JP2003251930A - Sheet for ink jet recording - Google Patents

Sheet for ink jet recording

Info

Publication number
JP2003251930A
JP2003251930A JP2002060810A JP2002060810A JP2003251930A JP 2003251930 A JP2003251930 A JP 2003251930A JP 2002060810 A JP2002060810 A JP 2002060810A JP 2002060810 A JP2002060810 A JP 2002060810A JP 2003251930 A JP2003251930 A JP 2003251930A
Authority
JP
Japan
Prior art keywords
weight
silica
receiving layer
ink receiving
ink
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Granted
Application number
JP2002060810A
Other languages
Japanese (ja)
Other versions
JP4012416B2 (en
Inventor
Hiromine Yamamoto
寛峰 山本
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Nisshinbo Holdings Inc
Original Assignee
Nisshinbo Industries Inc
Nisshin Spinning Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Nisshinbo Industries Inc, Nisshin Spinning Co Ltd filed Critical Nisshinbo Industries Inc
Priority to JP2002060810A priority Critical patent/JP4012416B2/en
Publication of JP2003251930A publication Critical patent/JP2003251930A/en
Application granted granted Critical
Publication of JP4012416B2 publication Critical patent/JP4012416B2/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

<P>PROBLEM TO BE SOLVED: To provide a sheet for ink jet recording which is excellent particularly in the water resistance and strength of an ink receiving layer and in the density and water resistance of an image and suitable for the outdoor use, e.g. for a poster or the like, while having the fundamental characteristics of a usual sheet for ink jet recording. <P>SOLUTION: The sheet has the ink receiving layer provided on a base. The ink receiving layer contains silica, a calcium carbonate of an aragonite quality, silanol modified polyvinyl alcohol and a hydrated aluminum oxide, and the silica contains 50 wt.% or more of silica of which the capacities of pores are 0.9-1.5 ml/g and the average particle length 2-5 μm. <P>COPYRIGHT: (C)2003,JPO

Description

【発明の詳細な説明】Detailed Description of the Invention

【0001】[0001]

【発明の属する技術分野】本発明はインクジェット記録
用シートに関し、さらに詳しくは、基材上にインク受理
層を有し、インク受理層の耐水性と強度及び画像の濃度
と耐水性に優れ、特に、ポスター等の屋外での使用に適
した、インクジェット記録用シートに関するものであ
る。
BACKGROUND OF THE INVENTION 1. Field of the Invention The present invention relates to an ink jet recording sheet, and more specifically, it has an ink receiving layer on a substrate and is excellent in water resistance and strength of the ink receiving layer and in image density and water resistance. The present invention relates to an inkjet recording sheet suitable for outdoor use such as a poster.

【0002】[0002]

【従来の技術】近年、コンピュータ利用技術の普及によ
り、コンピュータにより作成した資料をプリンターなど
を用いてプリントアウトすることが頻繁に行われるよう
になってきた。その際使用されるプリンターとしては、
ドットインパクトプリンター、レーザープリンター、サ
ーマルプリンターおよびインクジェットプリンターなど
が挙げられるが、プリントアウト時の機械的騒音がほと
んどなく、かつプリントアウトに伴うランニングコスト
の低さから、インクジェットプリンターが広く利用され
ている。
2. Description of the Related Art In recent years, due to the widespread use of computers, it has become common to print out materials created by computers using printers and the like. As a printer used at that time,
Examples include dot impact printers, laser printers, thermal printers, inkjet printers, and the like, but inkjet printers are widely used because they have almost no mechanical noise during printout and the running cost associated with printout is low.

【0003】かかるインクジェット記録方式には、基材
の上にインク受理層を設けた記録用シートが使用されて
いるが、用途の拡大に伴って、画像の精度だけではな
く、耐水性も求められている。従来、インク受理層とし
ては、シリカ、ポリビニルアルコール、アルミニウム酸
化物及び水溶性のカチオン樹脂を含むものが用いられる
ことが多いが、インク受理層の耐水性と強度及び画像の
濃度と耐水性(特に、水性顔料インク使用時)が不十分
であり、ポスター等として、屋外で使用するのには問題
があった。
In such an ink jet recording system, a recording sheet having an ink receiving layer provided on a base material is used. With the expansion of applications, not only image accuracy but also water resistance is required. ing. Conventionally, as the ink receiving layer, those containing silica, polyvinyl alcohol, aluminum oxide and a water-soluble cationic resin are often used, but the water resistance and strength of the ink receiving layer and the density and water resistance of the image (particularly, , When using the water-based pigment ink) was insufficient, and there was a problem in using it outdoors as a poster or the like.

【0004】[0004]

【発明が解決しようとする課題】本発明は、このような
状況で、従来のインクジェット記録用シートの基本的な
特性を有しながら、特に、インク受理層の耐水性と強度
及び画像の濃度と耐水性に優れたインクジェット記録用
シートを提供することを目的とするものである。
Under such circumstances, the present invention has the basic characteristics of the conventional ink jet recording sheet, and in particular, the water resistance and strength of the ink receiving layer and the density of the image. It is an object of the present invention to provide an inkjet recording sheet having excellent water resistance.

【0005】[0005]

【課題を解決するための手段】本発明者は、前記の優れ
た特性を有するインクジェット記録用シートを開発すべ
く鋭意研究を重ねた結果、特定の細孔容積と平均粒子径
のシリカを含むシリカ、アラゴナイト質の炭酸カルシウ
ム、シラノール変性ポリビニルアルコール及び水和アル
ミニウム酸化物を含有したインク受理層を設けたもの
が、その目的に適合し得ることを見出した。本発明はか
かる知見に基づいて完成したものである。すなわち、本
発明は、基材上にインク受理層を設けてなり、該インク
受理層が、シリカ、アラゴナイト質の炭酸カルシウム、
シラノール変性ポリビニルアルコール及び水和アルミニ
ウム酸化物を含有し、且つ、該シリカが、細孔容積が
0.9〜1.5ml/gで平均粒子径が2〜5μmのシ
リカを50重量%以上含有するシリカであることを特徴
とするインクジェット記録用シートを提供するものであ
る。
As a result of earnest studies to develop an ink jet recording sheet having the above-mentioned excellent properties, the present inventor has found that silica containing silica having a specific pore volume and average particle diameter. It has been found that those provided with an ink receiving layer containing aragonite calcium carbonate, silanol-modified polyvinyl alcohol and hydrated aluminum oxide can meet the purpose. The present invention has been completed based on such findings. That is, the present invention comprises an ink receiving layer provided on a substrate, wherein the ink receiving layer is silica, aragonite calcium carbonate,
It contains silanol-modified polyvinyl alcohol and hydrated aluminum oxide, and the silica contains 50% by weight or more of silica having a pore volume of 0.9 to 1.5 ml / g and an average particle diameter of 2 to 5 μm. It is intended to provide an inkjet recording sheet characterized by being silica.

【0006】[0006]

【発明の実施の形態】本発明のインクジェット記録用シ
ートは、基材の少なくとも一方の面に、インク受理層を
有するものである。本発明においては、基材は、シート
状のものであればよく、特に限定されるものではない。
プラスチックフィルム、紙、不織布等の種々のものが使
用可能であるが、特に、耐水性の点からプラスチックフ
ィルムが好適である。プラスチックの素材としては、塩
化ビニル、ポリエチレンテレフタレート、ポリプロピレ
ン、ポリスチレン、ポリカーボネート等の一般的な熱可
塑性樹脂フィルム、或いは、炭酸カルシウム等の無機粉
末や有機ピグメントを内添させたもの等から選択するこ
とが可能である。
BEST MODE FOR CARRYING OUT THE INVENTION The ink jet recording sheet of the present invention has an ink receiving layer on at least one surface of a substrate. In the present invention, the base material is not particularly limited as long as it is in the form of a sheet.
Various materials such as plastic films, papers, non-woven fabrics and the like can be used, but plastic films are particularly preferable from the viewpoint of water resistance. As the plastic material, it is possible to select a general thermoplastic resin film such as vinyl chloride, polyethylene terephthalate, polypropylene, polystyrene, or polycarbonate, or an inorganic powder such as calcium carbonate or an organic pigment internally added. It is possible.

【0007】又、発泡プラスチックフィルムも使用する
ことができる。ここで、発泡プラスチックフィルムと
は、フィルムの表面や内部に形成させる亀裂や欠所、或
いは、細かな気泡や空洞などを有するプラスチックフィ
ルムをいうが、これらの気泡や空洞などは、炭酸カルシ
ウム等の無機粉末を含有したフィルムを延伸して無機粉
末の周囲に発生させたり(ミクロボイドフィルムと称さ
れることがある)、発泡剤を含有させたフィルムにおい
て発泡剤を発泡させたりして形成したものなど、その名
称や形成方法或いは気泡や空洞の生成形態は問わない。
なお、ここでいうプラスチックフィルムには、合成紙と
称されるものも含まれる。
Foamed plastic films can also be used. Here, the foamed plastic film refers to a plastic film having cracks or voids formed on the surface or inside of the film, or fine bubbles or cavities, and these bubbles or cavities include those such as calcium carbonate. Formed by stretching a film containing inorganic powder and generating it around the inorganic powder (sometimes called a microvoid film), or foaming a foaming agent in a film containing a foaming agent, etc. The name, the forming method, or the generation form of bubbles or cavities does not matter.
The plastic film referred to here also includes what is called synthetic paper.

【0008】基材は、単層構造でも多層構造でもよく、
多層構造としては、例えば、接着剤を介して層同士を貼
り合せる方法、複数の押し出し機から複数の原料を押し
出し合流させて製膜するいわゆる共押出方法、フィルム
の上に押出機から直接フィルムを押し出しながら貼り合
わせて積層するいわゆる押し出しラミネート方法など、
公知の方法の何れで形成したものも用いることができ
る。
The substrate may have a single-layer structure or a multi-layer structure,
As the multilayer structure, for example, a method of laminating layers via an adhesive, a so-called co-extrusion method of extruding a plurality of raw materials from a plurality of extruders to join and form a film, a film directly from an extruder on a film. The so-called extrusion laminating method of laminating by laminating while extruding,
Those formed by any known method can be used.

【0009】基材には、インク受理層等との密着性や濡
れ性を向上させるなどの目的で、所望により、その片面
または両面に、酸化法や凹凸法などにより表面処理を施
すことができる。上記酸化法としては、例えばコロナ放
電処理、熱風処理などが挙げられ、また、凹凸法として
は、例えばサンドブラスト法、溶剤処理法などが挙げら
れる。これらの表面処理法は基材の種類に応じて適宜選
択されるが、一般にはコロナ放電処理法が効果および操
作性などの面から好ましく用いられる。また、易接着処
理を施すこともできる。
If desired, one or both surfaces of the base material may be subjected to a surface treatment by an oxidation method or a concavo-convex method for the purpose of improving the adhesion or wettability with the ink receiving layer or the like. . Examples of the oxidation method include corona discharge treatment and hot air treatment, and examples of the concavo-convex method include sandblast method and solvent treatment method. These surface treatment methods are appropriately selected according to the type of the base material, but in general, the corona discharge treatment method is preferably used in terms of effects and operability. Also, an easy adhesion treatment can be applied.

【0010】本発明においては、前記基材の少なくとも
一方の面に設けられるインク受理層は、シリカ、アラゴ
ナイト質の炭酸カルシウム、シラノール変性ポリビニル
アルコール及び水和アルミニウム酸化物を含有するもの
である。
In the present invention, the ink receiving layer provided on at least one surface of the substrate contains silica, aragonite calcium carbonate, silanol-modified polyvinyl alcohol and hydrated aluminum oxide.

【0011】インク受理層に填料として含有させるシリ
カとしては、細孔容積が0.9〜1.5ml/g、
平均粒子径が2〜5μm、の2条件をともに満たすシリ
カを50重量%以上含有するものを使用する。この細孔
容積及び平均粒子径のシリカの含有量が50重量%未満
である場合は、インク受理層の強度、画像の耐水性、に
じみの防止性能が低下する。填料として含有させるシリ
カの調整は、上記の2条件を満たすシリカが50重量%
以上になるように、別のシリカを混合すればよい。この
とき、細孔容積が0.9〜1.5ml/gで平均粒子径
が2〜5μmのシリカに、細孔容積が1.5ml/gを
超え2.2ml/g以下で、平均粒子径が5μmを超え
るシリカを加えると、にじみの防止性能や画像の濃度が
より向上するので、好ましい。その場合、細孔容積が
0.9〜1.5ml/gで平均粒子径が2〜5μmのシ
リカの含有量を50〜90重量%とし、細孔容積が1.
5ml/gを超え2.2ml/g以下で、平均粒子径が
5μmを超えるシリカの含有量を10〜40重量%とす
ればよく、シリカの粒度分布は2〜5μmの範囲と5μ
mを超えた範囲に2つのピークを有する、あるいは2〜
5μmの範囲にピークと5μmを超えた範囲に肩を有す
るものとなる。また、シリカは、ゲル法で製造されたも
のが好ましい。なお、細孔容積はBET法で測定したも
のを、また、平均粒子径はコールターカウンター法で測
定したものを、各々、意味する。
The silica contained as a filler in the ink receiving layer has a pore volume of 0.9 to 1.5 ml / g,
A silica containing 50% by weight or more of silica satisfying the two conditions of the average particle diameter of 2 to 5 μm is used. When the content of silica having the pore volume and the average particle diameter is less than 50% by weight, the strength of the ink receiving layer, the water resistance of the image, and the bleeding prevention performance deteriorate. The silica to be contained as a filler is adjusted to 50% by weight of silica satisfying the above two conditions.
As described above, another silica may be mixed. At this time, in the silica having a pore volume of 0.9 to 1.5 ml / g and an average particle diameter of 2 to 5 μm, the pore volume exceeds 1.5 ml / g and 2.2 ml / g or less, and the average particle diameter is Is more than 5 μm, the bleeding preventing performance and the image density are further improved, which is preferable. In that case, the content of silica having a pore volume of 0.9 to 1.5 ml / g and an average particle diameter of 2 to 5 μm is 50 to 90% by weight, and the pore volume is 1.
The content of silica exceeding 5 ml / g and 2.2 ml / g or less and having an average particle size of more than 5 μm may be 10 to 40% by weight, and the particle size distribution of silica is in the range of 2 to 5 μm and 5 μm.
It has two peaks in a range exceeding m, or 2 to
It has a peak in the range of 5 μm and a shoulder in the range exceeding 5 μm. Further, silica is preferably produced by a gel method. The pore volume means that measured by the BET method, and the average particle size means that measured by the Coulter counter method.

【0012】細孔容積が0.9〜1.5ml/gで平均
粒子径が2〜5μmのシリカを50重量%以上含有する
シリカのインク受理層中の含有率は、40〜70重量
%、特に45〜60重量%が好ましい。含有量がこの範
囲より少ないと、インク吸収性・乾燥性が低下しやすく
なり、逆に、この範囲より多いと、インク受理層の強度
が低下しやすくなる。
The content of silica containing 50% by weight or more of silica having a pore volume of 0.9 to 1.5 ml / g and an average particle size of 2 to 5 μm in the ink receiving layer is 40 to 70% by weight, Particularly, 45 to 60% by weight is preferable. If the content is less than this range, the ink absorbency / dryability tends to decrease, and conversely, if the content exceeds the range, the strength of the ink receiving layer tends to decrease.

【0013】インク受理層に填料として、シリカと共に
含有させる炭酸カルシウムは、アラゴナイト質の炭酸カ
ルシウムであり、特に好ましくは、平均粒子径が2〜6
μmで、三次元的に絡みあわせたウニ状の形状を有し、
吸油量が80〜110ml/100gのものである。ア
ラゴナイト質の炭酸カルシウムのインク受理層中の含有
率は、5〜25重量%、特に8〜20重量%が好まし
い。含有量がこの範囲より少ないと、画像が滲みやすく
なり、逆に、この範囲より多いと、インク受理層の耐水
性が低下しやすくなる。
The calcium carbonate contained together with silica as a filler in the ink receiving layer is an aragonite calcium carbonate, and particularly preferably, the average particle diameter is 2 to 6.
It has a sea urchin shape that is three-dimensionally intertwined with
The oil absorption is 80 to 110 ml / 100 g. The content of aragonite calcium carbonate in the ink receiving layer is preferably 5 to 25% by weight, particularly preferably 8 to 20% by weight. If the content is less than this range, the image tends to bleed, and conversely, if it is more than this range, the water resistance of the ink receiving layer tends to decrease.

【0014】インク受理層には、本発明の効果を損なわ
ない範囲で、前記シリカ及び炭酸カルシウム以外の填料
の一種又は二種以上を混合して用いることができる。か
かる、填料としては、例えば、タルク、クレー、けいそ
う土、水酸化アルミニウム、ポリスチレン、ポリメタク
リレート、酸化チタン、焼成カオリンなどが挙げられ
る。インク受理層中の填料全体の含有率は、45〜95
重量%、特に53〜80重量%が好ましい。填料がこの
範囲より少ないと、インク吸収性が不足しやすくなり、
逆に、この範囲より多いと、インク受理層の強度が低下
しやすくなる。
In the ink receiving layer, one or more kinds of fillers other than silica and calcium carbonate can be mixed and used within a range that does not impair the effects of the present invention. Examples of the filler include talc, clay, diatomaceous earth, aluminum hydroxide, polystyrene, polymethacrylate, titanium oxide, calcined kaolin and the like. The content ratio of the entire filler in the ink receiving layer is 45 to 95.
%, Especially 53 to 80% by weight is preferred. If the filler is less than this range, the ink absorbency tends to be insufficient,
On the other hand, if the amount is more than this range, the strength of the ink receiving layer tends to decrease.

【0015】結着剤としてインク受理層に含有させるシ
ラノール変性ポリビニルアルコールのインク受理層中の
含有率は、20〜50重量%、特に25〜35重量%が
好ましい。含有量がこの範囲より少ないと、インク受理
層の強度が低下しやすくなり、逆に、この範囲より多い
と、インク受理層のインク吸収性・乾燥性が低下しやす
くなる。
The content of silanol-modified polyvinyl alcohol contained in the ink receiving layer as a binder in the ink receiving layer is preferably 20 to 50% by weight, more preferably 25 to 35% by weight. When the content is less than this range, the strength of the ink receiving layer tends to decrease, and conversely, when the content is more than this range, the ink absorbability and drying property of the ink receiving layer tend to decrease.

【0016】結着剤としては、本発明の効果を損なわな
い範囲で、シラノール変性ポリビニルアルコール以外の
結着剤の一種又は二種以上を混合して用いることができ
る。かかる、結着剤としては、例えば、ポリビニルブチ
ラール、ゼラチン、ポリビニルアセタール、カルボキシ
メチルセルロース、ポリビニルピロリドン、ポリエステ
ル、アクリル樹脂、ウレタン樹脂及びこれらの共重体、
スチレン−アクリル共重合体、エチレン−酢酸ビニル共
重合体などを挙げることができる。インク受理層中の結
着剤全体の含有率(インク受理層中の固形分含有率)
は、20〜50重量%、特に25〜35重量%が好まし
い。
As the binder, one or two or more binders other than silanol-modified polyvinyl alcohol can be mixed and used as long as the effect of the present invention is not impaired. As such a binder, for example, polyvinyl butyral, gelatin, polyvinyl acetal, carboxymethyl cellulose, polyvinyl pyrrolidone, polyester, acrylic resin, urethane resin and their copolymers,
Examples thereof include styrene-acrylic copolymer, ethylene-vinyl acetate copolymer and the like. Content of the entire binder in the ink receiving layer (solid content in the ink receiving layer)
Is preferably 20 to 50% by weight, and particularly preferably 25 to 35% by weight.

【0017】インク受理層に含有させる水和アルミニウ
ム酸化物のインク受理層中の含有率は、2〜15重量
%、特に3〜7重量%が好ましい。含有量がこの範囲よ
り少ないと、インク受理層の耐水性が低下しやすくな
り、逆に、この範囲より多いと、記録用シートのカール
が強くなりやすくなる。
The content of the hydrated aluminum oxide contained in the ink receiving layer in the ink receiving layer is preferably 2 to 15% by weight, more preferably 3 to 7% by weight. When the content is less than this range, the water resistance of the ink receiving layer tends to be lowered, and conversely, when the content is more than this range, the curl of the recording sheet tends to be strong.

【0018】該インク受理層には、本発明の目的が損な
われない範囲で、必要に応じ、消泡剤、帯電防止剤、紫
外線吸収剤、蛍光増白剤、防腐剤、顔料分散剤、増粘剤
などの各種添加剤を含有させることができる。また、該
インク受理層は、にじみの防止性能や画像濃度に優れて
いるが、さらに微量のカチオン性物質を含有させること
により、にじみの防止性能をさらに向上させることがで
きる。かかるカチオン性物質としてはジシアンジアミ
ド、ジメチルアミンエピクロロヒドリン、ポリアミン系
樹脂、第4級アンモニウム塩などを挙げることが出来
る。カチオン性物質を含有させるには、カチオン性物質
以外のインク受理層形成材料を塗工・乾燥して形成した
層に、カチオン性物質を含浸させる方法を採るのが適当
である。層に含浸させる方法としては、カチオン性物質
を含む溶液に層を浸漬する方法、カチオン性物質を含む
溶液を層に塗工する方法、カチオン性物質を含む溶液を
層に散布する方法等があるが、操作の容易性の面から、
カチオン性物質を含む溶液を層に塗工する方法が好まし
い。塗工する場合は、リバースロールコート、エアナイ
フコート、グラビアコート、ブレードコート等の従来公
知の方法を用いることが可能である。
If necessary, the ink-receiving layer contains an antifoaming agent, an antistatic agent, an ultraviolet absorber, an optical brightening agent, an antiseptic agent, a pigment dispersant, and an increasing agent as long as the object of the present invention is not impaired. Various additives such as a sticky agent can be contained. Further, the ink receiving layer is excellent in the bleeding prevention performance and the image density, but the bleeding prevention performance can be further improved by further containing a slight amount of a cationic substance. Examples of such cationic substances include dicyandiamide, dimethylamine epichlorohydrin, polyamine resins, and quaternary ammonium salts. To contain the cationic substance, it is appropriate to adopt a method of impregnating the layer formed by coating and drying an ink receiving layer forming material other than the cationic substance with the cationic substance. The method of impregnating the layer includes a method of immersing the layer in a solution containing a cationic substance, a method of applying a solution containing a cationic substance to the layer, a method of spraying a solution containing a cationic substance on the layer, and the like. However, in terms of ease of operation,
A method of applying a solution containing a cationic substance to the layer is preferable. When coating, conventionally known methods such as reverse roll coating, air knife coating, gravure coating and blade coating can be used.

【0019】なお、カチオン性物質は層に含浸させる
が、層の上部に多くなるように局在させるのが好まし
い。その為には、塗工液は水、水溶性の有機溶媒と水の
混合液等で1〜15重量%、特に3〜6重量%に希釈
し、かつ結着剤を含まない液とするのが好ましく、ま
た、塗液量をカチオン性物質の固形分重量で0.4〜
1.2g/m2とするのが好ましい。カチオン性物質が
この範囲より少ないと、画像のにじみが生じやすくなる
とともに、画像の濃度が低下しやすくなり、逆に、この
範囲より多いと、画像の耐水性が低下しやすくなる。こ
のインク受理層の厚さは、20〜50μm、特に25〜
40μmの範囲が好ましい。この範囲より薄いと、イン
ク受理層のインク吸収性・乾燥性が低下しやすくなり、
逆に、この範囲より厚いと、インク受理層の強度及び耐
水性が低下しやすくなる。
Although the cationic substance is impregnated in the layer, it is preferable that the cationic substance is localized so as to be abundant in the upper portion of the layer. For that purpose, the coating solution should be diluted with water, a mixed solution of a water-soluble organic solvent and water to 1 to 15% by weight, particularly 3 to 6% by weight, and to be a solution containing no binder. Is preferable, and the coating liquid amount is 0.4 to 10 in terms of solid content weight of the cationic substance.
It is preferably 1.2 g / m 2 . If the amount of the cationic substance is less than this range, image bleeding tends to occur and the image density tends to decrease, while if it is more than this range, the water resistance of the image tends to decrease. The thickness of the ink receiving layer is 20 to 50 μm, and particularly 25 to
The range of 40 μm is preferable. When the thickness is less than this range, the ink absorbing layer tends to deteriorate in ink absorbency and dryness,
On the other hand, if the thickness is larger than this range, the strength and water resistance of the ink receiving layer are likely to decrease.

【0020】また、本発明のインクジェット記録シート
には、本発明の目的が損なわれない範囲で、インク受理
層以外の層を設けてもよい。例えば、基材とインク受理
層との密着力を向上する為に、アンカーコート層を設け
てもよい。インク受理層は、構成成分を適当な溶媒に溶
解又は分散させた塗工液を、リバースロールコート、エ
アナイフコート、グラビアコート、ブレードコートなど
の公知の方法により塗工し、乾燥させることにより形成
することができる。
The ink jet recording sheet of the present invention may be provided with a layer other than the ink receiving layer as long as the object of the present invention is not impaired. For example, an anchor coat layer may be provided in order to improve the adhesion between the base material and the ink receiving layer. The ink-receiving layer is formed by applying a coating solution obtained by dissolving or dispersing the constituent components in a suitable solvent by a known method such as reverse roll coating, air knife coating, gravure coating, blade coating, and drying. be able to.

【0021】[0021]

【実施例】次に、本発明を実施例によりさらに詳しく説
明するが、本発明は、これらの例によってなんら限定さ
れるものではない。なお、インクジェット記録用シート
の性能は、以下に示す要領に従って評価した。また、印
画は、セイコーエプソン社製のインクジェットプリンタ
(機種名:MC9000)で、純正の顔料タイプのイン
クを使用して行った。
EXAMPLES Next, the present invention will be described in more detail with reference to examples, but the present invention is not limited to these examples. The performance of the inkjet recording sheet was evaluated according to the following procedure. In addition, printing was performed with an inkjet printer (model name: MC9000) manufactured by Seiko Epson Corporation using genuine pigment type ink.

【0022】(1)インク受理層の耐水性(濡れた状態
での耐擦過性) 十分に濡れた綿棒で、荷重が100gになるようにイン
クジェット記録用シートのインク受理層表面を、インク
受理層が脱離するまで擦り、それに要した回数を数え
た。なお、1往復(片道50mm)を1回と数えた。ま
た、操作は100回まで行い、その時点でインク受理層
が脱離しなかったものも、100回とした。
(1) Water resistance of the ink receiving layer (scratch resistance in a wet state) With a cotton swab sufficiently wet, the surface of the ink receiving layer of the ink jet recording sheet is adjusted so that the load is 100 g. Was rubbed until it detached, and the number of times required for it was counted. In addition, one round trip (one way 50 mm) was counted as once. The operation was performed up to 100 times, and the number of times when the ink receiving layer was not detached at that time was 100 times.

【0023】(2)インク受理層の強度 インク受理層上にセロハンテープ(ニチバン社製「CT
405A−18」、長さ10cm)を2kgの圧着ロー
ル3往復で貼り付け、45°の角度で逆行する向きに剥
離した時の剥がれ具合を下記の判断基準で評価した。 ○:セロハンテープに付着した塗工層の面積が30%以
下 △:セロハンテープに付着した塗工層の面積が30%超
60%以下 ×:セロハンテープに付着した塗工層の面積が60%超
(2) Strength of ink receiving layer Cellophane tape (“CT manufactured by Nichiban Co., Ltd.” is placed on the ink receiving layer.
405A-18 ", length 10 cm) was pasted with 3 kg of 2 kg pressure rolls, and the degree of peeling when peeling in the direction opposite to the angle of 45 ° was evaluated according to the following criteria. ◯: Area of coating layer adhered to cellophane tape is 30% or less Δ: Area of coating layer adhered to cellophane tape is more than 30% and 60% or less ×: Area of coating layer adhered to cellophane tape is 60% Super

【0024】(3)画像の耐水性(滴下) シアン、マゼンタ、イエロー及びブラック混色の黒をベ
タ印画し、印画5分後に印画部にスポイトで蒸留水を一
滴垂らし、蒸留水が完全に吸収されたときのインク流出
の度合いを目視で観察し、下記の判定基準で評価した。 ◎:流出なし ○:流出が若干発生したが、実用上支障なし △:流出が発生し、実用上支障あり ×:流出が多く発生し、実用上支障あり
(3) Water resistance of image (dripping) Black of cyan, magenta, yellow and black mixed color is solidly printed, and after 5 minutes of printing, one drop of distilled water is dropped on the printing part with a dropper so that the distilled water is completely absorbed. The degree of ink outflow was visually observed and evaluated according to the following criteria. ◎: No outflow ○: Some outflow occurred, but there was no problem in practical use △: Outflow occurred, there was a problem in practical use ×: Many outflow occurred, there was a practical problem

【0025】(4)画像濃度 シアン、マゼンタ、イエロー各色と、混色の黒(シア
ン、マゼンタ、イエロー及びブラックを混色したもの)
をベタ印画し、画像の反射濃度をマクベス濃度計RD−
918で測定した。
(4) Image density Cyan, magenta, and yellow colors and mixed color black (mixed color of cyan, magenta, yellow, and black)
Is printed solidly, and the reflection density of the image is measured by Macbeth densitometer RD-
It was measured at 918.

【0026】(5)にじみの防止性能 レッド(マゼンタとイエローの混色)及びグリーン(シ
アンとイエローの混色)を使用し、マット印刷モード
(使用したプリンターのモードのうち、インクの噴射量
が多いランクに属する。)において、インク噴射量17
0%で白抜き文字を印画したときのインクのにじみの状
態を目視し、下記の判定基準で評価した。 ◎:にじみなし ○:にじみが若干発生したが、実用上支障なし △:にじみが発生し、実用上支障あり ×:にじみが多く発生し、実用上支障あり
(5) Anti-bleeding performance Using red (mixed color of magenta and yellow) and green (mixed color of cyan and yellow), matte printing mode (rank of ink jetting amount in the used printer modes) Ink ejection amount 17
The state of ink bleeding when a blank character was printed at 0% was visually observed and evaluated according to the following criteria. ◎: No bleeding ○: Some bleeding occurred, but there was no problem in practical use △: Bleeding occurred and there was practical problem ×: Many bleeding occurred, there was practical problem

【0027】実施例1 基材として、厚さ80μmのユポFPG80〔商品名、
ユポ・コーポレーション社製の白色の発泡ポリプロピレ
ンフィルム、ミクロボイドフィルム〕を用いた。アンカ
ーコート用塗工液として、次の成分の均一混合物を用い
た。 (a) アクロナールYJ−6221D〔商品名、BASF
ディスパージョン(株)製アクリル樹脂、固形分濃度4
9重量%、アニオン性〕60重量部 (b) カルライトSA〔商品名、白石中央研究所製炭酸カ
ルシウム、固形分濃度100重量%、アラゴナイト質〕
10重量部 (c) 水30重量%
Example 1 As a base material, YUPO FPG80 [trade name, having a thickness of 80 μm,
A white foamed polypropylene film and a micro void film manufactured by YUPO Corporation were used. A uniform mixture of the following components was used as an anchor coating liquid. (a) ACRONAL YJ-6221D [trade name, BASF
Dispersion Co., Ltd. acrylic resin, solid content concentration 4
9% by weight, anionic] 60 parts by weight (b) Callite SA [trade name, calcium carbonate manufactured by Shiraishi Central Research Institute, solid content concentration 100% by weight, aragonite]
10 parts by weight (c) 30% by weight of water

【0028】インク受理層用塗工液として、次の成分の
均一混合物を用いた。 (1) サイリシア440〔商品名、富士シリシア化学
(株)製シリカ、固形分濃度100重量%、平均粒子径
3.5μm、細孔容積1.2 5ml/g〕6.0重量
部 (2) サイロジェットP412〔商品名、Grace Davison
社製シリカ、固形分濃度100重量%、平均粒子径6〜
8μm、細孔容積2.05ml/g〕2.4重量部 (3) カルライトSA〔商品名、白石中央研究所製炭酸カ
ルシウム、固形分濃度100重量%、アラゴナイト質、
平均粒子径約3μm、形状:三次元的に絡み合わせたウ
ニ状、吸油量95ml/100g〕2.2重量部 (4) RポリマーR−1130〔クラレ(株)製シラノー
ル変性ポリビニルアルコール、固形分濃度100重量
%〕4.9重量部 (5) アルミナゾル200〔商品名、日産化学工業(株)
製水和アルミニウム酸化物、固形分濃度10重量%〕
7.6重量部 (6) 水76.7重量部
A uniform mixture of the following components was used as the coating liquid for the ink receiving layer. (1) Silysia 440 [trade name, silica manufactured by Fuji Silysia Chemical Ltd., solid content concentration 100% by weight, average particle diameter 3.5 μm, pore volume 1.25 ml / g] 6.0 parts by weight (2) Silojet P412 [trade name, Grace Davison
Silica, solid content concentration 100% by weight, average particle size 6 to
8 μm, pore volume 2.05 ml / g] 2.4 parts by weight (3) Callite SA [trade name, calcium carbonate manufactured by Shiraishi Central Research Institute, solid content concentration 100% by weight, aragonite,
Average particle diameter of about 3 μm, shape: sea urchin three-dimensionally intertwined, oil absorption 95 ml / 100 g] 2.2 parts by weight (4) R polymer R-1130 [silanol-modified polyvinyl alcohol manufactured by Kuraray Co., Ltd., solid content] Concentration 100% by weight] 4.9 parts by weight (5) Alumina sol 200 [trade name, Nissan Chemical Industries, Ltd.
Made hydrated aluminum oxide, solid content concentration 10% by weight]
7.6 parts by weight (6) Water 76.7 parts by weight

【0029】基材上に、アンカーコート用塗工液を塗工
して、厚さ3μm(乾燥後)のアンカーコート層を形成
し、その上にインク受理層用塗工液を塗工して、厚さ3
0μm(乾燥後)のインク受理層を形成させることによ
り、インクジェット記録用シートを作製した。
Anchor coat coating liquid is applied on the base material to form an anchor coat layer having a thickness of 3 μm (after drying), and the ink receiving layer coating liquid is applied thereon. , Thickness 3
An inkjet recording sheet was produced by forming an ink receiving layer having a thickness of 0 μm (after drying).

【0030】実施例2 インク受理層用塗工液におけるサイロジェットP412
〔シリカ〕2.4重量部をサイリシア440〔シリカ〕
2.4重量部に変えた、すなわち、シリカとしてサイリ
シア440〔シリカ〕8.4重量部のみを使用した以外
は実施例1と同様にして、インクジェット記録用シート
を作製した。
Example 2 Silojet P412 in a coating liquid for an ink receiving layer
[Silica] 2.4 parts by weight of Silysia 440 [silica]
An ink jet recording sheet was produced in the same manner as in Example 1 except that 2.4 parts by weight, that is, 8.4 parts by weight of Silysia 440 [silica] was used as silica.

【0031】実施例3 実施例1と全く同様に行って、厚さ30μm(乾燥後)
のインク受理層を形成させたのち、次の組成からなる、
カチオン性物質(ジシアンジアミド縮合物)含有溶液
を、インク受理層中のカチオン性物質の固形分含有量が
3重量%となるように該インク受理層に塗工した。この
溶液は新たな層は形成しなかった。 (イ) ネオフィックスE117〔商品名、日華化学(株)
製ジシアンジアミド縮合物、固形分濃度50重量%〕9
重量部 (ロ) 水91重量部
Example 3 Exactly the same as Example 1, and the thickness is 30 μm (after drying).
After forming the ink receiving layer of
A solution containing a cationic substance (dicyandiamide condensate) was applied to the ink receiving layer so that the solid content of the cationic substance in the ink receiving layer was 3% by weight. This solution did not form a new layer. (A) Neofix E117 [trade name, Nika Kagaku Co., Ltd.
Manufactured dicyandiamide condensate, solid content concentration 50% by weight] 9
Part by weight (b) Water 91 parts by weight

【0032】比較例1 実施例2におけるカルライトSA〔炭酸カルシウム〕
2.2重量部に代えて、軽質炭酸カルシウム〔丸尾カル
シウム社製炭酸カルシウム、固形分濃度100重量%、
カルサイト質、平均粒子径約1〜2μm、吸油量50m
l/100g〕2.2重量部を用いた以外は, 実施例2
と同様にして、インクジェット記録用シートを作製し
た。
Comparative Example 1 Callite SA [calcium carbonate] in Example 2
Instead of 2.2 parts by weight, light calcium carbonate [calcium carbonate manufactured by Maruo Calcium Co., solid content concentration 100% by weight,
Calcite quality, average particle size about 1-2 μm, oil absorption 50 m
1/100 g] Example 2 except that 2.2 parts by weight were used.
An ink jet recording sheet was produced in the same manner as in.

【0033】比較例2 実施例2におけるカルライトSA〔炭酸カルシウム〕
2.2重量部を使用しなかった以外は, 実施例2と同様
にして、インクジェット記録用シートを作製した。
Comparative Example 2 Callite SA [calcium carbonate] in Example 2
An inkjet recording sheet was produced in the same manner as in Example 2 except that 2.2 parts by weight was not used.

【0034】比較例3 実施例2におけるアルミナゾル200〔水和アルミニウ
ム酸化物〕7.6重量部を使用しなかった以外は, 実施
例2と同様にして、インクジェット記録用シートを作製
した。
Comparative Example 3 An ink jet recording sheet was prepared in the same manner as in Example 2 except that 7.6 parts by weight of alumina sol 200 [hydrated aluminum oxide] in Example 2 was not used.

【0035】比較例4 実施例2におけるサイリシア440〔シリカ〕8.4重
量部に代えて、ミズカシルP78F〔商品名、水澤化学
(株)製シリカ、固形分濃度100重量%、平均粒子径
12.5μm、細孔容積1.65ml/g〕8.4重量
部を使用した以外は, 実施例2と同様にして、インクジ
ェット記録用シートを作製した。
Comparative Example 4 Instead of 8.4 parts by weight of Sylysia 440 [silica] in Example 2, Mizukasil P78F [trade name, silica manufactured by Mizusawa Chemical Co., Ltd., solid content concentration 100% by weight, average particle size 12. 5 μm, pore volume 1.65 ml / g] An ink jet recording sheet was produced in the same manner as in Example 2 except that 8.4 parts by weight was used.

【0036】比較例5 実施例2のインク受理層用塗工液において、カルライト
SA〔炭酸カルシウム〕2.2重量部を使用せず、且
つ、該インク受理層用塗工液にジシアンジアミド縮合物
〔日華化学(株)製、商品名:ネオフィックスE11
7、固形分濃度50重量%、水溶性のカチオン性物質〕
4.1重量部を混合した以外は, 実施例2と同様にし
て、インクジェット記録用シートを作製した。
Comparative Example 5 In the coating liquid for the ink receiving layer of Example 2, 2.2 parts by weight of Callite SA [calcium carbonate] was not used, and the coating liquid for the ink receiving layer had a dicyandiamide condensation product [ Nichika Chemical Co., Ltd., trade name: Neofix E11
7, solid content concentration 50% by weight, water-soluble cationic substance]
An inkjet recording sheet was produced in the same manner as in Example 2 except that 4.1 parts by weight was mixed.

【0037】上記実施例1〜3及び比較例1〜5で得ら
れたインクジェット記録用シートそれぞれについて、イ
ンク受理層の耐水性(濡れた状態での耐擦過性)、イン
ク受理層の強度、画像の耐水性(滴下)、画像濃度、及
びにじみの防止性能を評価し、その結果を第1表に示
す。
For each of the ink jet recording sheets obtained in Examples 1 to 3 and Comparative Examples 1 to 5, the water resistance of the ink receiving layer (rubbing resistance in a wet state), the strength of the ink receiving layer, the image Of water resistance (dripping), image density, and bleeding prevention performance were evaluated, and the results are shown in Table 1.

【0038】[0038]

【表1】 [Table 1]

【0039】[0039]

【発明の効果】細孔容積が0.9〜1.5ml/gで、
平均粒子径が2〜5μmのシリカを50重量%以上含有
するシリカ、アラゴナイト質の炭酸カルシウム、シラノ
ール変性ポリビニルアルコール及び水和アルミニウム酸
化物を含有したインク受理層を設けた本発明のインクジ
ェット記録用シートは、従来のインクジェット記録用シ
ートの基本的な特性を有しながら、特に、インク受理層
の耐水性と強度及び画像の濃度と耐水性に優れ、ポスタ
ー等の屋外での使用に適したたものである。
The effect of the invention is that the pore volume is 0.9 to 1.5 ml / g,
The ink jet recording sheet of the present invention provided with an ink receiving layer containing silica containing 50% by weight or more of silica having an average particle diameter of 2 to 5 μm, aragonite calcium carbonate, silanol modified polyvinyl alcohol and hydrated aluminum oxide. Has the basic characteristics of conventional ink jet recording sheets, but is particularly suitable for outdoor use such as posters, because it is excellent in the water resistance and strength of the ink receiving layer and the image density and water resistance. Is.

Claims (4)

【特許請求の範囲】[Claims] 【請求項1】 基材上にインク受理層を設けてなり、該
インク受理層が、シリカ、アラゴナイト質の炭酸カルシ
ウム、シラノール変性ポリビニルアルコール及び水和ア
ルミニウム酸化物を含有し、且つ、該シリカが、細孔容
積が0.9〜1.5ml/gで、平均粒子径が2〜5μ
mのシリカを50重量%以上含有するシリカであること
を特徴とするインクジェット記録用シート。
1. An ink receiving layer is provided on a substrate, and the ink receiving layer contains silica, aragonite calcium carbonate, silanol-modified polyvinyl alcohol and hydrated aluminum oxide, and the silica is , The pore volume is 0.9 to 1.5 ml / g, and the average particle size is 2 to 5 μ.
An ink jet recording sheet, which comprises 50% by weight or more of m silica.
【請求項2】 前記シリカが、細孔容積が0.9〜1.
5ml/gで、平均粒子径が2〜5μmのシリカを50
〜90重量%と、細孔容積が1.5ml/gを超え2.
2ml/g以下で、平均粒子径が5μmを超えるシリカ
を10〜40重量%含有するシリカである、請求項1に
記載のインクジェット記録用シート。
2. The silica has a pore volume of 0.9-1.
50 ml of silica having an average particle size of 2 to 5 μm at 5 ml / g
˜90% by weight, the pore volume exceeds 1.5 ml / g and 2.
The inkjet recording sheet according to claim 1, which is a silica containing 10 to 40% by weight of silica having an average particle size of 5 μm or less at 2 ml / g or less.
【請求項3】 インク受理層中のシリカの含有量が40
〜70重量%であり、アラゴナイト質の炭酸カルシウム
の含有量が5〜25重量%であり、シラノール変性ポリ
ビニルアルコールの含有量が20〜50重量%であり、
水和アルミニウム酸化物の含有量が2〜15重量%であ
る、請求項1又は2に記載のインクジェット記録用シー
ト。
3. The content of silica in the ink receiving layer is 40.
-70% by weight, the content of aragonite calcium carbonate is 5 to 25% by weight, the content of silanol-modified polyvinyl alcohol is 20 to 50% by weight,
The inkjet recording sheet according to claim 1, wherein the content of the hydrated aluminum oxide is 2 to 15% by weight.
【請求項4】 色材として顔料を用いた水性インク用で
ある、請求項1〜3の何れかに記載のインクジェット記
録用シート。
4. The ink jet recording sheet according to claim 1, which is for a water-based ink using a pigment as a coloring material.
JP2002060810A 2002-03-06 2002-03-06 Inkjet recording sheet Expired - Fee Related JP4012416B2 (en)