合は、定着時の熱量の伝達が十分でなく定着性に優れ、かつ高画質(光沢・濃度・画像鮮明性等のばらつきが少ない)の画像を得ることは困難であった。   However, for users who are familiar with printing and silver halide photography, the images on full-color copiers are still not satisfactory, and there is a need for higher image quality that satisfies photography, high-definition, and high resolution. Yes. Especially when using thick paper or when printing at high speed, the heat quantity during fixing is not sufficiently transmitted, and the image has excellent fixing properties and high image quality (small variations in gloss, density, image sharpness, etc.). Was difficult.

さらにそのような低温定着システム、トナーを極めていくと、確かにトナーの軟化特性を低温化させることで低温定着に対応したトナーは製造可能であるが、今度は低温定着化したトナーの耐熱保存特性が低下して好ましくない。すなわち、トナー製造後の保管時、運搬時における高温高湿、低温低湿環境等はトナーにとって過酷な状況にあり、環境保存後においてもトナー同士が凝集せず、帯電特性、流動性、転写性、定着性の劣化のない、あるいは極めて少ない保存性に優れたトナーが要求されている。一方、それら究極の低温定着トナーにおいては、従来問題とならなかった、オフィス高温高湿環境における感光体フィルミング現象が発生し、その課題解決が困難であった。すなわち感光体表面にトナーの低温溶融物が付着することで、感光体表面が汚染され、本来の感光特性が発揮できないため、画像ボケ等が発生する現象で、いかなる使用環境においても安定的な画像を出力するニーズを満足する事ができず非常に困難な課題であった。   Furthermore, if such a low-temperature fixing system and toner are extremely advanced, it is possible to manufacture a toner that supports low-temperature fixing by lowering the softening characteristic of the toner, but this time the low-temperature fixing toner has heat-resistant storage characteristics. Is not preferable. In other words, high-temperature and high-humidity and low-temperature and low-humidity environments during storage and transportation after toner production are harsh conditions for the toner, and the toner does not aggregate even after storage in the environment. There is a demand for a toner having no deterioration in fixability or having very little storage stability. On the other hand, in these ultimate low-temperature fixing toners, a filming phenomenon of a photoreceptor in an office high-temperature and high-humidity environment, which has not been a problem in the past, has occurred, and it has been difficult to solve the problem. In other words, the low temperature melt of toner adheres to the surface of the photoconductor, which contaminates the surface of the photoconductor and cannot exhibit its original photosensitivity, resulting in image blurring and the like. It was a very difficult problem because it could not satisfy the needs of output.

特許文献1には、表面ワックス量を制御した少なくとも、窒素原子を含む官能基を有するポリエステルプレポリマー、ポリエステル、着色剤及び離型剤を有機溶媒中に分散させてなるトナー材料液を、水系媒体中で架橋及び/又は伸長反応させて得られるトナーの例が示されている。しかし、該トナーのコアシェル構造は十分でなく、またコアの軟化温度とシェル層の軟化温度に関しても十分な制御がなされていなかった。そのためさらなる低温定着性と耐熱保存性の両立の点で問題であった。 In Patent Document 1, a toner material liquid in which a polyester prepolymer having a functional group containing at least a nitrogen atom, a polyester, a colorant, and a release agent having a controlled surface wax amount is dispersed in an organic solvent is used as an aqueous medium. Examples of toner obtained by crosslinking and / or elongation reaction therein are shown. However, the core / shell structure of the toner is not sufficient, and the softening temperature of the core and the softening temperature of the shell layer have not been sufficiently controlled. Therefore, it was a problem in terms of both low-temperature fixability and heat-resistant storage stability.

上記のように、従来のトナー画像システムでは、特に使用条件の厳しい高速印字分野において、低温定着性、耐熱保存性、高温高湿環境での低感光体汚染性を高度に両立する画像形成装置を得ることは困難であった。   As described above, in the conventional toner image system, an image forming apparatus that has both low temperature fixing property, heat resistant storage stability, and low photoreceptor contamination in a high temperature and high humidity environment, particularly in the high-speed printing field where the use conditions are severe. It was difficult to get.

本発明の目的は上記のごとき問題点を解決した、以下を提供することにある。
高度の低温定着性、耐熱保存性、低感光体汚染性、高速印字対応性を確保したトナー、画像形成装置を提供すること。
An object of the present invention is to provide the following which solves the above problems.
To provide a toner and an image forming apparatus which ensure high low temperature fixability, heat resistant storage stability, low photoreceptor contamination, and high-speed printing compatibility.

本発明者らは前記課題を達成すべく鋭意検討した結果、少なくとも結着樹脂、着色剤、離型剤を含有するトナーにおいて、該トナーは内部にコアと、該コアの表面に厚みが0.01μm〜2μmのシェルとを有するコアシェル構造を有するトナーであって、前記コア部に少なくとも結晶性ポリエステル樹脂と非結晶性ポリエステル樹脂、着色剤、離型剤を含有してかつ、ヒーター内蔵のSPMプローブにより測定した前記シェル層の軟化温度ST(℃)と、内部コア部分の軟化温度CT(℃)が、以下の関係を示すトナーを用いることで、高度の低温定着性、耐熱保存性、低感光体汚染性、高速印字対応性を確保したトナー、画像形成装置を提供することができることを見いだした。
1.1≦ST/CT≦2.5
As a result of intensive studies to achieve the above-mentioned problems, the present inventors have found that in a toner containing at least a binder resin, a colorant, and a release agent, the toner has a core inside and a thickness of 0. 0 on the surface of the core. A toner having a core-shell structure having a shell of 01 μm to 2 μm, wherein the core portion contains at least a crystalline polyester resin, an amorphous polyester resin, a colorant, a release agent, and a heater built-in SPM probe By using a toner having the following relationship between the softening temperature ST (° C.) of the shell layer and the softening temperature CT (° C.) of the inner core portion measured by the above, a high degree of low-temperature fixing property, heat-resistant storage property, low photosensitivity It has been found that a toner and an image forming apparatus that ensure body contamination and high-speed printing compatibility can be provided.
1.1 ≦ ST / CT ≦ 2.5

(1)少なくとも結着樹脂、着色剤、離型剤を含有するトナーにおいて、該トナーは内部にコアと、該コアの表面にシェルとを有するコアシェル構造を有するトナーであって、前記コア部に少なくとも結晶性ポリエステル樹脂、非結晶性ポリエステル樹脂、着色剤、離型剤を含有してかつ、ヒーター内蔵のSPMプローブにより測定した前記シェル層の軟化温度ST(℃)と、内部コア部分の軟化温度CT(℃)が、以下の関係を示す事を特徴とするトナー。
1.1≦ST/CT≦2.5
(2)前記シェル層の厚さをSLとし、トナー粒子の最大径をTLとしたとき、SLとTLとが以下の関係を示すことを特徴とする(1)に記載のトナー。
0.01≦SL/TL≦0.20
(3)前記非結晶性ポリエステル樹脂が変性ポリエステル樹脂を含む事を特徴とする(1)または(2)に記載のトナー。
(4)前記トナーが、結晶性ポリエステル樹脂、着色剤、離型剤及び非結晶ポリエステル樹脂となるポリエステルプレポリマーを含むトナー組成物を溶解した有機溶媒の油滴を水系媒体中に分散させ、伸長反応および/または架橋反応により形成された粒子である事を特徴とする(1)〜(3)のいずれかに記載のトナー。
(5)前記ポリエステルプレポリマーが活性水素基を有する化合物と反応可能な部位を有する重合体である事を特徴とする(4)に記載のトナー。
(6)前記トナー組成物が更に非結晶性ポリエステルを含むことを特徴とする(4)又は(5)に記載のトナー。
(7)前記トナーのシェル層が少なくともビニル系樹脂を含有する事を特徴とする(1)〜(6)のいずれかに記載のトナー。
(8)前記トナーの平均円形度Eが0.93〜0.99である事を特徴とする(1)〜(7)のいずれかに記載のトナー。
(9)前記トナーの円形度SF−1値が100〜150、かつ円形度SF−2値が100〜140である事を特徴とする(1)〜(8)のいずれかに記載のトナー。
(10)前記トナー粒子の重量平均粒径D4が2〜7μmであり、重量平均粒径D4と個数平均粒径Dnの比D4/Dnが1.25以下である事を特徴とする(1)〜(9)のいずれかに記載のトナー。
(11)少なくとも(1)〜(10)のいずれかに記載のトナーとキャリアを含むことを特徴とする二成分現像剤。
(12)少なくとも(1)〜(10)のいずれかに記載のトナーとキャリアを含むことを特徴とする補給用トナー。
(13)(1)〜(10)のいずれかに記載のトナーを用いる事を特徴とする画像形成装置。
(14)(1)〜(10)のいずれか記載のトナーを用いてかつ、記録媒体上の可視像を熱と圧力により定着させる定着装置を備える画像形成装置であって、少なくとも4つ以上の現像色の異なる現像ユニットを直列に配置したタンデム型の現像方式でかつ、システム速度が500〜2500mm/secであり、かつ定着媒体の加圧面圧が、5N/cm2〜90N/cm2であることを特徴とするカラー画像形成装置。
(15)潜像担持体と、少なくとも現像手段を一体に支持し、画像形成装置本体に着脱可能であるプロセスカートリッジにおいて、該現像手段はトナーを保持し、該トナーは(1)〜(10)のいずれかに記載のトナーであることを特徴とするプロセスカートリッジ。
(1) In a toner containing at least a binder resin, a colorant, and a release agent, the toner has a core-shell structure having a core inside and a shell on the surface of the core, The softening temperature ST (° C.) of the shell layer, which contains at least a crystalline polyester resin, an amorphous polyester resin, a colorant, a release agent, and is measured by an SPM probe with a built-in heater, and the softening temperature of the inner core portion A toner characterized in that CT (° C.) shows the following relationship.
1.1 ≦ ST / CT ≦ 2.5
(2) The toner according to (1), wherein SL and TL have the following relationship, where SL is the thickness of the shell layer and TL is the maximum diameter of the toner particles.
0.01 ≦ SL / TL ≦ 0.20
(3) The toner according to (1) or (2), wherein the non-crystalline polyester resin contains a modified polyester resin.
(4) The toner is dispersed by dispersing oil droplets of an organic solvent in which a toner composition containing a polyester prepolymer that becomes a crystalline polyester resin, a colorant, a release agent, and an amorphous polyester resin is dispersed in an aqueous medium. The toner according to any one of (1) to (3), wherein the toner is particles formed by a reaction and / or a crosslinking reaction.
(5) The toner according to (4), wherein the polyester prepolymer is a polymer having a site capable of reacting with a compound having an active hydrogen group.
(6) The toner according to (4) or (5), wherein the toner composition further contains an amorphous polyester.
(7) The toner according to any one of (1) to (6), wherein the shell layer of the toner contains at least a vinyl resin.
(8) The toner according to any one of (1) to (7), wherein the toner has an average circularity E of 0.93 to 0.99.
(9) The toner according to any one of (1) to (8), wherein the toner has a circularity SF-1 value of 100 to 150 and a circularity SF-2 value of 100 to 140.
(10) The toner particles have a weight average particle diameter D4 of 2 to 7 μm and a ratio D4 / Dn of the weight average particle diameter D4 to the number average particle diameter Dn of 1.25 or less (1) The toner according to any one of to (9).
(11) A two-component developer comprising at least the toner according to any one of (1) to (10) and a carrier.
(12) A replenishing toner comprising at least the toner according to any one of (1) to (10) and a carrier.
(13) An image forming apparatus using the toner according to any one of (1) to (10).
(14) An image forming apparatus using the toner according to any one of (1) to (10) and including a fixing device that fixes a visible image on a recording medium by heat and pressure, and at least four or more and a tandem type developing system developing color different developing units arranged in series, the system speed is 500~2500mm / sec, and pressing surface pressure of the fixing medium, at 5N / cm 2 ~90N / cm 2 There is provided a color image forming apparatus.
(15) In a process cartridge that integrally supports the latent image carrier and at least the developing unit and is detachable from the main body of the image forming apparatus, the developing unit holds toner, and the toner is (1) to (10). A process cartridge comprising the toner according to any one of the above.

本発明によれば低温定着性、耐熱保存性、現像安定性、高速印字対応性を高度に確保したトナー、画像形成装置が提供できる。   According to the present invention, it is possible to provide a toner and an image forming apparatus that have highly secured low-temperature fixability, heat-resistant storage stability, development stability and high-speed printing compatibility.

ヒーター内臓のSPMプローブによりトナーのシェル層及びコア部の軟化温度の測定方法を示す図である。It is a figure which shows the measuring method of the softening temperature of the shell layer of a toner, and a core part by the SPM probe with a built-in heater. 本発明プロセスカートリッジを備える画像形成装置の構成を示す概略図である。1 is a schematic diagram illustrating a configuration of an image forming apparatus including a process cartridge of the present invention. 本発明のタンデム型のカラー画像形成装置の一例の構成を示す概略図である。1 is a schematic diagram illustrating a configuration of an example of a tandem color image forming apparatus according to the present invention. 本発明のタンデム型のカラー画像形成装置の他の例の構成を示す概略図である。It is the schematic which shows the structure of the other example of the tandem type color image forming apparatus of this invention. 本発明のタンデム型のカラー画像形成装置の他の例の構成を示す概略図である。It is the schematic which shows the structure of the other example of the tandem type color image forming apparatus of this invention. 本発明のタンデム型のカラー画像形成装置の他の例の構成を示す概略図である。It is the schematic which shows the structure of the other example of the tandem type color image forming apparatus of this invention. 本発明のトナーの断面のTEMで観察した図である。FIG. 3 is a view of a cross section of the toner of the present invention observed with a TEM.

以下、本発明について詳述する。ここで、本発明に用いられるトナー、現像剤の製法や材料、および電子写真プロセスに関するシステム全般に関しては条件を満たせば、公知のものが全て使用可能である。   Hereinafter, the present invention will be described in detail. Here, the toner, the manufacturing method and material of the developer, and the overall system relating to the electrophotographic process that are used in the present invention can be used as long as the conditions are satisfied.

本発明のトナーは内部にコアと、該コアの表面に厚みが0.01μm〜2μmのシェルとを有するコアシェル構造を有するトナーであって、前記コア部に少なくとも結晶性ポリエステル樹脂と非結晶性ポリエステル樹脂、着色剤、離型剤を含有してかつ、ヒーター内蔵のSPMプローブにより測定した前記シェル層の軟化温度ST(℃)と、内部コア部分の軟化温度CT(℃)が、以下の関係を示すトナーを用いることで、高度の低温定着性、耐熱保存性、低感光体汚染性、高速印字対応性を確保することができる。
1.1≦ST/CT≦2.5
The toner of the present invention is a toner having a core-shell structure having a core inside and a shell having a thickness of 0.01 μm to 2 μm on the surface of the core, and at least a crystalline polyester resin and an amorphous polyester in the core portion The softening temperature ST (° C.) of the shell layer measured with an SPM probe containing a resin, a colorant, and a release agent and having a built-in heater and the softening temperature CT (° C.) of the inner core portion have the following relationship: By using the toner shown, it is possible to ensure high low-temperature fixability, heat-resistant storage stability, low photoreceptor contamination, and high-speed printing compatibility.
1.1 ≦ ST / CT ≦ 2.5

本発明のトナーが上記のような格別の効果を奏するメカニズムは現在解明中であるが、いくつかの解析データから以下のことが推測された。
本発明のトナーはトナーの外側に厚さ0.01μm〜2μm、より好ましくは0.4μm〜1.5μmのシェルを有するコアシェル構造を有するトナーであって、前記コア部に少なくとも結晶性ポリエステル樹脂と非結晶性ポリエステル樹脂、離型剤、着色剤を含有する。ここで、シェル層はトナー内部の帯電特性、感光体汚染性(感光体フィルミング性)に悪影響を与える外的要因から離型剤、着色剤、低溶融成分、帯電不良成分を保護する。シェル層厚は、0.01μm未満であると層としての効果が十分でなく感光体汚染性、耐熱保存性が低下して好ましくない。また2μmを超えるとシェル層が厚すぎてコア内部の着色剤による発色性、離型剤の染み出し性が低下して好ましくない。またシェル層の低温定着性が十分確保できなくなるため好ましくない。
またコアに結着樹脂として少なくとも結晶性ポリエステル樹脂と非結晶性ポリエステル樹脂を含有する事で、結晶性ポリステルのシャープな溶融特性と非結晶性ポリエステルと相乗的に発揮される可塑効果でトナー全体としての低温定着性が確保できる。
The mechanism by which the toner of the present invention exhibits the above-mentioned special effects is currently being elucidated, but the following has been estimated from some analysis data.
The toner of the present invention is a toner having a core-shell structure having a shell having a thickness of 0.01 μm to 2 μm, more preferably 0.4 μm to 1.5 μm on the outside of the toner, and at least a crystalline polyester resin and Contains an amorphous polyester resin, a release agent, and a colorant. Here, the shell layer protects the release agent, the colorant, the low melting component, and the poorly charged component from external factors that adversely affect the charging characteristics inside the toner and the photoreceptor contamination (photoreceptor filming property). When the shell layer thickness is less than 0.01 μm, the effect as a layer is not sufficient, and the photoreceptor contamination and heat-resistant storage stability are unfavorable. On the other hand, if the thickness exceeds 2 μm, the shell layer is too thick, and the color developability due to the colorant inside the core and the bleeding property of the release agent are undesirably lowered. Further, it is not preferable because the low-temperature fixability of the shell layer cannot be sufficiently secured.
In addition, by containing at least a crystalline polyester resin and an amorphous polyester resin as a binder resin in the core, the toner as a whole has a sharp melting characteristic of the crystalline polyester and a plastic effect that is synergistically exhibited with the amorphous polyester. Can be secured at low temperature.

さらに、ヒーター内蔵のSPMプローブにより測定した前記シェル層の軟化温度STと、内側のコア部分の軟化温度CTが、1.1≦ST/CT≦2.5の関係を示すことが重要である。コアシェルの軟化特性を1.1≦ST/CT≦2.5に制御することで、シェル層が外環境(保管、輸送、各種使用状況)に起因する溶融、固着等を防止する。一方、コア部で画像形成定着時における定着溶融性を適切な定着圧力の下に確保する。上記のメカニズムで低温定着性だけでなく、耐熱保存性両立が可能となる。ここで、ST/CTが1.1未満の場合、シェル層とコア部の軟化温度差が少なすぎて、トナー軟化の保護としての本来の機能が発揮できない。さらにST/CTが2.5を超える場合、コア部の軟化温度に対してシェル層の軟化温度が高すぎて、低温定着性が達成できず好ましくない。またシェル層を十分低軟化した場合、コア部の軟化温度が低すぎて、トナー定着するに十分な粘性を有さず、その結果低温定着できず好ましくない。   Furthermore, it is important that the softening temperature ST of the shell layer measured by the SPM probe with a built-in heater and the softening temperature CT of the inner core portion show a relationship of 1.1 ≦ ST / CT ≦ 2.5. By controlling the softening property of the core shell to 1.1 ≦ ST / CT ≦ 2.5, the shell layer prevents melting, sticking, and the like due to the external environment (storage, transportation, various usage conditions). On the other hand, the fixing meltability at the time of image formation fixing at the core is ensured under an appropriate fixing pressure. With the above mechanism, not only low-temperature fixability but also heat-resistant storage stability can be achieved. Here, when ST / CT is less than 1.1, the difference in softening temperature between the shell layer and the core portion is too small, and the original function as protection for toner softening cannot be exhibited. Furthermore, when ST / CT exceeds 2.5, the softening temperature of the shell layer is too high with respect to the softening temperature of the core part, so that low temperature fixability cannot be achieved. Further, when the shell layer is sufficiently softened, the softening temperature of the core portion is too low and does not have sufficient viscosity to fix the toner, and as a result, low temperature fixing cannot be achieved.

シェル層の軟化温度STは50℃〜100℃であることが好ましく、より好ましくは60℃〜90℃である。また、コア部分の軟化温度CTは40℃〜90℃であることが好ましく、より好ましくは50℃〜80℃である。 The softening temperature ST of the shell layer is preferably 50 ° C to 100 ° C, more preferably 60 ° C to 90 ° C. Moreover, it is preferable that the softening temperature CT of a core part is 40 to 90 degreeC, More preferably, it is 50 to 80 degreeC.

また該トナーのシェル層は少なくともビニル系樹脂を含有することが好ましく、ビニル系樹脂の中でも特にスチレン・アクリル樹脂が好ましい。ビニル系樹脂の表面性、粘弾性他に起因する特性により、シェル層の環境負荷時における耐感光体スペント性がめざましく向上してより好ましい。   The shell layer of the toner preferably contains at least a vinyl resin, and among the vinyl resins, a styrene / acryl resin is particularly preferable. The properties due to the surface properties, viscoelasticity, and the like of the vinyl resin are more preferable because the spent resistance of the shell layer at the time of environmental load is remarkably improved.

また該トナーのコア部に少なくとも変性ポリエステル樹脂を含むことで、樹脂の熱特性、粘弾性特性の設計範囲が広がりより好ましい。
また、該トナーが、プレポリマーを含むトナー組成物を溶解した有機溶媒の油滴を水系媒体中に分散させ、伸長反応および/または架橋反応により形成された粒子からなるトナーであることにより、該コアシェル構造を有するトナーを形成することが可能となりより好ましい。
In addition, it is more preferable that the core portion of the toner contains at least a modified polyester resin, which expands the design range of the thermal characteristics and viscoelastic characteristics of the resin.
Further, the toner is a toner composed of particles formed by dispersing an oil droplet of an organic solvent in which a toner composition containing a prepolymer is dissolved in an aqueous medium, and extending and / or cross-linking. It is possible to form a toner having a core-shell structure, which is more preferable.

また、該トナーは、少なくとも、活性水素基を有する化合物と反応可能な部位を有する重合体、ポリエステル、着色剤、離型剤を含むトナー組成物を水系媒体中で樹脂微粒子の存在下で架橋及び/又は伸長反応させてなるトナーであることにより、同様に該コアシェル構造を有するトナーを形成し、かつシェル層とコア内部で適切な軟化特性を有するトナーが形成可能となりより好ましい。   Further, the toner includes a toner composition containing at least a polymer capable of reacting with a compound having an active hydrogen group, a polyester, a colorant, and a release agent in an aqueous medium in the presence of resin fine particles. A toner obtained by an elongation reaction is more preferable because a toner having the core-shell structure can be similarly formed and a toner having an appropriate softening property can be formed inside the shell layer and the core.

また、該トナーが、平均円形度Eが0.93〜0.99のトナーであることにより、適切に球形に近い形状でコアシェル構造を確保できより好ましい。
また、該トナーが、円形度SF−1値が100〜150、かつ円形度SF−2値が100〜140であるトナーであることにより、適切に球形に近い形状でコアシェル構造を確保できより好ましい。
また、該トナーが、重量平均粒径D4が2〜7μm、より好ましくは2〜5μmであり、重量平均粒径D4と個数平均粒径Dnの比D4/Dnが1.25以下、より好ましくは1.15以下であるトナーであることにより、トナーの帯電現像性、転写性、定着性を確保しつつ、均一なコアシェル構造のトナー粒子が形成可能でより好ましい。
In addition, the toner having a mean circularity E of 0.93 to 0.99 is more preferable because it can ensure a core-shell structure with a shape close to a sphere.
In addition, when the toner is a toner having a circularity SF-1 value of 100 to 150 and a circularity SF-2 value of 100 to 140, a core-shell structure can be appropriately secured in a shape close to a spherical shape, which is more preferable. .
The toner has a weight average particle diameter D 4 of 2 to 7 μm, more preferably 2 to 5 μm, and a ratio D 4 / Dn of the weight average particle diameter D 4 to the number average particle diameter Dn of 1.25 or less. More preferably, the toner is 1.15 or less because it is possible to form toner particles having a uniform core-shell structure while ensuring the charge developability, transferability, and fixability of the toner.

また、前記トナーと磁性粒子からなるキャリアを含むことを特徴とする二成分系の現像剤とすることで、コアシェル構造で低下するトナーの帯電ポテンシャルを短時間での摩擦帯電で十分な立ち上がり性を確保することが可能で、十分にシャープな帯電量分布が維持できてより好ましい。
また、記録媒体上の可視像を熱と圧力により定着させる定着装置を備える画像形成装置において、システム速度が500〜2500mm/secであり、かつ定着媒体の加圧面圧が、5N/cm2〜90N/cm2である画像形成装置において、本発明のトナーを用いることで、高速印字における低温定着の要求に応じることが可能で、供給定着熱量が不十分な状況でも十分に強固な定着強度を有した画像を得ることが可能となる。
In addition, by using a two-component developer containing the toner and a carrier composed of magnetic particles, the charging potential of the toner, which is lowered by the core-shell structure, can be sufficiently increased by frictional charging in a short time. It is more preferable because it can be ensured and a sufficiently sharp charge amount distribution can be maintained.
Further, in an image forming apparatus including a fixing device that fixes a visible image on a recording medium by heat and pressure, the system speed is 500 to 2500 mm / sec, and the pressing surface pressure of the fixing medium is 5 N / cm 2 to. In the image forming apparatus of 90 N / cm 2 , by using the toner of the present invention, it is possible to meet the demand for low-temperature fixing in high-speed printing, and a sufficiently strong fixing strength even in a situation where the supply fixing heat amount is insufficient. It becomes possible to obtain the possessed image.

(結晶性の評価)
本発明におけるポリエステル樹脂の結晶性の有無は、X線回折法により結晶性ピークの有無で評価した。装置と条件を以下に示す。
XRD:(株)リガク製 RINT−TTRIII型 広角X線回折装置
X線源 ;CuKα線
管電圧−管電流 ;50kV−300mA
ステップ幅 ;0.02deg.
測定範囲 ;2°〜60°
測定速度 ;5deg./min
スリット系 ;0.5deg.−0.15mm−0.5deg.
回折線湾曲結晶モノクロメータ
(Evaluation of crystallinity)
The presence or absence of crystallinity of the polyester resin in the present invention was evaluated by the presence or absence of the crystallinity peak by X-ray diffraction method. The equipment and conditions are shown below.
XRD: Rigaku Co., Ltd. RINT-TTRIII type wide angle X-ray diffractometer X-ray source; CuKα ray tube voltage-tube current; 50 kV-300 mA
Step width; 0.02 deg.
Measurement range: 2 ° -60 °
Measurement speed: 5 deg. / Min
Slit system; 0.5 deg. -0.15 mm-0.5 deg.
Diffraction line crystal monochromator

(トナーコアシェル構造・シェル層の厚さ評価)
本発明のトナーは、内部のコアと、該コアの表面のシェル層とを有するコアシェル構造のトナーである。
本発明のトナーにおいては、前記シェル層の厚さをSLとし、トナー粒子の最大径をTLとした時に、SLとTLとが以下の関係を有することが好ましい。
0.01≦SL/TL≦0.20
より好ましくは、シェル層の厚さSLは、10nm〜2000nm、さらに好ましくは50nm〜1500nmの範囲である。粒子の最大径TLは、2000nm〜7000nm、さらに好ましくは、3000nm〜5000nmである。
本発明者らは、シェル層厚さをトナーの最大粒子径と対応させて評価することで、トナー低温定着性、耐熱保存性、感光体汚染性他の特性との関係で優位差のある特性値として評価できることを見出したものである。
(Evaluation of toner core shell structure and shell layer thickness)
The toner of the present invention is a core-shell toner having an inner core and a shell layer on the surface of the core.
In the toner of the present invention, it is preferable that SL and TL have the following relationship, where SL is the thickness of the shell layer and TL is the maximum diameter of the toner particles.
0.01 ≦ SL / TL ≦ 0.20
More preferably, the thickness SL of the shell layer is in the range of 10 nm to 2000 nm, more preferably 50 nm to 1500 nm. The maximum diameter TL of the particles is 2000 nm to 7000 nm, more preferably 3000 nm to 5000 nm.
The present inventors have evaluated the shell layer thickness in correspondence with the maximum particle diameter of the toner, so that there are characteristics that have a significant difference in relation to other characteristics such as toner low-temperature fixability, heat-resistant storage stability, and photoreceptor contamination. It has been found that it can be evaluated as a value.

本発明におけるトナーシェル層の厚さは、以下の方法で評価することができる。
《TEM(透過型電子顕微鏡)による評価》
まずトナーをスパチュラ一杯程度エポキシ系樹脂に包埋して硬化させる。四酸化ルテニウムで試料を5分間ガス暴露することでシェル層とコア内部を識別染色する。ナイフで断面出ししてウルトラミクロトーム(Leica社製 ULTRACUT UCT 、ダイヤナイフ使用)でトナーの超薄切片(200nm厚さ)を作成する。その後TEM(透過型電子顕微鏡;H7000;日立ハイテク社製)により加速電圧100kVで観察する。
得られたTEM像の画像処理解析を実施して、粒子の最大径TLとシェル層厚さSLを算出する。粒子を無作為に1粒子選択し、該粒子の最大径を求める。次にその粒子のシェル層厚さを無作為に5箇所選択して求める。同様にして他の粒子を解析して、合計10粒子の平均値でTL、SLを求める。
The thickness of the toner shell layer in the present invention can be evaluated by the following method.
<< Evaluation by TEM (Transmission Electron Microscope) >>
First, the toner is embedded and cured in an epoxy resin about one full spatula. The shell layer and the inside of the core are differentially stained by exposing the sample to gas with ruthenium tetroxide for 5 minutes. An ultra-thin section (200 nm thickness) of the toner is prepared with an ultramicrotome (ULTRACUT UCT manufactured by Leica, using a diamond knife). Thereafter, observation is performed with a TEM (transmission electron microscope; H7000; manufactured by Hitachi High-Tech) at an acceleration voltage of 100 kV.
Image processing analysis of the obtained TEM image is performed to calculate the maximum particle diameter TL and the shell layer thickness SL. One particle is selected at random and the maximum diameter of the particle is determined. Next, the thickness of the shell layer of the particles is determined by randomly selecting five locations. Similarly, other particles are analyzed, and TL and SL are obtained by the average value of a total of 10 particles.

(ヒーター内臓のSPMプローブによるシェル層、コア内部の軟化温度評価)
本発明のヒーター内臓のSPMプローブによるシェル層、コア内部の軟化温度評価は、以下の方法で評価することが好ましいが、他の手段で評価可能であればその手段でもかまわない。
ヒーター内蔵のSPMプローブとしては、アナシスインスツルメント社のnano−TAユニットを用い、SPMに設置して評価した。SPMはVeeco社製 走査型プローブ顕微鏡;MMAFM型マルチモードを用いた。nano−TAは、ヒーター内蔵のSPMプローブによりサンプルの軟化特性(TMA)、熱特性を評価する手法である。プローブ(カンチレバー)を試料の測定位置に移動させ、カンチレバーのチップを昇温させ、カンチレバーのたわみ位置を評価することでチップ温度に対する沈み込みを評価する(図1)。たわみの変極点を軟化温度として評価する。
(Evaluation of softening temperature inside shell layer and core by SPM probe with built-in heater)
The evaluation of the softening temperature inside the shell layer and the core by the SPM probe incorporated in the heater of the present invention is preferably performed by the following method, but may be performed as long as it can be evaluated by other means.
As an SPM probe with a built-in heater, a nano-TA unit manufactured by Anasys Instruments Co., Ltd. was used and evaluated by installing it in the SPM. For SPM, a scanning probe microscope manufactured by Veeco; MMMAM type multimode was used. The nano-TA is a method for evaluating the softening characteristics (TMA) and thermal characteristics of a sample using an SPM probe with a built-in heater. The probe (cantilever) is moved to the measurement position of the sample, the tip of the cantilever is heated, and the deflection position of the cantilever is evaluated to evaluate the sinking with respect to the tip temperature (FIG. 1). The inflection point of deflection is evaluated as the softening temperature.

nano−TAシステムでは、原子間力顕微鏡と同等な鋭敏な専用カンチレバーを用い、20nmの分解能で狙いの場所の軟化特性(TMA特性)が評価可能である。測定位置合わせは通常の原子間力顕微鏡としてコンタクトモード、あるいはタッピングモードで位置決めが可能で狙いのトナー断面のシェル層、コア内部の軟化特性が個別に評価できる。測定のバラツキを考慮して、トナー5粒子の平均軟化温度を評価することが好ましい。カンチレバーの昇温速度は5℃/secとした。なお装置の軟化温度は、事前に軟化温度が分かっている標準樹脂3点を用いて校正する。   The nano-TA system can evaluate the softening characteristic (TMA characteristic) of the target location with a resolution of 20 nm using a sensitive dedicated cantilever equivalent to an atomic force microscope. Measurement positioning can be performed in contact mode or tapping mode as a normal atomic force microscope, and the shell layer of the target toner cross section and the softening characteristics inside the core can be individually evaluated. In consideration of measurement variations, it is preferable to evaluate the average softening temperature of the toner 5 particles. The heating rate of the cantilever was 5 ° C./sec. The softening temperature of the apparatus is calibrated using three standard resins whose softening temperatures are known in advance.

(平均円形度E)
本発明のトナーの平均円形度Eは、円形度E=(粒子投影面積と同じ面積の円の周囲長/粒子投影像の周囲長)×100%で定義される。フロー式粒子像分析装置(「FPIA−2100」;シスメックス社製)を用いて計測し、解析ソフト(FPIA-2100 Data Processing Program for FPIA version00-10)を用いて解析を行なった。具体的には、ガラス製100mlビーカーに10wt%界面活性剤(アルキルベンゼンスフォン酸塩ネオゲンSC−A;第一工業製薬性)を0.1〜0.5ml添加し、各トナー0.1〜0.5g添加しミクロスパーテルでかき混ぜ、次いでイオン交換水80mlを添加した。得られた分散液を超音波分散器(本多電子社製)で3分間分散処理した。前記分散液を前記FPIA−2100を用いて濃度を5000〜15000個/μlが得られるまでトナーの形状及び分布を測定した。本測定法は平均円形度の測定再現性の点から前記分散液濃度が5000〜15000個/μlにすることが重要である。前記分散液濃度を得るために前記分散液の条件、すなわち添加する界面活性剤量、トナー量を変更する必要がある。界面活性剤量は前述したトナー粒径の測定と同様にトナーの疎水性により必要量が異なり、多く添加すると泡によるノイズが発生し、少ないとトナーを十分にぬらすことができないため、分散が不十分となる。またトナー添加量は粒径のより異なり、小粒径の場合は少なく、また大粒径の場合は多くする必要があり、トナー粒径が3〜7μmの場合、トナー量を0.1〜0.5g添加することにより分散液濃度を5000〜15000個/μlにあわせることが可能となる。
(Average circularity E)
The average circularity E of the toner of the present invention is defined by circularity E = (peripheral length of a circle having the same area as the projected particle area / perimeter length of the projected particle image) × 100%. Measurement was performed using a flow type particle image analyzer (“FPIA-2100”; manufactured by Sysmex Corporation), and analysis was performed using analysis software (FPIA-2100 Data Processing Program for FPIA version 00-10). Specifically, 0.1 to 0.5 ml of 10 wt% surfactant (alkylbenzene sulfonate Neogen SC-A; Daiichi Kogyo Seiyaku) is added to a glass 100 ml beaker, and each toner 0.1 to 0 is added. 0.5 g was added and stirred with a micropartel, and then 80 ml of ion-exchanged water was added. The obtained dispersion was subjected to a dispersion treatment for 3 minutes with an ultrasonic disperser (manufactured by Honda Electronics Co., Ltd.). The shape and distribution of the toner were measured using the FPIA-2100 until the density of the dispersion was 5000 to 15000 / μl. In this measurement method, it is important that the concentration of the dispersion liquid is 5000 to 15000 / μl from the viewpoint of measurement reproducibility of the average circularity. In order to obtain the dispersion concentration, it is necessary to change the conditions of the dispersion, that is, the amount of surfactant to be added and the amount of toner. The amount of the surfactant varies depending on the hydrophobicity of the toner as in the measurement of the toner particle diameter described above. If it is added in a large amount, noise due to bubbles is generated. It will be enough. Further, the toner addition amount differs from the particle size, and it is necessary to decrease the small particle size and increase the large particle size. When the toner particle size is 3 to 7 μm, the toner amount is 0.1 to 0. By adding 0.5 g, the dispersion concentration can be adjusted to 5000 to 15000 / μl.

(円形度SF−1,SF−2)
本発明に用いられる円形度である形状係数SF−1、SF−2は、日立製作所製FE−SEM(S−4200)により測定して得られたトナーのFE−SEM像を300個無作為にサンプリングし、その画像情報をインターフェースを介してニレコ社製画像解析装置(Luzex AP)に導入し解析を行い、下式より算出し得られた値をSF−1、SF−2と定義した。SF−1、SF−2の値はLuzexにより求めた値が好ましいが、同様の解析結果が得られるのであれば特に上記FE−SEM装置、画像解析装置に限定されない。
SF−1=(L2/A)×(π/4)×100
SF−2=(P2/A)×(1/4π)×100
ここで、
トナーの絶対最大長をL
トナーの投影面積をA
トナーの最大周長をP
とする。真球であればいずれも100となり、100より値が大きくなるにつれて球形から不定形になる。また特にSF−1はトナー全体の形状(楕円や球等)を表し、SF−2は表面の凹凸程度を示す形状係数となる。
(Circularity SF-1, SF-2)
The shape factors SF-1 and SF-2, which are the circularity used in the present invention, are 300 random FE-SEM images of toner obtained by measurement with an FE-SEM (S-4200) manufactured by Hitachi, Ltd. Sampling was performed, and the image information was introduced into an image analysis apparatus (Luzex AP) manufactured by Nireco through an interface for analysis. Values obtained by the following equations were defined as SF-1 and SF-2. The values of SF-1 and SF-2 are preferably values obtained by Luzex, but are not particularly limited to the FE-SEM device and the image analysis device as long as similar analysis results can be obtained.
SF-1 = (L 2 / A) × (π / 4) × 100
SF-2 = (P 2 / A) × (1 / 4π) × 100
here,
The absolute maximum length of toner is L
The projected area of the toner is A
The maximum toner circumference is P
And In the case of a true sphere, all become 100, and from a spherical shape to an indefinite shape as the value becomes larger than 100. In particular, SF-1 represents the shape of the entire toner (ellipse, sphere, etc.), and SF-2 is a shape factor indicating the degree of surface irregularities.

(重量平均粒径、D4/Dn(重量平均粒径/個数平均粒径の比))
トナーの重量平均粒径(D4)と個数平均粒径(Dn)、その比(D4/Dn)は、以下の方法で測定できる。トナーの平均粒径及び粒度分布は、コールターカウンターTA−II、コールターマルチサイザーII(いずれもコールター社製)等を用いて測定することができる。特に本発明ではコールターマルチサイザーIIを使用した。以下に測定方法について述べる。
まず、電解水溶液100〜150ml中に分散剤として界面活性剤(好ましくはポリオキシエチレンアルキルエーテル(非イオン性の界面活性剤))を0.1〜5ml加える。ここで、電解液とは1級塩化ナトリウムを用いて約1%NaCl水溶液を調製したもので、例えばISOTON−II(コールター社製)が使用できる。ここで、更に測定試料を2〜20mg加える。試料を懸濁した電解液は、超音波分散器で約1〜3分間分散処理を行ない、前記測定装置により、アパーチャーとして100μmアパーチャーを用いて、トナー粒子又はトナーの体積、個数を測定して、体積分布と個数分布を算出する。得られた分布から、トナーの重量平均粒径(D)、個数平均粒径を求めることができる。
(Weight average particle diameter, D 4 / Dn (ratio of weight average particle diameter / number average particle diameter))
The weight average particle diameter (D 4 ), number average particle diameter (Dn), and ratio (D 4 / Dn) of the toner can be measured by the following method. The average particle size and particle size distribution of the toner can be measured using a Coulter Counter TA-II, Coulter Multisizer II (both manufactured by Coulter, Inc.) and the like. In particular, Coulter Multisizer II is used in the present invention. The measurement method is described below.
First, 0.1 to 5 ml of a surfactant (preferably polyoxyethylene alkyl ether (nonionic surfactant)) is added as a dispersant to 100 to 150 ml of an electrolytic aqueous solution. Here, the electrolytic solution is a solution prepared by preparing a 1% NaCl aqueous solution using primary sodium chloride. For example, ISOTON-II (manufactured by Coulter) can be used. Here, 2 to 20 mg of a measurement sample is further added. The electrolytic solution in which the sample is suspended is subjected to a dispersion treatment with an ultrasonic disperser for about 1 to 3 minutes, and the measurement device is used to measure the volume and number of toner particles or toner using a 100 μm aperture as an aperture. Volume distribution and number distribution are calculated. From the obtained distribution, the weight average particle diameter (D 4 ) and number average particle diameter of the toner can be obtained.

チャンネルとしては、2.00〜2.52μm未満;2.52〜3.17μm未満;3.17〜4.00μm未満;4.00〜5.04μm未満;5.04〜6.35μm未満;6.35〜8.00μm未満;8.00〜10.08μm未満;10.08〜12.70μm未満;12.70〜16.00μm未満;16.00〜20.20μm未満;20.20〜25.40μm未満;25.40〜32.00μm未満;32.00〜40.30μm未満の13チャンネルを使用し、粒径2.00μm以上乃至40.30μm未満の粒子を対象とする。   As channels, 2.00 to less than 2.52 μm; 2.52 to less than 3.17 μm; 3.17 to less than 4.00 μm; 4.00 to less than 5.04 μm; 5.04 to less than 6.35 μm; 6 Less than 35 to 8.00 μm; less than 8.00 to less than 10.08 μm; less than 10.08 to less than 12.70 μm; less than 12.70 to less than 16.00 μm; less than 16.00 to less than 20.20 μm; Uses 13 channels of less than 40 μm; 25.40 to less than 32.00 μm; 32.00 to less than 40.30 μm, and targets particles having a particle size of 2.00 μm to less than 40.30 μm.

(システム線速)
本発明において、システム線速は以下のようにして測定した。A4紙、縦方向通紙(通紙方向紙の長さ297mm)、連続100枚、該当画像形成装置で出力し、スタートから終了までの出力時間をA秒とし、システム速度をBとした場合、下記式にて、システム速度を求めた。
B(mm/sec)=100枚×297mm÷A秒
(System speed)
In the present invention, the system linear velocity was measured as follows. When A4 paper, longitudinal paper passage (length of paper passage paper: 297 mm), continuous 100 sheets, output by the corresponding image forming apparatus, the output time from the start to the end is A second, and the system speed is B, The system speed was calculated by the following formula.
B (mm / sec) = 100 sheets × 297 mm ÷ A seconds

(定着加圧面圧)
本発明における定着加圧面圧は、蒲田工業株式会社の圧力センサー(PINCH)を用いて評価した。
(Fixing pressure surface pressure)
The fixing pressure surface pressure in the present invention was evaluated using a pressure sensor (PINCH) manufactured by Iwata Industry Co., Ltd.

(プロセスカートリッジ)
図2は、本発明のプロセスカートリッジを備える画像形成装置の構成を示す概略図である。図2において、プロセスカートリッジは感光体(潜像担持体)、帯電手段、現像手段、クリーニング手段を有している。
本発明においては、上述の感光体、帯電装置手段、現像手段およびクリーニング手段等の構成要素のうち、少なくとも感光体および現像手段をプロセスカートリッジとして一体に結合して構成し、このプロセスカートリッジを複写機やプリンター等の画像形成装置本体に対して着脱可能に構成する。
(Process cartridge)
FIG. 2 is a schematic view showing a configuration of an image forming apparatus including the process cartridge of the present invention. In FIG. 2, the process cartridge has a photosensitive member (latent image carrier), a charging unit, a developing unit, and a cleaning unit.
In the present invention, at least the photosensitive member and the developing unit are integrally combined as a process cartridge among the above-described components such as the photosensitive member, the charging device, the developing unit, and the cleaning unit. And an image forming apparatus main body such as a printer.

(分子量分布;Mn、Mw)
本発明の数平均分子量Mn、重量平均分子量Mwの測定は、ゲルパーミュエーションクロマトグラフィ(GPC)により測定することができる。GPCによる分子量測定は、測定装置として東ソー製GPC・HLC−8120を用い、東ソー製カラム・TSKgel SuperHM−M(15cm)を使用し、THF溶媒で行った。各平均分子量は、この測定結果から単分散ポリスチレン標準試料により作成した分子量校正曲線を使用して算出したものである。
(Molecular weight distribution; Mn, Mw)
The number average molecular weight Mn and the weight average molecular weight Mw of the present invention can be measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC was performed with a THF solvent using a Tosoh column / TSKgel Super HM-M (15 cm) using a Tosoh GPC / HLC-8120 as a measuring device. Each average molecular weight is calculated from the measurement result using a molecular weight calibration curve prepared with a monodisperse polystyrene standard sample.

(ガラス転移点;Tg)
ガラス転移点(Tg)は理学電機社製TG−DSCシステムTAS−100を使用して測定した。
まず、試料約10mgをアルミ製試料容器に入れ、それをホルダユニットに載せて電気炉中にセットする。次に、室温から昇温速度10℃/minで150℃まで加熱した後、150℃で10分間放置し、その後室温まで試料を冷却して10分間放置する。更に、窒素雰囲気下で再度150℃まで昇温速度10℃/minで加熱し、DSC測定を行なう。Tgは、TAS−100システム中の解析システムを用いて、Tg近傍の吸熱カーブの接線とベースラインとの接点から算出する。
(Glass transition point; Tg)
The glass transition point (Tg) was measured using a TG-DSC system TAS-100 manufactured by Rigaku Corporation.
First, about 10 mg of a sample is placed in an aluminum sample container, which is placed on a holder unit and set in an electric furnace. Next, after heating from room temperature to 150 ° C. at a heating rate of 10 ° C./min, the sample is allowed to stand at 150 ° C. for 10 minutes, and then the sample is cooled to room temperature and left for 10 minutes. Further, the DSC measurement is performed by heating again to 150 ° C. at a heating rate of 10 ° C./min under a nitrogen atmosphere. Tg is calculated from the contact point between the tangent line and the base line of the endothermic curve near Tg, using the analysis system in the TAS-100 system.

(ビニル系樹脂を含有するシェル層とそれに用いる樹脂微粒子)
本発明では、必要に応じてトナーのシェル層にビニル系樹脂を含有することが好ましく、スチレン・アクリル樹脂を含有する事がより好ましい。シェル化は樹脂微粒子でトナー母体粒子を覆った後、溶媒等で均一化して(あるいは溶媒の揮発性を利用して)コーティングしても良いし、熱等より表面をアニーリングする事でコーティング状態を形成しても良い。
使用される樹脂微粒子は、ガラス転移点(Tg)が40〜100℃であり、重量平均分子量が3千〜30万がより好ましく、前述したようにガラス転移点(Tg)が40℃未満、及び/又は重量平均分子量が3千未満の場合、トナーの保存性が悪化してしまい、保管時および現像機内でブロッキングを発生してしまう。ガラス転移点(Tg)が100℃を超える場合、及び/又は重量平均分子量が30万を越える場合、樹脂微粒子が定着紙との接着性を阻害してしまい、定着下限温度が上がってしまう。
(Shell layer containing vinyl resin and resin fine particles used for it)
In the present invention, it is preferable to contain a vinyl resin in the toner shell layer as required, and more preferably to contain a styrene / acrylic resin. Shelling may be performed by covering the toner base particles with resin fine particles and then coating with a solvent or the like (or using the volatility of the solvent), or by annealing the surface with heat or the like to change the coating state. It may be formed.
The resin fine particles used have a glass transition point (Tg) of 40 to 100 ° C., a weight average molecular weight of 3,000 to 300,000 is more preferable, and as described above, the glass transition point (Tg) is less than 40 ° C., and If the weight average molecular weight is less than 3,000, the storage stability of the toner deteriorates, and blocking occurs during storage and in the developing machine. When the glass transition point (Tg) exceeds 100 ° C. and / or the weight average molecular weight exceeds 300,000, the resin fine particles inhibit the adhesiveness to the fixing paper, and the minimum fixing temperature increases.

トナー粒子に対する樹脂微粒子の残存率が0.5〜5.0wt%にすることがさらに好ましい。残存率が、0.5wt%未満の時、トナーの保存性が悪化してしまい、保管時および現像機内でブロッキングの発生が見られ、また、残存量が5.0wt%を超えると、樹脂微粒子がワックスのしみ出しを阻害し、ワックスの離型性効果が十分得られず、オフセットの発生が見られる。
樹脂微粒子の残存率は、トナー粒子に起因せず樹脂微粒子に起因する物質を熱分解ガスクロマトグラフ質量分析計で分析し、そのピーク面積から算出し測定することができる。検出器としては、質量分析計が好ましいが、特に制限はない。
More preferably, the residual ratio of the resin fine particles to the toner particles is 0.5 to 5.0 wt%. When the residual ratio is less than 0.5 wt%, the storage stability of the toner deteriorates, and blocking occurs during storage and in the developing machine. When the residual amount exceeds 5.0 wt%, the resin fine particles Inhibits the seepage of the wax, and the effect of releasing the wax cannot be sufficiently obtained, and the occurrence of offset is observed.
The residual rate of the resin fine particles can be measured by analyzing a substance caused by the resin fine particles, not by the toner particles, using a pyrolysis gas chromatograph mass spectrometer, and calculating from the peak area. The detector is preferably a mass spectrometer, but is not particularly limited.

シェル層に用いる樹脂微粒子としては、ビニル系樹脂を用いることが好ましい。
ビニル系樹脂としては、ビニル系モノマーを単独重合また共重合したポリマーで、例えば、スチレン−(メタ)アクリル酸エステル樹脂、スチレン−ブタジエン共重合体、(メタ)アクリル酸−アクリル酸エステル重合体、スチレン−アクリロニトリル共重合体、スチレン−無水マレイン酸共重合体、スチレン−(メタ)アクリル酸共重合体等が挙げられる。
As the resin fine particles used for the shell layer, it is preferable to use a vinyl resin.
The vinyl resin is a polymer obtained by homopolymerization or copolymerization of a vinyl monomer, such as a styrene- (meth) acrylate resin, a styrene-butadiene copolymer, a (meth) acrylic acid-acrylate polymer, Examples include styrene-acrylonitrile copolymers, styrene-maleic anhydride copolymers, styrene- (meth) acrylic acid copolymers, and the like.

他にも、ポリスチレン、ポリp−クロロスチレン、ポリビニルトルエンなどのスチレンおよびその置換体の重合体;スチレン−p−クロロスチレン共重合体、スチレン−プロピレン共重合体、スチレン−ビニルトルエン共重合体、スチレン−ビニルナフタリン共重合体、スチレン−アクリル酸メチル共重合体、スチレン−アクリル酸エチル共重合体、スチレン−アクリル酸ブチル共重合体、スチレン−アクリル酸オクチル共重合体、スチレン−メタクリル酸メチル共重合体、スチレン−メタクリル酸エチル共重合体、スチレン−メタクリル酸ブチル共重合体、スチレン−α−クロルメタクリル酸メチル共重合体、スチレン−アクリロニトリル共重合体、スチレン−ビニルメチルケトン共重合体、スチレン−ブタジエン共重合体、スチレン−イソプレン共重合体、スチレン−アクリロニトリル−インデン共重合体、スチレン−マレイン酸共重合体、スチレン−マレイン酸エステル共重合体などのスチレン系共重合体;ポリメチルメタクリレート、ポリブチルメタクリレート等が挙げられる。 In addition, polymers of styrene and its substitution products such as polystyrene, poly p-chlorostyrene, polyvinyltoluene; styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, Styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer, styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer Polymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-α-chloromethyl methacrylate copolymer, styrene-acrylonitrile copolymer, styrene-vinyl methyl ketone copolymer, styrene -Butadiene copolymer, styrene-a Puren copolymer, styrene - acrylonitrile - indene copolymer, styrene - maleic acid copolymer, styrene - styrene copolymer and maleic acid ester copolymers; polymethyl methacrylate, polybutyl methacrylate, and the like.

(結晶性ポリエステル樹脂)
本発明で用いる結晶性ポリエステル樹脂の融点は50〜100℃の範囲にあることが必要であり、55〜90℃の範囲にあることがより望ましく、60〜85℃の範囲にあることがさらに望ましい。融点が50℃を下回ると、保管トナーにブロックキングが生じるなどのトナー保管性や、定着後の定着画像の保管性が困難となる。また、融点が100℃を超える場合では十分な低温定着性が得られない。なお、上記結晶性ポリエステル樹脂の融点は、前記の示差走査熱量測定(DSC)により得られた吸熱ピークのピーク温度として求めた。
(Crystalline polyester resin)
The melting point of the crystalline polyester resin used in the present invention is required to be in the range of 50 to 100 ° C., more preferably in the range of 55 to 90 ° C., and further preferably in the range of 60 to 85 ° C. . When the melting point is lower than 50 ° C., it becomes difficult to store the toner such that block king occurs in the stored toner and to store the fixed image after fixing. Further, when the melting point exceeds 100 ° C., sufficient low-temperature fixability cannot be obtained. In addition, melting | fusing point of the said crystalline polyester resin was calculated | required as the peak temperature of the endothermic peak obtained by the said differential scanning calorimetry (DSC).

本発明において「結晶性ポリエステル樹脂」は、その構成成分が100%ポリエステル構造であるポリマー以外にも、ポリエステルを構成する成分と他の成分とを共に重合してなるポリマー(共重合体)も意味する。但し、後者の場合には、ポリマー(共重合体)を構成するポリエステル以外の他の構成成分が50質量%以下である。   In the present invention, “crystalline polyester resin” means a polymer (copolymer) obtained by polymerizing a component constituting a polyester and another component in addition to a polymer having a 100% polyester structure as a constituent component. To do. However, in the latter case, the component other than the polyester constituting the polymer (copolymer) is 50% by mass or less.

本発明のトナーに用いられる結晶性ポリエステル樹脂は、例えば多価カルボン酸成分と多価アルコール成分とから合成される。なお、本実施形態においては、前記結晶性ポリエステル樹脂として市販品を使用してもよいし、合成したものを使用してもよい。
多価カルボン酸成分としては、例えば、シュウ酸、コハク酸、グルタル酸、アジピン酸、スペリン酸、アゼライン酸、セバシン酸、1,9−ノナンジカルボン酸、1,10−デカンジカルボン酸、1,12−ドデカンジカルボン酸、1,14−テトラデカンジカルボン酸、1,18−オクタデカンジカルボン酸等の脂肪族ジカルボン酸;フタル酸、イソフタル酸、テレフタル酸、ナフタレン−2,6−ジカルボン酸、マロン酸、メサコニン酸等の二塩基酸等の芳香族ジカルボン酸;などが挙げられ、さらに、これらの無水物やこれらの低級アルキルエステルも挙げられるがこの限りではない。
The crystalline polyester resin used in the toner of the present invention is synthesized from, for example, a polyvalent carboxylic acid component and a polyhydric alcohol component. In the present embodiment, a commercially available product may be used as the crystalline polyester resin, or a synthesized product may be used.
Examples of the polyvalent carboxylic acid component include oxalic acid, succinic acid, glutaric acid, adipic acid, peric acid, azelaic acid, sebacic acid, 1,9-nonanedicarboxylic acid, 1,10-decanedicarboxylic acid, 1,12 -Aliphatic dicarboxylic acids such as dodecanedicarboxylic acid, 1,14-tetradecanedicarboxylic acid, 1,18-octadecanedicarboxylic acid; phthalic acid, isophthalic acid, terephthalic acid, naphthalene-2,6-dicarboxylic acid, malonic acid, mesaconic acid Aromatic dicarboxylic acids such as dibasic acids such as, and the like, and anhydrides and lower alkyl esters thereof are also included, but not limited thereto.

3価以上のカルボン酸としては、例えば、1,2,4−ベンゼントリカルボン酸、1,2,5−ベンゼントリカルボン酸、1,2,4−ナフタレントリカルボン酸等、及びこれらの無水物やこれらの低級アルキルエステルなどが挙げられる。これらは1種単独で使用してもよいし、2種以上を併用してもよい。   Examples of the trivalent or higher carboxylic acid include 1,2,4-benzenetricarboxylic acid, 1,2,5-benzenetricarboxylic acid, 1,2,4-naphthalenetricarboxylic acid, and the like, and anhydrides thereof. And lower alkyl esters. These may be used individually by 1 type and may use 2 or more types together.

また、酸成分としては、前記脂肪族ジカルボン酸や芳香族ジカルボン酸の他に、スルホン酸基を持つジカルボン酸成分が含まれていてもよい。さらに、前記脂肪族ジカルボン酸や芳香族ジカルボン酸の他に、2重結合を持つジカルボン酸成分を含有してもよい。   Moreover, as an acid component, the dicarboxylic acid component which has a sulfonic acid group other than the said aliphatic dicarboxylic acid and aromatic dicarboxylic acid may be contained. Furthermore, in addition to the aliphatic dicarboxylic acid and aromatic dicarboxylic acid, a dicarboxylic acid component having a double bond may be contained.

多価アルコール成分としては、脂肪族ジオールが好ましく、主鎖部分の炭素数が7〜20である直鎖型脂肪族ジオールがより望ましい。脂肪族ジオールが分岐型では、ポリエステル樹脂の結晶性が低下し、融点が降下してしまう場合がある。また、主鎖部分の炭素数が7未満であると、芳香族ジカルボン酸と縮重合させる場合、融解温度が高くなり、低温定着が困難となることがある一方、主鎖部分の炭素数が20を超えると実用上の材料の入手が困難となり易い。主鎖部分の炭素数としては14以下であることがより望ましい。   As the polyhydric alcohol component, an aliphatic diol is preferable, and a linear aliphatic diol having 7 to 20 carbon atoms in the main chain portion is more preferable. If the aliphatic diol is branched, the crystallinity of the polyester resin is lowered, and the melting point may be lowered. Further, when the main chain portion has less than 7 carbon atoms, when polycondensation with an aromatic dicarboxylic acid, the melting temperature becomes high and fixing at low temperature may be difficult, while the main chain portion has 20 carbon atoms. Exceeding the above range makes it difficult to obtain practical materials. The number of carbon atoms in the main chain portion is more preferably 14 or less.

本発明のトナーに用いられる結晶性ポリエステルの合成に好適に用いられる脂肪族ジオールとしては、具体的には、例えば、エチレングリコール、1,3−プロパンジオール、1,4−ブタンジオール、1,5−ペンタンジオール、1,6−ヘキサンジオール、1,7−ヘプタンジオール、1,8−オクタンジオール、1,9−ノナンジオール、1,10−デカンジオール、1,11−ウンデカンジオール、1,12−ドデカンジオール、1,13−トリデカンジオール、1,14−テトラデカンジオール、1,18−オクタデカンジオール、1,14−エイコサンデカンジオールなどが挙げられるが、これらに限定されるものではない。これらのうち、入手容易性を考慮すると1,8−オクタンジオール、1,9−ノナンジオール、1,10−デカンジオールが望ましい。   Specific examples of the aliphatic diol suitably used for the synthesis of the crystalline polyester used in the toner of the present invention include ethylene glycol, 1,3-propanediol, 1,4-butanediol, and 1,5. -Pentanediol, 1,6-hexanediol, 1,7-heptanediol, 1,8-octanediol, 1,9-nonanediol, 1,10-decanediol, 1,11-undecanediol, 1,12- Examples include, but are not limited to, dodecanediol, 1,13-tridecanediol, 1,14-tetradecanediol, 1,18-octadecanediol, 1,14-eicosandecanediol, and the like. Among these, considering availability, 1,8-octanediol, 1,9-nonanediol, and 1,10-decanediol are desirable.

3価以上のアルコールとしては、例えば、グリセリン、トリメチロールエタン、トリメチロールプロパン、ペンタエリスリトールなどが挙げられる。これらは1種単独で使用してもよいし、2種以上を併用してもよい。
多価アルコール成分のうち、前記脂肪族ジオールの含有量が80モル%以上であることが好ましく、より望ましくは90%以上である。脂肪族ジオールの含有量が80モル%未満では、ポリエステル樹脂の結晶性が低下し、融解温度が降下する為、耐トナーブロッキング性、画像保存性及び、低温定着性が悪化してしまう場合がある。
Examples of the trivalent or higher alcohol include glycerin, trimethylolethane, trimethylolpropane, pentaerythritol and the like. These may be used individually by 1 type and may use 2 or more types together.
Among the polyhydric alcohol components, the content of the aliphatic diol is preferably 80 mol% or more, and more preferably 90% or more. When the content of the aliphatic diol is less than 80 mol%, the crystallinity of the polyester resin is lowered and the melting temperature is lowered, so that toner blocking resistance, image storage stability, and low-temperature fixability may be deteriorated. .

なお、必要に応じて酸価や水酸基価の調製等の目的で、多価カルボン酸や多価アルコールを合成の最終段階で添加してもよい。多価カルボン酸の例としては、テレフタル酸、イソフタル酸、無水フタル酸、無水トリメリット酸、ピロメリット酸、ナフタレンジカルボン酸、などの芳香族カルボン酸類;無水マレイン酸、フマル酸、コハク酸、アルケニル無水コハク酸、アジピン酸などの脂肪族カルボン酸類;シクロヘキサンジカルボン酸などの脂環式カルボン酸類等が挙げられる。   If necessary, a polycarboxylic acid or a polyhydric alcohol may be added at the final stage of the synthesis for the purpose of adjusting the acid value or the hydroxyl value. Examples of polycarboxylic acids include aromatic carboxylic acids such as terephthalic acid, isophthalic acid, phthalic anhydride, trimellitic anhydride, pyromellitic acid, naphthalenedicarboxylic acid; maleic anhydride, fumaric acid, succinic acid, alkenyl Aliphatic carboxylic acids such as succinic anhydride and adipic acid; and alicyclic carboxylic acids such as cyclohexanedicarboxylic acid.

多価アルコールの例としては、エチレングリコール、ジエチレングリコール、トリエチレングリコール、プロピレングリコール、ブタンジオール、ヘキサンジオール、ネオペンチルグリコール、グリセリンなどの脂肪族ジオール類;シクロヘキサンジオール、シクロヘキサンジメタノール、水添ビスフェノールAなどの脂環式ジオール類;ビスフェノールAのエチレンオキサイド付加物、ビスフェノールAのプロピレンオキサイド付加物などの芳香族ジオール類等が挙げられる。   Examples of polyhydric alcohols include aliphatic diols such as ethylene glycol, diethylene glycol, triethylene glycol, propylene glycol, butanediol, hexanediol, neopentyl glycol, glycerin; cyclohexanediol, cyclohexanedimethanol, hydrogenated bisphenol A, etc. And aromatic diols such as bisphenol A ethylene oxide adduct and bisphenol A propylene oxide adduct.

前記結晶性ポリエステル樹脂の製造は、重合温度を180〜230℃として行うことができ、必要に応じて反応系内を減圧にし、縮合の際に発生する水やアルコールを除去しながら反応させる。
重合性単量体が、反応温度下で溶解または相溶しない場合は、高沸点の溶剤を溶解補助剤として加え溶解させてもよい。重縮合反応においては、溶解補助溶剤を留去しながら行う。共重合反応において相溶性の悪い重合性単量体が存在する場合は、あらかじめ相溶性の悪い重合性単量体とその重合性単量体と重縮合予定の酸またはアルコールとを縮合させておいてから主成分と共に重縮合させるとよい。
The crystalline polyester resin can be produced at a polymerization temperature of 180 to 230 ° C., and the reaction system is depressurized as necessary, and the reaction is carried out while removing water and alcohol generated during the condensation.
When the polymerizable monomer is not dissolved or compatible at the reaction temperature, a solvent having a high boiling point may be added as a solubilizer and dissolved. In the polycondensation reaction, the dissolution auxiliary solvent is distilled off. If there is a polymerizable monomer having poor compatibility in the copolymerization reaction, the polymerizable monomer having poor compatibility and the polymerizable monomer and the acid or alcohol to be polycondensed are condensed in advance. And then polycondensation with the main component.

前記ポリエステル樹脂の製造の際に使用可能な触媒としては、ナトリウム、リチウム等のアルカリ金属化合物;マグネシウム、カルシウム等のアルカリ土類金属化合物;亜鉛、マンガン、アンチモン、チタン、スズ、ジルコニウム、ゲルマニウム等の金属化合物;亜リン酸化合物;リン酸化合物;及びアミン化合物等が挙げられる。
具体的には、酢酸ナトリウム、炭酸ナトリウム、酢酸リチウム、炭酸リチウム、酢酸カルシウム、ステアリン酸カルシウム、酢酸マグネシウム、酢酸亜鉛、ステアリン酸亜鉛、ナフテン酸亜鉛、塩化亜鉛、酢酸マンガン、ナフテン酸マンガン、チタンテトラエトキシド、チタンテトラプロポキシド、チタンテトライソプロポキシド、チタンテトラブトキシド、三酸化アンチモン、トリフェニルアンチモン、トリブチルアンチモン、ギ酸スズ、シュウ酸スズ、テトラフェニルスズ、ジブチルスズジクロライド、ジブチルスズオキシド、ジフェニルスズオキシド、ジルコニウムテトラブトキシド、ナフテン酸ジルコニウム、炭酸ジルコニール、酢酸ジルコニール、ステアリン酸ジルコニール、オクチル酸ジルコニール、酸化ゲルマニウム、トリフェニルホスファイト、トリス(2,4−ジ−t−ブチルフェニル)ホスファイト、エチルトリフェニルホスホニウムブロマイド、トリエチルアミン、トリフェニルアミン等の化合物が挙げられる。
Catalysts usable in the production of the polyester resin include alkali metal compounds such as sodium and lithium; alkaline earth metal compounds such as magnesium and calcium; zinc, manganese, antimony, titanium, tin, zirconium, germanium and the like Metal compounds; phosphorous acid compounds; phosphoric acid compounds; and amine compounds.
Specifically, sodium acetate, sodium carbonate, lithium acetate, lithium carbonate, calcium acetate, calcium stearate, magnesium acetate, zinc acetate, zinc stearate, zinc naphthenate, zinc chloride, manganese acetate, manganese naphthenate, titanium tetraethoxy , Titanium tetrapropoxide, titanium tetraisopropoxide, titanium tetrabutoxide, antimony trioxide, triphenylantimony, tributylantimony, tin formate, tin oxalate, tetraphenyltin, dibutyltin dichloride, dibutyltin oxide, diphenyltin oxide, zirconium tetra Butoxide, Zirconium naphthenate, Zirconyl carbonate, Zirconyl acetate, Zirconyl stearate, Zirconyl octylate, Germanium oxide, Trif Alkenyl phosphite, tris (2,4-di -t- butyl-phenyl) phosphite, ethyltriphenylphosphonium bromide, triethylamine, compounds such as triphenyl amine.

本発明に用いる結晶性ポリエステル樹脂の酸価(樹脂1gを中和するに必要なKOHのmg数)は、3.0〜30.0mgKOH/gの範囲であることが望ましく、6.0〜25.0mgKOH/gの範囲にあることがより望ましく、8.0〜20.0mgKOH/gの範囲にあることがさらに望ましい。
酸価が3.0mgKOH/gよりも低いと水中への分散性が低下するため、湿式製法での粒子の作製が非常に困難となる場合がある。また凝集の際における重合粒子としての安定性が著しく低下するため、効率的なトナーの作製が困難になる場合がある。一方、酸価が30.0mgKOH/gを超えると、トナーとしての吸湿性が増してしまい、トナーとしての環境影響を受けやすくなることがある。
The acid value of the crystalline polyester resin used in the present invention (mg number of KOH required to neutralize 1 g of resin) is preferably in the range of 3.0 to 30.0 mgKOH / g, and 6.0 to 25 More desirably, it is in the range of 0.0 mgKOH / g, and further desirably in the range of 8.0 to 20.0 mgKOH / g.
When the acid value is lower than 3.0 mgKOH / g, the dispersibility in water is lowered, and thus it may be very difficult to produce particles by a wet process. In addition, since stability as polymerized particles during aggregation is significantly reduced, it may be difficult to produce an efficient toner. On the other hand, when the acid value exceeds 30.0 mgKOH / g, the hygroscopicity as a toner increases and the toner may be easily affected by the environment.

また、結晶性ポリエステル樹脂の重量平均分子量(Mw)は、6,000〜35,000であることが望ましい。分子量(Mw)が、6,000未満であると、定着の際にトナーが紙等の記録媒体の表面へしみ込んで定着ムラを生じたり、定着画像の折り曲げ耐性に対する強度が低下する場合がある。また、重量平均分子量(Mw)が35,000を超えると、溶融時の粘度が高くなりすぎて定着に適当な粘度まで至るための温度が高くなることがあり、結果として低温定着性が損なわれる場合がある。   The crystalline polyester resin preferably has a weight average molecular weight (Mw) of 6,000 to 35,000. When the molecular weight (Mw) is less than 6,000, the toner may permeate the surface of a recording medium such as paper at the time of fixing to cause fixing unevenness, or the strength of the fixed image against bending resistance may be reduced. On the other hand, when the weight average molecular weight (Mw) exceeds 35,000, the viscosity at the time of melting becomes too high, and the temperature for reaching a viscosity suitable for fixing may be increased, resulting in the deterioration of the low-temperature fixability. There is a case.

上記重量平均分子量の測定は、ゲルパーミュエーションクロマトグラフィ(GPC)により測定することができる。GPCによる分子量測定は、測定装置として東ソー製GPC・HLC−8120を用い、東ソー製カラム・TSKgel SuperHM−M(15cm)を使用し、THF溶媒で行った。重量平均分子量は、この測定結果から単分散ポリスチレン標準試料により作成した分子量校正曲線を使用して算出したものである。   The weight average molecular weight can be measured by gel permeation chromatography (GPC). The molecular weight measurement by GPC was performed with a THF solvent using a Tosoh column / TSKgel Super HM-M (15 cm) using a Tosoh GPC / HLC-8120 as a measuring device. The weight average molecular weight is calculated from the measurement result using a molecular weight calibration curve prepared with a monodisperse polystyrene standard sample.

トナーにおける結晶性ポリエステル樹脂の含有量としては、3〜40質量%の範囲であることが望ましく、より望ましく4〜35質量%の範囲であり、さらに望ましくは5〜30質量%の範囲である。結晶性ポリエステル樹脂の含有量が3質量%未満であると、十分な低温定着性が得られない場合があり、40質量%より多いと、十分なトナー強度や定着画像強度が得られず、また帯電性への悪影響も生じてしまう場合がある。   The content of the crystalline polyester resin in the toner is preferably in the range of 3 to 40% by mass, more preferably in the range of 4 to 35% by mass, and still more preferably in the range of 5 to 30% by mass. When the content of the crystalline polyester resin is less than 3% by mass, sufficient low-temperature fixability may not be obtained. When the content is more than 40% by mass, sufficient toner strength and fixed image strength cannot be obtained. There is a case where an adverse effect on the charging property is also caused.

以上の結晶性ポリエステル樹脂を含む結晶性樹脂は、脂肪族重合性単量体を用いて合成された結晶性ポリエステル樹脂(以下、「結晶性脂肪族ポリエステル樹脂」という場合がある)を主成分(50質量%以上)とすることが望ましい。さらにこの場合、前記結晶性脂肪族ポリエステル樹脂を構成する脂肪族重合性単量体の構成比は、60mol%以上であることが望ましく、90mol%以上であることがより望ましい。なお、脂肪族重合性単量体としては、前述の脂肪族のジオール類やジカルボン酸類を好適に用いることができる。   The crystalline resin containing the above crystalline polyester resin is mainly composed of a crystalline polyester resin synthesized from an aliphatic polymerizable monomer (hereinafter sometimes referred to as “crystalline aliphatic polyester resin”). 50 mass% or more) is desirable. Furthermore, in this case, the constituent ratio of the aliphatic polymerizable monomer constituting the crystalline aliphatic polyester resin is preferably 60 mol% or more, and more preferably 90 mol% or more. As the aliphatic polymerizable monomer, the above-mentioned aliphatic diols and dicarboxylic acids can be suitably used.

(非結晶性ポリエステル樹脂)
本発明のトナーは結着樹脂として非結晶性ポリエステル樹脂を含有する。非結晶性ポリエステル樹脂としては変性ポリエステル樹脂と未変性ポリエステル樹脂があるが、その両方を含有することがさらに好ましい。
非結晶性ポリエステル樹脂のトナー100重量部に対する含有割合は3〜20重量部、より好ましくは5〜12重量部である。
(Non-crystalline polyester resin)
The toner of the present invention contains an amorphous polyester resin as a binder resin. The non-crystalline polyester resin includes a modified polyester resin and an unmodified polyester resin, and it is more preferable to contain both.
The content ratio of the amorphous polyester resin to 100 parts by weight of the toner is 3 to 20 parts by weight, more preferably 5 to 12 parts by weight.

(変性ポリエステル樹脂)
変性ポリエステル樹脂とは、ポリエステル樹脂中に酸、アルコールのモノマーユニットに含まれる官能基とエステル結合以外の結合基が存在したり、また、ポリエステル樹脂中に構成の異なる樹脂成分が共有結合、イオン結合等により結合した状態のものをいう。
例えば、ポリエステル末端をエステル結合以外のもので反応させたもの、具体的には、末端に酸基、水酸基と反応するイソシアネート基等の官能基を導入し、活性水素化合物とさらに反応させ、末端を変性したり伸長反応させたものも含まれる。
さらに、活性水素基が複数存在する化合物であれば、ポリエステル末端同士を結合させたものも含まれる(ウレア変性ポリエステル、ウレタン変性ポリエステル等)。また、ポリエステル主鎖中に二重結合等の反応性基を導入し、そこからラジカル重合を起こして側鎖に炭素−炭素結合のグラフト成分を導入したり、二重結合同士を橋かけしたものも含まれる(スチレン変性、アクリル変性ポリエステル等)。
また、ポリエステルの主鎖中に構成の異なる樹脂成分を共重合させたり、末端のカルボキシル基や水酸基と反応させたもの、例えば、末端がカルボキシル基、水酸基、エポキシ基、メルカプト基によって変性されたシリコーン樹脂と共重合させたものも含まれる(シリコーン変性ポリエステル等)。
本発明においては、変性ポリエステル樹脂としてはイソシアネート基を有するポリエステルプレポリマーを用いて架橋及び/又は伸長させた変性ポリエステル樹脂を用いることが好ましい。イソシアネート基を有するポリエステルプレポリマー(A)としては、ポリオール(1)とポリカルボン酸(2)の重縮合物でかつ活性水素基を有するポリエステルをさらにポリイソシアネート(3)と反応させた物などが挙げられる。上記ポリエステルの有する活性水素基としては、水酸基(アルコール性水酸基およびフェノール性水酸基)、アミノ基、カルボキシル基、メルカプト基などが挙げられ、これらのうち好ましいものはアルコール性水酸基である。
(Modified polyester resin)
The modified polyester resin is a polyester resin in which a functional group contained in the acid or alcohol monomer unit and a bonding group other than an ester bond exist, or a resin component having a different structure is covalently bonded or ionic bond in the polyester resin. It is the state of being connected by, for example.
For example, the polyester terminal is reacted with something other than an ester bond, specifically, a functional group such as an isocyanate group that reacts with an acid group or a hydroxyl group is introduced at the terminal, and further reacted with an active hydrogen compound, and the terminal is terminated. Those that have been modified or extended are also included.
Furthermore, if it is a compound in which a plurality of active hydrogen groups are present, those in which the polyester ends are bonded together (urea-modified polyester, urethane-modified polyester, etc.) are also included. In addition, a reactive group such as a double bond is introduced into the polyester main chain, and radical polymerization is caused therefrom to introduce a carbon-carbon bond graft component into the side chain, or a double bond is bridged. (Styrene-modified, acrylic-modified polyester, etc.).
In addition, a resin component having a different structure is copolymerized in the main chain of the polyester, or reacted with a carboxyl group or a hydroxyl group at the terminal, for example, a silicone having a terminal modified with a carboxyl group, a hydroxyl group, an epoxy group, or a mercapto group Also included are those copolymerized with resins (silicone-modified polyesters, etc.).
In the present invention, it is preferable to use a modified polyester resin that has been crosslinked and / or elongated using a polyester prepolymer having an isocyanate group as the modified polyester resin. Examples of the polyester prepolymer (A) having an isocyanate group include a product obtained by further reacting a polyester having an active hydrogen group with a polyisocyanate (3), which is a polycondensate of polyol (1) and polycarboxylic acid (2). Can be mentioned. Examples of the active hydrogen group possessed by the polyester include hydroxyl groups (alcoholic hydroxyl groups and phenolic hydroxyl groups), amino groups, carboxyl groups, mercapto groups, and the like. Among these, alcoholic hydroxyl groups are preferred.

ポリオール(1)としては、ジオール(1−1)および3価以上のポリオール(1−2)が挙げられ、(1−1)単独、または(1−1)と少量の(1−2)の混合物が好ましい。ジオール(1−1)としては、アルキレングリコール(エチレングリコール、1,2−プロピレングリコール、1,3−プロピレングリコール、1,4−ブタンジオール、1,6−ヘキサンジオールなど);アルキレンエーテルグリコール(ジエチレングリコール、トリエチレングリコール、ジプロピレングリコール、ポリエチレングリコール、ポリプロピレングリコール、ポリテトラメチレンエーテルグリコールなど);脂環式ジオール(1,4−シクロヘキサンジメタノール、水素添加ビスフェノールAなど);ビスフェノール類(ビスフェノールA、ビスフェノールF、ビスフェノールSなど);上記脂環式ジオールのアルキレンオキサイド(エチレンオキサイド、プロピレンオキサイド、ブチレンオキサイドなど)付加物;上記ビスフェノール類のアルキレンオキサイド(エチレンオキサイド、プロピレンオキサイド、ブチレンオキサイドなど)付加物などが挙げられる。これらのうち好ましいものは、炭素数2〜12のアルキレングリコールおよびビスフェノール類のアルキレンオキサイド付加物であり、特に好ましいものはビスフェノール類のアルキレンオキサイド付加物、およびこれと炭素数2〜12のアルキレングリコールとの併用である。3価以上のポリオール(1−2)としては、3〜8価またはそれ以上の多価脂肪族アルコール(グリセリン、トリメチロールエタン、トリメチロールプロパン、ペンタエリスリトール、ソルビトールなど);3価以上のフェノール類(トリスフェノールPA、フェノールノボラック、クレゾールノボラックなど);上記3価以上のポリフェノール類のアルキレンオキサイド付加物などが挙げられる。   Examples of the polyol (1) include a diol (1-1) and a tri- or higher valent polyol (1-2). (1-1) alone or (1-1) and a small amount of (1-2) Mixtures are preferred. Diol (1-1) includes alkylene glycol (ethylene glycol, 1,2-propylene glycol, 1,3-propylene glycol, 1,4-butanediol, 1,6-hexanediol, etc.); alkylene ether glycol (diethylene glycol) , Triethylene glycol, dipropylene glycol, polyethylene glycol, polypropylene glycol, polytetramethylene ether glycol, etc.); alicyclic diols (1,4-cyclohexanedimethanol, hydrogenated bisphenol A, etc.); bisphenols (bisphenol A, bisphenol) F, bisphenol S, etc.); alkylene oxide (ethylene oxide, propylene oxide, butylene oxide, etc.) adduct of the above alicyclic diol; Alkylene oxide phenol compound (ethylene oxide, propylene oxide, butylene oxide, etc.), etc. adducts. Among them, preferred are alkylene glycols having 2 to 12 carbon atoms and alkylene oxide adducts of bisphenols, and particularly preferred are alkylene oxide adducts of bisphenols and alkylene glycols having 2 to 12 carbon atoms. It is a combined use. The trihydric or higher polyol (1-2) includes 3 to 8 or higher polyhydric aliphatic alcohols (glycerin, trimethylolethane, trimethylolpropane, pentaerythritol, sorbitol, etc.); trihydric or higher phenols (Trisphenol PA, phenol novolak, cresol novolak, etc.); and alkylene oxide adducts of the above trivalent or higher polyphenols.

ポリカルボン酸(2)としては、ジカルボン酸(2−1)および3価以上のポリカルボン酸(2−2)が挙げられ、(2−1)単独、および(2−1)と少量の(2−2)の混合物が好ましい。ジカルボン酸(2−1)としては、アルキレンジカルボン酸(コハク酸、アジピン酸、セバシン酸など);アルケニレンジカルボン酸(マレイン酸、フマール酸など);芳香族ジカルボン酸(フタル酸、イソフタル酸、テレフタル酸、ナフタレンジカルボン酸など)などが挙げられる。これらのうち好ましいものは、炭素数4〜20のアルケニレンジカルボン酸および炭素数8〜20の芳香族ジカルボン酸である。3価以上のポリカルボン酸(2−2)としては、炭素数9〜20の芳香族ポリカルボン酸(トリメリット酸、ピロメリット酸など)などが挙げられる。なお、ポリカルボン酸(2)としては、上述のものの酸無水物または低級アルキルエステル(メチルエステル、エチルエステル、イソプロピルエステルなど)を用いてポリオール(1)と反応させてもよい。   Examples of the polycarboxylic acid (2) include dicarboxylic acid (2-1) and trivalent or higher polycarboxylic acid (2-2). (2-1) alone and (2-1) with a small amount of ( The mixture of 2-2) is preferred. Dicarboxylic acid (2-1) includes alkylene dicarboxylic acid (succinic acid, adipic acid, sebacic acid, etc.); alkenylene dicarboxylic acid (maleic acid, fumaric acid, etc.); aromatic dicarboxylic acid (phthalic acid, isophthalic acid, terephthalic acid) And naphthalenedicarboxylic acid). Of these, preferred are alkenylene dicarboxylic acids having 4 to 20 carbon atoms and aromatic dicarboxylic acids having 8 to 20 carbon atoms. Examples of the trivalent or higher polycarboxylic acid (2-2) include aromatic polycarboxylic acids having 9 to 20 carbon atoms (trimellitic acid, pyromellitic acid, and the like). In addition, as polycarboxylic acid (2), you may make it react with polyol (1) using the acid anhydride or lower alkyl ester (methyl ester, ethyl ester, isopropyl ester, etc.) of the above-mentioned thing.

ポリオール(1)とポリカルボン酸(2)の比率は、水酸基[OH]とカルボキシル基[COOH]の当量比[OH]/[COOH]として、通常2/1〜1/1、好ましくは1.5/1〜1/1、さらに好ましくは1.3/1〜1.02/1である。   The ratio of the polyol (1) and the polycarboxylic acid (2) is usually 2/1 to 1/1, preferably 1. as the equivalent ratio [OH] / [COOH] of the hydroxyl group [OH] and the carboxyl group [COOH]. 5/1 to 1/1, more preferably 1.3 / 1 to 1.02 / 1.

ポリイソシアネート(3)としては、脂肪族ポリイソシアネート(テトラメチレンジイソシアネート、ヘキサメチレンジイソシアネート、2,6−ジイソシアナトメチルカプロエートなど);脂環式ポリイソシアネート(イソホロンジイソシアネート、シクロヘキシルメタンジイソシアネートなど);芳香族ジイソシアネート(トリレンジイソシアネート、ジフェニルメタンジイソシアネートなど);芳香脂肪族ジイソシアネート(α,α,α',α'−テトラメチルキシリレンジイソシアネートなど);イソシアヌレート類;前記ポリイソシアネートをフェノール誘導体、オキシム、カプロラクタムなどでブロックしたもの;およびこれら2種以上の併用が挙げられる。   Examples of the polyisocyanate (3) include aliphatic polyisocyanates (tetramethylene diisocyanate, hexamethylene diisocyanate, 2,6-diisocyanatomethylcaproate, etc.); alicyclic polyisocyanates (isophorone diisocyanate, cyclohexylmethane diisocyanate, etc.); Diisocyanates (tolylene diisocyanate, diphenylmethane diisocyanate, etc.); araliphatic diisocyanates (α, α, α ′, α′-tetramethylxylylene diisocyanate, etc.); isocyanurates; polyisocyanates such as phenol derivatives, oximes, caprolactam And a combination of two or more of these.

ポリイソシアネート(3)の比率は、イソシアネート基[NCO]と、水酸基を有するポリエステルの水酸基[OH]の当量比[NCO]/[OH]として、通常5/1〜1/1、好ましくは4/1〜1.2/1、さらに好ましくは2.5/1〜1.5/1である。[NCO]/[OH]が5を超えると低温定着性が悪化する。[NCO]のモル比が1未満では、変性ポリエステル中のウレア含量が低くなり、耐ホットオフセット性が悪化する。末端にイソシアネート基を有するプレポリマー(A)中のポリイソシアネート(3)構成成分の含有量は、通常0.5〜40重量%、好ましくは1〜30重量%、さらに好ましくは2〜20重量%である。0.5重量%未満では、耐ホットオフセット性が悪化するとともに、耐熱保存性と低温定着性の両立の面で不利になる。また、40重量%を超えると低温定着性が悪化する。   The ratio of the polyisocyanate (3) is usually 5/1 to 1/1, preferably 4 /, as the equivalent ratio [NCO] / [OH] of the isocyanate group [NCO] and the hydroxyl group [OH] of the polyester having a hydroxyl group. 1 to 1.2 / 1, more preferably 2.5 / 1 to 1.5 / 1. When [NCO] / [OH] exceeds 5, low-temperature fixability deteriorates. If the molar ratio of [NCO] is less than 1, the urea content in the modified polyester will be low, and the hot offset resistance will deteriorate. The content of the polyisocyanate (3) component in the prepolymer (A) having an isocyanate group at the terminal is usually 0.5 to 40% by weight, preferably 1 to 30% by weight, more preferably 2 to 20% by weight. It is. If it is less than 0.5% by weight, the hot offset resistance deteriorates, and it is disadvantageous in terms of both heat-resistant storage stability and low-temperature fixability. On the other hand, if it exceeds 40% by weight, the low-temperature fixability deteriorates.

イソシアネート基を有するプレポリマー(A)中の1分子当たりに含有するイソシアネート基は、通常1個以上、好ましくは、平均1.5〜3個、さらに好ましくは、平均1.8〜2.5個である。1分子当たり1個未満では、架橋及び/又は伸長後の変性ポリエステルの分子量が低くなり、耐ホットオフセット性が悪化する。   The number of isocyanate groups contained per molecule in the prepolymer (A) having an isocyanate group is usually 1 or more, preferably 1.5 to 3 on average, more preferably 1.8 to 2.5 on average. It is. If it is less than 1 per molecule, the molecular weight of the modified polyester after crosslinking and / or elongation becomes low, and the hot offset resistance deteriorates.

(架橋剤及び伸長剤)
本発明において、架橋剤及び/又は伸長剤として、アミン類を用いることができる。アミン類(B)としては、ジアミン(B1)、3価以上のポリアミン(B2)、アミノアルコール(B3)、アミノメルカプタン(B4)、アミノ酸(B5)、およびB1〜B5のアミノ基をブロックしたもの(B6)などが挙げられる。ジアミン(B1)としては、芳香族ジアミン(フェニレンジアミン、ジエチルトルエンジアミン、4,4’ジアミノジフェニルメタンなど);脂環式ジアミン(4,4’−ジアミノ−3,3’ジメチルジシクロヘキシルメタン、ジアミンシクロヘキサン、イソホロンジアミンなど);および脂肪族ジアミン(エチレンジアミン、テトラメチレンジアミン、ヘキサメチレンジアミンなど)などが挙げられる。3価以上のポリアミン(B2)としては、ジエチレントリアミン、トリエチレンテトラミンなどが挙げられる。アミノアルコール(B3)としては、エタノールアミン、ヒドロキシエチルアニリンなどが挙げられる。アミノメルカプタン(B4)としては、アミノエチルメルカプタン、アミノプロピルメルカプタンなどが挙げられる。アミノ酸(B5)としては、アミノプロピオン酸、アミノカプロン酸などが挙げられる。B1〜B5のアミノ基をブロックしたもの(B6)としては、前記B1〜B5のアミン類とケトン類(アセトン、メチルエチルケトン、メチルイソブチルケトンなど)から得られるケチミン化合物、オキサゾリン化合物などが挙げられる。これらアミン類(B)のうち好ましいものは、B1およびB1と少量のB2の混合物である。
(Crosslinking agent and extender)
In the present invention, amines can be used as a crosslinking agent and / or an extender. As amines (B), diamine (B1), trivalent or higher polyamine (B2), aminoalcohol (B3), aminomercaptan (B4), amino acid (B5), and amino acids B1-B5 blocked (B6) etc. are mentioned. Examples of the diamine (B1) include aromatic diamines (phenylenediamine, diethyltoluenediamine, 4,4′diaminodiphenylmethane, etc.); alicyclic diamines (4,4′-diamino-3,3′dimethyldicyclohexylmethane, diaminecyclohexane, Isophorone diamine etc.); and aliphatic diamines (ethylene diamine, tetramethylene diamine, hexamethylene diamine etc.) and the like. Examples of the trivalent or higher polyamine (B2) include diethylenetriamine and triethylenetetramine. Examples of amino alcohol (B3) include ethanolamine and hydroxyethylaniline. Examples of amino mercaptan (B4) include aminoethyl mercaptan and aminopropyl mercaptan. Examples of the amino acid (B5) include aminopropionic acid and aminocaproic acid. Examples of the B1 to B5 amino group blocked (B6) include ketimine compounds and oxazoline compounds obtained from the B1 to B5 amines and ketones (acetone, methyl ethyl ketone, methyl isobutyl ketone, etc.). Among these amines (B), preferred are B1 and a mixture of B1 and a small amount of B2.

さらに、必要により架橋及び/又伸長は停止剤を用いて反応終了後の変性ポリエステルの分子量を調整することができる。停止剤としては、モノアミン(ジエチルアミン、ジブチルアミン、ブチルアミン、ラウリルアミンなど)、およびそれらをブロックしたもの(ケチミン化合物)などが挙げられる。   Furthermore, if necessary, the molecular weight of the modified polyester after completion of the reaction can be adjusted by using a terminator for crosslinking and / or elongation. Examples of the terminator include monoamines (diethylamine, dibutylamine, butylamine, laurylamine, etc.), and those blocked (ketimine compounds).

アミン類(B)の比率は、イソシアネート基を有するプレポリマー(A)中のイソシアネート基[NCO]と、アミン類(B)中のアミノ基[NHx]の当量比[NCO]/[NHx]として、通常1/2〜2/1、好ましくは1.5/1〜1/1.5、さらに好ましくは1.2/1〜1/1.2である。[NCO]/[NHx]が2より大きかったり1/2未満では、ウレア変性ポリエステル(i)の分子量が低くなり、耐ホットオフセット性が悪化する。   The ratio of amines (B) is the equivalent ratio [NCO] / [NHx] of isocyanate groups [NCO] in the prepolymer (A) having isocyanate groups and amino groups [NHx] in amines (B). The ratio is usually 1/2 to 2/1, preferably 1.5 / 1 to 1 / 1.5, more preferably 1.2 / 1 to 1 / 1.2. If [NCO] / [NHx] is greater than 2 or less than 1/2, the molecular weight of the urea-modified polyester (i) becomes low and the hot offset resistance deteriorates.

(未変性ポリエステル)
本発明においては、非結晶性ポリエステル樹脂として前記変性されたポリエステル単独使用だけでなく、この変性ポリエステルと共に、変性されていないポリエステル(C)をトナーバインダー成分として含有させることが好ましい。(C)を併用することで、低温定着性およびフルカラー装置に用いた場合の光沢性、光沢均一性が向上する。(C)としては、前記(A)のポリエステル成分と同様なポリオール(1)とポリカルボン酸(2)との重縮合物などが挙げられ、好ましいものも変性ポリエステルについて述べたものと同様である。また、(C)は無変性のポリエステルだけでなく、ウレア結合以外の化学結合で変性されているものでもよく、例えばウレタン結合で変性されていてもよい。変性ポリエステルと(C)は少なくとも一部が相溶していることが低温定着性、耐ホットオフセット性の面で好ましい。従って、変性ポリエステルのポリエステル成分と(C)は類似の組成が好ましい。変性ポリエステルを含有させる場合の変性ポリエステルと(C)の重量比は、通常5/95〜75/25、好ましくは10/90〜25/75、さらに好ましくは12/88〜25/75、特に好ましくは12/88〜22/78である。変性ポリエステルの重量比が5%未満では、耐ホットオフセット性が悪化するとともに、耐熱保存性と低温定着性の両立の面で不利になる。
(Unmodified polyester)
In the present invention, it is preferable that not only the modified polyester alone is used as the non-crystalline polyester resin, but also the unmodified polyester (C) is contained as a toner binder component together with the modified polyester. By using (C) in combination, the low-temperature fixability and the glossiness and gloss uniformity when used in a full-color apparatus are improved. Examples of (C) include the same polycondensates of polyol (1) and polycarboxylic acid (2) as in the polyester component (A), and preferred ones are the same as those described for the modified polyester. . (C) is not limited to unmodified polyester, but may be modified with a chemical bond other than a urea bond, and may be modified with, for example, a urethane bond. The modified polyester and (C) are preferably at least partially compatible with each other in terms of low-temperature fixability and hot offset resistance. Accordingly, the polyester component of the modified polyester and (C) preferably have a similar composition. When the modified polyester is contained, the weight ratio of the modified polyester to (C) is usually 5/95 to 75/25, preferably 10/90 to 25/75, more preferably 12/88 to 25/75, particularly preferably. Is 12 / 88-22 / 78. If the weight ratio of the modified polyester is less than 5%, the hot offset resistance is deteriorated, and it is disadvantageous in terms of both heat-resistant storage stability and low-temperature fixability.

(C)のピーク分子量は、通常1000〜30000、好ましくは1500〜10000、さらに好ましくは2000〜8000である。1000未満では耐熱保存性が悪化し、10000を超えると低温定着性が悪化する。(C)の水酸基価は5mgKOH/g以上であることが好ましく、さらに好ましくは10〜120mgKOH/g、特に好ましくは20〜80mgKOH/gである。5mgKOH/g未満では耐熱保存性と低温定着性の両立の面で不利になる。(C)の酸価は通常0.5〜40mgKOH/g、好ましくは5〜35mgKOH/gである。酸価を持たせることで負帯電性となりやすい傾向がある。また、酸価及び水酸基価がそれぞれこの範囲を越えるものは高温高湿度下、低温低湿度下の環境下において、環境の影響を受けやすく、画像の劣化を招きやすい。   The peak molecular weight of (C) is usually 1000-30000, preferably 1500-10000, more preferably 2000-8000. If it is less than 1000, heat-resistant storage stability will deteriorate, and if it exceeds 10,000, low-temperature fixability will deteriorate. The hydroxyl value of (C) is preferably 5 mgKOH / g or more, more preferably 10 to 120 mgKOH / g, and particularly preferably 20 to 80 mgKOH / g. If it is less than 5 mgKOH / g, it is disadvantageous in terms of both heat-resistant storage stability and low-temperature fixability. The acid value of (C) is usually 0.5 to 40 mgKOH / g, preferably 5 to 35 mgKOH / g. By having an acid value, it tends to be negatively charged. Further, those having an acid value and a hydroxyl value exceeding these ranges are easily affected by the environment under high temperature and high humidity and low temperature and low humidity, and are liable to cause image deterioration.

本発明において、トナーのガラス転移点(Tg)は通常40〜70℃、好ましくは45〜55℃である。40℃未満ではトナーの耐熱保存性が悪化し、70℃を超えると低温定着性が不十分となる。架橋及び/又は伸長されたポリエステル樹脂の共存により、本発明の静電荷像現像用トナーにおいては、公知のポリエステル系トナーと比較して、ガラス転移点が低くても良好な保存性を示す。トナーの貯蔵弾性率としては、測定周波数20Hzにおいて10000dyne/cmとなる温度(TG’)が、通常100℃以上、好ましくは110〜200℃である。100℃未満では耐ホットオフセット性が悪化する。トナーの粘性としては、測定周波数20Hzにおいて1000ポイズとなる温度(Tη)が、通常180℃以下、好ましくは90〜160℃である。180℃を超えると低温定着性が悪化する。すなわち、低温定着性と耐ホットオフセット性の両立の観点から、TG’はTηより高いことが好ましい。言い換えるとTG’とTηの差(TG’−Tη)は0℃以上が好ましい。さらに好ましくは10℃以上であり、特に好ましくは20℃以上である。差の上限は特に限定されない。また、耐熱保存性と低温定着性の両立の観点から、TηとTgの差は0〜100℃が好ましい。さらに好ましくは10〜90℃であり、特に好ましくは20〜80℃である。 In the present invention, the glass transition point (Tg) of the toner is usually 40 to 70 ° C., preferably 45 to 55 ° C. If it is less than 40 ° C., the heat-resistant storage stability of the toner deteriorates, and if it exceeds 70 ° C., the low-temperature fixability becomes insufficient. Due to the coexistence of the crosslinked and / or elongated polyester resin, the toner for developing an electrostatic charge image of the present invention exhibits good storage stability even when the glass transition point is low, as compared with known polyester-based toners. As the storage elastic modulus of the toner, the temperature (TG ′) at which the measurement frequency is 20 Hz is 10000 dyne / cm 2 is usually 100 ° C. or higher, preferably 110 to 200 ° C. If it is less than 100 ° C., the resistance to hot offset deteriorates. As the viscosity of the toner, the temperature (Tη) at 1000 poise at a measurement frequency of 20 Hz is usually 180 ° C. or less, preferably 90 to 160 ° C. If it exceeds 180 ° C., the low-temperature fixability deteriorates. That is, TG ′ is preferably higher than Tη from the viewpoint of achieving both low temperature fixability and hot offset resistance. In other words, the difference between TG ′ and Tη (TG′−Tη) is preferably 0 ° C. or higher. More preferably, it is 10 degreeC or more, Most preferably, it is 20 degreeC or more. The upper limit of the difference is not particularly limited. Further, from the viewpoint of achieving both heat-resistant storage stability and low-temperature fixability, the difference between Tη and Tg is preferably 0 to 100 ° C. More preferably, it is 10-90 degreeC, Most preferably, it is 20-80 degreeC.

(着色剤)
本発明の着色剤としては公知の染料及び顔料が全て使用でき、例えば、カーボンブラック、ニグロシン染料、鉄黒、ナフトールイエローS、ハンザイエロー(10G、5G、G)、カドミュウムイエロー、黄色酸化鉄、黄土、黄鉛、チタン黄、ポリアゾイエロー、オイルイエロー、ハンザイエロー(GR、A、RN、R)、ピグメントイエローL、ベンジジンイエロー(G、GR)、パーマネントイエロー(NCG)、バルカンファストイエロー(5G、R)、タートラジンレーキ、キノリンイエローレーキ、アンスラザンイエローBGL、イソインドリノンイエロー、ベンガラ、鉛丹、鉛朱、カドミュウムレッド、カドミュウムマーキュリレッド、アンチモン朱、パーマネントレッド4R、パラレッド、ファイセーレッド、パラクロルオルトニトロアニリンレッド、リソールファストスカーレットG、ブリリアントファストスカーレット、ブリリアントカーンミンBS、パーマネントレッド(F2R、F4R、FRL、FRLL、F4RH)、ファストスカーレットVD、ベルカンファストルビンB、ブリリアントスカーレットG、リソールルビンGX、パーマネントレッドF5R、ブリリアントカーミン6B、ポグメントスカーレット3B、ボルドー5B、トルイジンマルーン、パーマネントボルドーF2K、ヘリオボルドーBL、ボルドー10B、ボンマルーンライト、ボンマルーンメジアム、エオシンレーキ、ローダミンレーキB、ローダミンレーキY、アリザリンレーキ、チオインジゴレッドB、チオインジゴマルーン、オイルレッド、キナクリドンレッド、ピラゾロンレッド、ポリアゾレッド、クロームバーミリオン、ベンジジンオレンジ、ペリノンオレンジ、オイルオレンジ、コバルトブルー、セルリアンブルー、アルカリブルーレーキ、ピーコックブルーレーキ、ビクトリアブルーレーキ、無金属フタロシアニンブルー、フタロシアニンブルー、ファストスカイブルー、インダンスレンブルー(RS、BC)、インジゴ、群青、紺青、アントラキノンブルー、ファストバイオレットB、メチルバイオレットレーキ、コバルト紫、マンガン紫、ジオキサンバイオレット、アントラキノンバイオレット、クロムグリーン、ジンクグリーン、酸化クロム、ピリジアン、エメラルドグリーン、ピグメントグリーンB、ナフトールグリーンB、グリーンゴールド、アシッドグリーンレーキ、マラカイトグリーンレーキ、フタロシアニングリーン、アントラキノングリーン、酸化チタン、亜鉛華、リトボン及びそれらの混合物が使用できる。着色剤の含有量はトナーに対して通常1〜15重量%、好ましくは3〜10重量%である。
(Coloring agent)
As the coloring agent of the present invention, all known dyes and pigments can be used. For example, carbon black, nigrosine dye, iron black, naphthol yellow S, Hansa yellow (10G, 5G, G), cadmium yellow, yellow iron oxide , Ocher, yellow lead, titanium yellow, polyazo yellow, oil yellow, Hansa yellow (GR, A, RN, R), pigment yellow L, benzidine yellow (G, GR), permanent yellow (NCG), Vulcan fast yellow ( 5G, R), Tartrazine Lake, Quinoline Yellow Lake, Anthrazan Yellow BGL, Isoindolinone Yellow, Bengala, Red Dan, Lead Zhu, Cadmium Red, Cadmium Mercury Red, Antimon Zhu, Permanent Red 4R, Para Red , Fais red, parachlorol Nitroaniline Red, Resol Fast Scarlet G, Brilliant Fast Scarlet, Brilliant Carmine B, Permanent Red (F2R, F4R, FRL, FRLL, F4RH), Fast Scarlet VD, Belkan Fast Rubin B, Brilliant Scarlet G, Resol Rubin GX, Permanent Red F5R, Brilliant Carmine 6B, Pigment Scarlet 3B, Bordeaux 5B, Tolujing Maroon, Permanent Bordeaux F2K, Helio Bordeaux BL, Bordeaux 10B, Bon Maroon Light, Bon Maroon Medium, Eosin Lake, Rhodamine Lake B, Rhodamine Lake Y, Alizarin Lake , Thioindigo red B, thioindigo maroon, oil red, quinacridone red, pyrazolone , Polyazo red, chrome vermillion, benzidine orange, perinone orange, oil orange, cobalt blue, cerulean blue, alkali blue rake, peacock blue rake, Victoria blue rake, metal-free phthalocyanine blue, phthalocyanine blue, fast sky blue, in Dunslen Blue (RS, BC), Indigo, Ultramarine Blue, Bitumen, Anthraquinone Blue, Fast Violet B, Methyl Violet Lake, Cobalt Purple, Manganese Purple, Dioxane Violet, Anthraquinone Violet, Chrome Green, Zinc Green, Chrome Oxide, Pyridian, Emerald Green, Pigment Green B, Naphthol Green B, Green Gold, Acid Green Lake, Malachite Green Lake Phthalocyanine green, anthraquinone green, titanium oxide, zinc white, litbon and mixtures thereof can be used. The content of the colorant is usually 1 to 15% by weight, preferably 3 to 10% by weight, based on the toner.

本発明で用いる着色剤は樹脂と複合化されたマスターバッチとして用いることもできる。 マスターバッチの製造またはマスターバッチとともに混練されるバインダー樹脂としては、先にあげた変性、未変性ポリエステル樹脂の他にポリスチレン、ポリp−クロロスチレン、ポリビニルトルエンなどのスチレン及びその置換体の重合体;スチレン−p−クロロスチレン共重合体、スチレン−プロピレン共重合体、スチレン−ビニルトルエン共重合体、スチレン−ビニルナフタリン共重合体、スチレン−アクリル酸メチル共重合体、スチレン−アクリル酸エチル共重合体、スチレン−アクリル酸ブチル共重合体、スチレン−アクリル酸オクチル共重合体、スチレン−メタクリル酸メチル共重合体、スチレン−メタクリル酸エチル共重合体、スチレン−メタクリル酸ブチル共重合体、スチレン−α−クロルメタクリル酸メチル共重合体、スチレン−アクリロニトリル共重合体、スチレン−ビニルメチルケトン共重合体、スチレン−ブタジエン共重合体、スチレン−イソプレン共重合体、スチレン−アクリロニトリル−インデン共重合体、スチレン−マレイン酸共重合体、スチレン−マレイン酸エステル共重合体などのスチレン系共重合体;ポリメチルメタクリレート、ポリブチルメタクリレート、ポリ塩化ビニル、ポリ酢酸ビニル、ポリエチレン、ポリプロピレン、ポリエステル、エポキシ樹脂、エポキシポリオール樹脂、ポリウレタン、ポリアミド、ポリビニルブチラール、ポリアクリル酸樹脂、ロジン、変性ロジン、テルペン樹脂、脂肪族叉は脂環族炭化水素樹脂、芳香族系石油樹脂、塩素化パラフィン、パラフィンワックスなどが挙げられ、単独あるいは混合して使用できる。   The colorant used in the present invention can also be used as a master batch combined with a resin. As the binder resin to be kneaded together with the production of the masterbatch or the masterbatch, in addition to the modified and unmodified polyester resins mentioned above, styrene such as polystyrene, poly p-chlorostyrene, polyvinyltoluene, and polymers of substituted products thereof; Styrene-p-chlorostyrene copolymer, styrene-propylene copolymer, styrene-vinyltoluene copolymer, styrene-vinylnaphthalene copolymer, styrene-methyl acrylate copolymer, styrene-ethyl acrylate copolymer Styrene-butyl acrylate copolymer, styrene-octyl acrylate copolymer, styrene-methyl methacrylate copolymer, styrene-ethyl methacrylate copolymer, styrene-butyl methacrylate copolymer, styrene-α- Chloromethyl methacrylate copolymer, Tylene-acrylonitrile copolymer, styrene-vinyl methyl ketone copolymer, styrene-butadiene copolymer, styrene-isoprene copolymer, styrene-acrylonitrile-indene copolymer, styrene-maleic acid copolymer, styrene-maleic acid Styrene copolymers such as acid ester copolymers; polymethyl methacrylate, polybutyl methacrylate, polyvinyl chloride, polyvinyl acetate, polyethylene, polypropylene, polyester, epoxy resin, epoxy polyol resin, polyurethane, polyamide, polyvinyl butyral, poly Acrylic resin, rosin, modified rosin, terpene resin, aliphatic or alicyclic hydrocarbon resin, aromatic petroleum resin, chlorinated paraffin, paraffin wax, etc. The

本マスターバッチはマスターバッチ用の樹脂と着色剤とを高せん断力をかけて混合、混練してマスターバッチを得る事ができる。この際着色剤と樹脂の相互作用を高めるために、有機溶剤を用いる事ができる。またいわゆるフラッシング法と呼ばれる着色剤の水を含んだ水性ペーストを樹脂と有機溶剤とともに混合混練を行い、着色剤を樹脂側に移行させ、水分と有機溶剤成分を除去する方法も着色剤のウエットケーキをそのまま用いる事ができるため乾燥する必要がなく、好ましく用いられる。混合混練するには3本ロールミル等の高せん断分散装置が好ましく用いられる。   This master batch can be obtained by mixing and kneading a resin for a master batch and a colorant under a high shear force to obtain a master batch. At this time, an organic solvent can be used to enhance the interaction between the colorant and the resin. In addition, a so-called flushing method, which is a wet cake of a coloring agent, is a method of mixing and kneading an aqueous paste containing water of a coloring agent together with a resin and an organic solvent, transferring the coloring agent to the resin side, and removing moisture and organic solvent components. Can be used as it is, so that it is not necessary to dry and is preferably used. For mixing and kneading, a high shear dispersion device such as a three-roll mill is preferably used.

(離型剤)
また、トナーバインダー、着色剤とともに離型剤としてワックスを含有させることもできる。本発明のワックスとしては公知のものが使用でき、例えばポリオレフィンワッックス(ポリエチレンワックス、ポリプロピレンワックスなど);長鎖炭化水素(パラフィンワッックス、サゾールワックスなど);カルボニル基含有ワックスなどが挙げられる。これらのうち好ましいものは、カルボニル基含有ワックスである。カルボニル基含有ワックスとしては、ポリアルカン酸エステル(カルナバワックス、モンタンワックス、トリメチロールプロパントリベヘネート、ペンタエリスリトールテトラベヘネート、ペンタエリスリトールジアセテートジベヘネート、グリセリントリベヘネート、1,18-オクタデカンジオールジステアレートなど);ポリアルカノールエステル(トリメリット酸トリステアリル、ジステアリルマレエートなど);ポリアルカン酸アミド(エチレンジアミンジベヘニルアミドなど);ポリアルキルアミド(トリメリット酸トリステアリルアミドなど);およびジアルキルケトン(ジステアリルケトンなど)などが挙げられる。これらカルボニル基含有ワックスのうち好ましいものは、ポリアルカン酸エステルである。本発明のワックスの融点は、通常40〜160℃であり、好ましくは50〜120℃、さらに好ましくは60〜90℃である。融点が40℃未満のワックスは耐熱保存性に悪影響を与え、160℃を超えるワックスは低温での定着時にコールドオフセットを起こしやすい。また、ワックスの溶融粘度は、融点より20℃高い温度での測定値として、5〜1000cpsが好ましく、さらに好ましくは10〜100cpsである。1000cpsを超えるワックスは、耐ホットオフセット性、低温定着性への向上効果に乏しい。トナー中のワックスの含有量は通常0〜40重量%であり、好ましくは3〜30重量%である。
(Release agent)
Further, a wax may be contained as a release agent together with the toner binder and the colorant. Known waxes can be used as the wax of the present invention, such as polyolefin wax (polyethylene wax, polypropylene wax, etc.); long chain hydrocarbon (paraffin wax, sazol wax, etc.); carbonyl group-containing wax, etc. It is done. Of these, carbonyl group-containing waxes are preferred. Carbonyl group-containing waxes include polyalkanoic acid esters (carnauba wax, montan wax, trimethylolpropane tribehenate, pentaerythritol tetrabehenate, pentaerythritol diacetate dibehenate, glycerin tribehenate, 1,18. -Octadecandiol diol distearate, etc.); polyalkanol esters (tristearyl trimellitic acid, distearyl maleate, etc.); polyalkanoic acid amides (ethylenediamine dibehenyl amide, etc.); And dialkyl ketones (such as distearyl ketone). Among these carbonyl group-containing waxes, polyalkanoic acid esters are preferred. The melting point of the wax of the present invention is usually 40 to 160 ° C, preferably 50 to 120 ° C, more preferably 60 to 90 ° C. A wax having a melting point of less than 40 ° C. has an adverse effect on heat resistant storage stability, and a wax having a melting point of more than 160 ° C. tends to cause a cold offset when fixing at a low temperature. Further, the melt viscosity of the wax is preferably 5 to 1000 cps, more preferably 10 to 100 cps as a measured value at a temperature 20 ° C. higher than the melting point. Waxes exceeding 1000 cps have poor effects for improving hot offset resistance and low-temperature fixability. The content of the wax in the toner is usually 0 to 40% by weight, preferably 3 to 30% by weight.

(帯電制御剤)
本発明のトナーは、必要に応じて帯電制御剤を含有してもよい。帯電制御剤としては公知のものが全て使用でき、例えばニグロシン系染料、トリフェニルメタン系染料、クロム含有金属錯体染料、モリブデン酸キレート顔料、ローダミン系染料、アルコキシ系アミン、4級アンモニウム塩(フッ素変性4級アンモニウム塩を含む)、アルキルアミド、燐の単体または化合物、タングステンの単体または化合物、フッ素系活性剤、サリチル酸金属塩及び、サリチル酸誘導体の金属塩等である。具体的にはニグロシン系染料のボントロン03、第四級アンモニウム塩のボントロンPー51、含金属アゾ染料のボントロンSー34、オキシナフトエ酸系金属錯体のEー82、サリチル酸系金属錯体のEー84、フェノール系縮合物のEー89(以上、オリエント化学工業社製)、第四級アンモニウム塩モリブデン錯体のTPー302、TP一415(以上、保土谷化学工業社製)、第四級アンモニウム塩のコピーチャージPSY VP2038、トリフェニルメタン誘導体のコピーブルーPR、第四級アンモニウム塩のコピーチャージ NEG VP2036、コピーチャージ NX VP434(以上、ヘキスト社製)、LRAー901、ホウ素錯体であるLRー147(日本カ一リット社製)、銅フタロシアニン、ペリレン、キナクリドン、アゾ系顔料、その他スルホン酸基、カルボキシル基、四級アンモニウム塩等の官能基を有する高分子系の化合物が挙げられる。
(Charge control agent)
The toner of the present invention may contain a charge control agent as necessary. All known charge control agents can be used, such as nigrosine dyes, triphenylmethane dyes, chromium-containing metal complex dyes, molybdate chelate pigments, rhodamine dyes, alkoxy amines, quaternary ammonium salts (fluorine-modified). Quaternary ammonium salts), alkylamides, phosphorus simple substances or compounds, tungsten simple substances or compounds, fluorine-based activators, salicylic acid metal salts, and metal salts of salicylic acid derivatives. Specifically, Nitronine dye Bontron 03, quaternary ammonium salt Bontron P-51, metal-containing azo dye Bontron S-34, oxynaphthoic acid metal complex E-82, salicylic acid metal complex E- 84, E-89 of a phenol-based condensate (above, Orient Chemical Industry Co., Ltd.), TP-302 of a quaternary ammonium salt molybdenum complex, TP 1415 (above, Hodogaya Chemical Industry Co., Ltd.), quaternary ammonium Copy charge PSY VP2038 of salt, copy blue PR of triphenylmethane derivative, copy charge of quaternary ammonium salt NEG VP2036, copy charge NX VP434 (above, manufactured by Hoechst), LRA-901, LR-147 which is a boron complex (Nippon Carlit Co., Ltd.), copper phthalocyanine, perylene, quinacridone Azo pigments, sulfonate group, carboxyl group, and polymer compounds having a functional group such as a quaternary ammonium salt.

本発明において荷電制御剤の使用量は、バインダー樹脂の種類、必要に応じて使用される添加剤の有無、分散方法を含めたトナー製造方法によって決定されるもので、一義的に限定されるものではないが、好ましくはバインダー樹脂100重量部に対して、0.1〜10重量部の範囲で用いられる。好ましくは、0.2〜5重量部の範囲がよい。10重量部を越える場合にはトナーの帯電性が大きすぎ、主帯電制御剤の効果を減退させ、現像ローラとの静電的吸引力が増大し、現像剤の流動性低下や、画像濃度の低下を招く。これらの帯電制御剤はマスターバッチ、樹脂とともに溶融混練した後溶解分散させる事もできるし、もちろん有機溶剤に直接溶解、分散する際に加えても良いし、トナー表面にトナー粒子作成後固定化させてもよい。   In the present invention, the amount of charge control agent used is determined by the toner production method including the type of binder resin, the presence or absence of additives used as necessary, and the dispersion method, and is uniquely limited. However, it is preferably used in the range of 0.1 to 10 parts by weight with respect to 100 parts by weight of the binder resin. The range of 0.2 to 5 parts by weight is preferable. When the amount exceeds 10 parts by weight, the chargeability of the toner is too high, the effect of the main charge control agent is reduced, the electrostatic attractive force with the developing roller is increased, the flowability of the developer is reduced, and the image density is reduced. Incurs a decline. These charge control agents can be dissolved and dispersed after being melt-kneaded with a masterbatch and resin, and of course, they can be added directly when dissolved and dispersed in an organic solvent, or fixed on the toner surface after preparation of toner particles. May be.

(外添剤)
本発明で得られた着色粒子の流動性や現像性、帯電性を補助するための外添剤としては、酸化物微粒子の他に、無機微粒子や疎水化処理無機微粒子を併用することができるが、疎水化処理された無機微粒子の一次粒子の平均粒径は1〜150nm、より好ましくは5nm〜70nmであり、この無機微粒子を少なくとも1種類以上含むことがより望ましい。この範囲より小さいと、無機微粒子がトナー中に埋没し、その機能が有効に発揮されにくい。またこの範囲より大きいと、感光体表面を不均一に傷つけ好ましくない。
さらに疎水化処理された一次粒子の平均粒径が20nm以下の無機微粒子を少なくとも1種類以上含みかつ、30nm以上の無機微粒子を少なくとも1種類以上含むことがより望ましい。また、BET法による比表面積は、20〜500m2/gであることが好ましい。
それらは、条件を満たせば公知のものすべて使用可能である。例えば、シリカ微粒子、疎水性シリカ、脂肪酸金属塩(ステアリン酸亜鉛、ステアリン酸アルミニウムなど)、金属酸化物(チタニア、アルミナ、酸化錫、酸化アンチモンなど)、フルオロポリマー等を含有してもよい。
前記の外添剤の添加量はトナーに対し0.1から5重量%、好ましくは0.3から3重量%を用いる事ができる。
(External additive)
As an external additive for assisting fluidity, developability and chargeability of the colored particles obtained in the present invention, inorganic fine particles and hydrophobic treated inorganic fine particles can be used in combination with oxide fine particles. The average particle size of the primary particles of the hydrophobized inorganic fine particles is from 1 to 150 nm, more preferably from 5 nm to 70 nm, and it is more desirable to contain at least one kind of these inorganic fine particles. If it is smaller than this range, the inorganic fine particles are buried in the toner, and the function is hardly exhibited effectively. On the other hand, if it is larger than this range, the surface of the photoreceptor is undesirably damaged.
Further, it is more preferable that the hydrophobized primary particles contain at least one kind of inorganic fine particles having an average particle diameter of 20 nm or less and at least one kind of inorganic fine particles of 30 nm or more. Moreover, it is preferable that the specific surface area by BET method is 20-500 m < 2 > / g.
Any of them can be used as long as the conditions are satisfied. For example, silica fine particles, hydrophobic silica, fatty acid metal salts (such as zinc stearate and aluminum stearate), metal oxides (such as titania, alumina, tin oxide, and antimony oxide), fluoropolymers, and the like may be contained.
The external additive may be added in an amount of 0.1 to 5% by weight, preferably 0.3 to 3% by weight, based on the toner.

特に好適な添加剤としては、疎水化されたシリカ、チタニア、酸化チタン、アルミナ微粒子があげられる。シリカ微粒子としては、HDK H 2000、HDK H 2000/4、HDK H 2050EP、HVK21、HDK H 1303(以上ヘキスト)やR972、R974、RX200、RY200、R202、R805、R812(以上日本アエロジル)がある。また、チタニア微粒子としては、P−25(日本アエロジル)やSTT−30、STT−65C−S(以上チタン工業)、TAF−140(富士チタン工業)、MT−150W、MT−500B、MT−600B、MT−150A(以上テイカ)などがある。特に疎水化処理された酸化チタン微粒子としては、T−805(日本アエロジル)やSTT−30A、STT−65S−S(以上チタン工業)、TAF−500T、TAF−1500T(以上富士チタン工業)、MT−100S、MT−100T(以上テイカ)、IT−S(石原産業)などがある。   Particularly suitable additives include hydrophobized silica, titania, titanium oxide, and alumina fine particles. Silica fine particles include HDK H 2000, HDK H 2000/4, HDK H 2050EP, HVK21, HDK H 1303 (above Hoechst) and R972, R974, RX200, RY200, R202, R805, and R812 (above Nippon Aerosil). Further, as titania fine particles, P-25 (Nippon Aerosil), STT-30, STT-65C-S (above Titanium Industry), TAF-140 (Fuji Titanium Industry), MT-150W, MT-500B, MT-600B MT-150A (taker above). Particularly, the hydrophobized titanium oxide fine particles include T-805 (Nippon Aerosil), STT-30A, STT-65S-S (above Titanium Industry), TAF-500T, TAF-1500T (above Fuji Titanium Industry), MT -100S, MT-100T (above Taka), IT-S (Ishihara Sangyo), etc.

疎水化処理された酸化物微粒子、シリカ微粒子及びチタニア微粒子、アルミナ微粒子を得るためには、親水性の微粒子をメチルトリメトキシシランやメチルトリエトキシシラン、オクチルトリメトキシシランなどのシランカップリング剤で処理して得ることができる。またシリコーンオイルを必要ならば熱を加えて無機微粒子に処理した、シリコーンオイル処理酸化物微粒子、無機微粒子も好適である。   In order to obtain hydrophobized oxide fine particles, silica fine particles, titania fine particles, and alumina fine particles, hydrophilic fine particles are treated with a silane coupling agent such as methyltrimethoxysilane, methyltriethoxysilane, or octyltrimethoxysilane. Can be obtained. In addition, silicone oil-treated oxide fine particles and inorganic fine particles obtained by treating silicone oil with heat if necessary to treat it with inorganic fine particles are also suitable.

シリコーンオイルとしては、例えばジメチルシリコーンオイル、メチルフェニルシリコーンオイル、クロルフェニルシリコーンオイル、メチルハイドロジェンシリコーンオイル、アルキル変性シリコーンオイル、フッ素変性シリコーンオイル、ポリエーテル変性シリコーンオイル、アルコール変性シリコーンオイル、アミノ変性シリコーンオイル、エポキシ変性シリコーンオイル、エポキシ・ポリエーテル変性シリコーンオイル、フェノール変性シリコーンオイル、カルボキシル変性シリコーンオイル、メルカプト変性シリコーンオイル、アクリル、メタクリル変性シリコーンオイル、αメチルスチレン変性シリコーンオイル等が使用できる。無機微粒子としては、例えばシリカ、アルミナ、酸化チタン、チタン酸バリウム、チタン酸マグネシウム、チタン酸カルシウム、チタン酸ストロンチウム、酸化鉄、酸化銅、酸化亜鉛、酸化スズ、ケイ砂、クレー、雲母、ケイ灰石、ケイソウ土、酸化クロム、酸化セリウム、ペンガラ、三酸化アンチモン、酸化マグネシウム、酸化ジルコニウム、硫酸パリウム、炭酸バリウム、炭酸カルシウム、炭化ケイ素、窒化ケイ素などを挙げることができる。その中でも特にシリカと二酸化チタンが好ましい。   Examples of the silicone oil include dimethyl silicone oil, methylphenyl silicone oil, chlorophenyl silicone oil, methyl hydrogen silicone oil, alkyl modified silicone oil, fluorine modified silicone oil, polyether modified silicone oil, alcohol modified silicone oil, amino modified silicone. Oil, epoxy-modified silicone oil, epoxy-polyether-modified silicone oil, phenol-modified silicone oil, carboxyl-modified silicone oil, mercapto-modified silicone oil, acrylic, methacryl-modified silicone oil, α-methylstyrene-modified silicone oil, and the like can be used. Examples of the inorganic fine particles include silica, alumina, titanium oxide, barium titanate, magnesium titanate, calcium titanate, strontium titanate, iron oxide, copper oxide, zinc oxide, tin oxide, quartz sand, clay, mica, and silica ash. Examples thereof include stone, diatomaceous earth, chromium oxide, cerium oxide, pengala, antimony trioxide, magnesium oxide, zirconium oxide, parium sulfate, barium carbonate, calcium carbonate, silicon carbide, and silicon nitride. Of these, silica and titanium dioxide are particularly preferred.

この他高分子系微粒子たとえばソープフリー乳化重合や懸濁重合、分散重合によって得られるポリスチレン、メタクリル酸エステルやアクリル酸エステル共重合体やシリコーン、ベンゾグアナミン、ナイロンなどの重縮合系、熱硬化性樹脂による重合体粒子が挙げられる。   Other polymer fine particles such as polystyrene, methacrylic acid ester and acrylic acid ester copolymer obtained by soap-free emulsion polymerization, suspension polymerization, and dispersion polymerization, polycondensation systems such as silicone, benzoguanamine, and nylon, and thermosetting resins Examples include polymer particles.

このような流動化剤は表面処理を行って、疎水性を上げ、高湿度下においても流動特性や帯電特性の悪化を防止することができる。例えばシランカップリング剤、シリル化剤、フッ化アルキル基を有するシランカップリング剤、有機チタネート系カップリング剤、アルミニウム系のカップリング剤、シリコーンオイル、変性シリコーンオイルなどが好ましい表面処理剤として挙げられる。   Such a fluidizing agent can be surface-treated to increase hydrophobicity and prevent deterioration of flow characteristics and charging characteristics even under high humidity. For example, silane coupling agents, silylating agents, silane coupling agents having an alkyl fluoride group, organic titanate coupling agents, aluminum coupling agents, silicone oils, modified silicone oils and the like are preferable surface treatment agents. .

感光体や一次転写媒体に残存する転写後の現像剤を除去するためのクリーニング性向上剤としては、例えばステアリン酸亜鉛、ステアリン酸カルシウム、ステアリン酸など脂肪酸金属塩、例えばポリメチルメタクリレート微粒子、ポリスチレン微粒子などのソープフリー乳化重合などによって製造された、ポリマー微粒子などを挙げることかできる。ポリマー微粒子は比較的粒度分布が狭く、体積平均粒径が0.01から1μmのものが好ましい。   Examples of the cleaning property improver for removing the developer after transfer remaining on the photoreceptor or the primary transfer medium include, for example, zinc stearate, calcium stearate, fatty acid metal salts such as stearic acid, such as polymethyl methacrylate fine particles, polystyrene fine particles, etc. And polymer fine particles produced by soap-free emulsion polymerization. The polymer fine particles preferably have a relatively narrow particle size distribution and a volume average particle size of 0.01 to 1 μm.

本発明の乾式トナーは以下の方法で製造することができるが勿論これらに限定されることはない。
(水系媒体中でのトナー製造法)
本発明に用いる水性相には、予め樹脂微粒子を添加することにより使用するとより好ましい。水性相に用いる水は、水単独でも良いが、水と混和可能な溶剤を併用することもできる。混和可能な溶剤としては、アルコール(メタノール、イソプロパノール、エチレングリコールなど)、ジメチルホルムアミド、テトラヒドロフラン、セルソルブ類(メチルセルソルブなど)、低級ケトン類(アセトン、メチルエチルケトンなど)などが挙げられる。
The dry toner of the present invention can be produced by the following method, but is not limited thereto.
(Toner production method in aqueous medium)
The aqueous phase used in the present invention is more preferably used by adding resin fine particles in advance. The water used in the aqueous phase may be water alone, or a solvent miscible with water may be used in combination. Examples of the miscible solvent include alcohol (methanol, isopropanol, ethylene glycol, etc.), dimethylformamide, tetrahydrofuran, cellosolves (methylcellosolve, etc.), lower ketones (acetone, methyl ethyl ketone, etc.) and the like.

トナー粒子は、水性相で有機溶媒に溶解、又は分散させたイソシアネート基を有するポリエステルプレポリマー(A)を含有する分散体を、アミン類(B)と反応させて形成することにより得られる。水性相でポリエステルプレポリマー(A)を含有する分散体を安定して形成させる方法としては、水性相に有機溶媒に溶解、又は分散させたポリエステルプレポリマー(A)からなるトナー原料の組成物を加えて、せん断力により分散させる方法などが挙げられる。有機溶媒に溶解、又は分散させたポリエステルプレポリマー(A)と他のトナー組成物である(以下トナー原料と呼ぶ)着色剤、着色剤マスターバッチ、離型剤、荷電制御剤、結晶性ポリエステル樹脂、未変性ポリエステル樹脂などは、水性相で分散体を形成させる際に混合してもよいが、あらかじめトナー原料を混合後、有機溶媒に溶解、又は分散させた後、水性相にその混合物を加えて分散させたほうがより好ましい。
また、本発明においては、荷電制御剤などの他のトナー原料は、必ずしも、水性相で粒子を形成させる時に混合しておく必要はなく、粒子を形成せしめた後、添加してもよい。
Toner particles are obtained by reacting a dispersion containing an isocyanate group-containing polyester prepolymer (A) dissolved or dispersed in an organic solvent in an aqueous phase with amines (B). As a method for stably forming a dispersion containing the polyester prepolymer (A) in the aqueous phase, a composition of a toner raw material comprising the polyester prepolymer (A) dissolved or dispersed in an organic solvent in the aqueous phase is used. In addition, a method of dispersing by shearing force may be mentioned. A polyester prepolymer (A) dissolved or dispersed in an organic solvent and other toner composition (hereinafter referred to as toner raw material), a colorant masterbatch, a release agent, a charge control agent, a crystalline polyester resin Unmodified polyester resin and the like may be mixed when forming the dispersion in the aqueous phase, but after the toner raw materials are mixed in advance and dissolved or dispersed in an organic solvent, the mixture is added to the aqueous phase. It is more preferable to disperse them.
In the present invention, other toner raw materials such as a charge control agent are not necessarily mixed when forming particles in an aqueous phase, and may be added after the particles are formed.

イソシアネート基を有するプレポリマー(A)は、ポリオール(1)とポリカルボン酸(2)を、テトラブトキシチタネート、ジブチルチンオキサイドなど公知のエステル化触媒の存在下、150〜280℃に加熱し、必要により減圧としながら生成する水を溜去して、水酸基を有するポリエステルを得て、次いで40〜140℃にて、これにポリイソシアネート(3)を反応させることにより得ることができる。   Prepolymer (A) having an isocyanate group is required to heat polyol (1) and polycarboxylic acid (2) to 150 to 280 ° C. in the presence of a known esterification catalyst such as tetrabutoxy titanate or dibutyltin oxide. The water produced while distilling under reduced pressure is distilled off to obtain a polyester having a hydroxyl group, which is then reacted at 40 to 140 ° C. with polyisocyanate (3).

分散の方法としては特に限定されるものではないが、低速せん断式、高速せん断式、摩擦式、高圧ジェット式、超音波などの公知の設備が適用できる。分散体の粒径を2〜20μmにするために高速せん断式が好ましい。高速せん断式分散機を使用した場合、回転数は特に限定はないが、通常1000〜30000rpm、好ましくは5000〜20000rpmである。分散時間は特に限定はないが、バッチ方式の場合は、通常0.1〜5分である。分散時の温度としては、通常、0〜150℃(加圧下)、好ましくは40〜98℃である。高温なほうが、ポリエステルプレポリマー(A)からなる分散体の粘度が低く、分散が容易な点で好ましい。   The dispersion method is not particularly limited, and known equipment such as a low-speed shear method, a high-speed shear method, a friction method, a high-pressure jet method, and an ultrasonic wave can be applied. In order to make the particle size of the dispersion 2 to 20 μm, a high-speed shearing type is preferable. When a high-speed shearing disperser is used, the rotational speed is not particularly limited, but is usually 1000 to 30000 rpm, preferably 5000 to 20000 rpm. The dispersion time is not particularly limited, but in the case of a batch method, it is usually 0.1 to 5 minutes. The temperature during dispersion is usually 0 to 150 ° C. (under pressure), preferably 40 to 98 ° C. Higher temperatures are preferred in that the dispersion of the polyester prepolymer (A) has a low viscosity and is easy to disperse.

ポリエステルプレポリマー(A)を含むトナー組成物100部に対する水性相の使用量は、通常50〜2000重量部、好ましくは100〜1000重量部である。50重量部未満ではトナー組成物の分散状態が悪く、所定の粒径のトナー粒子が得られない。20000重量部を超えると経済的でない。また、必要に応じて、分散剤を用いることもできる。分散剤を用いたほうが、粒度分布がシャープになるとともに分散が安定である点で好ましい。   The amount of the aqueous phase used is usually 50 to 2000 parts by weight, preferably 100 to 1000 parts by weight, based on 100 parts of the toner composition containing the polyester prepolymer (A). If the amount is less than 50 parts by weight, the dispersion state of the toner composition is poor, and toner particles having a predetermined particle diameter cannot be obtained. If it exceeds 20000 parts by weight, it is not economical. Moreover, a dispersing agent can also be used as needed. It is preferable to use a dispersant because the particle size distribution becomes sharp and the dispersion is stable.

トナー組成物が分散された油性相を水性相に乳化、分散するための分散剤としてアルキルベンゼンスルホン酸塩、αーオレフィンスルホン酸塩、リン酸エステルなどの陰イオン界面活性荊、アルキルアミン塩、アミノアルコール脂肪酸誘導体、ポリアミン脂肪酸誘導体、イミダゾリンなどのアミン塩型や、アルキルトリメチルアンモニム塩、ジアルキルジメチルアンモニウム塩、アルキルジメチルベンジルアンモニウム塩、ピリジニウム塩、アルキルイソキノリニウム塩、塩化ベンゼトニウムなどの四級アンモニウム塩型の陽イオン界面活性剤、脂肪酸アミド誘導体、多価アルコール誘導体などの非イオン界面活性剤、例えばアラニン、ドデシルジ(アミノエチル)グリシン、ジ(オクチルアミノエチル)グリシンやNーアルキルーN,Nージメチルアンモニウムベタインなどの両性界面活性剤が挙げられる。   Anionic surfactants such as alkylbenzene sulfonates, α-olefin sulfonates, phosphate esters, alkylamine salts, amino acids as dispersants for emulsifying and dispersing the oily phase in which the toner composition is dispersed in the aqueous phase Amine salt types such as alcohol fatty acid derivatives, polyamine fatty acid derivatives, imidazoline, and quaternary ammonium such as alkyltrimethylammonium salt, dialkyldimethylammonium salt, alkyldimethylbenzylammonium salt, pyridinium salt, alkylisoquinolinium salt, benzethonium chloride Nonionic surfactants such as salt-type cationic surfactants, fatty acid amide derivatives, polyhydric alcohol derivatives such as alanine, dodecyldi (aminoethyl) glycine, di (octylaminoethyl) glycine and N-alkyl-N, N-di Amphoteric surfactants such as chill ammonium betaine.

またフルオロアルキル基を有する界面活性剤を用いることにより、非常に少量でその効果をあげることができる。好ましく用いられるフルオロアルキル基を有するアニオン性界面活性剤としては、炭素数2〜10のフルオロアルキルカルボン酸及びその金属塩、パーフルオロオクタンスルホニルグルタミン酸ジナトリウム、3−[オメガ−フルオロアルキル(C6〜C11)オキシ]−1−アルキル(C3〜C4)スルホン酸ナトリウム、3−[オメガ−フルオロアルカノイル(C6〜C8)−N−エチルアミノ]−1−プロパンスルホン酸ナトリウム、フルオロアルキル(C11〜C20)カルボン酸及びその金属塩、パーフルオロアルキルカルボン酸(C7〜C13)及びその金属塩、パーフルオロアルキル(C4〜C12)スルホン酸及びその金属塩、パーフルオロオクタンスルホン酸ジエタノールアミド、N−プロピル−N−(2ヒドロキシエチル)パーフルオロオクタンスルホンアミド、パーフルオロアルキル(C6〜C10)スルホンアミドプロピルトリメチルアンモニウム塩、パーフルオロアルキル(C6〜C10)−N−エチルスルホニルグリシン塩、モノパーフルオロアルキル(C6〜C16)エチルリン酸エステルなどが挙げられる,   Further, by using a surfactant having a fluoroalkyl group, the effect can be obtained in a very small amount. Preferred anionic surfactants having a fluoroalkyl group include fluoroalkyl carboxylic acids having 2 to 10 carbon atoms and metal salts thereof, disodium perfluorooctanesulfonyl glutamate, 3- [omega-fluoroalkyl (C6-C11 ) Oxy] -1-alkyl (C3-C4) sodium sulfonate, 3- [omega-fluoroalkanoyl (C6-C8) -N-ethylamino] -1-propanesulfonic acid sodium, fluoroalkyl (C11-C20) carvone Acids and metal salts thereof, perfluoroalkylcarboxylic acids (C7 to C13) and metal salts thereof, perfluoroalkyl (C4 to C12) sulfonic acids and metal salts thereof, perfluorooctanesulfonic acid diethanolamide, N-propyl-N- (2-hydroxyethyl ) Perfluorooctanesulfonamide, perfluoroalkyl (C6-C10) sulfonamidopropyltrimethylammonium salt, perfluoroalkyl (C6-C10) -N-ethylsulfonylglycine salt, monoperfluoroalkyl (C6-C16) ethyl phosphate Etc.,

商品名としては、サーフロンS−111、S−112、S−113(旭硝子社製)、フロラードFC−93、FC−95、FC−98、FC−l29(住友3M社製)、ユニダインDS−101、DS−l02、(ダイキン工業社製)、メガファックF−ll0、F−l20、F−113、F−191、F−812、F−833(大日本インキ社製)、エクトップEF−102、l03、104、105、112、123A、123B、306A、501、201、204、(トーケムプロダクツ社製)、フタージェントF−100、F150(ネオス社製)などが挙げられる。   Product names include Surflon S-111, S-112, S-113 (Asahi Glass Co., Ltd.), Florard FC-93, FC-95, FC-98, FC-129 (Sumitomo 3M Co., Ltd.), Unidyne DS-101. DS-102 (Daikin Kogyo Co., Ltd.), Mega-Fac F-l0, F-l20, F-113, F-191, F-812, F-833 (Dainippon Ink Co., Ltd.), Xtop EF-102 , 103, 104, 105, 112, 123A, 123B, 306A, 501, 201, 204 (manufactured by Tochem Products), and Fagento F-100, F150 (manufactured by Neos).

また、カチオン界面活性剤としては、フルオロアルキル基を有する脂肪族一級、二級もしくは三級アミン酸、パーフルオロアルキル(C6〜C10)スルホンアミドプロピルトリメチルアンモニウム塩などの脂肪族4級アンモニウム塩、ベンザルコニウム塩、塩化ベンゼトニウム、ピリジニウム塩、イミダゾリニウム塩、商品名としてはサーフロンSーl21(旭硝子社製)、フロラードFC−135(住友3M社製)、ユニダインDS−202(ダイキン工業社製)、メガファックF−150、F−824(大日本インキ社製)、エクトップEF−l32(トーケムプロダクツ社製)、フタージェントF−300(ネオス社製)などが挙げられる。   Cationic surfactants include aliphatic primary, secondary or tertiary amine acids having a fluoroalkyl group, aliphatic quaternary ammonium salts such as perfluoroalkyl (C6-C10) sulfonamidopropyltrimethylammonium salts, benzaza Luconium salt, benzethonium chloride, pyridinium salt, imidazolinium salt, trade names include Surflon S-21 (Asahi Glass), Florard FC-135 (Sumitomo 3M), Unidyne DS-202 (Daikin Industries) , Megafac F-150, F-824 (Dainippon Ink Co., Ltd.), Xtop EF-132 (Tochem Products Co., Ltd.), Footgent F-300 (Neos Co., Ltd.), and the like.

また水に難溶の無機化合物分散剤としてリン酸三カルシウム、炭酸カルシウム、酸化チタン、コロイダルシリカ、ヒドロキシアパタイトなども用いる事が出来る。
また高分子系保護コロイドにより分散液滴を安定化させても良い。例えばアクリル酸、メタクリル酸、α−シアノアクリル酸、α−シアノメタクリル酸、イタコン酸、クロトン酸、フマール酸、マレイン酸または無水マレイン酸などの酸類、あるいは水酸基を含有する(メタ)アクリル系単量体、例えばアクリル酸β−ヒドロキシエチル、メタクリル酸β−ヒドロキシエチル、アクリル酸β−ヒドロキシプロピル、メタクリル酸β−ヒドロキシプロピル、アクリル酸γ−ヒドロキシプロピル、メタクリル酸γ−ヒドロキシプロピル、アクリル酸3−クロロ2−ヒドロキシプロピル、メタクリル酸3−クロロ−2−ヒドロキシプロピル、ジエチレングリコールモノアクリル酸エステル、ジエチレングリコールモノメタクリル酸エステル、グリセリンモノアクリル酸エステル、グリセリンモノメタクリル酸エステル、N−メチロールアクリルアミド、N−メチロールメタクリルアミドなど、ビニルアルコールまたはビニルアルコールとのエーテル類、例えばビニルメチルエーテル、ビニルエチルエーテル、ビニルプロピルエーテルなど、またはビニルアルコールとカルボキシル基を含有する化合物のエステル類、例えば酢酸ビニル、プロピオン酸ビニル、酪酸ビニルなど、アクリルアミド、メタクリルアミド、ジアセトンアクリルアミドあるいはこれらのメチロール化合物、アクリル酸クロライド、メタクリル酸クロライドなどの酸クロライド類、ビニルピリジン、ビニルピロリドン、ビニルイミダゾール、エチレンイミンなどの窒素原子、またはその複素環を有するものなどのホモポリマーまたは共重合体、ポリオキシエチレン、ポリオキシプロピレン、ポリオキシエチレンアルキルアミン、ポリオキシプロピレンアルキルアミン、ポリオキシエチレンアルキルアミド、ポリオキシプロピレンアルキルアミド、ポリオキシエチレンノニルフエニルエーテル、ポリオキシエチレンラウリルフェニルエーテル、ポリオキシエチレンステアリルフェニルエステル、ポリオキシエチレンノニルフェニルエステルなどのポリオキシエチレン系、メチルセルロース、ヒドロキシエチルセルロース、ヒドロキシプロピルセルロースなどのセルロース類などが使用できる。
Further, tricalcium phosphate, calcium carbonate, titanium oxide, colloidal silica, hydroxyapatite and the like can be used as an inorganic compound dispersant which is hardly soluble in water.
Further, the dispersed droplets may be stabilized by a polymer protective colloid. For example, acrylic acid, methacrylic acid, α-cyanoacrylic acid, α-cyanomethacrylic acid, itaconic acid, crotonic acid, fumaric acid, maleic acid or maleic anhydride and other (meth) acrylic monomers containing hydroxyl groups Such as β-hydroxyethyl acrylate, β-hydroxyethyl methacrylate, β-hydroxypropyl acrylate, β-hydroxypropyl methacrylate, γ-hydroxypropyl acrylate, γ-hydroxypropyl methacrylate, 3-chloroacrylate 2-hydroxypropyl, 3-chloro-2-hydroxypropyl methacrylate, diethylene glycol monoacrylate, diethylene glycol monomethacrylate, glycerol monoacrylate, glycerol monomethacrylate, N -Methylol acrylamide, N-methylol methacrylamide, etc., vinyl alcohol or ethers with vinyl alcohol, such as vinyl methyl ether, vinyl ethyl ether, vinyl propyl ether, etc., or esters of compounds containing vinyl alcohol and carboxyl groups, such as Vinyl acetate, vinyl propionate, vinyl butyrate, etc., acrylamide, methacrylamide, diacetone acrylamide or their methylol compounds, acid chlorides such as acrylic acid chloride, methacrylic acid chloride, vinyl pyridine, vinyl pyrrolidone, vinyl imidazole, ethyleneimine, etc. Homopolymers or copolymers such as those having a nitrogen atom or a heterocyclic ring thereof, polyoxyethylene, polyoxypropylene, Oxyethylene alkylamine, polyoxypropylene alkylamine, polyoxyethylene alkylamide, polyoxypropylene alkylamide, polyoxyethylene nonyl phenyl ether, polyoxyethylene lauryl phenyl ether, polyoxyethylene stearyl phenyl ester, polyoxyethylene nonylphenyl Polyoxyethylenes such as esters, celluloses such as methyl cellulose, hydroxyethyl cellulose, and hydroxypropyl cellulose can be used.

なお、分散安定剤としてリン酸カルシウム塩などの酸、アルカリに溶解可能な物を用いた場合は、塩酸等の酸により、リン酸カルシウム塩を溶解した後、水洗するなどの方法によって、微粒子からリン酸カルシウム塩を除去する。その他酵素による分解などの操作によっても除去できる。
分散剤を使用した場合には、該分散剤がトナー粒子表面に残存したままとすることもできるが、伸長および/または架橋反応後、洗浄除去するほうがトナーの帯電面から好ましい。
In addition, when an acid such as calcium phosphate salt or an alkali-soluble substance is used as the dispersion stabilizer, the calcium phosphate salt is removed from the fine particles by a method such as dissolving the calcium phosphate salt with an acid such as hydrochloric acid and washing with water. To do. It can also be removed by operations such as enzymatic degradation.
When a dispersant is used, the dispersant may remain on the surface of the toner particles, but it is preferable from the charged surface of the toner that the dispersant is washed and removed after the elongation and / or crosslinking reaction.

伸長および/または架橋反応時間は、プレポリマー(A)の有するイソシアネート基構造とアミン類(B)の組み合わせによる反応性により選択されるが、通常10分〜40時間、好ましくは2〜24時間である。反応温度は、通常、0〜150℃、好ましくは40〜98℃である。また、必要に応じて公知の触媒を使用することができる。具体的にはジブチルチンラウレート、ジオクチルチンラウレートなどが挙げられる。   The elongation and / or cross-linking reaction time is selected depending on the reactivity of the isocyanate group structure of the prepolymer (A) and the amines (B), but is usually 10 minutes to 40 hours, preferably 2 to 24 hours. is there. The reaction temperature is generally 0 to 150 ° C, preferably 40 to 98 ° C. Moreover, a well-known catalyst can be used as needed. Specific examples include dibutyltin laurate and dioctyltin laurate.

得られた乳化分散体から有機溶媒を除去するためには、系全体を徐々に昇温し、液滴中の有機溶媒を完全に蒸発除去する方法を採用することができる。あるいはまた、乳化分散体を乾燥雰囲気中に噴霧して、液滴中の非水溶性有機溶媒を完全に除去してトナー微粒子を形成し、合せて水系分散剤を蒸発除去することも可能である。乳化分散体が噴霧される乾燥雰囲気としては、空気、窒素、炭酸ガス、燃焼ガス等を加熱した気体、特に使用される最高沸点溶媒の沸点以上の温度に加熱された各種気流が一般に用いられる。スプレイドライアー、ベルトドライアー、ロータリーキルンなどの短時間の処理で十分目的とする品質が得られる。
また有機溶媒を除去する方法として、ロータリーエバポレータ等でエアーを吹き込み除去させることが可能である。
In order to remove the organic solvent from the obtained emulsified dispersion, a method in which the temperature of the entire system is gradually raised to completely evaporate and remove the organic solvent in the droplets can be employed. Alternatively, the emulsified dispersion can be sprayed into a dry atmosphere to completely remove the water-insoluble organic solvent in the droplets to form toner fine particles, and the aqueous dispersant can be removed by evaporation together. . As a dry atmosphere in which the emulsified dispersion is sprayed, a gas obtained by heating air, nitrogen, carbon dioxide gas, combustion gas, or the like, in particular, various air streams heated to a temperature equal to or higher than the boiling point of the highest boiling solvent used are generally used. Sufficient quality can be obtained with a short treatment such as spray dryer, belt dryer or rotary kiln.
Further, as a method for removing the organic solvent, air can be blown away by a rotary evaporator or the like.

その後、遠心分離により粗分離を行い、洗浄タンクにて乳化分散体を洗浄、温風乾燥機にて乾燥の工程を繰り返し、溶媒を除去、乾燥させてトナー母体を得ることができる。
乾燥後に熟成工程を入れることが好ましく、その熟成条件は30〜55℃(より好ましくは40〜50℃)で、5〜36時間(より好ましくは10〜24時間)である。
Thereafter, rough separation is performed by centrifugal separation, the emulsified dispersion is washed in a washing tank, and the drying process is repeated in a hot air dryer, and the solvent is removed and dried to obtain a toner base.
It is preferable to put an aging step after drying, and the aging conditions are 30 to 55 ° C. (more preferably 40 to 50 ° C.) and 5 to 36 hours (more preferably 10 to 24 hours).

乳化分散時の粒度分布が広く、その粒度分布を保って洗浄、乾燥処理が行われた場合、所望の粒度分布に分級して粒度分布を整えることができる。
分級操作は液中でサイクロン、デカンター、遠心分離等により、微粒子部分を取り除くことができる。もちろん乾燥後に粉体として取得した後に分級操作を行っても良いが、液体中で行うことが効率の面で好ましい。得られた不要の微粒子、または粗粒子は再び混練工程に戻して粒子の形成に用いることができる。その際微粒子、または粗粒子はウェットの状態でも構わない。
用いた分散剤は得られた分散液からできるだけ取り除くことが好ましいが、先に述べた分級操作と同時に行うのが好ましい。
When the particle size distribution at the time of emulsification dispersion is wide and washing and drying processes are performed while maintaining the particle size distribution, the particle size distribution can be adjusted by classifying into a desired particle size distribution.
In the classification operation, the fine particle portion can be removed in the liquid by a cyclone, a decanter, centrifugation, or the like. Of course, the classification operation may be performed after obtaining the powder as a powder after drying. The unnecessary fine particles or coarse particles obtained can be returned to the kneading step and used for the formation of particles. At that time, fine particles or coarse particles may be wet.
The dispersant used is preferably removed from the obtained dispersion as much as possible, but it is preferable to carry out it simultaneously with the classification operation described above.

得られた乾燥後のトナーの粉体と帯電制御性微粒子、流動化剤微粒子、などの異種粒子とともに混合を行ったり、混合粉体に機械的衝撃力を与えることによって表面で固定化、融合化させ、得られる複合体粒子の表面からの異種粒子の脱離を防止することができる。
具体的手段としては、高速で回転する羽根によって混合物に衝撃力を加える方法、高速気流中に混合物を投入し、加速させ、粒子同士または複合化した粒子を適当な衝突板に衝突させる方法などがある。装置としては、オングミル(ホソカワミクロン社製)、I式ミル(日本ニューマチック社製)を改造して、粉砕エアー圧カを下げた装置、ハイブリダイゼイションシステム(奈良機械製作所社製)、クリプトロンシステム(川崎重工業社製)、自動乳鉢などがあげられる。
最後に無機微粒子等の外添剤とトナーをヘンシェルミキサー等で混合し、超音波篩い等で粗大粒子を除去して、最終的なトナーを得る。
The obtained dried toner powder is mixed and mixed with different particles such as charge control fine particles and fluidizer fine particles, and mechanical impact force is applied to the mixed powder to fix and fuse on the surface. Thus, detachment of the foreign particles from the surface of the obtained composite particle can be prevented.
Specific means include a method of applying an impact force to the mixture by blades rotating at high speed, a method of injecting and accelerating the mixture in a high-speed air stream, and causing particles or composite particles to collide with an appropriate collision plate, etc. is there. As equipment, Ong mill (manufactured by Hosokawa Micron Co., Ltd.), I-type mill (manufactured by Nippon Pneumatic Co., Ltd.) is modified to reduce the pulverization air pressure, hybridization system (manufactured by Nara Machinery Co., Ltd.), kryptron System (manufactured by Kawasaki Heavy Industries, Ltd.), automatic mortar, etc.
Finally, an external additive such as inorganic fine particles and a toner are mixed with a Henschel mixer or the like, and coarse particles are removed with an ultrasonic sieve or the like to obtain a final toner.

(二成分現像剤用キャリア)
本発明のトナーを2成分系現像剤に用いる場合には、磁性キャリアと混合して用いれば良く、現像剤中のキャリアとトナーの含有比は、キャリア100重量部に対してトナー1〜10重量部が好ましい。磁性キャリアとしては、粒子径20〜200μm程度の鉄粉、フェライト粉、マグネタイト粉、磁性樹脂キャリアなど従来から公知のものが使用できる。また、被覆材料としては、アミノ系樹脂、例えば尿素−ホルムアルデヒド樹脂、メラミン樹脂、ベンゾグアナミン樹脂、ユリア樹脂、ポリアミド樹脂、エポキシ樹脂等があげられる。またポリビニルおよびポリビニリデン系樹脂、例えばアクリル樹脂、ポリメチルメタクリレート樹脂、ポリアクリロニトリル樹脂、ポリ酢酸ビニル樹脂、ポリビニルアルコール樹脂、ポリビニルブチラール樹脂、ポリスチレン樹脂およびスチレンアクリル共重合樹脂等のポリスチレン系樹脂、ポリ塩化ビニル等のハロゲン化オレフィン樹脂、ポリエチレンテレフタレート樹脂およびポリブチレンテレフタレート樹脂等のポリエステル系樹脂、ポリカーボネート系樹脂、ポリエチレン樹脂、ポリ弗化ビニル樹脂、ポリ弗化ビニリデン樹脂、ポリトリフルオロエチレン樹脂、ポリヘキサフルオロプロピレン樹脂、弗化ビニリデンとアクリル単量体との共重合体、弗化ビニリデンと弗化ビニルとの共重合体、テトラフルオロエチレンと弗化ビニリデンと非弗化単量体とのターポリマー等のフルオロターポリマー、およびシリコーン樹脂等が使用できる。また必要に応じて、導電粉等を被覆樹脂中に含有させてもよい。導電粉としては、金属粉、カーボンブラック、酸化チタン、酸化錫、酸化亜鉛等が使用できる。これらの導電粉は、平均粒子径1μm以下のものが好ましい。平均粒子径が1μmよりも大きくなると、電気抵抗の制御が困難になる。
また、本発明のトナーはキャリアを使用しない1成分系の磁性トナー或いは、非磁性トナーとしても用いることができる。
(Carrier for two-component developer)
When the toner of the present invention is used for a two-component developer, it may be used by mixing with a magnetic carrier. The carrier to toner content ratio in the developer is 1 to 10 weights of toner with respect to 100 parts by weight of carrier. Part is preferred. As the magnetic carrier, conventionally known ones such as iron powder, ferrite powder, magnetite powder, magnetic resin carrier having a particle diameter of about 20 to 200 μm can be used. Examples of the coating material include amino resins such as urea-formaldehyde resin, melamine resin, benzoguanamine resin, urea resin, polyamide resin, and epoxy resin. Polyvinyl and polyvinylidene resins such as acrylic resins, polymethyl methacrylate resins, polyacrylonitrile resins, polyvinyl acetate resins, polyvinyl alcohol resins, polyvinyl butyral resins, polystyrene resins and styrene acrylic copolymer resins, Halogenated olefin resins such as vinyl, polyester resins such as polyethylene terephthalate resin and polybutylene terephthalate resin, polycarbonate resins, polyethylene resins, polyvinyl fluoride resins, polyvinylidene fluoride resins, polytrifluoroethylene resins, polyhexafluoro Propylene resin, copolymer of vinylidene fluoride and acrylic monomer, copolymer of vinylidene fluoride and vinyl fluoride, tetrafluoroethylene and vinylidene fluoride And fluoro such as terpolymers of non-fluoride monomers including, and silicone resins. Moreover, you may contain electrically conductive powder etc. in coating resin as needed. As the conductive powder, metal powder, carbon black, titanium oxide, tin oxide, zinc oxide or the like can be used. These conductive powders preferably have an average particle diameter of 1 μm or less. When the average particle diameter is larger than 1 μm, it becomes difficult to control electric resistance.
The toner of the present invention can also be used as a one-component magnetic toner that does not use a carrier or a non-magnetic toner.

(補給用トナー)
本発明では、補給用トナーとして、トナーに0〜20重量%程度キャリアを含有させたキャリア入りトナーを補給用トナーとする事が可能である。
二成分現像剤を使用する画像形成装置においては、キャリアは、画像出力枚数が増加するとキャリアが劣化して、徐々にキャリアコート層の削れあるいは、トナーの低温溶融成分、外添剤等がキャリア表面に付着するキャリアスペントの現象が発生して、キャリア本来の帯電能力は発揮できず、画像地肌汚れ等の画像劣化の原因となり好ましくない。そこで劣化キャリアを徐々に排出して、代わりに新しいキャリアを補給する事でトータルのキャリア寿命を延ばす事が可能である。
(Supply toner)
In the present invention, as the replenishment toner, a toner containing a carrier containing about 0 to 20% by weight of the carrier in the toner can be used as the replenishment toner.
In an image forming apparatus using a two-component developer, the carrier deteriorates as the number of output images increases, and the carrier coat layer is gradually scraped or the low-temperature melting component of the toner, external additives, etc. The phenomenon of carrier spent adhering to the toner occurs, and the charging ability inherent to the carrier cannot be exhibited, which is not preferable because it causes image deterioration such as image background contamination. Therefore, it is possible to extend the total carrier life by gradually discharging the deteriorated carriers and supplying new carriers instead.

(タンデム型カラー画像形成装置)
本発明では、少なくとも4つ以上の現像色の異なる現像ユニットを直列に配置したタンデム型の現像方式のカラー画像形成装置としても使用できる。タンデム型カラー画像形成装置の実施形態の一例について説明する。タンデム型の電子写真装置には、図3に示すように、各感光体1上の画像を転写装置2により、シート搬送ベルト3で搬送するシートsに順次転写する直接転写方式のものと、図4に示すように、各感光体1上の画像を1次転写装置2によりいったん中間転写体4に順次転写して後、その中間転写体4上の画像を2次転写装置5によりシートsに一括転写する間接転写方式のものとがある。転写装置5は転写搬送ベルトであるが,ローラ形状も方式もある。
(Tandem type color image forming device)
The present invention can also be used as a color image forming apparatus of a tandem development system in which at least four development units having different development colors are arranged in series. An example of an embodiment of a tandem type color image forming apparatus will be described. As shown in FIG. 3, the tandem type electrophotographic apparatus includes a direct transfer system in which an image on each photoconductor 1 is sequentially transferred onto a sheet s conveyed by a sheet conveying belt 3 by a transfer apparatus 2; As shown in FIG. 4, the images on the respective photoconductors 1 are once sequentially transferred to the intermediate transfer member 4 by the primary transfer device 2, and then the images on the intermediate transfer member 4 are transferred to the sheet s by the secondary transfer device 5. There are indirect transfer systems that perform batch transfer. The transfer device 5 is a transfer conveyance belt, but there are also roller shapes and methods.

直接転写方式のものと,間接転写方式のものとを比較すると、前者は、感光体1を並べたタンデム型画像形成装置Tの上流側に給紙装置6を、下流側に定着装置7を配置しなければならず、シート搬送方向に大型化する欠点がある。
これに対し、後者は、2次転写位置を比較的自由に設置することができる。
給紙装置6,および定着装置7をタンデム型画像形成装置Tと重ねて配置することができ、小型化が可能となる利点がある。
Comparing the direct transfer type with the indirect transfer type, the former arranges the sheet feeding device 6 on the upstream side of the tandem type image forming apparatus T on which the photoconductors 1 are arranged, and the fixing device 7 on the downstream side. There is a drawback in that the size increases in the sheet conveying direction.
On the other hand, the latter can set the secondary transfer position relatively freely.
The sheet feeding device 6 and the fixing device 7 can be arranged so as to overlap with the tandem image forming apparatus T, and there is an advantage that downsizing is possible.

また、前者は、シート搬送方向に大型化しないためには,定着装置7をタンデム型画像形成装置Tに接近して配置することとなる。そのため,シートsがたわむことができる十分な余裕をもって定着装置7を配置することができず、シートsの先端が定着装置7に進入するときの衝撃(特に厚いシートで顕著となる)や,定着装置7を通過するときのシート搬送速度と,転写搬送ベルトによるシート搬送速度との速度差により、定着装置7が上流側の画像形成に影響を及ぼしやすい欠点がある。
これに対し、後者は、シートsがたわむことができる十分な余裕をもって定着装置7を配置することができるから、定着装置7がほとんど画像形成に影響を及ぼさないようにすることができる。
In the former, in order not to increase the size in the sheet conveying direction, the fixing device 7 is arranged close to the tandem type image forming apparatus T. Therefore, the fixing device 7 cannot be disposed with a sufficient margin that the sheet s can bend, and an impact (particularly with a thick sheet) when the leading edge of the sheet s enters the fixing device 7 or fixing. Due to the difference in speed between the sheet conveyance speed when passing through the apparatus 7 and the sheet conveyance speed by the transfer conveyance belt, there is a drawback that the fixing device 7 tends to affect image formation on the upstream side.
On the other hand, in the latter case, the fixing device 7 can be disposed with a sufficient margin that the sheet s can be bent, so that the fixing device 7 can hardly affect the image formation.

以上のようなことから、最近は、タンデム型電子写真装置の中の、特に間接転写方式のものが注目されてきている。
そして、この種のカラー電子写真装置では、図4に示すように、1次転写後に感光体1上に残留する転写残トナーを、感光体クリーニング装置8で除去して感光体1表面をクリーニングし、再度の画像形成に備えていた。また、2次転写後に中間転写体4上に残留する転写残トナーを、中間転写体クリーニング装置9で除去して中間転写体4表面をクリーニングし、再度の画像形成に備えていた。
In view of the above, recently, an indirect transfer type of tandem type electrophotographic apparatus has attracted attention.
In this type of color electrophotographic apparatus, as shown in FIG. 4, the transfer residual toner remaining on the photoreceptor 1 after the primary transfer is removed by the photoreceptor cleaning device 8 to clean the surface of the photoreceptor 1. In preparation for another image formation. Further, the transfer residual toner remaining on the intermediate transfer body 4 after the secondary transfer is removed by the intermediate transfer body cleaning device 9 to clean the surface of the intermediate transfer body 4 to prepare for image formation again.

以下、図面を参照しつつ、この発明の実施の形態につき説明する。
図5は、この発明の一実施の形態を示すもので、タンデム型間接転写方式の電子写真装置である。図中符号100は複写装置本体、200はそれを載せる給紙テーブル、300は複写装置本体100上に取り付けるスキャナ、400はさらにその上に取り付ける原稿自動搬送装置(ADF)である。複写装置本体100には、中央に、無端ベルト状の中間転写体10を設ける。
そして、図5に示すとおり、図示例では3つの支持ローラ14・15・16に掛け回して図中時計回りに回転搬送可能とする。
この図示例では、3つのなかで第2の支持ローラ15の左に、画像転写後に中間転写体10上に残留する残留トナーを除去する中間転写体クリーニング装置17を設ける。
また、3つのなかで第1の支持ローラ14と第2の支持ローラ15間に張り渡した中間転写体10上には、その搬送方向に沿って、イエロー,シアン,マゼンタ,ブラックの4つの画像形成手段18を横に並べて配置してタンデム画像形成装置20を構成する。
Hereinafter, embodiments of the present invention will be described with reference to the drawings.
FIG. 5 shows an embodiment of the present invention, which is a tandem indirect transfer type electrophotographic apparatus. In the figure, reference numeral 100 is a copying apparatus main body, 200 is a paper feed table on which the copying apparatus is placed, 300 is a scanner mounted on the copying apparatus main body 100, and 400 is an automatic document feeder (ADF) mounted thereon. The copying machine main body 100 is provided with an endless belt-shaped intermediate transfer member 10 at the center.
Then, as shown in FIG. 5, in the illustrated example, it is wound around three support rollers 14, 15, and 16 so that it can be rotated and conveyed clockwise in the figure.
In this illustrated example, an intermediate transfer body cleaning device 17 for removing residual toner remaining on the intermediate transfer body 10 after image transfer is provided on the left of the second support roller 15 among the three.
Among the three images, four images of yellow, cyan, magenta, and black are arranged on the intermediate transfer member 10 stretched between the first support roller 14 and the second support roller 15 along the conveyance direction. The tandem image forming apparatus 20 is configured by arranging the forming units 18 side by side.

そのタンデム画像形成装置20の上には、図5に示すように、さらに露光装置21を設ける。一方、中間転写体10を挟んでタンデム画像形成装置20と反対の側には、2次転写装置22を備える。2次転写装置22は、図示例では、2つのローラ23間に、無端ベルトである2次転写ベルト24を掛け渡して構成し、中間転写体10を介して第3の支持ローラ16に押し当てて配置し、中間転写体10上の画像をシートに転写する。
2次転写装置22の横には、シート上の転写画像を定着する定着装置25を設ける。定着装置25は、無端ベルトである定着ベルト26に加圧ローラ27を押し当てて構成する。
上述した2次転写装置22には、画像転写後のシートをこの定着装置25へと搬送するシート搬送機能も備えてなる。もちろん、2次転写装置22として、転写ローラや非接触のチャージャを配置してもよく、そのような場合は、このシート搬送機能を併せて備えることは難しくなる。
なお、図示例では、このような2次転写装置22および定着装置25の下に、上述したタンデム画像形成装置20と平行に、シートの両面に画像を記録すべくシートを反転するシート反転装置28を備える。
An exposure device 21 is further provided on the tandem image forming apparatus 20 as shown in FIG. On the other hand, a secondary transfer device 22 is provided on the side opposite to the tandem image forming apparatus 20 with the intermediate transfer body 10 interposed therebetween. In the illustrated example, the secondary transfer device 22 is configured by spanning a secondary transfer belt 24, which is an endless belt, between two rollers 23, and is pressed against the third support roller 16 via the intermediate transfer body 10. The image on the intermediate transfer body 10 is transferred to a sheet.
A fixing device 25 for fixing the transfer image on the sheet is provided beside the secondary transfer device 22. The fixing device 25 is configured by pressing a pressure roller 27 against a fixing belt 26 that is an endless belt.
The secondary transfer device 22 described above is also provided with a sheet transport function for transporting the image-transferred sheet to the fixing device 25. Of course, a transfer roller or a non-contact charger may be arranged as the secondary transfer device 22, and in such a case, it is difficult to provide this sheet conveying function together.
In the illustrated example, under such a secondary transfer device 22 and a fixing device 25, a sheet reversing device 28 for reversing the sheet so as to record images on both sides of the sheet in parallel with the tandem image forming device 20 described above. Is provided.

さて、いまこのカラー電子写真装置を用いてコピーをとるときは、原稿自動搬送装置400の原稿台30上に原稿をセットする。または、原稿自動搬送装置400を開いてスキャナ300のコンタクトガラス32上に原稿をセットし、原稿自動搬送装置400を閉じてそれで押さえる。
そして、不図示のスタートスイッチを押すと、原稿自動搬送装置400に原稿をセットしたときは、原稿を搬送してコンタクトガラス32上へと移動して後、他方コンタクトガラス32上に原稿をセットしたときは、直ちにスキャナ300を駆動し、第1走行体33および第2走行体34を走行する。そして、第1走行体33で光源から光を発射するとともに原稿面からの反射光をさらに反射して第2走行体34に向け、第2走行体34のミラーで反射して結像レンズ35を通して読取りセンサ36に入れ、原稿内容を読み取る。
Now, when making a copy using this color electrophotographic apparatus, a document is set on the document table 30 of the automatic document feeder 400. Alternatively, the automatic document feeder 400 is opened, a document is set on the contact glass 32 of the scanner 300, and the automatic document feeder 400 is closed and pressed by it.
When a start switch (not shown) is pressed, when the document is set on the automatic document feeder 400, the document is transported and moved onto the contact glass 32, and then the document is set on the other contact glass 32. At that time, the scanner 300 is immediately driven to travel the first traveling body 33 and the second traveling body 34. Then, the first traveling body 33 emits light from the light source and further reflects the reflected light from the document surface toward the second traveling body 34, and is reflected by the mirror of the second traveling body 34 and passes through the imaging lens 35. The document is placed in the reading sensor 36 and the original content is read.

また、不図示のスタートスイッチを押すと、不図示の駆動モータで支持ローラ14・15・16の1つを回転駆動して他の2つの支持ローラを従動回転し、中間転写体10を回転搬送する。同時に、個々の画像形成手段18でその感光体40を回転して各感光体40上にそれぞれ、ブラック・イエロー・マゼンタ・シアンの単色画像を形成する。そして、中間転写体10の搬送とともに、それらの単色画像を順次転写して中間転写体10上に合成カラー画像を形成する。
一方、不図示のスタートスイッチを押すと、給紙テーブル200の給紙ローラ42の1つを選択回転し、ペーパーバンク43に多段に備える給紙カセット44の1つからシートを繰り出し、分離ローラ45で1枚ずつ分離して給紙路46に入れ、搬送ローラ47で搬送して複写機本体100内の給紙路48に導き、レジストローラ49に突き当てて止める。
または、給紙ローラ50を回転して手差しトレイ51上のシートを繰り出し、分離ローラ52で1枚ずつ分離して手差し給紙路53に入れ、同じくレジストローラ49に突き当てて止める。
そして、中間転写体10上の合成カラー画像にタイミングを合わせてレジストローラ49を回転し、中間転写体10と2次転写装置22との間にシートを送り込み、2次転写装置22で転写してシート上にカラー画像を記録する。
When a start switch (not shown) is pressed, one of the support rollers 14, 15, and 16 is driven to rotate by a drive motor (not shown), and the other two support rollers are driven to rotate to convey the intermediate transfer member 10. To do. At the same time, the individual image forming means 18 rotates the photoconductor 40 to form black, yellow, magenta, and cyan monochrome images on each photoconductor 40. Then, along with the conveyance of the intermediate transfer member 10, the single color images are sequentially transferred to form a composite color image on the intermediate transfer member 10.
On the other hand, when a start switch (not shown) is pressed, one of the paper feed rollers 42 of the paper feed table 200 is selectively rotated, and the sheet is fed out from one of the paper feed cassettes 44 provided in multiple stages in the paper bank 43, and the separation roller 45. Then, the sheets are separated one by one into the paper feed path 46, transported by the transport roller 47, guided to the paper feed path 48 in the copying machine main body 100, and abutted against the registration roller 49 and stopped.
Alternatively, the sheet feed roller 50 is rotated to feed out the sheets on the manual feed tray 51, separated one by one by the separation roller 52, put into the manual feed path 53, and abutted against the registration roller 49 and stopped.
Then, the registration roller 49 is rotated in synchronization with the composite color image on the intermediate transfer member 10, the sheet is fed between the intermediate transfer member 10 and the secondary transfer device 22, and transferred by the secondary transfer device 22. A color image is recorded on the sheet.

画像転写後のシートは、2次転写装置22で搬送して定着装置25へと送り込み、定着装置25で熱と圧力とを加えて転写画像を定着して後、切換爪55で切り換えて排出ローラ56で排出し、排紙トレイ57上にスタックする。または、切換爪55で切り換えてシート反転装置28に入れ、そこで反転して再び転写位置へと導き、裏面にも画像を記録して後、排出ローラ56で排紙トレイ57上に排出する。
一方、画像転写後の中間転写体10は、中間転写体クリーニング装置17で、画像転写後に中間転写体10上に残留する残留トナーを除去し、タンデム画像形成装置20による再度の画像形成に備える。
ここで、レジストローラ49は一般的には接地されて使用されることが多いが,シートの紙粉除去のためにバイアスを印加することも可能である。
The sheet after the image transfer is conveyed by the secondary transfer device 22 and sent to the fixing device 25, and heat and pressure are applied to the fixing device 25 to fix the transferred image. The paper is discharged at 56 and stacked on the paper discharge tray 57. Alternatively, it is switched by the switching claw 55 and put into the sheet reversing device 28, where it is reversed and guided again to the transfer position, and an image is recorded also on the back surface, and then discharged onto the discharge tray 57 by the discharge roller 56.
On the other hand, the intermediate transfer body 10 after the image transfer is removed by the intermediate transfer body cleaning device 17 to remove residual toner remaining on the intermediate transfer body 10 after the image transfer, so that the tandem image forming apparatus 20 can prepare for another image formation.
Here, the registration roller 49 is generally used while being grounded, but it is also possible to apply a bias for removing paper dust from the sheet.

さて、上述したタンデム画像形成装置20において、個々の画像形成手段18は、詳しくは、例えば図6に示すように、ドラム状の感光体40のまわりに、帯電装置60、現像装置61、1次転写装置62、感光体クリーニング装置63、除電装置64などを備えてなる。   Now, in the tandem image forming apparatus 20 described above, the individual image forming means 18 includes, for example, a charging device 60, a developing device 61, and a primary device around a drum-shaped photoconductor 40 as shown in FIG. The image forming apparatus includes a transfer device 62, a photoconductor cleaning device 63, a charge removal device 64, and the like.

以下実施例により本発明を更に説明するが、本発明はこれに限定されるものではない。
以下、部は重量部を示す。
EXAMPLES The present invention will be further described below with reference to examples, but the present invention is not limited thereto.
Hereinafter, a part shows a weight part.

(評価機)
評価機として、imagio MP C6000の現像部と定着部を改造して用いた。改造した内容は、線速が1700mm/secになるように、現像ギャップは1.26mm、ドクタブレードギャップは1.6mm、反射型フォトセンサ機能をOFFとした状態で使用した。また定着部の定着ユニットは、定着面圧39N/cmとし、定着ニップ幅10mmとした。定着媒体表面はテトラフルオロエチレン−パーフルオロアルキルビニルエーテル共重合体樹脂(PFA)を塗布、成形、表面調整して使用した。像担持体、現像装置及び転写装置部の実温度領域は30〜40℃になるように制御した。定着ローラの加熱温度は130℃に設定した。
(Evaluation machine)
The developing unit and fixing unit of imagio MP C6000 were modified and used as an evaluation machine. The modified contents were used in a state where the development gap was 1.26 mm, the doctor blade gap was 1.6 mm, and the reflective photosensor function was turned off so that the linear velocity was 1700 mm / sec. The fixing unit of the fixing unit had a fixing surface pressure of 39 N / cm 2 and a fixing nip width of 10 mm. The fixing medium surface was coated with tetrafluoroethylene-perfluoroalkyl vinyl ether copolymer resin (PFA), molded, and surface-adjusted. The actual temperature regions of the image carrier, the developing device, and the transfer device unit were controlled to be 30 to 40 ° C. The heating temperature of the fixing roller was set to 130 ° C.

(2成分現像剤評価)
2成分系現像剤で画像評価する場合は、以下のように、シリコーン樹脂により0.5μmの平均厚さでコーティングされた平均粒径35μmのフェライトキャリアを用い、キャリア100重量部に対し各色トナー7重量部を容器が転動して攪拌される型式のターブラーミキサーを用いて均一混合し帯電させて、現像剤を作製した。
(Evaluation of two-component developer)
When evaluating an image with a two-component developer, a ferrite carrier having an average particle diameter of 35 μm coated with a silicone resin at an average thickness of 0.5 μm is used as follows, and toner 7 of each color is used with respect to 100 parts by weight of the carrier. A developer was prepared by uniformly mixing and charging parts by weight using a tumbler mixer of a type in which the container was rolled and stirred.

(キャリアの製造)
・芯材
Mnフェライト粒子(重量平均径:35μm) 5000部
・コート材
トルエン 50部
シリコーン樹脂SR2400(東レ・ダウコーニング・シリコーン製、不揮発分50%)
450部
アミノシランSH6020(東レ・ダウコーニング・シリコーン製) 10部
カーボンブラック 10部
上記コート材を10分間スターラーで分散してコート液を調製し、このコート液と芯材を流動床内に回転式底板ディスクと攪拌羽根を設けた旋回流を形成させながらコートを行うコーティング装置に投入して、当該コート液を芯材上に塗布した。得られた塗布物を電気炉で250℃、2時間焼成し上記キャリアを得た。
(Carrier production)
・ Core material Mn ferrite particles (weight average diameter: 35 μm) 5000 parts ・ Coating material Toluene 50 parts Silicone resin SR2400 (made by Toray Dow Corning Silicone, nonvolatile content 50%)
450 parts Aminosilane SH6020 (manufactured by Toray Dow Corning Silicone) 10 parts Carbon black 10 parts The above coating material is dispersed with a stirrer for 10 minutes to prepare a coating liquid, and the coating liquid and the core material are rotated in the fluidized bed. The coating liquid was applied to the core material by applying the coating liquid while forming a swirling flow provided with a disk and stirring blades. The obtained coated material was baked in an electric furnace at 250 ° C. for 2 hours to obtain the carrier.

(樹脂微粒子の合成)
冷却管、撹拌器、ガス導入管及び温度計を取り付けた反応容器にイオン交換水及びモノマーを仕込む。その処方例は表1の[樹脂微粒子分散液1、2、3]として記す。液は撹拌しながら加熱し、規定の反応温度まで昇温し反応する時間は全て8時間とし、ビニル系樹脂の水性分散液[樹脂微粒子分散液1、2、3]を得た。
[樹脂微粒子分散液1、2、3]を堀場製作所製レーザ回折/散乱式粒度分布測定装置(LA−920)で測定した体積平均粒径は、それぞれ360nm、270nm、190nmであった。[樹脂微粒子分散液1、2、3]の一部を乾燥して樹脂分を単離し、[樹脂微粒子1、2、3]を得た。該樹脂微粒子のTgはそれぞれ68℃、66℃、62℃であり、ピーク平均分子量はそれぞれ、13000、11000、8000であった。
(Synthesis of resin fine particles)
Charge ion exchange water and monomer into a reaction vessel equipped with a cooling tube, a stirrer, a gas introduction tube and a thermometer. The formulation example is described as [resin fine particle dispersion 1, 2, 3] in Table 1. The liquid was heated with stirring, the temperature was raised to the specified reaction temperature, and the reaction time was all 8 hours, and vinyl resin aqueous dispersions [resin fine particle dispersions 1, 2, 3] were obtained.
The volume average particle diameters of the [resin fine particle dispersions 1, 2, 3] measured by a laser diffraction / scattering particle size distribution analyzer (LA-920) manufactured by HORIBA, Ltd. were 360 nm, 270 nm, and 190 nm, respectively. A part of [resin fine particle dispersions 1, 2, 3] was dried to isolate the resin component to obtain [resin fine particles 1, 2, 3]. The Tg of the resin fine particles was 68 ° C., 66 ° C. and 62 ° C., respectively, and the peak average molecular weights were 13000, 11000 and 8000, respectively.

[実施例1]
〜水相の調製〜
水500部、[樹脂微粒子分散液1]83部、ドデシルジフェニルエーテルジスルホン酸ナトリウムの48.3%水溶液(エレミノールMON−7):三洋化成工業製)23部、酢酸エチル50部を混合撹拌し、乳白色の液体を得た。これを[水相1]とする。
[Example 1]
~ Preparation of aqueous phase ~
500 parts of water, 83 parts of [resin fine particle dispersion 1], 23 parts of a 48.3% aqueous solution of sodium dodecyldiphenyl ether disulfonate (Eleminol MON-7) manufactured by Sanyo Chemical Industries, Ltd., and 50 parts of ethyl acetate were mixed and stirred to give a milky white color Obtained liquid. This is designated as [Aqueous Phase 1].

〜非結晶性ポリエステル樹脂の合成〜
冷却管、撹拌機および窒素導入管の付いた反応容器中に、ビスフェノールAエチレンオキサイド2モル付加物229部、ビスフェノールAプロピレンオキサイド3モル付加物329部、テレフタル酸208部、アジピン酸80部およびジブチルチンオキサイド2部を入れ、常圧で230℃で7時間反応し、さらに10〜15mmHgの減圧で5時間反応した後、反応容器に無水トリメリット酸35部を入れ、180℃、常圧で2時間反応し、[非結晶性ポリエステル樹脂1]を得た。[非結晶性ポリエステル樹脂1]は、数平均分子量2000、重量平均分子量3800,Tg40℃、酸価25mgKOH/gであった。
~ Synthesis of non-crystalline polyester resin ~
In a reaction vessel equipped with a condenser, a stirrer and a nitrogen inlet tube, 229 parts of bisphenol A ethylene oxide 2-mole adduct, 329 parts of bisphenol A propylene oxide 3-mole adduct, 208 parts terephthalic acid, 80 parts adipic acid and dibutyl 2 parts of tin oxide was added, reacted at 230 ° C. for 7 hours at normal pressure, and further reacted for 5 hours at a reduced pressure of 10-15 mmHg. Then, 35 parts of trimellitic anhydride was added to the reaction vessel, and 2 parts at 180 ° C. under normal pressure. By reacting for a time, [amorphous polyester resin 1] was obtained. [Amorphous polyester resin 1] had a number average molecular weight of 2000, a weight average molecular weight of 3800, Tg of 40 ° C., and an acid value of 25 mgKOH / g.

〜非結晶性中間体ポリエステルの合成〜
冷却管、撹拌機および窒索導入管の付いた反応容器中に、ビスフェノールAエチレンオキサイド2モル付加物682部、ビスフェノールAプロピレンオキサイド2モル付加物81部、テレフタル酸283部、無水トリメリット酸22部およびジブチルチンオキサイド2部を入れ、常圧で230℃で7時間反応し、さらに10〜15mmHgの減圧で5時間反応して[非結晶性中間体ポリエステル1]を得た。[非結晶性中間体ポリエステル1]は、数平均分子量2200、重量平均分子量9700、Tg54℃、酸価0.5mgKOH/g、水酸基価52mgKOH/gであった。
次に、冷却管、撹拌機および窒素導入管の付いた反応容器中に、[非結晶性中間体ポリエステル1]410部、イソホロンジイソシアネート89部、酢酸エチル500部を入れ100℃で5時間反応し、[プレポリマー1]を得た。[プレポリマー1]の遊離イソシアネート重量%は、1.53%であった。
~ Synthesis of non-crystalline intermediate polyester ~
In a reaction vessel equipped with a cooling pipe, a stirrer and a nitrogen introduction pipe, 682 parts of bisphenol A ethylene oxide 2-mole adduct, 81 parts of bisphenol A propylene oxide 2-mole adduct, 283 parts of terephthalic acid, trimellitic anhydride 22 And 2 parts of dibutyltin oxide were added, reacted at 230 ° C. at normal pressure for 7 hours, and further reacted at reduced pressure of 10 to 15 mmHg for 5 hours to obtain [Amorphous Intermediate Polyester 1]. [Amorphous Intermediate Polyester 1] had a number average molecular weight of 2200, a weight average molecular weight of 9700, Tg of 54 ° C., an acid value of 0.5 mgKOH / g, and a hydroxyl value of 52 mgKOH / g.
Next, 410 parts of [Amorphous Intermediate Polyester 1], 89 parts of isophorone diisocyanate, and 500 parts of ethyl acetate are placed in a reaction vessel equipped with a cooling pipe, a stirrer, and a nitrogen introduction pipe, and reacted at 100 ° C. for 5 hours. [Prepolymer 1] was obtained. [Prepolymer 1] had a free isocyanate weight% of 1.53%.

〜ケチミンの合成〜
撹拌棒および温度計をセットした反応容器に、イソホロンジアミン170部とメチルエチルケトン75部を仕込み、50℃で4時間半反応を行い、[ケチミン化合物1]を得た。[ケチミン化合物1]のアミン価は417であった。
~ Synthesis of ketimine ~
In a reaction vessel equipped with a stirrer and a thermometer, 170 parts of isophoronediamine and 75 parts of methyl ethyl ketone were charged and reacted at 50 ° C. for 4 and a half hours to obtain [ketimine compound 1]. The amine value of [ketimine compound 1] was 417.

〜結晶性ポリエステル樹脂の合成
冷却管、撹拌機および窒素導入管の付いた反応容器中に、1,6−ヘキサンジオール1200部と、デカン2酸1200部と、触媒としてジブチル錫オキサイド0.4部と、を入れた後、減圧操作により容器内の空気を窒素ガスで不活性雰囲気とし、機械攪拌にて180rpmで5時間攪拌を行った。その後、減圧下にて220℃まで徐々に昇温を行い2時間攪拌し、粘稠な状態となったところで空冷し、反応を停止させ、[結晶性ポリエステル樹脂1]を得た。[結晶性ポリエステル樹脂1]は、数平均分子量3700、重量平均分子量16000、融点69℃であった。
~ Synthesis of crystalline polyester resin In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen introduction tube, 1200 parts of 1,6-hexanediol, 1200 parts of decanedioic acid, and 0.4 parts of dibutyltin oxide as a catalyst Then, the air in the container was made an inert atmosphere with nitrogen gas by depressurization, and the mixture was stirred at 180 rpm with mechanical stirring for 5 hours. Thereafter, the temperature was gradually raised to 220 ° C. under reduced pressure, and the mixture was stirred for 2 hours. When it became viscous, it was air-cooled to stop the reaction, thereby obtaining [Crystalline Polyester Resin 1]. [Crystalline polyester resin 1] had a number average molecular weight of 3700, a weight average molecular weight of 16000, and a melting point of 69 ° C.

〜マスターバッチ(MB)の合成〜
水1200部、カーボンブラック(Printex35 デクサ製)540部〔DBP吸油量=42ml/100mg、pH=9.5〕、ポリエステル樹脂1200部を加え、ヘンシェルミキサー(三井鉱山社製)で混合し、混合物を2本ロールを用いて110℃で1時間混練後、圧延冷却しパルペライザーで粉砕、[マスターバッチ1]を得た。
~ Synthesis of master batch (MB) ~
1200 parts of water, 540 parts of carbon black (made by Printex 35 Dexa) [DBP oil absorption = 42 ml / 100 mg, pH = 9.5] and 1200 parts of polyester resin are added and mixed with a Henschel mixer (made by Mitsui Mining Co., Ltd.). After kneading at 110 ° C. for 1 hour using two rolls, the product was rolled and cooled, and pulverized with a pulverizer to obtain [Masterbatch 1].

〜油相の作成〜
撹拌棒および温度計をセットした容器に、[非結晶性ポリエステル樹脂1]378部、パラフィンWAX(融点90℃)120部、[結晶性ポリエステル樹脂1]200部、酢酸エチル947部を仕込み、撹拌下80℃に昇温し、80℃のまま5時間保持した後、1時問で30℃に冷却した。次いで容器に[マスターバッチ1]500部、酢酸エチル500部を仕込み、1時間混合し[原料溶解液1]を得た。
[原料溶解液1]1324部を容器に移し、ビーズミル(ウルトラビスコミル、アイメックス社製)を用いて、送液速度1kg/hr、ディスク周速度6m/秒、0.5mmジルコニアビーズを80体積%充填、3パスの条件で、カーボンブラック、WAXの分散を行った。次いで、[非結晶性ポリエステル樹脂1]の65%酢酸エチル溶液1324部加え、上記条件のビーズミルで2パスし、[顔料・WAX分散液1]を得た。[顔料・WAX分散液1]の固形分濃度(130℃、30分)は50%であった。
~ Creation of oil phase ~
378 parts of [Non-crystalline polyester resin 1], 120 parts of paraffin WAX (melting point 90 ° C.), 200 parts of [crystalline polyester resin 1] and 947 parts of ethyl acetate are charged in a container equipped with a stir bar and a thermometer. The temperature was raised to 80 ° C., kept at 80 ° C. for 5 hours, and then cooled to 30 ° C. over 1 hour. Next, 500 parts of [Masterbatch 1] and 500 parts of ethyl acetate were charged in a container and mixed for 1 hour to obtain [Raw material solution 1].
[Raw material solution 1] 1324 parts are transferred to a container, and using a bead mill (Ultra Visco Mill, manufactured by Imex Co., Ltd.), a liquid feeding speed of 1 kg / hr, a disk peripheral speed of 6 m / sec, and 0.5 mm zirconia beads are 80% by volume. Carbon black and WAX were dispersed under conditions of filling and 3 passes. Next, 1324 parts of a 65% ethyl acetate solution of [Amorphous Polyester Resin 1] was added, followed by two passes with a bead mill under the above conditions to obtain [Pigment / WAX Dispersion 1]. The solid content concentration of [Pigment / WAX Dispersion 1] (130 ° C., 30 minutes) was 50%.

〜乳化⇒脱溶剤〜
[顔料・WAX分散液1]749部、[プレポリマー1]を115部、[ケチミン化合物1]2.9部を容器に入れ、TKホモミキサー(特殊機化製)で5,000rpmで2分間混合した後、容器に[水相1]1200部を加え、TKホモミキサーで、回転数13,000rpmで25分間混合し[乳化スラリー1]を得た。
撹拌機および温度計をセットした容器に、[乳化スラリー1]を投入し、30℃で8時間脱溶剤した後、40℃で24時間熟成を行い、[分散スラリー1]を得た。
~ Emulsification⇒Desolvation ~
[Pigment / WAX Dispersion 1] 749 parts, [Prepolymer 1] 115 parts, [Ketimine Compound 1] 2.9 parts in a container and TK homomixer (manufactured by Tokushu Kika) at 5,000 rpm for 2 minutes After mixing, 1200 parts of [Aqueous phase 1] was added to the container, and mixed with a TK homomixer at 13,000 rpm for 25 minutes to obtain [Emulsion slurry 1].
[Emulsion slurry 1] was charged into a container equipped with a stirrer and a thermometer, and after removing the solvent at 30 ° C. for 8 hours, aging was carried out at 40 ° C. for 24 hours to obtain [Dispersion slurry 1].

〜洗浄⇒乾燥〜
[分散スラリー1]100部を減圧濾過した後、
(1):濾過ケーキにイオン交換水100部を加え、TKホモミキサーで混合(回転数12,000rpmで10分間)した後濾過した。
(2):(1)の濾過ケーキに10%水酸化ナトリウム水溶液100部を加え、TKホモミキサーで混合(回転数12,000rpmで30分間)した後、減圧濾過した。
(3):(2)の濾過ケーキに10%塩酸100部を加え、TKホモミキサーで混合(回転数12,000rpmで10分間)した後濾過した。
(4):(3)の濾過ケーキにイオン交換水300部を加え、TKホモミキサーで混合(回転数12,000rpmで10分間)した後濾過する操作を2回行い[濾過ケーキ1]を得た。
[濾過ケーキ1]を循風乾燥機にて45℃で48時間乾燥した。その後目開き75μmメッシュで篩い[トナー母体粒子1]を得た。
その後、[トナー母体粒子1]100部、粒径13nmの疎水化処理シリカ1部をヘンシェルミキサーにて混合してトナーを得た。得られたトナーの物性は表2、評価結果は表3に示した。
~ Washing⇒Drying ~
[Dispersion Slurry 1] After filtering 100 parts under reduced pressure,
(1): 100 parts of ion-exchanged water was added to the filter cake, mixed with a TK homomixer (rotation speed: 12,000 rpm for 10 minutes), and then filtered.
(2): 100 parts of 10% aqueous sodium hydroxide solution was added to the filter cake of (1), mixed with a TK homomixer (30 minutes at 12,000 rpm), and then filtered under reduced pressure.
(3): 100 parts of 10% hydrochloric acid was added to the filter cake of (2), mixed with a TK homomixer (rotation speed: 12,000 rpm for 10 minutes), and then filtered.
(4): 300 parts of ion-exchanged water was added to the filter cake of (3), mixed with a TK homomixer (10 minutes at 12,000 rpm), and then filtered twice to obtain [filter cake 1]. It was.
[Filter cake 1] was dried at 45 ° C. for 48 hours in a circulating dryer. Thereafter, sieved with a mesh of 75 μm, [Toner Base Particle 1] was obtained.
Thereafter, 100 parts of [toner base particle 1] and 1 part of hydrophobized silica having a particle diameter of 13 nm were mixed with a Henschel mixer to obtain a toner. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.

[実施例2]
実施例1において、用いた[樹脂微粒子分散液1]を[樹脂微粒子分散液2]に変更した以外は実施例1と同様にしてトナーを得た。得られたトナーの物性は表2、評価結果は表3に示した。
[実施例3]
実施例1において、用いた[樹脂微粒子分散液1]を[樹脂微粒子分散液3]に変更した以外は実施例1と同様にしてトナーを得た。得られたトナーの物性は表2、評価結果は表3に示した。
[Example 2]
A toner was obtained in the same manner as in Example 1 except that [resin fine particle dispersion 1] used in Example 1 was changed to [resin fine particle dispersion 2]. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.
[Example 3]
A toner was obtained in the same manner as in Example 1 except that [resin fine particle dispersion 1] used in Example 1 was changed to [resin fine particle dispersion 3]. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.

[実施例4]
実施例1において、用いた[樹脂微粒子分散液1]を以下の[樹脂微粒子分散液4]に変更した以外は実施例1と同様にしてトナーを得た。得られたトナーの物性は表2、評価結果は表3に示した。
〜樹脂微粒子分散液4の調製〜
冷却管、撹拌機及び窒素導入管の付いた反応槽中に、ビスフェノールAのエチレンオキサイド2モル付加物350部、ビスフェノールAのプロピオンオキサイド3モル付加物326部、テレフタル酸278部、無水フタル酸40部及び縮合触媒としてチタニウムジヒドロキシビス(トリエタノールアミネート)2部を入れ、230℃で窒素気流下に生成する水を留去しながら10時間反応させた。次いで5〜20mmHgの減圧下に反応させ、酸価が2mgKOH/g以下になった時点で180℃に冷却し、無水トリメリット酸62部を加え、常圧密閉下2時間反応後取り出し、室温まで冷却後、粉砕して[非結晶性ポリエステル樹脂2]を得た。
得られた[非結晶性ポリエステル樹脂2]は、その酸価は35mgKOH/g、水酸基価は17mgKOH/g、Tgは69℃、Mnは3980、Mwは24400であった。
[Example 4]
A toner was obtained in the same manner as in Example 1 except that [resin fine particle dispersion 1] used in Example 1 was changed to the following [resin fine particle dispersion 4]. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.
-Preparation of resin fine particle dispersion 4-
In a reaction vessel equipped with a cooling tube, a stirrer and a nitrogen introduction tube, 350 parts of an ethylene oxide 2-mole adduct of bisphenol A, 326 parts of a propion oxide 3-mole adduct of bisphenol A, 278 parts of terephthalic acid, 40 of phthalic anhydride 2 parts of titanium dihydroxybis (triethanolamate) as a condensation catalyst was added, and the reaction was carried out for 10 hours while distilling off the water produced at 230 ° C. under a nitrogen stream. Next, the reaction is carried out under reduced pressure of 5 to 20 mmHg. When the acid value becomes 2 mgKOH / g or less, it is cooled to 180 ° C., 62 parts of trimellitic anhydride is added, taken out after reaction for 2 hours under normal pressure sealing, and taken to room temperature. After cooling, it was pulverized to obtain [Amorphous Polyester Resin 2].
The obtained [Non-crystalline polyester resin 2] had an acid value of 35 mgKOH / g, a hydroxyl value of 17 mgKOH / g, Tg of 69 ° C., Mn of 3980, and Mw of 24400.

前述の[非結晶性ポリエステル樹脂2]をハンマーミルで粗粉砕し、樹脂粒子分散液を調製した。
攪拌動力を与えるアンカー翼、還流装置、および真空ポンプによる減圧装置の備えられた2Lセパラブルフラスコに酢酸エチル50重量部、IPA 110重量部を添加、N2を0.2L/mの速度で送気し、系内の空気をN2で置換した。次いで、系内オイルバス装置により60℃に過熱しながら結晶性ポリエステル樹脂1を200重量部ゆっくりと添加し攪拌しながら溶解させた。ついで、これに5%アンモニア水20重量部を添加したのち、定量ポンプを用い、攪拌しながらこれにイオン交換水460重量部を4.0g/mの速度で投入した。乳化系内が乳白色を呈し、且つ攪拌粘度が低下した時点を乳化終了とした。
ついで、これに−700Torrまで減圧し、攪拌しながら40分攪拌した。更にこれに60℃の純水50重量部を添加し、20分減圧下攪拌を継続した。還流量が210重量部に達した際、これを終点とし、過熱をやめ攪拌しながら常温まで冷却した。得られた樹脂粒子の粒度をレーザー回折/散乱式粒度分布測定装置(堀場製作所社製、LA−920)を用いて行った。得られた樹脂微粒子の平均粒度は、344nmであった。
[Non-crystalline polyester resin 2] was coarsely pulverized with a hammer mill to prepare a resin particle dispersion.
50 parts by weight of ethyl acetate and 110 parts by weight of IPA were added to a 2 L separable flask equipped with an anchor blade for supplying stirring power, a reflux device, and a decompression device using a vacuum pump, and N 2 was fed at a rate of 0.2 L / m. The air in the system was replaced with N 2 . Next, 200 parts by weight of the crystalline polyester resin 1 was slowly added while being heated to 60 ° C. by an in-system oil bath device, and dissolved while stirring. Next, 20 parts by weight of 5% ammonia water was added thereto, and then 460 parts by weight of ion-exchanged water was added thereto at a rate of 4.0 g / m with stirring using a metering pump. Emulsification was completed when the emulsification system was milky white and the stirring viscosity was reduced.
Next, the pressure was reduced to -700 Torr, and the mixture was stirred for 40 minutes while stirring. Further, 50 parts by weight of pure water at 60 ° C. was added thereto, and stirring was continued for 20 minutes under reduced pressure. When the reflux amount reached 210 parts by weight, this was taken as the end point, and overheating was stopped and the mixture was cooled to room temperature while stirring. The particle size of the obtained resin particles was measured using a laser diffraction / scattering particle size distribution analyzer (LA-920, manufactured by Horiba, Ltd.). The average particle size of the obtained resin fine particles was 344 nm.

[実施例5]
実施例2において、[プレポリマー1]とケチミン化合物を含有させずに、他は実施例2と同様にしてトナーを得た。トナーには変性ポリエステルを含まず、伸長、あるいは架橋が形成されていないトナーとなった。得られたトナーの物性は表2、評価結果は表3に示した。
[Example 5]
In Example 2, a toner was obtained in the same manner as in Example 2 except that [Prepolymer 1] and the ketimine compound were not contained. The toner contained no modified polyester, and no toner was stretched or crosslinked. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.

[比較例1]
実施例1において、用いた[樹脂微粒子分散液1]を以下の[樹脂微粒子分散液5]に変更した以外は実施例1と同様にしてトナーを得た。得られたトナーの物性は表2、評価結果は表3に示した。
〜樹脂微粒子分散液5の調製〜
撹拌棒および温度計をセットした反応容器に、水683部、メタクリル酸エチレンオキサイド付加物硫酸エステルのナトリウム塩(エレミノールRS−30、三洋化成工業製)10部、メタクリル酸170部、アクリル酸ブチル100部、過硫酸アンモニウム1部を仕込み、3800回転/分で30分間撹拌したところ、白色の乳濁液が得られた。加熱して、系内温度75℃まで昇温し3時間反応させた。さらに、1%過硫酸アンモニウム水溶液30部加え、70℃で5時間熟成してビニル系樹脂(メタクリル酸−アクリル酸ブチル−メタクリル酸エチレンオキサイド付加物硫酸エステルのナトリウム塩の共重合体)の水性分散液[樹脂微粒子分散液5]を得た。[樹脂微粒子分散液5]をLA−920で測定した体積平均粒径は、60nmであった。[樹脂微粒子分散液5]の一部を乾燥して樹脂分を単離した。該樹脂分のTgは60℃であり、重量平均分子量は11万であった。
得られた樹脂微粒子の粒径が小さく、トナー母体粒子は十分識別可能なコアシェル構造を有さなかった。
[Comparative Example 1]
A toner was obtained in the same manner as in Example 1 except that [resin fine particle dispersion 1] used in Example 1 was changed to the following [resin fine particle dispersion 5]. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.
-Preparation of resin fine particle dispersion 5-
In a reaction vessel equipped with a stir bar and a thermometer, 683 parts of water, 10 parts of sodium salt of ethylene oxide methacrylate adduct sulfate (Eleminol RS-30, manufactured by Sanyo Chemical Industries), 170 parts of methacrylic acid, 100 butyl acrylate Parts and 1 part of ammonium persulfate were added and stirred at 3800 rpm for 30 minutes to obtain a white emulsion. The system was heated to raise the system temperature to 75 ° C. and reacted for 3 hours. Further, 30 parts of a 1% ammonium persulfate aqueous solution was added, and the mixture was aged at 70 ° C. for 5 hours, and an aqueous dispersion of vinyl resin (methacrylic acid-butyl acrylate-methacrylic acid ethylene oxide adduct sulfate sodium salt copolymer). [Resin fine particle dispersion 5] was obtained. The volume average particle diameter of [resin fine particle dispersion 5] measured with LA-920 was 60 nm. A portion of [resin fine particle dispersion 5] was dried to isolate the resin component. The Tg of the resin was 60 ° C., and the weight average molecular weight was 110,000.
The resin fine particles obtained had a small particle size, and the toner base particles did not have a sufficiently distinguishable core-shell structure.

[比較例2]
実施例1において、結晶性ポリエステル樹脂を含有させずに処方した以外は実施例1と同様にしてトナーを得た。得られたトナーの物性は表2、評価結果は表3に示した。
[Comparative Example 2]
A toner was obtained in the same manner as in Example 1 except that it was formulated without containing a crystalline polyester resin. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.

[比較例3]
実施例1において、用いた[樹脂微粒子分散液1]を以下の[樹脂微粒子分散液67]に変更した以外は実施例1と同様にしてトナーを得た。得られたトナーの物性は表2、評価結果は表3に示した。
−樹脂微粒子分散液6の調製−
前述の結晶性ポリエステル樹脂1、非結晶性ポリエステル樹脂1をハンマーミルで粗粉砕し、樹脂粒子分散液を調製した。
攪拌動力を与えるアンカー翼、還流装置、および真空ポンプによる減圧装置の備えられた2Lセパラブルフラスコに酢酸エチル50重量部、IPA 110重量部を添加、N2を0.2L/mの速度で送気し、系内の空気をN2で置換した。次いで、系内オイルバス装置により60℃に過熱しながら結晶性ポリエステル樹脂1を20重量部、非結晶性ポリエステル樹脂1を180重量部ゆっくりと添加し攪拌しながら溶解させた。ついで、これに10%アンモニア水20重量部を添加したのち、定量ポンプを用い、攪拌しながらこれにイオン交換水460重量部を9.6g/mの速度で投入した。乳化系内が乳白色を呈し、且つ攪拌粘度が低下した時点を乳化終了とした。
ついで、これに−700Torrまで減圧し、攪拌しながら40分攪拌した。更にこれに60℃の純水50重量部を添加し、20分減圧下攪拌を継続した。還流量が210重量部に達した際、これを終点とし、過熱をやめ攪拌しながら常温まで冷却した。得られた樹脂粒子の粒度をレーザー回折/散乱式粒度分布測定装置(堀場製作所社製、LA−920)を用いて行った。得られた樹脂微粒子の平均粒度は、260nmであった。
[Comparative Example 3]
A toner was obtained in the same manner as in Example 1 except that [resin fine particle dispersion 1] used in Example 1 was changed to the following [resin fine particle dispersion 67]. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.
-Preparation of resin fine particle dispersion 6-
The above-mentioned crystalline polyester resin 1 and non-crystalline polyester resin 1 were coarsely pulverized with a hammer mill to prepare a resin particle dispersion.
50 parts by weight of ethyl acetate and 110 parts by weight of IPA were added to a 2 L separable flask equipped with an anchor blade for supplying stirring power, a reflux device, and a decompression device using a vacuum pump, and N 2 was fed at a rate of 0.2 L / m. The air in the system was replaced with N 2 . Next, 20 parts by weight of the crystalline polyester resin 1 and 180 parts by weight of the amorphous polyester resin 1 were slowly added while being heated to 60 ° C. by an in-system oil bath apparatus, and dissolved while stirring. Next, 20 parts by weight of 10% ammonia water was added thereto, and then 460 parts by weight of ion-exchanged water was added thereto at a rate of 9.6 g / m while stirring using a metering pump. Emulsification was completed when the emulsification system was milky white and the stirring viscosity was reduced.
Next, the pressure was reduced to -700 Torr, and the mixture was stirred for 40 minutes while stirring. Further, 50 parts by weight of pure water at 60 ° C. was added thereto, and stirring was continued for 20 minutes under reduced pressure. When the reflux amount reached 210 parts by weight, this was taken as the end point, and overheating was stopped and the mixture was cooled to room temperature while stirring. The particle size of the obtained resin particles was measured using a laser diffraction / scattering particle size distribution analyzer (LA-920, manufactured by Horiba, Ltd.). The average particle size of the obtained resin fine particles was 260 nm.

[比較例4]
実施例1において、[プレポリマー1]とケチミン化合物を含有させずに、他は実施例1と同様にしてトナーを得た。トナーは変性ポリエステルを含まず、伸長、あるいは架橋が形成されていないトナーとなった。得られたトナーの物性は表2、評価結果は表3に示した。
[Comparative Example 4]
In Example 1, a toner was obtained in the same manner as in Example 1 except that [Prepolymer 1] and a ketimine compound were not contained. The toner contained no modified polyester and was a toner that was not stretched or crosslinked. The physical properties of the obtained toner are shown in Table 2, and the evaluation results are shown in Table 3.

(評価項目)
1)低温定着性
得られた二成分現像剤と評価機を用いて5%画像面積チャートを10,000枚出力した後、定着ユニットの温度を5℃づつ変化させ、画像出しをし、定着性を測定した。転写紙はリコーフルカラーPPC用紙タイプ6000を用いた。
定着機の定着温度を変え、X−Rite 938による画像濃度が1.2となるようなプリント画像を得た。コールドオフセット未発生の最低温度を定着下限温度として評価した。コールドオフセットとは、トナーが低温で十分溶融せずに用紙でなく定着部材(ベルト、ローラ)に付着して定着部材を汚染して、一周回転して次の用紙に定着部材に付着したオフセットトナーが再付着して、本来画像を形成すべきでない箇所を汚してしまう画像不具合である。
評価結果は以下のように示した。
◎;110〜120℃
○;125〜130℃
△;135〜140℃
×;140℃以上
(Evaluation item)
1) Low-temperature fixability After outputting 10,000 sheets of 5% image area chart using the obtained two-component developer and an evaluator, the temperature of the fixing unit is changed by 5 ° C., and an image is output to fix the image. Was measured. Ricoh full color PPC paper type 6000 was used as the transfer paper.
By changing the fixing temperature of the fixing machine, a print image having an image density of 1.2 by X-Rite 938 was obtained. The lowest temperature at which no cold offset occurred was evaluated as the minimum fixing temperature. Cold offset is an offset toner in which the toner does not melt sufficiently at a low temperature and adheres to the fixing member (belt, roller), not the paper, contaminates the fixing member, rotates once, and adheres to the fixing member on the next paper. Is an image defect that reattaches and stains a portion where an image should not be originally formed.
The evaluation results are shown as follows.
A: 110-120 ° C
○: 125-130 ° C
Δ: 135-140 ° C.
×: 140 ° C or higher

2)耐熱保存性
トナーを10gずつ計量し、20mlのガラス容器に入れ、ガラス瓶をタッピングマ装置にて100回タッピングした後、温度55℃、湿度80%にセットした恒温槽に100時間放置した後、針入度試験器(日科エンジニアリング マニュアル記載条件)にて針入度を測定した。良好なものから、◎:20mm以上、○:15mm以上20mm未満、△:10mm以上〜15mm未満、×:10mm未満、とした。
2) Heat-resistant storage stability Weigh 10 g of toner, put it in a 20 ml glass container, tap the glass bottle 100 times with a tapping machine, and leave it in a thermostatic chamber set at 55 ° C. and 80% humidity for 100 hours. The penetration was measured with a penetration tester (conditions described in the Nikka Engineering Manual). From the good one, ◎: 20 mm or more, ◯: 15 mm or more and less than 20 mm, Δ: 10 mm or more to less than 15 mm, x: less than 10 mm.

3)感光体汚染性
得られた二成分現像剤と評価機を用いて画像面積率20%チャート、BWモード、 100Print/Job(インターバル5分) 5,000枚/Day 計50,000枚出力耐久試験を実施した。評価環境条件は、27℃80%のオフィッス高温、高湿環境にて実施した。転写紙はリコーフルカラーPPC用紙タイプ6200を用いた。
そのときの感光体を取り出し、感光体フィルミング(付着異物)を表面凹凸物として観察した。レーザテック社製の共焦点顕微鏡であるフルカラーコンフォーカル顕微鏡C130を用いて、500μm角領域における表面粗さRaについて次の基準で評価した。
◎ 0.05μm未満
○ 0.05μm以上0.09μm未満
△ 0.09μm以上0.13μm未満
× 0.13μm以上
3) Photoconductor contamination Using the obtained two-component developer and an evaluation machine, an image area ratio 20% chart, BW mode, 100 Print / Job (interval 5 minutes) 5,000 sheets / day, total output of 50,000 sheets The test was conducted. Evaluation environmental conditions were carried out in an office high temperature and high humidity environment of 27 ° C. and 80%. Ricoh full color PPC paper type 6200 was used as the transfer paper.
The photoreceptor at that time was taken out, and the photoreceptor filming (adhered foreign matter) was observed as surface irregularities. Using a full-color confocal microscope C130, which is a confocal microscope manufactured by Lasertec, the surface roughness Ra in a 500 μm square region was evaluated according to the following criteria.
◎ Less than 0.05μm ○ 0.05μm or more and less than 0.09μm △ 0.09μm or more and less than 0.13μm × 0.13μm or more

(図3、図4について)
1 感光体
2 転写装置、1次転写装置
3 シート搬送ベルト
4 中間転写体
5 2次転写装置
6 給紙装置
7 定着装置
8 感光体クリーニング装置
9 中間転写体クリーニング装置
s シート
T タンデム型画像形成装置
(About Fig. 3 and Fig. 4)
DESCRIPTION OF SYMBOLS 1 Photoconductor 2 Transfer apparatus, Primary transfer apparatus 3 Sheet conveyance belt 4 Intermediate transfer body 5 Secondary transfer apparatus 6 Paper feed apparatus 7 Fixing apparatus 8 Photoconductor cleaning apparatus 9 Intermediate transfer body cleaning apparatus s Sheet T Tandem type image forming apparatus

(図5について)
10 中間転写体
14,15,16 支持ローラ
17 中間転写クリーニング装置
18 画像形成手段
20 タンデム画像形成装置
21 露光装置
22 2次転写装置
23 ローラ
24 2次転写ベルト
25 定着装置
26 定着ベルト
27 加圧ローラ
28 シート反転装置
30 原稿台
32 コンタクトガラス
33 第1走行体
34 第2走行体
35 結像レンズ
36 読取りセンサ
40 感光体
42 給紙ローラ
43 ペーパーバンク
44 給紙カセット
45 分離ローラ
46 給紙路
47 搬送ローラ
48 給紙路
49 レジストローラ
50 給紙ローラ
51 手差しトレイ
52 分離ローラ
53 手差し給紙路
55 切換爪
56 排出ローラ
57 排出トレイ
100 複写装置本体
200 給紙テーブル
300 スキャナ
400 原稿自動搬送装置
(図6について)
40 感光体
60 帯電装置
61 現像装置
62 1次転写装置
63 感光体クリーニング装置
64 除電装置
(About Figure 5)
DESCRIPTION OF SYMBOLS 10 Intermediate transfer bodies 14, 15, 16 Support roller 17 Intermediate transfer cleaning device 18 Image forming means 20 Tandem image forming device 21 Exposure device 22 Secondary transfer device 23 Roller 24 Secondary transfer belt 25 Fixing device 26 Fixing belt 27 Pressure roller 28 Sheet reversing device 30 Document base 32 Contact glass 33 First traveling body 34 Second traveling body 35 Imaging lens 36 Reading sensor 40 Photosensitive body 42 Paper feed roller 43 Paper bank 44 Paper feed cassette 45 Separating roller 46 Paper feed path 47 Conveyance Roller 48 Paper feed path 49 Registration roller 50 Paper feed roller 51 Manual feed tray 52 Separation roller 53 Manual feed path 55 Switching claw 56 Ejection roller 57 Ejection tray 100 Copying apparatus main body 200 Paper feed table 300 Scanner 400 Automatic document feeder (FIG. 6) about)
40 Photoconductor 60 Charging device 61 Developing device 62 Primary transfer device 63 Photoconductor cleaning device 64 Static eliminating device

特開2008−276269号JP 2008-276269 A

Claims (15)

少なくとも結着樹脂、着色剤、離型剤を含有するトナーにおいて、該トナーは内部にコアと、該コアの表面にシェルとを有するコアシェル構造を有するトナーであって、前記コア部に少なくとも結晶性ポリエステル樹脂、非結晶性ポリエステル樹脂、着色剤、離型剤を含有してかつ、ヒーター内蔵のSPMプローブにより測定した前記シェル層の軟化温度ST(℃)と、内部コア部分の軟化温度CT(℃)が、以下の関係を示す事を特徴とするトナー。
1.1≦ST/CT≦2.5
In a toner containing at least a binder resin, a colorant, and a release agent, the toner has a core-shell structure having a core inside and a shell on the surface of the core, and at least crystalline in the core part A softening temperature ST (° C.) of the shell layer measured by an SPM probe with a built-in heater and a polyester resin, an amorphous polyester resin, a colorant, a release agent, and a softening temperature CT (° C. of the inner core portion) ) Shows the following relationship:
1.1 ≦ ST / CT ≦ 2.5
前記シェル層の厚さをSLとし、トナー粒子の最大径をTLとしたとき、SLとTLとが以下の関係を示すことを特徴とする請求項1に記載のトナー。
0.01≦SL/TL≦0.20
The toner according to claim 1, wherein SL and TL have the following relationship, where SL is the thickness of the shell layer and TL is the maximum diameter of the toner particles.
0.01 ≦ SL / TL ≦ 0.20
前記非結晶性ポリエステル樹脂が変性ポリエステル樹脂を含む事を特徴とする請求項1又は2に記載のトナー。   The toner according to claim 1, wherein the non-crystalline polyester resin contains a modified polyester resin. 前記トナーが、結晶性ポリエステル樹脂、着色剤、離型剤及び非結晶ポリエステル樹脂となるポリエステルプレポリマーを含むトナー組成物を溶解した有機溶媒の油滴を水系媒体中に分散させ、伸長反応および/または架橋反応により形成された粒子である事を特徴とする請求項1〜3のいずれかに記載のトナー。   In the toner, oil droplets of an organic solvent in which a toner composition containing a polyester prepolymer that becomes a crystalline polyester resin, a colorant, a release agent, and an amorphous polyester resin is dispersed in an aqueous medium, and an extension reaction and / or The toner according to claim 1, wherein the toner is a particle formed by a crosslinking reaction. 前記ポリエステルプレポリマーが活性水素基を有する化合物と反応可能な部位を有する重合体である事を特徴とする請求項4に記載のトナー。   The toner according to claim 4, wherein the polyester prepolymer is a polymer having a site capable of reacting with a compound having an active hydrogen group. 前記トナー組成物が更に非結晶性ポリエステルを含むことを特徴とする請求項4又は5に記載のトナー。   The toner according to claim 4, wherein the toner composition further contains an amorphous polyester. 前記トナーのシェル層が少なくともビニル系樹脂を含有する事を特徴とする請求項1〜6のいずれかに記載のトナー。   The toner according to claim 1, wherein the shell layer of the toner contains at least a vinyl resin. 前記トナーの平均円形度Eが0.93〜0.99である事を特徴とする請求項1〜7のいずれかに記載のトナー。   The toner according to claim 1, wherein an average circularity E of the toner is 0.93 to 0.99. 前記トナーの円形度SF−1値が100〜150、かつ円形度SF−2値が100〜140である事を特徴とする請求項1〜8のいずれかに記載のトナー。   The toner according to claim 1, wherein the toner has a circularity SF-1 value of 100 to 150 and a circularity SF-2 value of 100 to 140. 前記トナー粒子の重量平均粒径D4が2〜7μmであり、重量平均粒径D4と個数平均粒径Dnの比D4/Dnが1.25以下である事を特徴とする請求項1〜9のいずれかに記載のトナー。   The weight average particle diameter D4 of the toner particles is 2 to 7 μm, and the ratio D4 / Dn of the weight average particle diameter D4 to the number average particle diameter Dn is 1.25 or less. The toner according to any one of the above. 少なくとも請求項1〜10のいずれかに記載のトナーとキャリアを含むことを特徴とする二成分現像剤。   A two-component developer comprising at least the toner according to claim 1 and a carrier. 少なくとも請求項1〜10のいずれかに記載のトナーとキャリアを含むことを特徴とする補給用トナー。   A toner for replenishment comprising at least the toner according to claim 1 and a carrier. 請求項1〜10のいずれかに記載のトナーを用いる事を特徴とする画像形成装置。   An image forming apparatus using the toner according to claim 1. 請求項1〜10のいずれか記載のトナーを用いてかつ、記録媒体上の可視像を熱と圧力により定着させる定着装置を備える画像形成装置であって、少なくとも4つ以上の現像色の異なる現像ユニットを直列に配置したタンデム型の現像方式でかつ、システム速度が500〜2500mm/secであり、かつ定着媒体の加圧面圧が、5N/cm2〜90N/cm2であることを特徴とするカラー画像形成装置。 An image forming apparatus comprising the fixing device using the toner according to claim 1 and fixing a visible image on a recording medium by heat and pressure, wherein at least four or more development colors are different. and a tandem type developing system arranged a developing unit in series, the system speed is 500~2500mm / sec, and pressing surface pressure of the fixing medium, and characterized by a 5N / cm 2 ~90N / cm 2 A color image forming apparatus. 潜像担持体と、少なくとも現像手段を一体に支持し、画像形成装置本体に着脱可能であるプロセスカートリッジにおいて、該現像手段はトナーを保持し、該トナーは請求項1〜10のいずれかに記載のトナーであることを特徴とするプロセスカートリッジ。   11. A process cartridge that integrally supports a latent image carrier and at least developing means and is detachable from an image forming apparatus main body, the developing means holds toner, and the toner is defined in any one of claims 1 to 10. A process cartridge characterized by being a toner.
JP2010047847A 2010-03-04 2010-03-04 Toner for developing electrostatic charge image, image forming apparatus, process cartridge, and developer Pending JP2011185973A (en)