[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP2000246843A - Multilayer film for packaging storage meat - Google Patents

Multilayer film for packaging storage meat

Info

Publication number
JP2000246843A
JP2000246843A JP11056552A JP5655299A JP2000246843A JP 2000246843 A JP2000246843 A JP 2000246843A JP 11056552 A JP11056552 A JP 11056552A JP 5655299 A JP5655299 A JP 5655299A JP 2000246843 A JP2000246843 A JP 2000246843A
Authority
JP
Japan
Prior art keywords
ethylene
meat
resin
resin composition
weight
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP11056552A
Other languages
Japanese (ja)
Inventor
Tomonori Murata
知規 村田
Hiroyuki Shimo
浩幸 下
Hitoshi Tateno
均 舘野
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Kuraray Co Ltd
Original Assignee
Kuraray Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Kuraray Co Ltd filed Critical Kuraray Co Ltd
Priority to JP11056552A priority Critical patent/JP2000246843A/en
Publication of JP2000246843A publication Critical patent/JP2000246843A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To improve barrier properties, a mechanical strength, and storage meat charging efficiency by incorporating at least one layer of a resin composition containing a specific ethylene-vinyl alcohol copolymer, a polyamide resin and an ethylene-unsaturated carboxylic acid copolymer or its metal salt in a multilayer film for packaging storage meat. SOLUTION: The multilayer film for packaging storage meat comprises one resin composition layer containing 50 to 95 wt.% of an ethylene-vinyl alcohol copolymer containing 20 to 60 mol% of an ethylene content and a saponification degree of 85% or above of a vinylester component by using an alkali catalyst from the copolymer of the ethylene and the vinylester, 0.2 to 25 wt.% of polyamide resin such as a polycaproamide (nylon-6), a polyundecaneamide (nylon-11), polylauryl lactam (nylon-12) or the like, and 0.5 to 40 wt.% of an ethylene-unsaturated carboxylic acid copolymer or its metal salt.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、バリア性、機械強
度、柔軟性、延伸性、収縮性、外観、畜肉の充填作業効
率に優れた、エチレン−ビニルアルコール共重合体
(A)、ポリアミド樹脂(B)およびエチレン−不飽和
カルボン酸共重合体またはその金属塩(C)からなる樹
脂組成物層、または、エチレン−ビニルアルコール共重
合体(A)、ポリアミド樹脂(B)、エチレン−不飽和
カルボン酸共重合体またはその金属塩(C)および11
以下の溶解性パラメーター(Fedorsの式から算
出)を有する前記樹脂以外の熱可塑性樹脂(D)からな
る樹脂組成物層を、少なくとも1層含む畜肉包装用多層
フィルムに関する。
TECHNICAL FIELD The present invention relates to an ethylene-vinyl alcohol copolymer (A) and a polyamide resin which are excellent in barrier properties, mechanical strength, flexibility, stretchability, shrinkage, appearance and work efficiency of filling meat. (B) and a resin composition layer composed of an ethylene-unsaturated carboxylic acid copolymer or a metal salt thereof (C), or an ethylene-vinyl alcohol copolymer (A), a polyamide resin (B), an ethylene-unsaturated Carboxylic acid copolymer or its metal salt (C) and 11
The present invention relates to a multilayer film for meat and meat packaging containing at least one resin composition layer composed of a thermoplastic resin (D) other than the above resin having the following solubility parameter (calculated from the Fedors equation).

【0002】[0002]

【従来の技術】ポリオレフィンやポリスチレンのような
疎水性熱可塑性樹脂は、その優れた溶融成形性、二次加
工性、機械特性、経済性から、食品包装分野においては
フィルム、ボトル、カップ等の容器等に、非食品分野に
おいては、生活用品、家電部品、自動車部品等に巾広く
使用されている。また、これらの樹脂とエチレン−ビニ
ルアルコール共重合体(以下、EVOHと略す)との多
層構造体は、酸素、フレーバー等に対するバリア性が必
要とされる食品分野等において広く使用されている。
2. Description of the Related Art Hydrophobic thermoplastic resins such as polyolefins and polystyrenes are used in containers such as films, bottles and cups in the field of food packaging because of their excellent melt moldability, secondary processing properties, mechanical properties and economy. In the non-food field, it is widely used for daily necessities, home electric parts, automobile parts and the like. In addition, multilayer structures of these resins and ethylene-vinyl alcohol copolymer (hereinafter abbreviated as EVOH) are widely used in the field of foods and the like that require a barrier property against oxygen, flavor and the like.

【0003】上記性能を生かし、EVOH系フィルムを
畜肉包装用多層フィルムとして用いることが試みられて
いるが、EVOH系フィルムがポリ塩化ビニリデン(以
下、PVDCと略す)系フィルムに比べ柔軟性に欠ける
ため、EVOH系フィルムは特に畜肉を保存するような
低温での落下強度が弱く、破損しやすいという欠点を有
している。
Attempts have been made to use EVOH-based films as a multilayer film for meat and meat packaging by taking advantage of the above-mentioned properties. However, EVOH-based films are less flexible than polyvinylidene chloride (hereinafter abbreviated as PVDC) -based films. In addition, EVOH-based films have the disadvantage that the drop strength at low temperatures, especially for preserving meat, is weak, and they are easily broken.

【0004】また、骨付き肉を包装する場合、特に熱収
縮包装する場合には、EVOH系フィルムの突刺し強度
が弱いため、骨の先端が畜肉包装用フィルムに突き刺さ
り破損を生じることがある。そこで、現在では布等で骨
の部分を被覆した後、包装を行っているが十分ではな
く、真空包装時もしくは熱収縮包装時に破損を生じるこ
とがある。さらに、EVOH系フィルムは一般的に硬
く、他のフィルムに比べ、肉の充填作業効率が悪いとい
う問題点が残されている。
[0004] In addition, when meat with bone is packaged, particularly in the case of heat shrink wrapping, the piercing strength of the EVOH-based film is low, so that the tip of the bone may pierce the meat packaging film and cause breakage. Therefore, at present, packaging is performed after covering the bone portion with a cloth or the like, but this is not sufficient, and damage may occur during vacuum packaging or heat shrink packaging. Furthermore, EVOH-based films are generally hard, and there is still a problem that the filling efficiency of meat is lower than other films.

【0005】また、EVOH系フィルムを熱収縮畜肉包
装用フィルムとして用いた場合では、熱収縮工程でメル
トホールが生じやすいという欠点を有している。なお、
本発明で言うメルトホールとは、熱収縮畜肉包装用フィ
ルムを用いて畜肉を包装する際に、フィルムを熱収縮さ
せるために熱風または熱水を吹き付ける工程において、
フィルムと畜肉表面が密着していない部分に熱風または
熱水が吹き付けられるためにフィルムに生じる穴のこと
を言う。
[0005] Further, when an EVOH-based film is used as a heat shrinkable meat packaging film, there is a drawback that a melt hole is easily generated in the heat shrinking step. In addition,
Melt hole referred to in the present invention, when packaging meat using a heat shrinkable meat packaging film, in the step of blowing hot air or hot water to thermally shrink the film,
A hole formed in the film because hot air or hot water is sprayed on the portion where the film and the meat surface do not adhere.

【0006】また、熱収縮畜肉包装用フィルムは、通
常、延伸されたものが用いられるが、EVOH系フィル
ムは一般に延伸性に乏しいため、 EVOH系フィルム
を用いた熱収縮畜肉包装用フィルムでは、延伸ムラや収
縮ムラによる厚み分布不良によるガスバリア性の低下、
更には外観不良が問題になる。
The heat-shrinkable meat and meat packaging film is usually stretched. However, since the EVOH-based film generally has poor stretchability, the heat-shrinkable meat and meat packaging film using the EVOH-based film is not stretched. Deterioration of gas barrier properties due to poor thickness distribution due to unevenness and shrinkage unevenness,
Furthermore, poor appearance is a problem.

【0007】そこで、EVOH系フィルムを他の熱可塑
性樹脂と積層し、かかる問題を解決することも考えられ
るが、必ずしも十分ではない。
To solve such a problem, it is conceivable to laminate the EVOH film with another thermoplastic resin, but this is not always sufficient.

【0008】[0008]

【発明が解決しようとする課題】本発明の目的は、本発
明は、バリア性、機械強度、柔軟性、延伸性、収縮性、
畜肉の充填作業効率、外観に優れた、畜肉包装用多層フ
ィルムを得ることである。
SUMMARY OF THE INVENTION An object of the present invention is to provide a barrier, mechanical strength, flexibility, stretchability, shrinkage,
An object of the present invention is to obtain a multi-layer film for packaging meat, which is excellent in meat filling work efficiency and appearance.

【0009】[0009]

【課題を解決するための手段】上記目的は、エチレン含
有量20〜60モル%、ビニルエステル成分のケン化度
が85%以上のエチレン−ビニルアルコール共重合体
(A)50〜95重量%、ポリアミド樹脂(B)0.2
〜25重量%およびエチレン−不飽和カルボン酸共重合
体またはその金属塩(C)0.5〜40重量%からなる
樹脂組成物層、または、エチレン含有量20〜60モル
%、ビニルエステル成分のケン化度が85%以上のエチ
レン−ビニルアルコール共重合体(A)50〜85重量
%、ポリアミド樹脂(B)0.2〜25重量%、エチレ
ン−不飽和カルボン酸共重合体またはその金属塩(C)
0.5〜40重量%および11以下の溶解性パラメータ
ー(Fedorsの式から算出)を有する前記樹脂以外
の熱可塑性樹脂(D)0.5〜40重量%からなる樹脂
組成物層を、少なくとも1層含む畜肉包装用多層フィル
ムを用いることにより達成される。
The object of the present invention is to provide an ethylene-vinyl alcohol copolymer (A) having an ethylene content of 20 to 60% by mole and a degree of saponification of a vinyl ester component of 85% or more by 50 to 95% by weight; Polyamide resin (B) 0.2
A resin composition layer consisting of 0.5 to 25% by weight and 0.5 to 40% by weight of an ethylene-unsaturated carboxylic acid copolymer or a metal salt thereof (C), or an ethylene content of 20 to 60% by mole, Ethylene-vinyl alcohol copolymer (A) having a degree of saponification of 85% or more (A) 50 to 85% by weight, polyamide resin (B) 0.2 to 25% by weight, ethylene-unsaturated carboxylic acid copolymer or a metal salt thereof (C)
A resin composition layer consisting of 0.5 to 40% by weight and 0.5 to 40% by weight of a thermoplastic resin (D) other than the above resin having a solubility parameter (calculated from the Fedors equation) of 11 or less, This is achieved by using a multi-layer film for animal meat packaging containing layers.

【0010】本発明においては、用いられる熱可塑性樹
脂(D)の20℃における弾性モジュラスが500kg
/cm以下であることが好ましい。
In the present invention, the thermoplastic resin (D) used has an elastic modulus at 20 ° C. of 500 kg.
/ Cm 2 or less.

【0011】本発明においては、前記樹脂組成物層の両
側に、接着剤層を介することなくポリアミド樹脂からな
る層を積層することが好ましい。
In the present invention, it is preferable to laminate a layer made of a polyamide resin on both sides of the resin composition layer without interposing an adhesive layer.

【0012】本発明においては、前記樹脂組成物中のア
ルカリ金属イオン含有量が1〜35,000ppmであ
ることが好ましい。
In the present invention, the content of alkali metal ions in the resin composition is preferably 1 to 35,000 ppm.

【0013】本発明においては、前記樹脂組成物中の亜
鉛、マグネシウム、カルシウムから選択される、少なく
とも1種の金属のイオン含有量が400〜50,000
ppmであることが好ましい。
In the present invention, the ion content of at least one metal selected from zinc, magnesium and calcium in the resin composition is 400 to 50,000.
It is preferably ppm.

【0014】[0014]

【発明の実施の形態】本発明で用いられるエチレン−ビ
ニルアルコール共重合体(A)(以下、EVOHと記
す。)は、エチレンとビニルエステルからなる共重合体
をアルカリ触媒等を用いてケン化して得られる。ビニル
エステルとしては酢酸ビニルが代表的なものとして挙げ
られるが、その他の脂肪酸ビニルエステル(プロピオン
酸ビニル、ピバリン酸ビニルなど)も使用できる。ま
た、EVOHは共重合成分としてビニルシラン化合物
0.0002〜0.2モル%を含有することができる。
ここで、ビニルシラン系化合物としては、たとえば、ビ
ニルトリメトキシシラン、ビニルトリエトキシシラン、
ビニルトリ(β−メトキシ−エトキシ)シラン、γ−メ
タクリルオキシプロピルメトキシシランが挙げられる。
なかでも、ビニルトリメトキシシラン、ビニルトリエト
キシシランが好適に用いられる。さらに、本発明の目的
が阻害されない範囲で、他の共単量体、例えば、プロピ
レン、ブチレン、あるいは(メタ)アクリル酸、(メ
タ)アクリル酸メチル、(メタ)アクリル酸エチルなど
の不飽和カルボン酸又はそのエステル、およびN−ビニ
ルピロリドンなどのビニルピロリドンを共重合すること
も出来る。
BEST MODE FOR CARRYING OUT THE INVENTION The ethylene-vinyl alcohol copolymer (A) (hereinafter referred to as EVOH) used in the present invention is obtained by saponifying a copolymer comprising ethylene and vinyl ester using an alkali catalyst or the like. Obtained. A typical example of the vinyl ester is vinyl acetate, but other fatty acid vinyl esters (such as vinyl propionate and vinyl pivalate) can also be used. EVOH can contain 0.0002 to 0.2 mol% of a vinylsilane compound as a copolymerization component.
Here, as the vinylsilane-based compound, for example, vinyltrimethoxysilane, vinyltriethoxysilane,
Vinyl tri (β-methoxy-ethoxy) silane and γ-methacryloxypropylmethoxysilane.
Among them, vinyltrimethoxysilane and vinyltriethoxysilane are preferably used. Further, other comonomer such as propylene, butylene, or unsaturated carboxylic acid such as (meth) acrylic acid, methyl (meth) acrylate, ethyl (meth) acrylate and the like, as long as the object of the present invention is not hindered. Acids or esters thereof and vinylpyrrolidone such as N-vinylpyrrolidone can also be copolymerized.

【0015】本発明に用いられるEVOH(A)のエチ
レン含量は20〜60モル%であり、好適には25〜5
5モル%、より好適には25〜50モル%である。エチ
レン含量が20モル%未満では、高湿度下でのガスバリ
ア性が低下し溶融成形性も悪化する。また60モル%を
超えると十分なガスバリア性が得られない。
The ethylene content of EVOH (A) used in the present invention is 20 to 60 mol%, preferably 25 to 5 mol%.
It is 5 mol%, more preferably 25 to 50 mol%. If the ethylene content is less than 20 mol%, the gas barrier property under high humidity is reduced, and the melt moldability is also deteriorated. If it exceeds 60 mol%, sufficient gas barrier properties cannot be obtained.

【0016】また、本発明に用いられるEVOH(A)
のビニルエステル成分のケン化度は85%以上であり、
好適には95%以上、より好適には98%以上である。
ケン化度が85%未満では、高湿度時のガスバリア性が
低下するだけでなく、EVOHの熱安定性が悪化し、成
形物にゲルが発生しやすくなる。
The EVOH (A) used in the present invention
The degree of saponification of the vinyl ester component is 85% or more,
It is preferably at least 95%, more preferably at least 98%.
If the degree of saponification is less than 85%, not only does the gas barrier property at high humidity decrease, but also the thermal stability of EVOH deteriorates, and gels are likely to be generated in molded products.

【0017】本発明に用いられるEVOH(A)の好適
なメルトフローレート(MFR)(190℃、2160
g荷重下)は0.1〜50g/10min.、最適には
0.5〜30g/10min.である。但し、融点が1
90℃付近あるいは190℃を超えるものは2160g
荷重下、融点以上の複数の温度で測定し、片対数グラフ
で絶対温度の逆数を横軸、MFRの対数を縦軸にプロッ
トし、190℃に外挿した値で表す。これらのEVOH
樹脂は、それぞれ単独で用いることもできるし、2種以
上を混合して用いることもできる。
The preferred melt flow rate (MFR) of the EVOH (A) used in the present invention (190 ° C., 2160
g load) is 0.1 to 50 g / 10 min. , Optimally 0.5 to 30 g / 10 min. It is. However, the melting point is 1
2160g if near 90 ° C or above 190 ° C
It is measured at a plurality of temperatures above the melting point under load, and the reciprocal of the absolute temperature is plotted on the abscissa and the logarithm of the MFR is plotted on the ordinate in a semilogarithmic graph. These EVOH
The resins can be used alone or in combination of two or more.

【0018】本発明で用いられるポリアミド樹脂(B)
は、アミド結合を有する重合体であって、例えば、ポリ
カプロアミド(ナイロン−6)、ポリウンデカンアミド
(ナイロン−11)、ポリラウリルラクタム(ナイロン
−12)、ポリヘキサメチレンアジパミド(ナイロン−
6,6)、ポリヘキサメチレンセバカミド(ナイロン−
6,12)の如き単独重合体、カプロラクタム/ラウリ
ルラクタム共重合体(ナイロン−6/12)、カプロラ
クタム/アミノウンデカン酸重合体(ナイロン−6/1
1)、カプロラクタム/ω−アミノノナン酸重合体(ナ
イロン−6,9)、カプロラクタム/ヘキサメチレンジ
アンモニウムアジペート共重合体(ナイロン−6/6,
6)、カプロラクタム/ヘキサメチレンジアンモニウム
アジペート/ヘキサメチレンジアンモニウムセバケート
共重合体(ナイロン−6/6,6/6,12)、アジピ
ン酸とメタキシリレンジアミンとの重合体、あるいはヘ
キサメチレンジアミンとm,p−フタル酸との重合体で
ある芳香族系ナイロンなどが挙げられる。これらのポリ
アミド樹脂は、それぞれ単独で用いることもできるし、
2種以上を混合して用いることもできる。
The polyamide resin (B) used in the present invention
Is a polymer having an amide bond, for example, polycaproamide (nylon-6), polyundecaneamide (nylon-11), polylauryl lactam (nylon-12), polyhexamethylene adipamide (nylon-
6,6), polyhexamethylene sebacamide (nylon-
6,12), caprolactam / lauryl lactam copolymer (nylon-6 / 12), caprolactam / aminoundecanoic acid polymer (nylon-6 / 1)
1), a caprolactam / ω-aminononanoic acid polymer (nylon-6, 9), a caprolactam / hexamethylenediammonium adipate copolymer (nylon-6 / 6,
6), caprolactam / hexamethylenediammonium adipate / hexamethylenediammonium sebacate copolymer (nylon-6 / 6,6 / 6,12), polymer of adipic acid and meta-xylylenediamine, or hexamethylenediamine And aromatic nylon which is a polymer of m, p-phthalic acid and the like. Each of these polyamide resins can be used alone,
Two or more kinds may be used as a mixture.

【0019】また、ポリアミド樹脂(B)の融点は、好
ましくは、175〜240℃、より好ましくは178〜
235℃、最も好ましくは180〜230℃である。ポ
リアミド樹脂(B)の融点が240℃を超えると、延伸
性、および収縮性が低下する。 また、EVOHとポリ
アミド樹脂は高温での溶融過程で反応してゲル化するた
め、ブレンド組成物の熱劣化を抑制する点から、ポリア
ミド樹脂(B)の融点は240℃以下が好ましく、23
0℃以下であることがより好ましい。
The melting point of the polyamide resin (B) is preferably 175 to 240 ° C., more preferably 178 to 240 ° C.
235 ° C, most preferably 180-230 ° C. When the melting point of the polyamide resin (B) exceeds 240 ° C., the stretchability and the shrinkage deteriorate. Further, since the EVOH and the polyamide resin react and gel during the melting process at a high temperature, the melting point of the polyamide resin (B) is preferably 240 ° C. or less from the viewpoint of suppressing the thermal deterioration of the blend composition.
It is more preferable that the temperature is 0 ° C. or lower.

【0020】本発明に用いられるポリアミド樹脂(B)
の好適なメルトフローレート(MFR)(210℃、2
160g荷重下)は0.1〜50g/10min.、最
適には0.5〜30g/10min.である。但し、融
点が210℃付近あるいは210℃を超えるものは21
60g荷重下、融点以上の複数の温度で測定し、片対数
グラフで絶対温度の逆数を横軸、MFRの対数を縦軸に
プロットし、210℃に外挿した値で表す。
The polyamide resin (B) used in the present invention
Suitable melt flow rate (MFR) (210 ° C., 2
(Under a load of 160 g) is 0.1 to 50 g / 10 min. , Optimally 0.5 to 30 g / 10 min. It is. However, those having a melting point of around 210 ° C. or exceeding 210 ° C.
Measured at a plurality of temperatures above the melting point under a load of 60 g, the reciprocal of the absolute temperature is plotted on the horizontal axis and the logarithm of MFR is plotted on the vertical axis in a semilogarithmic graph.

【0021】本発明で用いられるエチレン−不飽和カル
ボン酸共重合体またはその金属塩(C)とは、エチレン
と不飽和カルボン酸を共重合して得られる重合体、ある
いはそのカルボン酸成分を中和して得られる金属塩のこ
とをいう。ここで、エチレンと不飽和カルボン酸がラン
ダムに共重合していることが特に好ましく、ポリエチレ
ンに不飽和カルボン酸をグラフトさせた共重合体を用い
た場合と比較して、本発明の効果を大幅に向上させるこ
とができる。ランダム共重合体またはその金属塩がグラ
フト共重合体に比べて優れている理由は、グラフト共重
合体では相容性を発揮するのに必要な高い酸含量を得る
ことが難しいためである。更に、不飽和カルボン酸、例
えば無水マレイン酸のグラフト共重合体の場合は、EV
OH中の水酸基とグラフト共重合体中のカルボキシル基
が反応するためか、ゲル・フィッシュアイが発生の原因
となるため、好ましくない場合がある。特に、長時間に
渡る溶融成形を行う場合にゲル・フィッシュアイの発生
が増加することがある。
The ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) used in the present invention refers to a polymer obtained by copolymerizing ethylene and an unsaturated carboxylic acid, or a carboxylic acid component thereof. It means a metal salt obtained by summing. Here, it is particularly preferable that ethylene and the unsaturated carboxylic acid are randomly copolymerized, and the effect of the present invention is significantly increased as compared with the case where a copolymer obtained by grafting the unsaturated carboxylic acid to polyethylene is used. Can be improved. The reason that the random copolymer or its metal salt is superior to the graft copolymer is that it is difficult to obtain a high acid content necessary for exhibiting compatibility with the graft copolymer. Further, in the case of a graft copolymer of an unsaturated carboxylic acid, for example, maleic anhydride, EV
It may not be preferable because a hydroxyl group in OH reacts with a carboxyl group in the graft copolymer or gel fisheye is generated. In particular, when melt molding is performed for a long time, the generation of gel fish eyes may increase.

【0022】不飽和カルボン酸の含有量は、好ましくは
2〜15モル%、さらに好ましくは3〜12モル%であ
る。不飽和カルボン酸としては、例えば、アクリル酸、
メタアクリル酸、エタアクリル酸、マレイン酸、マレイ
ン酸モノメチル、マレイン酸モノエチル、無水マレイン
酸などが例示され、特にアクリル酸あるいはメタアクリ
ル酸が好ましい。また、共重合体に含有されても良い他
の単量体としては、酢酸ビニル、プロピオン酸ビニルの
ようなビニルエステル、アクリル酸メチル、アクリル酸
エチル、アクリル酸イソプロピル、アクリル酸イソブチ
ル、アクリル酸n−ブチル、アクリル酸2−エチルヘキ
シル、メタアクリル酸メチル、メタアクリル酸イソブチ
ル、マレイン酸ジエチルのような不飽和カルボン酸エス
テル、一酸化炭素などが例示される。
The content of the unsaturated carboxylic acid is preferably 2 to 15 mol%, more preferably 3 to 12 mol%. As unsaturated carboxylic acids, for example, acrylic acid,
Examples thereof include methacrylic acid, ethacrylic acid, maleic acid, monomethyl maleate, monoethyl maleate, and maleic anhydride, and acrylic acid or methacrylic acid is particularly preferable. Other monomers that may be included in the copolymer include vinyl acetate, vinyl esters such as vinyl propionate, methyl acrylate, ethyl acrylate, isopropyl acrylate, isobutyl acrylate, and n-acrylate. -Butyl, 2-ethylhexyl acrylate, methyl methacrylate, isobutyl methacrylate, unsaturated maleic esters such as diethyl maleate, carbon monoxide and the like.

【0023】本発明においては、上述のようにエチレン
−不飽和カルボン酸共重合体(C)として、エチレンと
不飽和カルボン酸のランダム共重合体を用いることが特
に好適であるが、その金属塩であるアイオノマーがより
好ましく用いられる。アイオノマーの方が優れている理
由は、アイオノマーの方が極性が高くなるために、ポリ
アミド樹脂(B)に対する相容性が増すためと考えられ
る。
In the present invention, it is particularly preferable to use a random copolymer of ethylene and an unsaturated carboxylic acid as the ethylene-unsaturated carboxylic acid copolymer (C) as described above. Is more preferably used. It is considered that the reason why the ionomer is superior is that the ionomer has a higher polarity and therefore has higher compatibility with the polyamide resin (B).

【0024】エチレン−不飽和カルボン酸共重合体の金
属塩における金属イオンとしては、リチウム、ナトリウ
ム、カリウムなどのアルカリ金属、マグネシウム、カル
シウムなどのアルカリ土類金属、亜鉛などの遷移金属が
例示され、特に亜鉛を用いた場合がポリアミド樹脂に対
する相容性の点で好ましい。オレフィン−不飽和カルボ
ン酸共重合体の金属塩における中和度は、100%以
下、特に90%以下、さらに70%以下の範囲が望まし
い。中和度の下限値については、通常5%以上、特に1
0%以上、さらには30%以上が望ましい。
Examples of the metal ion in the metal salt of the ethylene-unsaturated carboxylic acid copolymer include alkali metals such as lithium, sodium and potassium, alkaline earth metals such as magnesium and calcium, and transition metals such as zinc. Particularly, the case where zinc is used is preferable in view of compatibility with the polyamide resin. The degree of neutralization of the metal salt of the olefin-unsaturated carboxylic acid copolymer is preferably 100% or less, particularly preferably 90% or less, and more preferably 70% or less. The lower limit of the degree of neutralization is usually 5% or more, especially 1%.
0% or more, more preferably 30% or more.

【0025】本発明に用いられるエチレン−不飽和カル
ボン酸共重合体またはその金属塩(C)の好適なメルト
フローレート(MFR)(190℃、2160g荷重
下)は、0.05〜50g/10分、さらに好ましくは
0.5〜30g/10分である。これらのエチレン−不
飽和カルボン酸共重合体またはその金属塩は、それぞれ
単独で用いることもできるし、2種以上を混合して用い
ることもできる。
The preferred melt flow rate (MFR) of the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) (at 190 ° C. under a load of 2160 g) used in the present invention is 0.05 to 50 g / 10. Min, more preferably 0.5 to 30 g / 10 min. These ethylene-unsaturated carboxylic acid copolymers or metal salts thereof can be used alone or in combination of two or more.

【0026】本発明で用いられる熱可塑性樹脂(D)
は、成分(A)、(B)、(C)とは異なる熱可塑性樹
脂であり、溶解性パラメーターが11以下である事が重
要である。熱可塑性樹脂(D)の溶解性パラメーターが
11を超える場合、4成分(A)、(B)、(C)、
(D)間の相容性が低下し、畜肉包装用多層フィルムの
機械強度、柔軟性、延伸性、収縮性、外観、畜肉の充填
作業効率等が著しく低下する。
The thermoplastic resin (D) used in the present invention
Is a thermoplastic resin different from the components (A), (B) and (C), and it is important that the solubility parameter is 11 or less. When the solubility parameter of the thermoplastic resin (D) exceeds 11, the four components (A), (B), (C),
The compatibility between (D) is reduced, and the mechanical strength, flexibility, stretchability, shrinkage, appearance, filling efficiency of meat, etc. of the multilayer film for meat packaging are significantly reduced.

【0027】溶解性パラメーターが11以下の熱可塑性
樹脂(D)として、ポリオレフィン系樹脂、スチレン系
樹脂、ポリ塩化ビニル系樹脂などが挙げられる。その中
でも、ポリオレフィン系樹脂が最も好ましく、高密度も
しくは低密度ポリエチレン、ポリプロピレン、ポリブテ
ン−1などのα−オレフィンの単独重合体、エチレン、
プロピレン、ブテン−1、ヘキセン−1などから選ばれ
たα−オレフィン同士の共重合体などが例示される。ま
た、α−オレフィンに以下の成分:ジオレフィン、塩化
ビニル、酢酸ビニルなどのビニル化合物、アクリル酸エ
ステル、メタクリル酸エステルなどの不飽和カルボン酸
エステルなど;を共重合したものも含まれる。また、ス
チレン系樹脂としては、ポリスチレン、アクリロニトリ
ル−ブタジエン−スチレン共重合樹脂(ABS)、アク
リロニトリル−スチレン共重合樹脂(AS)、ビニル芳
香族化合物と共役ジエン化合物の共重合体等が挙げられ
る。これらの熱可塑性樹脂は、それぞれ単独で用いるこ
ともできるし、2種以上を混合して用いることもでき
る。
Examples of the thermoplastic resin (D) having a solubility parameter of 11 or less include polyolefin-based resins, styrene-based resins, and polyvinyl chloride-based resins. Among them, polyolefin-based resins are most preferable, and high-density or low-density polyethylene, polypropylene, homopolymers of α-olefins such as polybutene-1, ethylene,
Copolymers of α-olefins selected from propylene, butene-1, hexene-1 and the like are exemplified. Further, those obtained by copolymerizing the following components with an α-olefin: diolefin, vinyl compounds such as vinyl chloride and vinyl acetate, and unsaturated carboxylic esters such as acrylic acid esters and methacrylic acid esters are also included. Examples of the styrene resin include polystyrene, acrylonitrile-butadiene-styrene copolymer resin (ABS), acrylonitrile-styrene copolymer resin (AS), and a copolymer of a vinyl aromatic compound and a conjugated diene compound. These thermoplastic resins can be used alone or in combination of two or more.

【0028】本発明においては、用いられる熱可塑性樹
脂(D)の20℃における弾性モジュラス(ASTM
D882)が500kg/cm以下であることが好ま
しい。より好適には400kg/cm以下であり、さ
らに好適には300kg/cm以下である。
In the present invention, the elastic modulus (ASTM) of the thermoplastic resin (D) used at 20 ° C.
D882) is preferably 500 kg / cm 2 or less. More preferably, it is 400 kg / cm 2 or less, and still more preferably, it is 300 kg / cm 2 or less.

【0029】本発明でいう畜肉とは、生肉の他にその加
工品、例えばハム、ソーセージ、焼豚等を含むが、この
ような不定形のものを包装する畜肉包装用多層フィルム
においては、高い柔軟性と、屈曲に対する高い耐性を有
することが好ましい。また、本発明の好適な実施態様の
一つとして、熱収縮畜肉包装用多層フィルムが挙げられ
る。このような用途においては、望ましい収縮性を得る
ために、一般的に該フィルムは延伸してから用いられ
る。しかし、延伸工程のあるプロセスでは、延伸ムラに
よる熱成形物の厚み分布不良によるガスバリア性の悪
化、更には外観不良が問題となる。そこで、良好な耐屈
曲性、延伸性を発現させるために、より小さい力で延伸
可能な低ヤング率の畜肉包装用多層フィルムが望まれて
いる。かかる要望に対し、EVOH(A)に対し熱可塑
性樹脂(D)を配合することが有効であり、熱可塑性樹
脂(D)の20℃における弾性モジュラスを500kg
/cm 以下とすることが特に有効である。
In the present invention, beef meat refers to raw meat in addition to raw meat.
Artefacts, such as ham, sausage, baked pork, etc.
Multilayer film for livestock meat packaging such as irregular shaped
Has high flexibility and high resistance to bending.
Is preferred. In addition, in a preferred embodiment of the present invention,
One example is a heat-shrinkable meat packaging multilayer film.
You. In such applications, the desired shrinkage is obtained
In general, the film is used after being stretched.
You. However, in a process with a stretching step,
Barrier property due to poor thickness distribution of thermoformed product
And furthermore, poor appearance is a problem. Therefore, good bending resistance
Stretching with smaller force to develop bendability and stretchability
Multilayer film for meat packaging with low possible Young's modulus is desired
I have. In response to such demands, thermoplastics for EVOH (A)
It is effective to mix the thermoplastic resin (D),
The elastic modulus of the fat (D) at 20 ° C. is 500 kg
/ Cm 2The following is particularly effective.

【0030】弾性モジュラスが500kg/cm以下
である熱可塑性樹脂(D)の例としては、超低密度ポリ
エチレン(VLDPE)、エチレン−酢酸ビニル共重合
体(EVA)、エチレン−メチルメタクリレート共重合
体(EMMA)、エチレン−エチルアクリレート共重合
体(EEA)、エチレン−プロピレン共重合体(EP
R)、スチレン系エラストマー(SEBS樹脂等)など
が挙げられる。
Examples of the thermoplastic resin (D) having an elastic modulus of 500 kg / cm 2 or less include very low density polyethylene (VLDPE), ethylene-vinyl acetate copolymer (EVA), and ethylene-methyl methacrylate copolymer. (EMMA), ethylene-ethyl acrylate copolymer (EEA), ethylene-propylene copolymer (EP
R), styrene-based elastomers (SEBS resin and the like) and the like.

【0031】本発明に用いられる熱可塑性樹脂(D)の
メルトフローレート(MFR)(190℃、2160g
荷重下)は、好ましくは0.05〜100g/10分、
さらに好ましくは0.05〜50g/10分、最適には
0.5〜30g/10分である。但し、融点が190℃
付近あるいは190℃を超えるものは2160g荷重
下、融点以上の複数の温度で測定し、片対数グラフで絶
対温度の逆数を横軸、MFRの対数を縦軸にプロット
し、190℃に外挿した値で表す。これらの熱可塑性樹
脂(D)は、それぞれ単独で用いることもできるし、2
種以上を混合して用いることもできる。
The thermoplastic resin (D) used in the present invention has a melt flow rate (MFR) (190 ° C., 2160 g).
Under load) is preferably 0.05 to 100 g / 10 minutes,
More preferably, it is 0.05 to 50 g / 10 minutes, and most preferably 0.5 to 30 g / 10 minutes. However, the melting point is 190 ° C
Those near or exceeding 190 ° C were measured at a plurality of temperatures above the melting point under a load of 2160 g, and the reciprocal of the absolute temperature was plotted on the abscissa and the logarithm of MFR was plotted on the ordinate in a semilogarithmic graph, and extrapolated to 190 ° C. Expressed by value. Each of these thermoplastic resins (D) can be used alone,
Mixtures of more than one species can be used.

【0032】本発明の目的は、エチレン含有量20〜6
0モル%、ケン化度85%以上のエチレン−ビニルアル
コール共重合体(A)50〜95重量%、ポリアミド樹
脂(B)0.2〜25重量%およびエチレン−不飽和カ
ルボン酸共重合体またはその金属塩(C)0.5〜40
重量%からなる樹脂組成物層を少なくとも一層含む畜肉
包装用多層フィルムを用いることにより達成され、バリ
ア性、機械強度、柔軟性、延伸性、収縮性、外観、畜肉
の充填作業効率に優れた畜肉包装用多層フィルムを得る
ことができる。中でも、かかる構成を採用する畜肉包装
用多層フィルムは高い透明性を有するため、外観におけ
る改善効果が極めて大きい。
The object of the present invention is to provide an ethylene content of 20 to 6
0 mol%, an ethylene-vinyl alcohol copolymer (A) having a saponification degree of 85% or more (A) 50 to 95% by weight, a polyamide resin (B) 0.2 to 25% by weight, and an ethylene-unsaturated carboxylic acid copolymer or The metal salt (C) 0.5-40
Meat meat which is achieved by using a multilayer film for meat packing containing at least one resin composition layer consisting of wt% and has excellent barrier properties, mechanical strength, flexibility, stretchability, shrinkage, appearance and meat filling work efficiency. A multilayer film for packaging can be obtained. Above all, since the multilayer film for meat and meat packaging employing such a configuration has high transparency, the effect of improving the appearance is extremely large.

【0033】前記樹脂組成物中のEVOH(A)の含有
量は50〜95重量%、好適には55〜90重量%、さ
らに好適には60〜85重量%である。樹脂組成物中の
EVOH(A)の含有量 が50重量%未満の場合には
本来EVOHが有しているガスバリア性が不足し、 E
VOH(A)の含有量 が95重量%を超える場合には
畜肉包装用多層フィルムの機械強度、柔軟性および延伸
性の改善効果が不充分である。
The content of EVOH (A) in the resin composition is 50 to 95% by weight, preferably 55 to 90% by weight, more preferably 60 to 85% by weight. If the content of EVOH (A) in the resin composition is less than 50% by weight, the gas barrier properties inherent in EVOH are insufficient, and
When the content of VOH (A) exceeds 95% by weight, the effects of improving the mechanical strength, flexibility and stretchability of the multilayer film for livestock meat are insufficient.

【0034】前記樹脂組成物中のポリアミド樹脂(B)
の含有量 は0.2〜25重量%、好適には0.5〜1
5重量%、さらに好適には1〜10重量%である。樹脂
組成物中のポリアミド樹脂(B)の重量比が25重量%
を超える場合には、EVOH(A)に対するポリアミド
樹脂(B)の比率が上昇するため、両者の反応によるゲ
ルが生じ易くなり、延伸性、および収縮性の改善効果が
不充分になる。また、樹脂組成物中のポリアミド樹脂
(B)の重量比が0.2重量%未満の場合には、EVO
H(A)とエチレン−不飽和カルボン酸共重合体または
その金属塩(C)の相容性が低下し、畜肉包装用多層フ
ィルムの機械強度、柔軟性、および外観の改善効果が不
充分となる。
The polyamide resin (B) in the resin composition
Is 0.2 to 25% by weight, preferably 0.5 to 1% by weight.
It is 5% by weight, more preferably 1 to 10% by weight. The weight ratio of the polyamide resin (B) in the resin composition is 25% by weight.
When the ratio exceeds the above, the ratio of the polyamide resin (B) to the EVOH (A) increases, so that a gel is easily generated by the reaction between the two, and the effect of improving stretchability and shrinkage becomes insufficient. When the weight ratio of the polyamide resin (B) in the resin composition is less than 0.2% by weight, EVO
The compatibility between H (A) and the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) decreases, and the effect of improving the mechanical strength, flexibility, and appearance of the multilayer film for livestock meat is insufficient. Become.

【0035】樹脂組成物中のエチレン−不飽和カルボン
酸共重合体またはその金属塩(C)の含有量は0.5〜
40重量%、好適には1〜35重量%、さらに好適には
2〜20重量%である。樹脂組成物中のエチレン−不飽
和カルボン酸共重合体またはその金属塩(C)の含有量
が0.5重量%未満の場合には畜肉包装用多層フィルム
の機械強度および柔軟性の改善効果が不充分となり、エ
チレン−不飽和カルボン酸共重合体またはその金属塩
(C)の含有量が40重量%を超える場合には畜肉包装
用多層フィルムのガスバリア性が不足する。
The content of the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) in the resin composition is from 0.5 to
It is 40% by weight, preferably 1 to 35% by weight, more preferably 2 to 20% by weight. If the content of the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) in the resin composition is less than 0.5% by weight, the effect of improving the mechanical strength and flexibility of the multilayer film for livestock meat packaging is reduced. If the content becomes insufficient and the content of the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) exceeds 40% by weight, the gas barrier properties of the multilayer film for meat and meat packaging will be insufficient.

【0036】また、本発明の目的は、エチレン含有量2
0〜60モル%、ケン化度85%以上のエチレン−ビニ
ルアルコール共重合体(A)50〜95重量%、ポリア
ミド樹脂(B)0.2〜25重量%、エチレン−不飽和
カルボン酸共重合体またはその金属塩(C)0.5〜4
0重量%および11以下の溶解性パラメーター(Fed
orsの式から算出)を有する前記樹脂以外の熱可塑性
樹脂(D)0.5〜45重量%からなる樹脂組成物層
を、少なくとも1層含む畜肉包装用多層フィルムを用い
ることによっても達成される。熱可塑性樹脂(D)が樹
脂組成物中に添加されることにより、透明性が若干低下
するため、外観における改善効果はやや減じられるが、
得られる畜肉包装用多層フィルムの外観は充分に実用に
供しうるものであり、また、熱可塑性樹脂(D)を含有
することにより、本発明における機械強度、柔軟性、延
伸性の改善効果をさらに向上させることができる。
The object of the present invention is to provide an ethylene content of 2
0 to 60 mol%, ethylene-vinyl alcohol copolymer having a saponification degree of 85% or more (A) 50 to 95% by weight, polyamide resin (B) 0.2 to 25% by weight, ethylene-unsaturated carboxylic acid copolymer Combined or its metal salt (C) 0.5-4
0% by weight and a solubility parameter of less than 11 (Fed
(calculated from the ors formula) can be achieved by using a multi-layer film for livestock meat containing at least one resin composition layer composed of 0.5 to 45% by weight of a thermoplastic resin (D) other than the resin having the above-mentioned resin. . When the thermoplastic resin (D) is added to the resin composition, the transparency is slightly reduced, so that the effect of improving the appearance is slightly reduced.
The appearance of the obtained multi-layer film for livestock meat packaging can sufficiently be put to practical use, and by containing the thermoplastic resin (D), the effect of improving the mechanical strength, flexibility and stretchability in the present invention can be further improved. Can be improved.

【0037】前記樹脂組成物中の熱可塑性樹脂(D)の
含有量は0.5〜45重量%、好適には5〜40重量
%、さらに好適には10〜30重量%である。樹脂組成
物中の熱可塑性樹脂(D)の含有量 が0.5重量%未
満の場合には畜肉包装用多層フィルムの機械強度、柔軟
性および延伸性の改善効果が不充分であり、 熱可塑性
樹脂(D)の含有量 が45重量%を超える場合には畜
肉包装用多層フィルムのガスバリア性が不足する。
The content of the thermoplastic resin (D) in the resin composition is 0.5 to 45% by weight, preferably 5 to 40% by weight, more preferably 10 to 30% by weight. When the content of the thermoplastic resin (D) in the resin composition is less than 0.5% by weight, the effect of improving the mechanical strength, flexibility and stretchability of the multilayer film for livestock meat is insufficient. When the content of the resin (D) is more than 45% by weight, the gas barrier property of the multilayer film for livestock meat is insufficient.

【0038】本発明に用いられる樹脂組成物中に含まれ
るアルカリ金属イオンの添加方法としては、特に限定さ
れるものではないが、塩化リチウム、塩化カリウム、酢
酸カリウム、塩化ナトリウム等を、あらかじめEVOH
や他の樹脂とドライブレンドした後溶融する方法などが
挙げられる。中でも、EVOH生産時のケン化工程で副
生成する酢酸ナトリウムを用いることが、生産性および
コスト的に好ましい。
The method for adding the alkali metal ion contained in the resin composition used in the present invention is not particularly limited, but lithium chloride, potassium chloride, potassium acetate, sodium chloride and the like are previously added to EVOH.
And a method of dry blending with another resin and then melting. Among them, it is preferable to use sodium acetate by-produced in the saponification step at the time of EVOH production in terms of productivity and cost.

【0039】本発明に用いられる樹脂組成物中に含まれ
る好適なアルカリ金属イオンの含有量は1〜35,00
0ppmであり、さらに好ましくは2〜20,000p
pm、最も好ましくは3〜10,000ppmである。
アルカリ金属イオンを添加することにより、本発明の畜
肉包装フィルムの延伸性および収縮性が更に向上する
が、樹脂組成物中のアルカリ金属イオン含有量が35,
000ppmを超えた場合、着色し易くなり外観に悪影
響を及ぼす。
The preferred content of the alkali metal ion contained in the resin composition used in the present invention is from 1 to 35,00
0 ppm, more preferably 2 to 20,000 p
pm, most preferably 3 to 10,000 ppm.
By adding the alkali metal ion, the stretchability and shrinkage of the meat packaging film of the present invention are further improved, but the alkali metal ion content in the resin composition is 35,
If it exceeds 000 ppm, the coloring becomes easy and the appearance is adversely affected.

【0040】一方、樹脂組成物中に含まれる、亜鉛、マ
グネシウム、カルシウムから選択される、少なくとも1
種の金属のイオンの含有量は、400〜50,000p
pmであることが好ましく、450〜30,000pp
m、さらに好ましくは500〜10,000ppmであ
り、最も好ましくは1,000〜7,000ppmであ
る。亜鉛、マグネシウム、カルシウムから選択される、
少なくとも1種の金属のイオンを含有することにより、
本発明の畜肉包装フィルムの機械的強度、柔軟性および
外観の改善効果がさらに向上する。しかし、亜鉛、マグ
ネシウム、カルシウムから選択される、少なくとも1種
の金属のイオンの含有量が50,000ppmを超えた
場合、機械強度が悪化し、しかも延伸性も悪化する。亜
鉛、マグネシウム、カルシウムから選択される、少なく
とも1種の金属のイオンの添加方法としては、組成物中
に酢酸カルシウム、ステアリン酸カルシウム、塩化カル
シウム、酢酸マグネシウム、ステアリン酸マグネシウ
ム、塩化マグネシウム、酢酸亜鉛、ステアリ酸亜鉛、塩
化亜鉛等の金属塩を直接添加する方法もあるが、エチレ
ン−不飽和カルボン酸共重合体の亜鉛、マグネシウム、
カルシウムの金属塩を予め用意し、これを組成物の成分
として用いることもできる。
On the other hand, at least one selected from zinc, magnesium and calcium contained in the resin composition
The species metal ion content is 400-50,000p
pm, preferably from 450 to 30,000 pp
m, more preferably from 500 to 10,000 ppm, most preferably from 1,000 to 7,000 ppm. Selected from zinc, magnesium, calcium,
By containing at least one metal ion,
The effect of improving the mechanical strength, flexibility and appearance of the meat packaging film of the present invention is further improved. However, when the content of the ion of at least one metal selected from zinc, magnesium and calcium exceeds 50,000 ppm, the mechanical strength deteriorates and the stretchability also deteriorates. As a method for adding at least one metal ion selected from zinc, magnesium, and calcium, the composition may contain calcium acetate, calcium stearate, calcium chloride, magnesium acetate, magnesium stearate, magnesium chloride, zinc acetate, stearate. Zinc acid, a method of directly adding a metal salt such as zinc chloride, but zinc, magnesium, ethylene-unsaturated carboxylic acid copolymer,
A calcium metal salt may be prepared in advance and used as a component of the composition.

【0041】各樹脂組成物は、通常の溶融混練装置によ
り各成分を溶融混練することにより容易に得ることがで
きる。ブレンドする方法に関しては、特に限定されるも
のではないが、EVOH(A)、ポリアミド樹脂
(B)、エチレン−不飽和カルボン酸共重合体またはそ
の金属塩(C)、必要に応じて熱可塑性樹脂(D)を同
時に単軸または二軸スクリュー押出機などでペレット化
し乾燥する方法、あるいはまず最初にポリアミド樹脂
(B)とエチレン−不飽和カルボン酸共重合体またはそ
の金属塩(C)を溶融混合−冷却−ペレット化した後、
EVOH(A)、必要に応じて熱可塑性樹脂(D)にド
ライブレンドし、単軸または二軸スクリュー押出機など
でペレット化し乾燥する方法等があげられる。
Each of the resin compositions can be easily obtained by melt-kneading the components with a usual melt-kneading apparatus. The method of blending is not particularly limited, but EVOH (A), polyamide resin (B), ethylene-unsaturated carboxylic acid copolymer or its metal salt (C), if necessary, thermoplastic resin A method in which (D) is simultaneously pelletized and dried with a single-screw or twin-screw extruder or the like, or first, a polyamide resin (B) and an ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) are melt-mixed. -After cooling-pelletizing,
A method of dry blending the EVOH (A) with the thermoplastic resin (D) if necessary, and pelletizing and drying with a single screw or twin screw extruder, etc.

【0042】なかでも、後述する実施例で示されている
ように、まず最初に、ポリアミド樹脂(B)とオレフィ
ン−不飽和カルボン酸共重合体(C)とを溶融混合し、
造粒・乾燥してから、 EVOH(A)単独、あるいは
EVOHと熱可塑性樹脂(D)にドライブレンドし、単
軸または二軸スクリュー押出機などで造粒し、乾燥する
方法が好ましい。この理由として、各成分を同時に溶融
混練する場合は、相容性の良い成分同士(例えば、EV
OH(A)とポリアミド樹脂(B))の混合が優先して
進む場合があるために、3成分あるいは4成分からなる
樹脂組成物のモルフォロジーを安定に制御することが難
しいことがある。しかしながら、ポリアミド樹脂(B)
とオレフィン−不飽和カルボン酸共重合体(C)とのブ
レンド物を予め作製しておくことにより、溶融混合時の
条件にあまり影響を受けずに、モルフォロジーの安定し
た3成分または4成分からなる樹脂組成物を得ることが
できる。特に、この効果は熱可塑性樹脂(D)をブレン
ドする4成分からなる樹脂組成物において顕著であり、
安定したEVOH(A)と熱可塑性樹脂(D)との相容
化効果を得ることが可能である。
In particular, as shown in Examples described later, first, the polyamide resin (B) and the olefin-unsaturated carboxylic acid copolymer (C) are melt-mixed,
After granulation and drying, a method is preferable in which EVOH (A) is used alone, or EVOH and a thermoplastic resin (D) are dry-blended, granulated by a single screw or twin screw extruder, and dried. The reason for this is that when components are simultaneously melt-kneaded, components having good compatibility (for example, EV
Since the mixing of the OH (A) and the polyamide resin (B)) may proceed preferentially, it may be difficult to stably control the morphology of the resin composition composed of three or four components. However, polyamide resin (B)
And a olefin-unsaturated carboxylic acid copolymer (C) are prepared in advance so that the morphologically stable three-component or four-component compound is obtained without being greatly affected by the conditions at the time of melt mixing. A resin composition can be obtained. In particular, this effect is remarkable in a resin composition composed of four components in which the thermoplastic resin (D) is blended,
It is possible to obtain a stable compatibilizing effect between the EVOH (A) and the thermoplastic resin (D).

【0043】なお、溶融配合操作においては、ブレンド
が不均一になったり、ゲル、ブツが発生、混入したりす
る可能性があるので、ブレンドペレット化はなるべく混
練度の高い押出機を使用し、ホッパー口を窒素ガスでシ
ールし、低温で押出しすることが望ましい。
In the melt compounding operation, there is a possibility that the blend becomes non-uniform, and gels and lumps are generated and mixed. Therefore, an extruder having a high degree of kneading is used for the blend pelletizing. It is desirable to seal the hopper port with nitrogen gas and extrude at a low temperature.

【0044】EVOH(A)とポリアミド樹脂(B)が
反応することによるEVOHの熱劣化を防ぐ観点から、
本発明に用いる樹脂組成物には、高級脂肪族カルボン酸
の金属塩およびハイドロタルサイト化合物の少なくとも
1種を含有させることが好ましい。
From the viewpoint of preventing thermal degradation of EVOH due to reaction between EVOH (A) and polyamide resin (B),
The resin composition used in the present invention preferably contains at least one of a metal salt of a higher aliphatic carboxylic acid and a hydrotalcite compound.

【0045】ここで、ハイドロタルサイト化合物として
は特にMAl(OH)2x+3 y−2z(A)
aHO(MはMg、CaまたはZn、AはCOまた
はHPO、x、y、z、aは正数)で示される複塩で
あるハイドロタルサイト化合物を挙げることができ、こ
のようなもので、特に好適なものとして次のようなもの
が例示される。
Here, as the hydrotalcite compound, in particular, M x Al y (OH) 2x + 3 y-2z (A) z ·
A hydrotalcite compound which is a double salt represented by aH 2 O (M is Mg, Ca or Zn, A is CO 3 or HPO 4 , x, y, z, and a is a positive number) can be mentioned. In particular, the following are exemplified as particularly preferable ones.

【0046】 MgAl(OH)16CO・4HO MgAl(OH)20CO・5HO MgAl(OH)14CO・4HO Mg10Al(OH)22(CO・4HO MgAl(OH)16HPO・4HO CaAl(OH)16CO・4HO ZnAl(OH)16CO・4HO Mg4.5Al(OH)13CO・3.5H[0046] Mg 6 Al 2 (OH) 16 CO 3 · 4H 2 O Mg 8 Al 2 (OH) 20 CO 3 · 5H 2 O Mg 5 Al 2 (OH) 14 CO 3 · 4H 2 O Mg 10 Al 2 ( OH) 22 (CO 3) 2 · 4H 2 O Mg 6 Al 2 (OH) 16 HPO 4 · 4H 2 O Ca 6 Al 2 (OH) 16 CO 3 · 4H 2 O Zn 6 Al 6 (OH) 16 CO 3 .4H 2 O Mg 4.5 Al 2 (OH) 13 CO 3 .3.5H 2 O

【0047】また、ハイドロタルサイト化合物として、
特開平1−308439号(USP4954557)に
記載されているハイドロタルサイト系固溶体である、
[Mg 0.75Zn0.250.67Al
0.33(OH)(CO0.167・0.45H
Oのようなものも用いることができる。
Further, as the hydrotalcite compound,
JP-A-1-308439 (US Pat. No. 4,954,557)
The hydrotalcite-based solid solution described,
[Mg 0.75Zn0.25]0.67Al
0.33(OH)2(CO3)0.167・ 0.45H
2Something like O can also be used.

【0048】高級脂肪族カルボン酸の金属塩とは炭素数
8〜22の高級脂肪酸の金属塩であり、炭素数8〜22
の高級脂肪酸としては、ラウリン酸、ステアリン酸、ミ
リスチン酸などがあげられ、また金属としては、ナトリ
ウム、カリウム、マグネシウム、カルシウム、亜鉛、バ
リウム、アルミニウムなどがあげられる。このうちマグ
ネシウム、カルシウム、バリウム等のアルカリ土類金属
が好適である。
The metal salt of a higher aliphatic carboxylic acid is a metal salt of a higher fatty acid having 8 to 22 carbon atoms.
Examples of higher fatty acids include lauric acid, stearic acid, and myristic acid, and examples of metals include sodium, potassium, magnesium, calcium, zinc, barium, and aluminum. Of these, alkaline earth metals such as magnesium, calcium and barium are preferred.

【0049】これらの高級脂肪族カルボン酸の金属塩お
よびハイドロタルサイト化合物の含有量は、樹脂組成物
の合計重量に対して0.01〜3重量部が好ましく、よ
り好適には0.05〜2.5重量部である。
The content of the metal salt of these higher aliphatic carboxylic acids and the hydrotalcite compound is preferably 0.01 to 3 parts by weight, more preferably 0.05 to 3 parts by weight, based on the total weight of the resin composition. 2.5 parts by weight.

【0050】また、本発明に用いられる樹脂組成物に
は、上記の樹脂成分の他に適切な添加剤(例えば、熱安
定剤、可塑剤、紫外線吸収剤、酸化防止剤、着色剤、フ
ィラー、他の樹脂など)を本発明の目的が阻害されない
範囲で使用することは自由である。
The resin composition used in the present invention may contain, in addition to the above resin components, appropriate additives (for example, heat stabilizer, plasticizer, ultraviolet absorber, antioxidant, coloring agent, filler, It is free to use other resins and the like as long as the object of the present invention is not hindered.

【0051】本発明の多層フィルムを得る方法として
は、特に限定されるものではない。一般のポリオレフィ
ン等の分野で実施されている成形方法、例えば、Tダイ
成形、インフレーション成形、ドライラミネート成形、
押出コーティング、共押出成形などの方法が採用でき
る。中でも、各々の樹脂を押出機で溶融させ、丸ダイま
たはTダイより多層で吐出・冷却する共押出成形による
方法が工程を簡略化でき、製造コストを抑えられる面か
らも好ましい。成形温度は170〜270℃の範囲で選
ぶことが多い。また、これらの成形方法を組み合わせ
て、共押出成形にて特定の構成のフィルムを作製後、さ
らにドライラミネート成形を行って、多層フィルムを得
る方法も採用できる。
The method for obtaining the multilayer film of the present invention is not particularly limited. Molding methods practiced in the field of general polyolefins, for example, T-die molding, inflation molding, dry laminate molding,
Methods such as extrusion coating and coextrusion molding can be employed. Among them, a method of co-extrusion molding in which each resin is melted by an extruder and discharged and cooled in multiple layers from a round die or a T-die is preferable from the viewpoint that the process can be simplified and the production cost can be suppressed. The molding temperature is often selected in the range of 170 to 270 ° C. Further, a method of obtaining a multilayer film by producing a film having a specific configuration by co-extrusion molding and then performing dry lamination molding by combining these molding methods can also be adopted.

【0052】本発明の畜肉包装用多層フィルムは他の各
種基材と2種以上の多層構成のフィルムとして使用され
るが、その厚み、構成に関しても特に限定されるもので
はない。この本発明の樹脂組成物層に隣接する熱可塑性
樹脂層としては、高密度、中密度、あるいは低密度のポ
リエチレン、酢酸ビニル、アクリル酸エステル、あるい
はブテン、ヘキセンなどのα−オレフィン類を共重合し
たポリエチレン(直鎖状低密度ポリエチレン(LLDP
E)、超低密度ポリエチレン(VLDPE)を含む)、
アイオノマー樹脂、ポリプロピレンホモポリマー、ある
いは、エチレン、ブテン、ヘキセンなどのα−オレフィ
ン類を共重合したポリプロピレン、ゴム系ポリマーをブ
レンドした変性ポリプロピレンなどのポリオレフィン
類、あるいはこれらの樹脂に無水マレイン酸を付加、あ
るいはグラフトした熱可塑性樹脂、ポリアミド系樹脂、
ポリエステル系樹脂、ポリスチレン樹脂、ポリ塩化ビニ
ル系樹脂、アクリル系樹脂、ポリウレタン系樹脂、ポリ
カーボネート樹脂、ポリ酢酸ビニル系樹脂などが挙げら
れる。この中でも、ポリアミド樹脂を用いることが特に
好ましい。
The multi-layer film for livestock meat of the present invention is used as a film having a multi-layer structure composed of at least two kinds of other base materials and two or more types, but the thickness and structure are not particularly limited. As the thermoplastic resin layer adjacent to the resin composition layer of the present invention, high-density, medium-density, or low-density polyethylene, vinyl acetate, acrylate, or copolymerized with α-olefins such as butene and hexene. Polyethylene (linear low density polyethylene (LLDP)
E), including very low density polyethylene (VLDPE)),
Ionomer resins, polypropylene homopolymers, or ethylene, butene, polyolefins such as modified polypropylene blended with rubber-based polymers, such as polypropylene copolymerized with α-olefins such as hexene, or maleic anhydride added to these resins, Or grafted thermoplastic resin, polyamide resin,
Examples include polyester resins, polystyrene resins, polyvinyl chloride resins, acrylic resins, polyurethane resins, polycarbonate resins, polyvinyl acetate resins, and the like. Among them, it is particularly preferable to use a polyamide resin.

【0053】本発明の畜肉包装用多層フィルムの具体的
構成例は、EVOH(EVOHを含む樹脂組成物)、P
A(ポリアミド樹脂)、AD(接着剤)、TR(熱可塑
性樹脂)として表記すると、TR/AD/EVOH/A
D/TR、TR/AD/EVOH/PA/AD/TR、
TR/AD/PA/EVOH/PA、TR/AD/P
A/EVOH/PA/AD/TRなどが好適なものとし
て例示される。ただし、本発明の熱成形用多層フィルム
の層構成は上記の層構成例に限定されるものではない。
両外層に熱可塑性樹脂層を設ける場合は、異なる樹脂を
用いてもよいし、同じものを用いてもよい。また、押出
成形、ブロー成形、熱成形等を行う際に発生するスクラ
ップを、熱可塑性樹脂層にブレンドしたり、別途回収層
として設けてもよい。接着性樹脂は特に限定されるもの
ではないが、不飽和カルボン酸またはその無水物(無水
マレイン酸など)をオレフィン系重合体または共重合体
(例えば、LLDPE、VLDPEなど)、エチレン−
酢酸ビニル共重合体、エチレン−(メタ)アクリル酸エ
ステル共重合体にグラフトしたものが代表的なものとし
て挙げられる。
Specific examples of the constitution of the multilayer film for meat packaging of the present invention include EVOH (resin composition containing EVOH), P
When expressed as A (polyamide resin), AD (adhesive), TR (thermoplastic resin), TR / AD / EVOH / A
D / TR, TR / AD / EVOH / PA / AD / TR,
TR / AD / PA / EVOH / PA, TR / AD / P
A / EVOH / PA / AD / TR and the like are exemplified as suitable ones. However, the layer configuration of the multilayer film for thermoforming of the present invention is not limited to the above layer configuration examples.
When a thermoplastic resin layer is provided on both outer layers, different resins may be used, or the same resin may be used. Further, scrap generated when performing extrusion molding, blow molding, thermoforming, or the like may be blended with the thermoplastic resin layer or separately provided as a recovery layer. The adhesive resin is not particularly limited, but may be an unsaturated carboxylic acid or its anhydride (such as maleic anhydride), an olefin-based polymer or copolymer (such as LLDPE, VLDPE, etc.), ethylene-
Those grafted to a vinyl acetate copolymer or an ethylene- (meth) acrylate copolymer are typical examples.

【0054】本発明の畜肉包装用多層フィルムの構成と
しては、樹脂組成物層の両側に接着剤層を介さずに直接
ポリアミド樹脂を積層すること(PA/EVOH/P
A)が特に好ましい。かかる構成を採用することによ
り、畜肉包装用多層フィルムの、延伸性、収縮性および
耐ピンホール性などに代表される機械強度の点で、大き
な改善効果が得られる。
The multilayer film for meat packaging of the present invention is constituted by directly laminating a polyamide resin on both sides of a resin composition layer without an adhesive layer (PA / EVOH / P).
A) is particularly preferred. By adopting such a configuration, a great improvement effect can be obtained in terms of mechanical strength represented by stretchability, shrinkage and pinhole resistance of the multilayer film for livestock meat packaging.

【0055】また、その少なくとも一方の側に接着剤層
を介して熱可塑性樹脂層を設けること(TR/AD/P
A/EVOH/PA)が好適であり、両側に接着剤層を
介して熱可塑性樹脂層を設けること(TR/AD/PA
/EVOH/PA/AD/TR)がさらに好適である。
Further, a thermoplastic resin layer is provided on at least one side thereof via an adhesive layer (TR / AD / P).
A / EVOH / PA) is preferable, and a thermoplastic resin layer is provided on both sides via an adhesive layer (TR / AD / PA).
/ EVOH / PA / AD / TR) are more preferred.

【0056】本発明の畜肉包装用多層フィルムは、無延
伸フィルムのままで製袋し真空包装用の畜肉包装用多層
フィルムとして用いることができる。また、本発明の樹
脂組成物層を含む多層シートを延伸し、収縮性を向上さ
せた、熱収縮畜肉包装用多層フィルムとすることができ
る。該多層シートの延伸方法としては特に限定するもの
ではないが、作製した多層シートを、EVOHの融点以
下の温度範囲で再加熱し、パンタグラフ式二軸延伸機等
で、縦方向、横方向共に少なくとも2.0倍以上延伸を
行う方法が好適である。
The multi-layer film for meat packaging of the present invention can be used as a multi-layer film for meat packaging for vacuum packaging by making a bag without stretching. Further, the multilayer sheet containing the resin composition layer of the present invention can be stretched to improve the shrinkability, thereby obtaining a multilayer film for heat shrinkable meat packaging. Although there is no particular limitation on the method for stretching the multilayer sheet, the produced multilayer sheet is reheated in a temperature range equal to or lower than the melting point of EVOH, and is subjected to at least a longitudinal direction and a lateral direction by a pantograph-type biaxial stretching machine or the like. A method of stretching 2.0 times or more is preferable.

【0057】真空包装とは、畜肉包装用多層フィルムに
畜肉を充填し、内部を脱気した後に口部をシールする包
装形式である。かかる包装形式においては、畜肉が不定
形であることから、多層フィルムには特に機械強度、柔
軟性が良好であることが要求される。また、内容物を視
認するために、フィルムの透明性が高く、外観に優れる
ことが好ましい。
The vacuum packaging is a packaging type in which meat is filled in a meat packaging multi-layer film, the inside is evacuated, and the mouth is sealed. In such a packaging format, since the meat is indefinite, the multilayer film is required to have particularly good mechanical strength and flexibility. Further, in order to visually recognize the contents, the film preferably has high transparency and excellent appearance.

【0058】熱収縮包装とは、畜肉包装用多層フィルム
に畜肉を充填し、内部を脱気して口部をシールした後
に、フィルムに熱風または熱水を吹き付けることにより
フィルムを熱収縮させる包装形式である。かかる手法を
用いることにより、フィルムが内容物と密着し、かつフ
ィルムの皺が少ない外観に優れた包装体を得ることがで
きる。熱収縮畜肉包装用フィルムは、真空包装畜肉包装
用フィルムに求められる要求性能に加えて、特に収縮性
が要求されることから、該フィルムは延伸されたものを
用いることが好ましい。
The heat shrink wrapping is a packaging method in which meat is filled in a multi-layer film for meat wrapping, the inside is evacuated, the mouth is sealed, and the film is thermally shrunk by blowing hot air or hot water on the film. It is. By using such a technique, it is possible to obtain a package in which the film adheres to the contents and has excellent appearance with less wrinkling of the film. Since the heat shrinkable meat packaging film is required to have particularly shrinkability in addition to the required performance required for the vacuum packaging meat packaging film, it is preferable to use a stretched film.

【0059】[0059]

【実施例】以下、実施例により本発明をさらに説明する
が、本発明はこの実施例に限定されるものではない。
EXAMPLES The present invention will be further described below with reference to examples, but the present invention is not limited to these examples.

【0060】以下の実施例については、以下の表1〜4
に示す樹脂を原料として用いた。ここで、表1はEVO
H(A)、表2はポリアミド樹脂(B)、表3はエチレ
ン−不飽和カルボン酸共重合体またはその金属塩
(C)、表4は熱可塑性樹脂(D)を記載した。
The following examples are shown in Tables 1 to 4 below.
Was used as a raw material. Here, Table 1 shows EVO
H (A), Table 2 describes the polyamide resin (B), Table 3 describes the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C), and Table 4 describes the thermoplastic resin (D).

【0061】[0061]

【表1】 [Table 1]

【0062】[0062]

【表2】 [Table 2]

【0063】[0063]

【表3】 [Table 3]

【0064】[0064]

【表4】 [Table 4]

【0065】(実施例1)表1〜4に示す樹脂を用い、
EVOH (A−1)85重量%、ポリアミド樹脂(B
−1)5重量%、およびエチレン−メタクリル酸共重合
体亜鉛塩(C−2)15重量%からなる畜肉包装用フィ
ルム用樹脂組成物を以下の方法で得た。すなわち、まず
ポリアミド樹脂(B−1)とエチレン−メタクリル酸共
重合体亜鉛塩(C−2)をドライブレンドした後、二軸
スクリュータイプのベント押出機に入れ、220℃で押
出しペレット化を行い、得られたブレンドペレットと、
EVOH(A−1)を再度同様の方法でブレンドし、目
的の樹脂組成物を得た。
Example 1 Using the resins shown in Tables 1 to 4,
85% by weight of EVOH (A-1), polyamide resin (B
-1) A resin composition for a meat packaging film comprising 5% by weight and 15% by weight of an ethylene-methacrylic acid copolymer zinc salt (C-2) was obtained by the following method. That is, after the polyamide resin (B-1) and the ethylene-methacrylic acid copolymer zinc salt (C-2) are dry-blended, the mixture is put into a twin-screw vent extruder, and extruded at 220 ° C. into pellets. , The resulting blended pellets,
EVOH (A-1) was blended again by the same method to obtain a target resin composition.

【0066】得られた樹脂組成物のアルカリ金属イオン
含有量および亜鉛含有量の測定は、以下の方法で行っ
た。試料とする乾燥済み樹脂組成物10gを0.01規
定の塩酸水溶液に50mlに投入し、95℃で6時間撹
拌した。撹拌後の水溶液をイオンクロマトグラフィーを
用いて定量分析し、アルカリ金属イオン含有量および亜
鉛含有量を得た。カラムは、(株)横川電機製のCIS
−C25を使用し、溶離液は5.0mMの酒石酸水溶液
と1.0mMの2,6−ピリジンジカルボン酸水溶液の
混合液とした。なお、定量に際しては各種金属の塩酸塩
水溶液(例えば、NaCl)で作製した検量線を用い
た。
The alkali metal ion content and the zinc content of the obtained resin composition were measured by the following methods. 10 g of the dried resin composition as a sample was put into 50 ml of a 0.01 N hydrochloric acid aqueous solution, and stirred at 95 ° C. for 6 hours. The aqueous solution after the stirring was quantitatively analyzed using ion chromatography to obtain an alkali metal ion content and a zinc content. The column is CIS manufactured by Yokogawa Electric Corporation.
-C25 was used, and the eluent was a mixed solution of a 5.0 mM aqueous tartaric acid solution and a 1.0 mM 2,6-pyridinedicarboxylic acid aqueous solution. In the determination, a calibration curve prepared with aqueous solutions of various metal hydrochlorides (for example, NaCl) was used.

【0067】得られた樹脂組成物、直鎖状低密度ポリエ
チレン(LLDPE){三井化学製「ウルトゼックス2
022L」、MFR=2.1g/10分(210℃、2
160g荷重)}、接着性樹脂(カルボン酸変性ポリプ
ロピレン){三井化学製「アドマーNF500」、MF
R=3.5g/10分(210℃、2160g荷
重)}、ポリアミド樹脂{宇部興産製「宇部ナイロン1
030B」}を別々の押出機に入れ、4種7層の共押出
し設備を用いて、LLDPE/接着性樹脂/ポリアミド
樹脂/樹脂組成物/ポリアミド樹脂/接着性樹脂/LL
DPE(30/8/15/15/15/8/30μm)
の構成になるように共押出して無延伸7層フィルム(全
層厚み121μm)を作製した。押出成形は、LLDP
Eを一軸スクリュー(65mmφ)を用いて220℃
で、接着樹脂を一軸スクリュー(40mmφ)を用いて
220℃で、ポリアミド樹脂を一軸スクリュー(40m
mφ)を用いて250℃で、樹脂組成物を一軸スクリュ
ー(40mmφ)を用いて220℃の温度で、それぞれ
押出すことによって行った。
The obtained resin composition, linear low-density polyethylene (LLDPE) “Ultzex 2 manufactured by Mitsui Chemicals, Inc.
022L ", MFR = 2.1 g / 10 min (210 ° C., 2
160g load), adhesive resin (carboxylic acid-modified polypropylene), "Admer NF500" manufactured by Mitsui Chemicals, MF
R = 3.5 g / 10 min (210 ° C., 2160 g load)}, polyamide resin {“Ube Nylon 1 manufactured by Ube Industries”
030B ") in separate extruders, and using four types and seven layers of coextrusion equipment, LLDPE / adhesive resin / polyamide resin / resin composition / polyamide resin / adhesive resin / LL
DPE (30/8/15/15/15/8/30 μm)
To obtain a non-stretched seven-layer film (total layer thickness: 121 μm). Extrusion molding is LLDP
E at 220 ° C. using a single screw (65 mmφ)
At 220 ° C. using a single screw (40 mmφ), the polyamide resin was mixed with a single screw (40 m).
(mφ) at 250 ° C., and the resin composition was extruded at a temperature of 220 ° C. using a single screw (40 mmφ).

【0068】得られたフィルムは、フィルムの流れ方向
およびそれに垂直な方向に垂直な面で切断し、その切断
面のEVOH(A)をヨウ素で染色し、中央付近を光学
電子顕微鏡で観察することにより、 樹脂組成物層で
は、 EVOHが連続相、その他の樹脂が分散相である
ことを確認した。
The obtained film is cut along a plane perpendicular to the flow direction of the film and a direction perpendicular thereto, the EVOH (A) on the cut surface is stained with iodine, and the vicinity of the center is observed with an optical electron microscope. As a result, it was confirmed that, in the resin composition layer, EVOH was a continuous phase and other resins were a dispersed phase.

【0069】こうして得られたフィルムを用いて、以下
の方法で低温落下強度、突刺し強度、畜肉の充填作業効
率、メルトホール、外観、バリア性を評価した。
The film thus obtained was evaluated for low-temperature drop strength, piercing strength, meat filling efficiency, melt hole, appearance, and barrier properties by the following methods.

【0070】(1)低温落下強度 低温落下強度は、得られたフィルムを用いて作製した3
0cm×50cmの袋に、5kgの骨無し肉を充填し内
部を脱気した後、口部をシールすることで得た畜肉真空
包装体を5℃−65%RHに充分調湿後、10個の包装
体を5℃の室内でコンクリート床上に1mの高さから、
袋面と床面が平行になるように落下させ、破損状況を目
視で観察し、下記の1〜5の基準に従って評価した。 5:破損が無く、商品価値が極めて大。 4:破損がほとんど無く、商品価値大。 3:ごく微小な破損はあるものの、商品価値有り。 2:破損があり、商品価値は小。 1:破損が極めて大きく、商品価値無し。
(1) Low-temperature drop strength The low-temperature drop strength was determined by using the obtained film.
After filling 5 kg of boneless meat in a bag of 0 cm × 50 cm and deaeration of the inside, the meat vacuum package obtained by sealing the mouth was sufficiently humidified at 5 ° C.-65% RH. Place the package from a height of 1m on a concrete floor in a room at 5 ° C.
The bag surface and the floor surface were dropped so as to be parallel to each other, the state of damage was visually observed, and evaluated according to the following criteria 1 to 5. 5: No damage and extremely high commercial value. 4: There is almost no damage and the commercial value is high. 3: There is commercial value, although there is very slight damage. 2: There is damage, and the commercial value is small. 1: Extremely large damage, no commercial value.

【0071】(2)突刺し強度 肉の代替品として、直径3cm、長さ35cmの杉の丸棒を
10本束ねたものを、低温落下強度評価と同様に得られ
たフィルムを用いて作製した30cm×50cmの袋に
詰め、内部を脱気した後、口部をシールすることで真空
包装体を得た。5℃−65%RHに充分調湿後、10個
の包装体を5℃の室内でコンクリート床上に1mの高さ
から、袋面と床面が平行になるように落下させ、破損状
況を目視で観察し、下記の1〜5の基準に従って評価し
た。 5:破損が無く、商品価値が極めて大。 4:破損がほとんど無く、商品価値大。 3:ごく微小な破損はあるものの、商品価値有り。 2:破損があり、商品価値は小。 1:破損が極めて大きく、商品価値は無し。
(2) Puncture Strength As a substitute for meat, a bundle of 10 round cedar rods having a diameter of 3 cm and a length of 35 cm was prepared using a film obtained in the same manner as in the evaluation of the low-temperature drop strength. After packing in a bag of 30 cm × 50 cm and degassing the inside, the mouth was sealed to obtain a vacuum package. After sufficiently adjusting the humidity to 5 ° C.-65% RH, 10 packages are dropped on a concrete floor from a height of 1 m in a room at 5 ° C. so that the bag surface and the floor surface are parallel to each other. And evaluated according to the following criteria 1 to 5. 5: No damage and extremely high commercial value. 4: There is almost no damage and the commercial value is high. 3: There is commercial value, although there is very slight damage. 2: There is damage, and the commercial value is small. 1: Extremely large damage, no commercial value.

【0072】(3)畜肉の充填作業効率 得られたフィルムを用いて作製した30cm×50cm
の袋への、5kgの骨付き肉を充填しやすさに着目して
評価した。袋が硬すぎる場合、充填の際引っかかりや破
れが生じやすく、柔らかすぎる場合、骨付き肉にまとわ
りつき、充填効率が低下する。 良 5>4>3>2>1 悪
(3) Efficiency of Filling Livestock Meat 30 cm × 50 cm prepared using the obtained film
The evaluation was made by paying attention to the ease of filling 5 kg of meat with bone into the bag. If the bag is too hard, it tends to catch or break during filling, and if it is too soft, it sticks to the meat with bone and the filling efficiency decreases. Good 5>4>3>2> 1 bad

【0073】(4)外観 外観に関しては、実際に約5kgの骨付き肉を真空包装
した畜肉真空包装体を、スジ、ムラ、しわ等に着目し
て、目視にて判定した。 良 5>4>3>2>1 悪
(4) External Appearance The external appearance was evaluated by visual observation of a meat meat vacuum package in which about 5 kg of meat with bone was vacuum-packaged, focusing on streaks, unevenness, wrinkles, and the like. Good 5>4>3>2> 1 bad

【0074】(5)バリア性 酸素透過性は、得られたフィルムを用いて作製した30
cm×50cmの袋に、5kgの骨無し牛肉を充填し内
部を脱気した後、口部をシールすることで得た10個の
畜肉真空包装体を、5℃−65%RHの恒温高湿槽に放
置し、14日後の肉の変色状態に着目し、目視にて判定
した。 良 5>4>3>2>1 悪
(5) Barrier Property The oxygen permeability was measured using the obtained film.
After filling 5 kg of boneless beef in a bag of 5 cm × 50 cm, degassing the inside, and sealing the mouth, 10 pieces of the meat meat vacuum package were obtained and kept at a constant temperature and high humidity of 5 ° C. to 65% RH. And 14 days later, the state of discoloration of the meat was noted, and visually judged. Good 5>4>3>2> 1 bad

【0075】(実施例2)実施例1で作成した樹脂組成
物と、実施例1で使用した樹脂を用いて、 LLDPE
/接着性樹脂/ポリアミド樹脂/樹脂組成物/ポリアミ
ド樹脂/接着性樹脂/LLDPEの構成を有する多層シ
ート(270/70/140/140/140/70/
270μm)を得た後、パンタグラフ式二軸延伸機を用
いて、60℃で横方向,縦方向共に3.0倍に延伸し、
LLDPE/接着性樹脂/ポリアミド樹脂/樹脂組成物
/ポリアミド樹脂/接着性樹脂/LLDPE(30/8
/15/15/15/8/30μm)の構成の延伸フィ
ルムを作成した。
(Example 2) Using the resin composition prepared in Example 1 and the resin used in Example 1, LLDPE
/ Adhesive resin / polyamide resin / resin composition / polyamide resin / adhesive resin / multilayer sheet having a structure of LLDPE (270/70/140/140/140/70 /
270 μm), and stretched 3.0 times in both the horizontal and vertical directions at 60 ° C. using a pantograph-type biaxial stretching machine.
LLDPE / adhesive resin / polyamide resin / resin composition / polyamide resin / adhesive resin / LLDPE (30/8
/ 15/15/15/8/30 μm).

【0076】得られたフィルムを用いて、実施例1と同
様の評価を行った。結果を表5に示す。ただし、実施例
2においては、低温落下強度、落下突刺強度、外観、酸
素透過性に関して、以下の方法で熱収縮包装した畜肉熱
収縮包装体を用いて評価を行った。畜肉熱収縮包装体は
次の方法で得た。すなわち、得られたフィルムを用い
て、畜肉を充填するのに支障の無い程度の大きさに作ら
れた袋に畜肉を充填し、内部を脱気した後、口部をシー
ルする。そして該包装体に90℃の熱水を5秒間噴霧
し、該包装用フィルムを熱収縮させた後、直ちに冷水を
噴霧して冷却し畜肉熱収縮包装体を得た。
The same evaluation as in Example 1 was performed using the obtained film. Table 5 shows the results. However, in Example 2, low-temperature drop strength, drop piercing strength, appearance, and oxygen permeability were evaluated using heat-shrink wrapped meat meat that was heat-shrink-packed by the following method. The meat shrink wrap was obtained by the following method. That is, using the obtained film, the meat is filled in a bag made to a size that does not hinder the filling of the meat, the inside is evacuated, and the mouth is sealed. Then, the package was sprayed with hot water of 90 ° C. for 5 seconds to thermally shrink the packaging film, and then immediately cooled by spraying with cold water to obtain a meat shrink package.

【0077】また、以下の方法で、フィルムの延伸性、
およびメルトホール発生状況を評価した。結果は表5に
示す。
The stretchability of the film is determined by the following method.
And the state of melt hole generation was evaluated. The results are shown in Table 5.

【0078】(6)延伸性 フィルムの延伸性は、延伸フィルムのスジ、ムラ、しわ
等に着目し、目視にて評価した。 良 5>4>3>2>1 悪
(6) Stretchability The stretchability of the film was evaluated by visual observation, focusing on streaks, unevenness and wrinkles of the stretched film. Good 5>4>3>2> 1 bad

【0079】(7)メルトホール発生状況 水平に張った一定面積の円形フィルムの中央に、90℃
の熱風を風速20m/min.で吹き付け、メルトホー
ル発生状況をメルトホール発生までの時間と、メルトホ
ールの拡大速度に着目し、目視にて評価した。 良 5>4>3>2>1 悪
(7) Melt hole generation state A 90 ° C.
Hot air at a wind speed of 20 m / min. Then, the state of melt hole generation was visually evaluated, focusing on the time until melt hole generation and the speed of melt hole expansion. Good 5>4>3>2> 1 bad

【0080】(実施例3〜22、 比較例1〜10)実
施例1および2で作製した使用した樹脂組成物の代わり
に、表5〜表7に記載の樹脂組成のペレットが得られる
ように樹脂種類および配合比率を変更した他は、実施例
1および2と同様にして無延伸フィルム、延伸フィルム
を作成し評価した。結果を表5〜表7に示す。なお、ア
ルカリ金属濃度が150ppm未満の樹脂組成物に関し
ては、EVOHとして、EVOH(A−1)を生産時に
洗浄回数を増加させ、ケン化工程で副生成する酢酸ナト
リウム等の金属塩を除去したものをブレンドして作製し
た。また、アルカリ金属含有量が150ppmより大き
い樹脂組成物に関しては、表5または表6に記載のアル
カリ金属含有量となるように、酢酸ナトリウムをあらか
じめEVOH(A−1)にドライブレンドしてからペレ
タイズした。一方、亜鉛含有量が4,600ppmより
大きい樹脂組成物に関しては、表5または表6に記載の
亜鉛含有量となるように、ステアリン酸亜鉛をあらかじ
めエチレン−不飽和カルボン酸共重合体の亜鉛塩(C−
1)にドライブレンドしてからペレタイズした。
(Examples 3 to 22, Comparative Examples 1 to 10) Instead of the resin compositions used in Examples 1 and 2, pellets having the resin compositions shown in Tables 5 to 7 were obtained. A non-stretched film and a stretched film were prepared and evaluated in the same manner as in Examples 1 and 2, except that the resin type and the mixing ratio were changed. The results are shown in Tables 5 to 7. In addition, as for the resin composition having an alkali metal concentration of less than 150 ppm, EVOH (A-1) is used as an EVOH in which the number of washings is increased during production and metal salts such as sodium acetate by-produced in the saponification step are removed. Was blended. For the resin composition having an alkali metal content of more than 150 ppm, sodium acetate was previously dry-blended with EVOH (A-1) so that the alkali metal content shown in Table 5 or Table 6 was obtained, and then pelletized. did. On the other hand, with respect to the resin composition having a zinc content of more than 4,600 ppm, zinc stearate was previously added to the zinc salt of the ethylene-unsaturated carboxylic acid copolymer so that the zinc content shown in Table 5 or Table 6 was obtained. (C-
Pelletized after dry blending in 1).

【0081】[0081]

【表5】 [Table 5]

【0082】[0082]

【表6】 [Table 6]

【0083】[0083]

【表7】 [Table 7]

【0084】実施例1〜10の3成分系および実施例1
1〜22の4成分系の多層フィルムは、無延伸、延伸共
に優れた効果を発揮している。3成分系の多層フィルム
は、4成分系の多層フィルムよりやや外観とバリア性に
優れており、4成分系の多層フィルムは、3成分系の多
層フィルムより、やや強度の点で優れている。他方でポ
リアミド樹脂(B)又はエチレン−不飽和カルボン酸共
重合体又はその金属塩(C)を欠く比較例の多層フィル
ムは、いずれも強度も弱く、外観もあまりよくなかっ
た。
The three-component system of Examples 1 to 10 and Example 1
The four-component multilayer films of Nos. 1 to 22 exhibit excellent effects in both non-stretching and stretching. The three-component multilayer film is slightly superior in appearance and barrier properties to the four-component multilayer film, and the four-component multilayer film is slightly superior in strength to the three-component multilayer film. On the other hand, the multilayer films of Comparative Examples lacking the polyamide resin (B) or the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) were all weak in strength and not very good in appearance.

【0085】(実施例23)実施例1で作製した樹脂組
成物、および実施例1で使用したLLDPE、接着性樹
脂を別々の押出機に入れ、3種5層の共押出し設備を用
いて、 LLDPE/接着性樹脂/樹脂組成物/接着性
樹脂/LLDPE(45/8/15/8/45μm)の
構成になるように共押出して得た無延伸5層フィルム
(全層厚み121μm)に関して、実施例1と同様の評
価を行った。結果を表8に示す。
(Example 23) The resin composition prepared in Example 1, the LLDPE used in Example 1, and the adhesive resin were put into separate extruders, and three types and five layers of coextrusion equipment were used. Regarding a non-stretched five-layer film (total layer thickness 121 μm) obtained by co-extrusion to have a structure of LLDPE / adhesive resin / resin composition / adhesive resin / LLDPE (45/8/15/8/45 μm) The same evaluation as in Example 1 was performed. Table 8 shows the results.

【0086】(実施例24)実施例1で作製した樹脂組
成物、および実施例1で使用した、LLDPE、接着性
樹脂を用いて、 LLDPE/接着性樹脂/樹脂組成物
/接着性樹脂/LLDPE(405/70/135/7
0/405μm)の多層シートを得た後、パンタグラフ
式二軸延伸機を用いて、60℃で横方向,縦方向共に
3.0倍に延伸して得た、 LLDPE/接着性樹脂/
樹脂組成物/接着性樹脂/LLDPE(45/8/15
/8/45μm)の延伸5層フィルムに関して、実施例
2と同様の評価を行った。結果を表8に示す。
Example 24 Using the resin composition prepared in Example 1 and the LLDPE and adhesive resin used in Example 1, LLDPE / adhesive resin / resin composition / adhesive resin / LLDPE (405/70/135/7
0/405 μm), and stretched 3.0 times in both the horizontal and vertical directions at 60 ° C. using a pantograph-type biaxial stretching machine. LLDPE / adhesive resin /
Resin composition / adhesive resin / LLDPE (45/8/15
/ 8/45 μm) was evaluated in the same manner as in Example 2. Table 8 shows the results.

【0087】(実施例25)樹脂組成物として、実施例
11で作製したものを用いた以外は、実施例23と同様
にして無延伸5層フィルムを得て、実施例1と同様の評
価を行った。結果を表8に示す。
(Example 25) An unstretched five-layer film was obtained in the same manner as in Example 23 except that the resin composition prepared in Example 11 was used, and the same evaluation as in Example 1 was performed. went. Table 8 shows the results.

【0088】(実施例26)樹脂組成物として、実施例
11で作製したものを用いた以外は、実施例24と同様
にして延伸5層フィルムを得て、実施例1と同様の評価
を行った。結果を表8に示す。
Example 26 A stretched five-layer film was obtained in the same manner as in Example 24 except that the resin composition prepared in Example 11 was used, and the same evaluation as in Example 1 was performed. Was. Table 8 shows the results.

【0089】[0089]

【表8】 [Table 8]

【0090】本発明で用いる樹脂組成物を有する多層フ
ィルムは、層構成を変えても優れた外観とバリア性を有
しており、落下強度、突刺し強度等もかなりよいもので
あった。
The multilayer film having the resin composition used in the present invention had excellent appearance and barrier properties even when the layer structure was changed, and also had excellent drop strength and piercing strength.

【0091】[0091]

【発明の効果】エチレン含有量20〜60モル%、ビニ
ルエステル成分のケン化度が85%以上のエチレン−ビ
ニルアルコール共重合体(A)50〜95重量%、ポリ
アミド樹脂(B)0.2〜25重量%およびエチレン−
不飽和カルボン酸共重合体またはその金属塩(C)0.
5〜40重量%からなる樹脂組成物層、または、エチレ
ン含有量20〜60モル%、ビニルエステル成分のケン
化度が85%以上のエチレン−ビニルアルコール共重合
体(A)50〜85重量%、ポリアミド樹脂(B)0.
2〜25重量%、エチレン−不飽和カルボン酸共重合体
またはその金属塩(C)0.5〜40重量%および11
以下の溶解性パラメーター(Fedorsの式から算
出)を有する前記樹脂以外の熱可塑性樹脂(D)0.5
〜40重量%からなる樹脂組成物層を、少なくとも1層
含む多層フィルムは、バリア性、機械強度、柔軟性、延
伸性、収縮性、畜肉の充填作業効率、外観に優れた、畜
肉包装用多層フィルムとして有用である。
According to the present invention, an ethylene-vinyl alcohol copolymer (A) having an ethylene content of 20 to 60 mol% and a saponification degree of a vinyl ester component of 85% or more is 50 to 95% by weight, and a polyamide resin (B) 0.2. ~ 25% by weight and ethylene-
Unsaturated carboxylic acid copolymer or its metal salt (C)
5 to 40% by weight of a resin composition layer, or 50 to 85% by weight of an ethylene-vinyl alcohol copolymer (A) having an ethylene content of 20 to 60% by mole and a vinyl ester component having a saponification degree of 85% or more. , Polyamide resin (B)
2 to 25% by weight, 0.5 to 40% by weight of the ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) and 11
Thermoplastic resin (D) 0.5 other than the above resin having the following solubility parameter (calculated from Fedors equation):
The multilayer film containing at least one resin composition layer consisting of up to 40% by weight has excellent barrier properties, mechanical strength, flexibility, stretchability, shrinkage, meat filling work efficiency, and appearance, and is a multilayer for meat packaging. Useful as a film.

───────────────────────────────────────────────────── フロントページの続き (51)Int.Cl.7 識別記号 FI テーマコート゛(参考) C08L 77:00 23:08 101:12) Fターム(参考) 3E086 AD01 AD16 AD19 BA04 BA15 BB01 BB66 BB67 BB85 BB90 CA04 CA22 4F100 AK01A AK01K AK07 AK46 AK46A AK46B AK46C AK63 AK69A AK69K AK70A AL05A AL05K AL07 AT00B AT00C BA03 BA06 BA44 CB03 EH20 GB23 JB16A JB16K JD01 JK07A JK08 JL01 YY00A 4J002 BB004 BB034 BB054 BB064 BB074 BB082 BB092 BB104 BB124 BB144 BB154 BB164 BB174 BB184 BB221 BB232 BC024 BC034 BC054 BC064 BD034 BE031 BH022 BN154 CL003 CL013 CL033 CL053 DD066 DD076 EG036 EG046 FD070 GF00 GG02 ──────────────────────────────────────────────────続 き Continued on the front page (51) Int.Cl. 7 Identification symbol FI Theme coat ゛ (Reference) C08L 77:00 23:08 101: 12) F-term (Reference) 3E086 AD01 AD16 AD19 BA04 BA15 BB01 BB66 BB67 BB85 BB90 CA04 CA22 4F100 AK01A AK01K AK07 AK46 AK46A AK46B AK46C AK63 AK69A AK69K AK70A AL05A AL05K AL07 AT00B AT00C BA03 BA06 BA44 CB03 EH20 GB23 JB16A JB16K JD01 JK07A JK08 JL01 YY00A 4J002 BB004 BB034 BB054 BB064 BB074 BB082 BB092 BB104 BB124 BB144 BB154 BB164 BB174 BB184 BB221 BB232 BC024 BC034 BC054 BC064 BD034 BE031 BH022 BN154 CL003 CL013 CL033 CL053 DD066 DD076 EG036 EG046 FD070 GF00 GG02

Claims (7)

【特許請求の範囲】[Claims] 【請求項1】 エチレン含有量20〜60モル%、ビニ
ルエステル成分のケン化度が85%以上のエチレン−ビ
ニルアルコール共重合体(A)50〜95重量%、ポリ
アミド樹脂(B)0.2〜25重量%およびエチレン−
不飽和カルボン酸共重合体またはその金属塩(C)0.
5〜40重量%からなる樹脂組成物層を、少なくとも1
層含む畜肉包装用多層フィルム。
1. An ethylene-vinyl alcohol copolymer (A) having an ethylene content of 20 to 60 mol% and a degree of saponification of a vinyl ester component of 85% or more, 50 to 95% by weight, and a polyamide resin (B) 0.2. ~ 25% by weight and ethylene-
Unsaturated carboxylic acid copolymer or its metal salt (C)
5 to 40% by weight of a resin composition layer,
Multilayer film for meat packaging including layers.
【請求項2】 エチレン含有量20〜60モル%、ビニ
ルエステル成分のケン化度が85%以上のエチレン−ビ
ニルアルコール共重合体(A)50〜85重量%、ポリ
アミド樹脂(B)0.2〜25重量%、エチレン−不飽
和カルボン酸共重合体またはその金属塩(C)0.5〜
40重量%および11以下の溶解性パラメーター(Fe
dorsの式から算出)を有する前記樹脂以外の熱可塑
性樹脂(D)0.5〜45重量%からなる樹脂組成物層
を、少なくとも1層含む畜肉包装用多層フィルム。
2. An ethylene-vinyl alcohol copolymer (A) having an ethylene content of 20 to 60 mol% and a saponification degree of a vinyl ester component of 85% or more, 50 to 85% by weight, and a polyamide resin (B) 0.2. -25% by weight, ethylene-unsaturated carboxylic acid copolymer or its metal salt (C) 0.5-
40% by weight and a solubility parameter of less than 11 (Fe
A multi-layer film for livestock meat packaging, comprising at least one resin composition layer composed of 0.5 to 45% by weight of a thermoplastic resin (D) other than the resin having the following formula (calculated from dors formula).
【請求項3】 前記熱可塑性樹脂(D)の20℃におけ
る弾性モジュラスが500kg/cm以下である請求
項2記載の畜肉包装用多層フィルム。
3. The multilayer film for meat packaging according to claim 2, wherein the elastic modulus of the thermoplastic resin (D) at 20 ° C. is 500 kg / cm 2 or less.
【請求項4】 前記樹脂組成物層の両側に、接着剤層を
介することなく直接ポリアミド樹脂からなる層を積層す
ることを特徴とする請求項1ないし3のいずれかに記載
の畜肉包装用多層フィルム。
4. The multi-layered meat packaging according to claim 1, wherein a layer made of a polyamide resin is directly laminated on both sides of the resin composition layer without interposing an adhesive layer. the film.
【請求項5】 前記樹脂組成物中のアルカリ金属イオン
含有量が1〜35,000ppmである請求項1ないし
4のいずれかに記載の畜肉包装用多層フィルム。
5. The multilayer film for meat and meat packaging according to claim 1, wherein the content of alkali metal ions in the resin composition is 1 to 35,000 ppm.
【請求項6】 前記樹脂組成物中の亜鉛、マグネシウ
ム、カルシウムから選択される、少なくとも1種の金属
のイオン含有量が400〜50,000ppmである請
求項1ないし5のいずれかに記載の畜肉包装用多層フィ
ルム。
6. The animal meat according to claim 1, wherein the ion content of at least one metal selected from zinc, magnesium, and calcium in the resin composition is 400 to 50,000 ppm. Multilayer film for packaging.
【請求項7】 前記樹脂組成物がエチレン−ビニルアル
コール共重合体(A)を連続相成分とする請求項1ない
し6のいずれかに記載の畜肉包装用多層フィルム。
7. The multi-layer film for livestock meat packaging according to claim 1, wherein said resin composition contains an ethylene-vinyl alcohol copolymer (A) as a continuous phase component.
JP11056552A 1999-03-04 1999-03-04 Multilayer film for packaging storage meat Pending JP2000246843A (en)