[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

JP2000172021A - Production of liquid toner and liquid toner - Google Patents

Production of liquid toner and liquid toner

Info

Publication number
JP2000172021A
JP2000172021A JP10349518A JP34951898A JP2000172021A JP 2000172021 A JP2000172021 A JP 2000172021A JP 10349518 A JP10349518 A JP 10349518A JP 34951898 A JP34951898 A JP 34951898A JP 2000172021 A JP2000172021 A JP 2000172021A
Authority
JP
Japan
Prior art keywords
liquid toner
resin
producing
mill
ionomer
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
JP10349518A
Other languages
Japanese (ja)
Inventor
Toshio Waku
寿男 和久
Shigekazu Kitamura
繁和 北村
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Artience Co Ltd
Original Assignee
Toyo Ink Mfg Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Toyo Ink Mfg Co Ltd filed Critical Toyo Ink Mfg Co Ltd
Priority to JP10349518A priority Critical patent/JP2000172021A/en
Publication of JP2000172021A publication Critical patent/JP2000172021A/en
Pending legal-status Critical Current

Abstract

PROBLEM TO BE SOLVED: To enhance productivity and quality by dry-comminuting specified colored chips and carrying out further wet comminution in a nonaqueous solvent. SOLUTION: A colorant, a resin and ionomer are heated and kneaded at a temperature above the softening point of the resin, the kneaded material is coarsely comminuted and the resulting colored chips are dry-comminuted and further wet-comminuted in a nonaqueous solvent. A pigment effective in prolonging the life of an interim transfer body as well as an ordinarily used pigment or dye may be used as the colorant. An acrylic resin such as a polyacrylic ester, a polyethylene type resin such as polyethylene or a mixture of such resins may be used as the resin. The ionomer is obtained, e.g. by neutralizing an ethylene-acrylic acid copolymer with a metal. A hummer mill, a jet mill or the like is used for the dry comminution. A media crusher such as an attriter, a sand mill or a mill can be used for the wet comminution without causing any trouble.

Description

【発明の詳細な説明】DETAILED DESCRIPTION OF THE INVENTION

【0001】[0001]

【発明の属する技術分野】本発明は、静電潜像の顕在化
に適用される液体トナーの製造方法およびその液体トナ
ーに関する。例えば、カラーレーザプリンタやフルカラ
ーデジタルオンデマンド印刷機の画像形成材料として使
われる液体トナーの製造方法およびその液体トナーに関
する。
[0001] 1. Field of the Invention [0002] The present invention relates to a method for producing a liquid toner applied to visualizing an electrostatic latent image, and to the liquid toner. For example, the present invention relates to a method for producing a liquid toner used as an image forming material of a color laser printer or a full-color digital on-demand printing machine, and a liquid toner thereof.

【0002】[0002]

【従来の技術】静電潜像を顕在化するシステム、例えば
フルカラーデジタルオンデマンド印刷機において、粉体
トナーを用いたシステムと液体トナーを用いたシステム
が市場に出始めており、従来のオフィス用途のプリンタ
に比べて更に高速化、高画質化が図らて来ている。中で
も液体トナーは粒子径が粉体に比べて小さいことから、
高画質化を図るのに有利である。また、フルカラーデジ
タルオンデマンド印刷機が従来の印刷機と差別化を図る
ポイントは、無版であることによる「オンデマンド」
「ページバリアブル」といった機能であるが、もちろん
従来の印刷機に求められるような様々な種類の基材に適
応可能であるという点も重要であり、その解決の手段と
して「中間転写方式」を採用しているシステムもある。
2. Description of the Related Art In a system for realizing an electrostatic latent image, for example, in a full-color digital on-demand printer, a system using a powder toner and a system using a liquid toner have begun to appear on the market. Higher speed and higher image quality have been achieved compared to printers. Above all, liquid toner has a smaller particle size than powder,
This is advantageous for achieving high image quality. In addition, the point that the full-color digital on-demand printing machine is differentiating from the conventional printing machine is that the "on-demand"
Although it is a function such as "page variable", it is also important that it can be applied to various types of base materials required for conventional printing presses, and "intermediate transfer method" is adopted as a solution Some systems do.

【0003】液体トナーの製造方法としては、大別する
と、着色剤の処理にポイントを置いたものと、トナー粒
子の生成法に着目したものがある。前者は着色剤である
顔料等を凝集せずに分散させることにより画像濃度やそ
の他の画像品質を保つ目的であり、後者には、樹脂重合
法、着色剤との混練法、樹脂粉砕法、樹脂溶解析出法な
ど様々なものがあり、その殆どのものが画像品質の向上
を目的としている。それらの中で冷凍粉砕方式に関して
は、次のようなものがある。特開平7−234551号
公報には、バインダー成分である熱可塑性樹脂を冷凍粉
砕、分級したのち着色剤とともに湿式粉砕を行うことが
開示されている。この発明は樹脂原料を溶剤とともに加
熱し溶媒和させた後に冷却析出させる工程を乾式の冷凍
粉砕に代替し、得られる中間組成物の保管安定性と製造
コストの削減を意図したものでありそれは達成可能であ
るが、冷凍粉砕した比較的固い樹脂粉の中に着色剤を分
散させるのに不利であり、その結果画像濃度が充分でな
いことも起こり得る。
[0003] As a method of producing a liquid toner, when roughly classified, there are a method emphasizing the treatment of a colorant and a method focusing on a method of producing toner particles. The former is for the purpose of maintaining image density and other image quality by dispersing pigments and the like as colorants without agglomeration, and the latter is a resin polymerization method, a kneading method with a colorant, a resin pulverizing method, There are various methods such as a dissolution precipitation method, and most of them are aimed at improving image quality. Among them, there are the following regarding the freeze grinding method. JP-A-7-234551 discloses that a thermoplastic resin as a binder component is freeze-pulverized and classified, and then wet-pulverized together with a colorant. This invention is intended to replace the process of heating and solvating a resin raw material with a solvent to solvate and then cooling and precipitating it to dry freezing and pulverization, and to achieve storage stability of the obtained intermediate composition and reduction of production cost. Although possible, it is disadvantageous to disperse the colorant in relatively hardened and ground resin powder, which may result in insufficient image density.

【0004】特開平10−10796号公報には、顔料
と樹脂を混練後、冷凍粉砕し、次いで非水系溶媒中に溶
解分散して生成させた顔料組成物をもとにトナー粒子を
作ることが記載されている。特開平10−10797号
公報には、顔料と樹脂を混練後、冷凍粉砕し、次いで非
水系溶媒中に溶解分散して液体トナー用顔料組成物を作
ることについて記載されている。また、アイオノマーを
液体トナーの材料として使用したものには、次のような
ものがある。
[0004] Japanese Patent Application Laid-Open No. 10-10796 discloses that toner particles are produced based on a pigment composition produced by kneading a pigment and a resin, followed by freeze-pulverization, and then dissolving and dispersing in a non-aqueous solvent. Has been described. JP-A-10-10797 describes that a pigment and a resin are kneaded, then frozen and pulverized, and then dissolved and dispersed in a non-aqueous solvent to prepare a pigment composition for a liquid toner. Further, there are the following using ionomer as a material of a liquid toner.

【0005】特表平9−500976号公報には、帯電
性の良好でない液体トナー粒子をアイオノマーで被覆す
ることにより、帯電性を向上させることが開示されてい
る。
Japanese Patent Publication No. 9-500976 discloses that the chargeability is improved by coating liquid toner particles having poor chargeability with an ionomer.

【0006】[0006]

【発明が解決しようとする課題】カラーレーザプリンタ
やフルカラーデジタルオンデマンド印刷機の画像形成材
料として使われる液体トナーは、高速化、高画質化およ
び液体トナー生産性の向上が望まれている。高速化、高
画質化は殆どの場合その粒子の構成材料の改良によって
なされつつある。しかしながら、それだけでは不充分で
あり、液体トナー生産性の向上のため新規な製造方法が
求められ、着色剤の分散工程、樹脂の溶解工程、着色樹
脂の粉砕工程をいかに短時間に出来、かつより高速化に
対応し高画質であるものを作る方法およびその方法によ
って作られた液体トナーが必要とされている。
The liquid toner used as an image forming material for a color laser printer or a full-color digital on-demand printing machine is required to have a higher speed, a higher image quality and an improved liquid toner productivity. Higher speed and higher image quality are almost always achieved by improving the constituent materials of the particles. However, this alone is insufficient, and a new manufacturing method is required to improve the productivity of liquid toner, and the dispersing step of the colorant, the dissolving step of the resin, and the pulverizing step of the colored resin can be performed in a short time. There is a need for a method of producing high quality images with high speed and a liquid toner produced by the method.

【0007】[0007]

【課題を解決するための手段】本発明者らは、着色剤と
樹脂とアイオノマーを添加し、加熱混練し、それを粗粉
砕して得られた着色チップを乾式粉砕し、さらに非水系
溶剤中で湿式粉砕することにより、生産性、品質の向上
を達成した液体トナーを製造することを可能にした。第
1の発明は、着色剤と樹脂とアイオノマーを添加し、加
熱混練し、得られた着色チップを乾式粉砕し、さらに非
水系溶剤中で湿式粉砕することを特徴とする液体トナー
の製造方法である。
Means for Solving the Problems The present inventors added a colorant, a resin, and an ionomer, kneaded by heating, coarsely pulverized the resulting mixture, and dry-pulverized a colored chip, and further added a non-aqueous solvent. By performing wet pulverization with, a liquid toner having improved productivity and quality can be manufactured. The first invention is a method for producing a liquid toner, comprising adding a colorant, a resin and an ionomer, kneading under heating, dry-grinding the obtained colored chips, and further wet-grinding in a non-aqueous solvent. is there.

【0008】第2の発明は、アイオノマーがカルボキシ
ル基を含むオレフィン系樹脂を金属で中和した酸価10
0mgKOH/g以下のものであることを特徴とする請
求項1記載の液体トナーの製造方法である。第3の発明
は、アイオノマーの重量平均分子量が、500〜100
00であることを特徴とする第1または第2発明記載の
液体トナーの製造方法である。第4の発明は、乾式粉砕
が冷凍粉砕である第1〜第3いずれか記載の液体トナー
の製造方法である。第5の発明は、湿式粉砕の際に帯電
助剤を添加することを特徴とする第1〜第4いずれか記
載の液体トナーの製造方法である。
The second invention provides an ionomer obtained by neutralizing an olefin resin containing a carboxyl group with a metal by an acid value of 10%.
2. The method for producing a liquid toner according to claim 1, wherein the amount is 0 mgKOH / g or less. According to a third aspect, the weight average molecular weight of the ionomer is from 500 to 100.
00. The method for producing a liquid toner according to the first or second invention, wherein The fourth invention is the method for producing a liquid toner according to any one of the first to third inventions, wherein the dry pulverization is freeze pulverization. A fifth invention is the method for producing a liquid toner according to any one of the first to fourth inventions, wherein a charging aid is added during wet pulverization.

【0009】第6の発明は、静電潜像担持体上に顕在化
されたトナー粒子による画像を中間転写体に転写後、最
終的に基材に転写する画像形成システムに適用される第
1〜第4いずれか記載の液体トナーの製造方法である。
第7の発明は、第1〜第6発明いずれかの記載の方法に
よって得られたことを特徴とする液体トナーである。
A sixth aspect of the present invention is applied to an image forming system in which an image formed by toner particles revealed on an electrostatic latent image carrier is transferred to an intermediate transfer member and finally transferred to a substrate. 5. A method for producing a liquid toner according to any one of claims 4 to 4.
A seventh invention is a liquid toner obtained by the method according to any one of the first to sixth inventions.

【0010】[0010]

【発明の実施の形態】以下、本発明を説明する。着色チ
ップは、着色剤と樹脂とアイオノマーを樹脂の軟化点以
上の温度で加熱混練し、それを粗粉砕する。次いで得ら
れた着色チップを乾式粉砕し、さらに非水系溶剤中で湿
式粉砕することにより液体トナーとする。本発明で用い
られる着色剤は、通常使用されている顔料や染料は勿論
のこと、中間転写体のライフを伸ばすのに有効な顔料を
使用しても差し支えない。それらのものを例示すると、
ハンザイエロー、ジスアゾイエロー、キノリンイエロ
ー、パーマネントイエロー、イソインドリノン、ベンジ
ジンオレンジ、ベンガラ、ファーストレッド、リソール
レッド、パーマネントレッド、ウォッチャンレッドカル
シウム塩、ウォッチャンレッドマンガン塩、キナクリド
ン、ピラゾロンレッド、レーキレッドC、レーキレッド
D、ブリリアントカーミン3Bまたは6B、紺青、フタ
ロシアニンブルー、ビクトリアブルー、ニグロシン、カ
ーボンブラック等が挙げられる。これらの着色剤は単独
で、或いは混合して使用出来る。樹脂に対しての顔料の
含有比率は、0.1〜50重量%の範囲が良い。
DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described below. The coloring chip heats and kneads the coloring agent, the resin, and the ionomer at a temperature equal to or higher than the softening point of the resin, and coarsely pulverizes the mixture. Next, the obtained colored chips are dry-pulverized and further wet-pulverized in a non-aqueous solvent to obtain a liquid toner. As the coloring agent used in the present invention, not only pigments and dyes which are usually used, but also pigments effective for extending the life of the intermediate transfer member may be used. To illustrate them,
Hansa Yellow, Disazo Yellow, Quinoline Yellow, Permanent Yellow, Isoindolinone, Benzidine Orange, Vengara, Fast Red, Lisole Red, Permanent Red, Watchyan Red Calcium Salt, Watchyan Red Manganese Salt, Quinacridone, Pyrazolone Red, Lake Red C , Lake Red D, Brilliant Carmine 3B or 6B, Navy Blue, Phthalocyanine Blue, Victoria Blue, Nigrosine, Carbon Black and the like. These colorants can be used alone or as a mixture. The content ratio of the pigment to the resin is preferably in the range of 0.1 to 50% by weight.

【0011】本発明で使用される樹脂としては、ポリア
クリル酸エステル、ポリメタクリル酸エステル等のアク
リル樹脂、ポリスチレン、ポリエチレンーアクリル酸共
重合体、ポリエチレン−メタクリル酸共重合体、ポリエ
チレン−酢酸ビニル共重合体、エチレンメタクリル酸共
重合体のNa塩,Zn塩,Ca塩、エチレンアクリル酸
共重合体のNa塩,Zn塩,Ca塩,Mg塩、エチレン
エチルアクリレ−ト共重合体、エチレンマレイン酸共重
合体等のポリエチレン系樹脂その他ポリ塩化ビニル樹
脂、ニトロセルロース、アルキッド樹脂、フェノール樹
脂、ポリエステル樹脂、ポリビニルブチラール樹脂、ポ
リイソシアネート樹脂、ポリウレタン樹脂、ポリアミド
樹脂,エポキシ樹脂を単独または混合して使用する。
The resins used in the present invention include acrylic resins such as polyacrylates and polymethacrylates, polystyrenes, polyethylene-acrylic acid copolymers, polyethylene-methacrylic acid copolymers, and polyethylene-vinyl acetate copolymers. Polymer, Na salt, Zn salt, Ca salt of ethylene methacrylic acid copolymer, Na salt, Zn salt, Ca salt, Mg salt of ethylene acrylic acid copolymer, ethylene ethyl acrylate copolymer, ethylene maleate Use of polyethylene resin such as acid copolymer, other polyvinyl chloride resin, nitrocellulose, alkyd resin, phenol resin, polyester resin, polyvinyl butyral resin, polyisocyanate resin, polyurethane resin, polyamide resin, epoxy resin alone or in combination I do.

【0012】アイオノマーは、例えばエチレン−アクリ
ル酸共重合体を金属で中和したものであり、アライドシ
グナル社からAClynの商標名で市販されているもの
がある。Ca塩,Mg塩,Na塩,Zn塩タイプがそれ
ぞれあり、いずれも顔料分散の効果がある。添加量とし
ては、顔料1部に対し、0.01〜10部まで添加可能
である。酸価は、樹脂との親和性を考慮すると100m
gKOH/g以下の範囲が好ましく、より好ましくは6
0mgKOH/g以下であり、酸価を有しなくても良
い。また重量平均分子量は、500〜10000の範囲
が好ましい。着色剤と樹脂とアイオノマーの加熱混練に
は、2本ロール、2軸押し出し機、バンバリーミキサー
等が用いられる。
The ionomer is, for example, a product obtained by neutralizing an ethylene-acrylic acid copolymer with a metal, and is commercially available from Allied Signal under the trade name AClyn. There are Ca salt, Mg salt, Na salt, and Zn salt types, all of which have the effect of pigment dispersion. As the amount of addition, 0.01 to 10 parts can be added to 1 part of the pigment. The acid value is 100 m in consideration of the affinity with the resin.
gKOH / g or less, more preferably 6 gKOH / g or less.
It is 0 mgKOH / g or less, and may not have an acid value. Further, the weight average molecular weight is preferably in the range of 500 to 10,000. For the heating and kneading of the colorant, the resin, and the ionomer, a two-roll, twin-screw extruder, a Banbury mixer, or the like is used.

【0013】乾式粉砕には、ハンマーミル、ジェットミ
ル、ピンミル、ターボミル、カッターミル、ボールミ
ル、振動ミル、遊星ミルなどをもちいるが、粉砕する組
成物が柔らかい場合、たとえば軟化点が100℃以下の
場合は、液体窒素あるいは固体の二酸化炭素等で粉砕す
べき組成物を冷却し、脆化し、同様の粉砕機で粉砕す
る。粉砕後は、必要に応じて分級装置を用いて粗大粒子
を取り除く。この分級工程での分級装置の目開きを細か
くする事により、次工程の湿式粉砕工程にかかる時間を
短縮することも可能である。湿式粉砕には、メジア粉砕
機である、アトライタ、サンドミル、ダイノミル、ボー
ルミル、アペックスミル、スパイクミル、コボールミ
ル、ダイヤモンドファインミル、パールミル、DCPミ
ル、アクアマイザー、マイクロス、ピュアミル、NPミ
ルなどが問題なく使用可能で、メジアレス粉砕機ではホ
モジナイザー、トリゴナル、スラッシャー、コロイダル
ミル、キャビトロン、ゴラトール、デスパーミル、エバ
ラマイルダー、ナノマイザー、アクアテック、マイロイ
ダーなどが本発明のアイオノマーの量を若干増やせば使
用可能である。
For the dry pulverization, a hammer mill, a jet mill, a pin mill, a turbo mill, a cutter mill, a ball mill, a vibration mill, a planetary mill and the like are used. In this case, the composition to be pulverized with liquid nitrogen or solid carbon dioxide is cooled, embrittled, and pulverized by a similar pulverizer. After the pulverization, coarse particles are removed using a classification device as necessary. By making the openings of the classifier finer in this classifying step, the time required for the next wet pulverizing step can be reduced. For wet milling, there are no problems with medial mills such as attritor, sand mill, dyno mill, ball mill, apex mill, spike mill, coball mill, diamond fine mill, pearl mill, DCP mill, aquamizer, micros, pure mill, NP mill, etc. It can be used, and in a medial crusher, a homogenizer, a trigonal, a slasher, a colloidal mill, a cavitron, a gatorol, a desper mill, an ebaramilder, a nanomizer, an aquatech, a myloider, etc. can be used if the amount of the ionomer of the present invention is slightly increased. .

【0014】本発明において湿式粉砕の際に添加される
帯電助剤は、飽和脂肪酸の金属塩または不飽和脂肪酸の
金属塩が好ましい。例えば、ステアリン酸カルシウム、
ステアリン酸アルミニウム、ラウリン酸アルミニウム、
ラウリン酸バリウム、オレイン酸ソーダが特にトナー粒
子の帯電ひいては電気泳動性には好ましい。また、この
帯電助剤の湿式粉砕時に於ける添加時期は、粉砕開始時
から粉砕終了直前のいずれの時期でも構わない。加熱混
練の際に帯電助剤を入れたもの、湿式粉砕の時に入れた
ものとでは、明らかに後者の方が電気泳動性が高いた
め、湿式粉砕時に帯電助剤を添加するのが好ましい。
In the present invention, the charging aid added during wet grinding is preferably a metal salt of a saturated fatty acid or a metal salt of an unsaturated fatty acid. For example, calcium stearate,
Aluminum stearate, aluminum laurate,
Barium laurate and sodium oleate are particularly preferred for charging toner particles and thus for electrophoresis. In addition, the timing of addition of the charging aid during wet pulverization may be any time from the start of pulverization to immediately before the end of pulverization. It is apparent that the latter has a higher electrophoretic property than the one in which the charging aid is added during the heat kneading and the one in which the charging aid is added during the wet pulverization. Therefore, it is preferable to add the charging aid during the wet pulverization.

【0015】本発明の製造法による液体トナーが中間転
写方式の画像形成に良い理由は、溶剤とともに加熱して
溶媒和させて析出する工程が省かれるため、液体トナー
粒子中の溶剤量が少ないことで、中間転写体上で溶剤を
蒸発させる熱をトナー粒子の溶解に利用出来るので、基
材への定着性が向上する。本発明の液体トナーに用いる
溶媒としては、誘電率3.5以下、体積抵抗10 7 オー
ムセンチ以上の炭化水素系溶剤である。これらの好まし
い例としては、150〜220°Cの範囲に沸点を有す
る脂肪族炭化水素、芳香族炭化水素であり、アイソパ
G,H,L(エクソンケミカル製)、シェルゾールA,
AB(シェル製)、ナフテゾルL,M,H(日本石油
製)等が挙げられる。
The liquid toner according to the production method of the present invention is
A good reason for image formation in the copying method is that heating with a solvent
Liquid toner is eliminated because the step of solvation and precipitation is omitted.
Due to the small amount of solvent in the particles, the solvent
The heat that evaporates can be used to dissolve the toner particles.
The fixing property to the material is improved. Used for the liquid toner of the present invention
As the solvent, the dielectric constant is 3.5 or less, and the volume resistance is 10 or less. 7Oh
It is a hydrocarbon-based solvent with a centimeter or more. These preferred
As an example, it has a boiling point in the range of 150 to 220 ° C.
Aliphatic hydrocarbons and aromatic hydrocarbons
G, H, L (Exxon Chemical), Shersol A,
AB (manufactured by Shell), Naphthesol L, M, H (Nippon Oil
Manufactured).

【0016】本発明の液体トナーは、電荷調整剤を添加
することにより、より高い電気泳動性を発揮する。通常
液体トナーの電荷調整剤に使用されている界面活性剤は
勿論のこと、高速印刷対応の電荷調整剤も問題なく使用
出来る。例えば、ナフテン酸コバルト、ナフテン酸亜
鉛、ナフテン酸銅、ナフテン酸マンガン、レシチン、オ
クチル酸コバルト、オクチル酸ジルコニウム、アルキル
アリルスルフォネート類、石油系スルフォン酸金属塩、
ポリビニルピロリドン、アルキル化ポリビニルピロリド
ン、リン酸エステルなどを単独または複数のものを混合
して使うことができる。高速印刷対応型としては、特開
平6−208255〜7号公報および特表平7−509
074号公報記載のものも使用出来る。
The liquid toner of the present invention exhibits higher electrophoretic properties by adding a charge control agent. Not only surfactants which are usually used as charge adjusting agents for liquid toners, but also charge adjusting agents for high-speed printing can be used without any problem. For example, cobalt naphthenate, zinc naphthenate, copper naphthenate, manganese naphthenate, lecithin, cobalt octylate, zirconium octylate, alkyl allyl sulfonates, petroleum metal sulfonate,
Polyvinylpyrrolidone, alkylated polyvinylpyrrolidone, phosphoric acid ester and the like can be used alone or in combination of two or more. Japanese Patent Application Laid-Open No. Hei 6-208255-7 and Japanese Patent Laid-Open Publication No. Hei 7-509
No. 074 can also be used.

【0017】添加量はトナー粒子固型分0.1〜5.5
重量%の現像液1000部に対して0.01〜50部の
範囲で適宜加える。
The amount of addition is 0.1 to 5.5 in terms of solid content of toner particles.
It is appropriately added in the range of 0.01 to 50 parts to 1000 parts by weight of the developer.

【0018】[0018]

【実施例】以下実施例に基づいて本発明を説明する。 (実施例1〜5)表6の記号のそれぞれ該当する表1〜
表5の条件で試作し、表7の結果を得た。具体例とし
て、実施例1について以下に記述する。表1の記号Aに
該当するカーボンブラック顔料と表1の記号Bに該当す
る樹脂エチレン−メタクリル酸共重合体と表2の記号D
に該当するCaで中和された酸価42mgKOH/gの
アイオノマーを表3による配合比で表4の記号Hに該当
する二本ロールで樹脂の軟化点を超える100°Cで混
練し、1〜10mm角に粗粉砕し、着色チップを得た。
次いで、液体窒素にて冷却しながらピンミルで粉砕し、
150ミクロンの目開きのメッシュで分級すると、平均
粒子径42ミクロン(SA−CP3L、島津製作所製遠
心沈降式粒度分布測定機)でシャープな粒度分布をもつ
粉砕物が得らた。
DESCRIPTION OF THE PREFERRED EMBODIMENTS The present invention will be described below based on embodiments. (Examples 1 to 5) Tables 1 to 5 corresponding to the symbols in Table 6 respectively.
A prototype was produced under the conditions shown in Table 5, and the results shown in Table 7 were obtained. Example 1 will be described below as a specific example. The carbon black pigment corresponding to the symbol A in Table 1, the resin ethylene-methacrylic acid copolymer corresponding to the symbol B in Table 1, and the symbol D in Table 2
The ionomer having an acid value of 42 mgKOH / g neutralized with Ca corresponding to the above is kneaded at 100 ° C. exceeding the softening point of the resin with two rolls corresponding to the symbol H in Table 4 in a mixing ratio according to Table 3, and It was coarsely pulverized into 10 mm square to obtain a colored chip.
Then, pulverize with a pin mill while cooling with liquid nitrogen,
When the particles were classified using a mesh having a mesh size of 150 microns, a pulverized product having an average particle size of 42 microns (SA-CP3L, a centrifugal sedimentation type particle size distribution measuring device manufactured by Shimadzu Corporation) and having a sharp particle size distribution was obtained.

【0019】この粉砕物を下記の処方で混合しアトライ
タ(ユニオンプロセス社)で湿式粉砕を行った。 上記粉砕物 25部 アイソパ H(エクソンケミカル社製) 74部 表5の記号Kに該当するステアリン酸アルミニウム 1部 3時間の粉砕で平均粒子径2.1ミクロン(SA−CP
3L、島津製作製遠心沈降式粒度分布測定機)の液体ト
ナー粒子を得た。またこの液体トナー粒子は球形でなく
複数のファイバーを持つことから、光散乱回折式の粒度
分布測定機(SALD−2000A、島津製作所製)で
測定すると表7の「粒子径」に該当する7.1ミクロン
の平均粒子径であった。この液体トナー粒子をアイソパ
ーHで不揮発分2.0%に調整し、その希釈液1000
部に対し、電荷調整剤であるレシチン1.0部を添加し
液体トナーを得た。
The pulverized material was mixed according to the following formulation and wet pulverized by an attritor (Union Process). 25 parts of the above pulverized product 74 parts Isopa H (manufactured by Exxon Chemical Co.) 74 parts Aluminum stearate corresponding to symbol K in Table 5 1 part
3 L, liquid toner particles of a centrifugal sedimentation type particle size distribution analyzer manufactured by Shimadzu) were obtained. Further, since the liquid toner particles are not spherical but have a plurality of fibers, they correspond to “particle diameter” in Table 7 when measured with a light scattering diffraction type particle size distribution analyzer (SALD-2000A, manufactured by Shimadzu Corporation). The average particle size was 1 micron. The liquid toner particles are adjusted to a non-volatile content of 2.0% with Isopar H,
The liquid toner was obtained by adding 1.0 part of lecithin as a charge control agent to the parts.

【0020】電気泳動性は、高電場導電率と低電場導電
率の差である粒子導電率と呼ばれるものを評価したもの
である。粒子単独の導電率を意味し、高い方が高速印刷
に適しているということになる。高電場導電率は、1.
5V/マイクロメーター(DC)で測定され、低電場導
電率は、5V/mm(AC:5Hz)で測定される。測
定結果は表7の「電気泳動性」に示すとおり150pS
/cm(ピコジーメンス/cm)であった。この液体ト
ナーをフルカラーデジタルオンデマンド印刷機であるE
−Print1000(インディゴ社製)の液体トナー
タンクに入れ、現像電圧を400Vに固定し出力画像を
評価した。
The electrophoretic property is an evaluation of what is called particle conductivity, which is the difference between high electric field conductivity and low electric field conductivity. The conductivity of the particles alone means that the higher the particle, the more suitable it is for high-speed printing. The high electric field conductivity is:
Measured at 5 V / micrometer (DC), low field conductivity is measured at 5 V / mm (AC: 5 Hz). The measurement result was 150 pS as shown in “Electrophoresis” in Table 7.
/ Cm (pico siemens / cm). This liquid toner is used as a full-color digital on-demand printer E
-Print 1000 (manufactured by Indigo Corporation) was placed in a liquid toner tank, and the output voltage was fixed at 400 V, and the output image was evaluated.

【0021】「画像濃度」は、X−Rite408(X
−Rite社製)で測定し、表7の1.78を得た。
「接着性」は(テープ剥離耐性)(消しゴム擦り耐性)
(爪引っ掻き耐性)の評価結果を集計し、7段階評価し
表7の7(値が高い方が良好)を得た。 (比較例1)二本ロールでの混練時にアイオノマーを添
加しない事以外は、実施例1と同じ条件で試作、評価し
た。 (比較例2)帯電助剤の添加時期を二本ロールでの混練
時にしたこと以外は、実施例1と同じ条件で試作、評価
した。 (比較例3)着色チップの冷凍粉砕を行う代わりに、着
色チップ40部に対しアイソパ H(エクソンケミカル
社製)60部を攪拌加熱溶解し、その後冷却析出して、
下記の処方で混合しアトライタ(ユニオンプロセス社)
で湿式粉砕を行ったこと以外は、実施例1と同じ条件で
試作、評価した。
The "image density" is defined as X-Rite 408 (X
-Rite) to obtain 1.78 in Table 7.
"Adhesiveness" is (tape peeling resistance) (rubber resistance to eraser)
The evaluation results of (claw scratch resistance) were totaled and evaluated on a 7-point scale to obtain 7 in Table 7 (the higher the value, the better). (Comparative Example 1) A prototype was produced and evaluated under the same conditions as in Example 1 except that no ionomer was added during kneading with two rolls. (Comparative Example 2) A trial production and evaluation were performed under the same conditions as in Example 1 except that the charging aid was added at the time of kneading with two rolls. (Comparative Example 3) Instead of freezing and pulverizing the colored chips, 60 parts of Isopa H (manufactured by Exxon Chemical Co., Ltd.) was stirred and heated and dissolved in 40 parts of the colored chips.
Attritor mixed with the following formula (Union Process)
A trial production and evaluation were performed under the same conditions as in Example 1 except that wet grinding was performed.

【0022】 上記析出物 62.5部 アイソパ H(エクソンケミカル社製) 36.5部 表5の記号Kに該当するステアリン酸アルミニウム 1部 (比較例4)着色チップを作らずに、表1の記号Aに該
当するカーボンブラック顔料と表1の記号Bに該当する
樹脂エチレン−メタクリル酸共重合体とを下記の処方で
攪拌加熱溶解し、その後冷却析出した。 カーボンブラック顔料 6部 エチレン−メタクリル酸共重合体 32部 アイソパ H(エクソンケミカル社製) 62部 次いで、下記の処方で混合しアトライタ(ユニオンプロ
セス社)で湿式粉砕を行ったこと以外は、実施例1と同
じ条件で試作、評価した。
62.5 parts of the above precipitate 36.5 parts of Isopa H (manufactured by Exxon Chemical Co.) 1 part of aluminum stearate corresponding to the symbol K in Table 5 (Comparative Example 4) The carbon black pigment corresponding to the symbol A and the resin ethylene-methacrylic acid copolymer corresponding to the symbol B in Table 1 were dissolved by stirring and heating according to the following formulation, and then cooled and precipitated. Carbon black pigment 6 parts Ethylene-methacrylic acid copolymer 32 parts Isopa H (manufactured by Exxon Chemical Co.) 62 parts Then, the mixture was mixed according to the following formulation and wet-pulverized with an attritor (Union Process). A prototype was produced and evaluated under the same conditions as in Example 1.

【0023】 上記析出物 62.5部 アイソパ H(エクソンケミカル社製) 36.5部 表5の記号Kに該当するステアリン酸アルミニウム 1部62.5 parts of the above precipitates 36.5 parts of Isopa H (manufactured by Exxon Chemical Co.) 1 part of aluminum stearate corresponding to the symbol K in Table 5

【0024】[0024]

【表1】 [Table 1]

【0025】[0025]

【表2】 [Table 2]

【0026】[0026]

【表3】 [Table 3]

【0027】[0027]

【表4】 [Table 4]

【0028】[0028]

【表5】 [Table 5]

【0029】[0029]

【表6】 [Table 6]

【0030】[0030]

【表7】 [Table 7]

【0031】[0031]

【発明の効果】本発明の製造方法で製造された液体トナ
ーを使用することにより、電気泳動性にとんだ画像濃度
の高い、また定着強度の高い画像を電子写真式の印刷シ
ステムに於いて得られ、生産性が向上した。生産性の向
上については、樹脂の溶剤中で加熱溶解・冷却析出した
後に着色剤等とともに湿式粉砕する方式から、予め着色
剤等を加熱混練する方式に代えることにより達成され、
さらにその後溶剤中で加熱溶解・冷却析出を行わず乾式
粉砕を行うことでより高い効果を得た。
By using the liquid toner produced by the production method of the present invention, an electrophoretic image having a high image density and a high fixing strength can be obtained in an electrophotographic printing system. , Increased productivity. Improvement in productivity is achieved by replacing the method of wet grinding with a colorant etc. after heating and dissolving / cooling and precipitating in a resin solvent, by replacing the method of heating and kneading the colorant etc. in advance,
Furthermore, a higher effect was obtained by performing dry pulverization without heating dissolution / cooling precipitation in a solvent thereafter.

【0032】電気泳動性の向上および画像濃度の向上
は、帯電助剤を湿式粉砕時に添加すること、本発明のア
イオノマーの添加、着色チップを溶剤中で加熱溶解・冷
却析出せず乾式粉砕することにより達成され、また定着
性は着色チップあるいは樹脂を溶剤中で加熱溶解・冷却
析出せず乾式粉砕することによって達成された。
To improve the electrophoretic property and the image density, the charge aid should be added during wet grinding, the ionomer of the present invention should be added, and the colored chips should be dry-ground without heating, dissolving and cooling in a solvent. The fixability was achieved by dry pulverization of a colored chip or resin in a solvent without heating, dissolving or cooling.

Claims (7)

【特許請求の範囲】[Claims] 【請求項1】着色剤と樹脂とアイオノマーを添加し、加
熱混練し、得られた着色チップを乾式粉砕し、さらに非
水系溶剤中で湿式粉砕することを特徴とする液体トナー
の製造方法。
1. A method for producing a liquid toner, comprising adding a colorant, a resin and an ionomer, kneading under heating, dry-grinding the obtained colored chips, and further wet-grinding in a non-aqueous solvent.
【請求項2】アイオノマーがカルボキシル基を含むオレ
フィン系樹脂を金属で中和した酸価100mgKOH/
g以下のものであることを特徴とする請求項1記載の液
体トナーの製造方法。
2. An acid value obtained by neutralizing an olefin resin containing a carboxyl group with a metal with a metal having an acid value of 100 mg KOH /
The method for producing a liquid toner according to claim 1, wherein the amount is not more than g.
【請求項3】アイオノマーの重量平均分子量が、500
〜10000であることを特徴とする請求項1または2
記載の液体トナーの製造方法。
3. The ionomer has a weight average molecular weight of 500.
3. The method according to claim 1, wherein the number is from 10,000 to 10,000.
A method for producing the liquid toner according to the above.
【請求項4】乾式粉砕が冷凍粉砕である請求項1〜3い
ずれか記載の液体トナーの製造方法。
4. The method for producing a liquid toner according to claim 1, wherein the dry pulverization is freeze pulverization.
【請求項5】湿式粉砕の際に帯電助剤を添加することを
特徴とする請求項1〜4いずれか記載の液体トナーの製
造方法。
5. The method for producing a liquid toner according to claim 1, wherein a charging aid is added during wet pulverization.
【請求項6】静電潜像担持体上に顕在化されたトナー粒
子による画像を中間転写体に転写後、最終的に基材に転
写する画像形成システムに適用される請求項1〜5いず
れか記載の液体トナーの製造方法。
6. The image forming system according to claim 1, wherein the image formed by the toner particles revealed on the electrostatic latent image carrier is transferred to an intermediate transfer member and finally transferred to a substrate. Or a method for producing a liquid toner according to the above.
【請求項7】請求項1〜6いずれかの記載の方法によっ
て得られたことを特徴とする液体トナー。
7. A liquid toner obtained by the method according to claim 1.
JP10349518A 1998-12-09 1998-12-09 Production of liquid toner and liquid toner Pending JP2000172021A (en)