CN1724387A - 从石煤钒矿中提取五氧化二钒的方法 - Google Patents
从石煤钒矿中提取五氧化二钒的方法 Download PDFInfo
- Publication number
- CN1724387A CN1724387A CN 200510031726 CN200510031726A CN1724387A CN 1724387 A CN1724387 A CN 1724387A CN 200510031726 CN200510031726 CN 200510031726 CN 200510031726 A CN200510031726 A CN 200510031726A CN 1724387 A CN1724387 A CN 1724387A
- Authority
- CN
- China
- Prior art keywords
- water
- vanadium
- tank
- slag
- roasting
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Pending
Abstract
本发明涉及一种从石煤钒矿中提取五氧化二钒的方法,它是一种加钙氧化焙烧,弱碱性浸出,离子交换,从低碳硅质石煤钒矿中提取五氧化二钒。其特征在于:矿石配加15%以内的钙盐进行球磨,制粒料进沸腾炉氧化焙烧后,在弱碱性溶液中搅拌浸出,含钒溶液用离子交换富集,脱洗、沉钒、热解,得到五氧化二钒产品。本发明的生产过程完全消除了废气、废水、废渣对环境的污染,钒收得率高于65%,生产成本比钠法和酸法更低。本发明工艺可靠,实施方便,建厂投资省。能充分利用现有钒厂的设施,改造费用低,见效快;它是一种理想的从石煤钒矿中提取五氧化二钒的方法。
Description
技术领域
本发明涉及从矿石提取五氧化二钒的工艺。
背景技术
钒是高熔点稀有金属,具有许多优良的性能。在冶金、化工等行业有广泛的用途,随着我国现代化建设的高速发展,钒及其化合物的需求量越来越大。但是钒矿资源稀少而且分散,当前主要来源是从含钒铁矿的冶炼过程提取,产量远远不能满足需求。几十年来,国内外对低含量的石煤钒矿提炼做了许多研究和生产实践,一直未得到满意的效果。比较成熟的工艺是矿石加氯化钠焙烧,水浸出,设备普遍采用平窑,钒收得率低,环境污染严重。近十多年来,出现了竖炉焙烧、平窑减钠焙烧、“二氯化钙+氢氧化钙”焙烧等方法,这些方法只能部分降低焙烧烟气中氯气和氯化氢的浓度,不能完全解决废气对环境的污染问题。有的采用中间盐法或酸浸-萃取法,虽然克服了废气污染环境问题,但酸浸过程会把砷、镉、铅、铜、锌、铁、锰等有害杂质同时浸出,溶液净化和废水处理负担重,与酸接触的设备要防腐,故而设备投资大、运行费用高,废水和废渣对环境的污染难以完全消除。
发明内容
本发明的目的在于克服上述缺陷,提供一种成本低、无污染、操作方便、产品质量好的从石煤钒矿中提取五氧化二钒的方法。
本发明技术解决方案是:用碳酸钙或氧化钙或其混合物代替氯化钠作焙烧添加剂,物料磨碎采用润湿式球磨机,磨细料制成Φ3-12mm的球粒,焙烧采用高效率、自动化的沸腾炉,也可以用回转窑,焙烧温度为700--1000℃,产出热料加水进湿球磨,球磨矿浆用机械搅拌槽在35--100℃浸出,加碳酸盐调整溶液PH7.5-9.0,浸出矿浆放入重力沉降池沉渣,上清液送贮液池冷却到50℃以下,池底浓泥送流态化洗涤槽用热水洗涤,冷却后的含钒溶液送阴离子交换树脂柱,吸附的钒经脱洗、沉淀结晶、热解得到五氧化二钒产品。
矿石磨碎采用润湿式球磨机,物料含水分率3~10%,雨季生产不受阻,无粉尘污染,噪音也比干磨下降约30分贝,大大改善工厂和周边环境。矿石配入钙盐为碳酸钙或氧化钙、其钙盐量为矿石量的5-15%,根据矿石成分调整。
球磨料需先制粒,球粒直径控制在Φ3-12mm的范围内。焙烧采用沸腾炉(或用回转窑),焙烧温度为700--1000℃,焙烧时间为2-5小时,根据物料性质和产量调整。
焙烧烟气在降尘室通过间接换热,把沸腾炉的炉底鼓风从常温加热到150--200℃,再通过水箱冷却器间接加热生产用水,最后在烟囱内淋水洗涤,烟气所含热量得到充分回收利用,排烟含尘量≤150mg/m3,低于国家允许排放标准。焙烧排出热料直接溜入水槽,混合进入湿式球磨机浆化球磨,热料使水温升到50--100℃,不需外加热,通过调整水量来控制温度不使水沸腾,料∶水==1∶3-5。
球磨热矿浆送机械搅拌槽浸出,温度为35--100℃,浸出时间为1-4小时。浸出剂为碳酸盐,加入量为矿石量的5-10%,调整溶液PH7.5-9.0。浸出过程在机械搅拌的同时,向槽内鼓入部分焙烧烟气,而利用烟气中的CO2和热量,节省碳酸盐的用量,保持反应温度,可省去供热锅炉。
浸出矿浆的渣液分离采用重力沉降和流态化洗涤的巧妙方法,省去了过滤设备的大量投资,生产运行费用也大大降低。浸出矿浆在重力沉降池沉降2小时以上,上清率可达到75%以上。抽取70~75%的上清液到贮液池,进一步澄清并降温到50℃以下。
浸出矿浆沉降池的底部浓泥送流态化洗涤槽,从上部中心加入,洗水从底部旋流向上,洗水量为渣量的2-3倍,即渣∶水=1∶2~3;洗水温度为50℃~100℃,洗涤槽的上口溢出的洗液返回冲热料进湿球磨;底部排出渣送堆渣池,渣在池中堆放72小时以上,经重力挤压使渣含水从50%以上降到25%左右。水返回使用,渣可送去生产水泥,也可集中堆放以后再用,还可返回矿区铺填山地直接恢复植被。
经澄清和冷却的含钒溶液送到阴离子交换树脂柱吸附钒,排出液主要含铵离子和少量钠、钾、硅、铝、磷等阳离子,送到阳离子交换树脂柱中吸附铵和其他阳离子。两次吸附后的排出水较纯净,可全部返回使用。需要排放时也不会对水体造成任何危害。
阳离子树脂吸附饱和后,用稀酸溶液脱洗,得到的浓铵盐溶液含有少量其它阳离子,简单的处理方法是做复合肥料,规模大的厂可以提纯得到工业纯铵盐,返回使用。
吸附饱和钒的阴离子树脂,用NaCl+NH4Cl的混合液脱洗,得到钒酸铵和钒酸钠的浓溶液。
钒酸铵钠溶液送到沉淀池中,加入过量的NH4Cl,使钒以偏钒酸铵的形式结晶沉淀,NH4Cl的加量保证NH4+离子浓度为理论量的2.5倍以上;沉淀时间8小时以上。
偏钒酸铵沉淀经洗涤、甩干后,送到焙解炉中,在400--550℃下热解得到99%以上的V2O5产品。
综上所述,本发明的生产过程自动化程度高,操作方便,运行稳定可靠,可以大规模生产,钒收得率大于65%,生产成本比钠法和酸法更低,特别是完全消除了三废对环境的影响,对环境无污染,矿产资源和热能得到充分利用,建厂投资省,年产500吨V2O5的生产厂,投入600万元就可建成,建厂周期4-6个月。如果对现有钠法平窑进行技术改造也很经济,平窑改建,其材料可利用,其它设施都可直接利用,因地制宜补加必需设施,即可恢复生产,本发明具有广阔的应用前景和实用价值。
附图说明
附图为本发明的工艺流程图:
具体实施方式
下面结合附图对本发明作进一步的说明:一种从石煤钒矿中提取五氧化二钒的方法,其特征在于:矿石初碎后,配入矿石量5~15%的钙盐,混合进入球磨,制粒后送沸腾炉在700--1000℃焙烧,焙烧料加水进入湿式球磨机浆化球磨,加碳酸盐调溶液PH7.5-9.0,温度35--100℃条件下,机械搅拌浸出,溶液用离子交换树脂吸附,脱洗液沉淀偏钒酸铵,热解得到五氧化二钒产品。配加的钙盐为碳酸钙或氧化钙,其配加量为矿石量的5-15%,根据矿石成分调整加量。
物料球磨在润湿式球磨机中进行,物料的含水率为3~10%,球磨料制粒的球粒直径为3-12mm。焙烧是在沸腾炉中或在回转窑中进行,焙烧温度700--1000℃,焙烧时间2-5小时。
焙烧出炉料随即溜入水槽混合进入湿式球磨机浆化球磨,温度50--100℃,加水量为:料∶水==1∶3-5;湿磨料浆送机械搅拌槽浸出,温度35--100℃,加碳酸盐量为矿石量的5-10%,调整溶液PH值为7.5-9.0,浸出时间为1-4小时。可以将焙烧中的部分烟气鼓入浸出而利用其中的二氧化碳和热量。
浸出矿浆放入重力沉降池,自然沉降2小时以上,重力沉降池的上清液送贮液池冷却到50℃以下,沉降池的底部浓泥送流态化洗涤槽,浓泥从上部中心加入,洗水从底部旋流向上,洗水量为渣量的2~3倍洗水温度50--100℃,渣∶水==1∶2-3;洗涤槽的上部溢流液送湿球磨,底部排渣送堆渣池,渣在池中堆放72小时以上,重力挤压使渣含水从50%以上降到25%左右,水返回使用,渣中不含酸、碱和其它任何有害离子。
贮液池中冷却到50℃以下的含钒溶液送到阴离子交换树脂柱吸附钒,排出液再送到阳离子交换树脂柱吸附铵和其它阳离子,两次吸附后的排出水已较纯净,可以返回使用或向外排放
吸附饱和钒的阴离子树脂用NaCl+NH4Cl的混合液脱洗,得到钒酸铵和钒酸钠的浓溶液,钒酸铵钠溶液送到沉钒池中加入NH4Cl,沉淀出偏钒酸铵结晶,偏钒酸铵经洗涤、甩干后,在400--550℃下热解得到99%以上的V2O5产品。
1、矿石的配加剂可以是CaCO3、Na2CO3、K2CO3、CaO、Na2O、K2O等,也可以是其混合物,其共同特点是钒被氧化,而烟气中不带出氯气和氯化氢等毒害性气体。从实施效果和原料来源等综合比较,推荐用CaCO3或CaO或两者混合物。
2、球磨料的粒度范围为90%的矿粉粒度在0.075-0.18mm(80-200目)以内。
3、物料球磨制粒的球粒直径要适当,太大烧不透,太小烟尘多。故选用球直径为Φ3-12mm。
4、焙烧是本工艺流程的关键步骤,焙烧采用可调式沸腾炉进行,操作方便,运行可靠,工艺参数调节幅度很大,对原料变化和产量波动有很强的适应能力。焙烧温度700--1000℃,焙烧时间2-5小时,炉内料层高度400-1200mm,炉床生产量4-12t/m2.d的大范围变化,不会降低焙烧质量,对工厂的连续稳定生产十分有利。是本发明显著优于其它工艺方法的关键点。焙烧过程的主要化学反应如下:
(1)
(2)
(3)
(4)
(5)
(6)
5、焙烧料的趁热加水湿球磨有三方面的优点:一是充分利用热能,浸出过程不需外加热,省去了供热锅炉;二是节省浸出时间;三是有效破碎CaCO3的沉积层。
6、浸出过程的添加剂可以是钠、钾、铵的碳酸盐,从实施效果和经济性比较,推荐用碳酸铵或者碳酸氢铵。其主要化学反应是:
(1)
(2)
(3)
(4)
(5)
(6)
(7)
(8)
7、将部分焙烧烟气鼓入浸出槽,其中的CO2参与浸出反应,可以减少碳酸盐加入量;热量可以保持反应温度大多在55℃以上,在寒冷季节尤其有用,不用供热锅炉而全年生产可以平稳运行。
8、浸出矿浆的渣液分离采用重力沉浆和流态化洗涤,由于矿浆中的CaCO3容易沉积,堵塞设备,滤布老化失效快,生产运行费用高,难于连续稳定作业。本发明的方法证明,只要磨料粒度适当,石煤矿的沉降性能良好,自然沉降1小时,上清液可达总体积的75%以上。为确保溶液质量,推荐沉清2小时以上。本发明采用流态化洗涤技术,洗水用量仅为渣量的2--3倍,渣被洗到中性,渣含钒(离子)小于0.05%;并且设施投资不到过滤设备的四分之一,操作费用很低,约为过滤的十分之一。
9、从含钒溶液中离子交换、脱洗、沉钒、热解得到产品的工艺方法已很成熟,不需作详细说明。本发明优于其它方法是进入钒溶液的杂质少;特别是用阳离子交换树脂处理生产水,既消除了废水对环境的污染,资源得到充分利用,又使系统中的杂质及时完全开路,返回系统的是去离子水,比一般江河水还纯净,从而可保证产品质量稳定优良。
本发明的生产过程自动化程度高,操作方便,运行可靠,可以大规模生产,钒收得率大于65%,生产成本比钠法和酸法更低,特别是完全消除了三废对环境的影响,矿产资源和热能得到充分利用,它是一种理想的从石煤钒矿中提取五氧化二钒的方法。
Claims (9)
1、一种从石煤钒矿中提取五氧化二钒的方法,其特征在于:矿石初碎后,配入矿石量5~15%的钙盐,混合进入球磨,制粒后送沸腾炉在700-1000℃焙烧,焙烧料加水进入湿式球磨机浆化球磨,加碳酸盐调溶液PH7.5-9.0,温度35-100℃条件下,机械搅拌浸出,溶液用离子交换树脂吸附,脱洗液沉淀偏钒酸铵,热解得到五氧化二钒产品。
2、根据权利要求1所述的方法,其特征在于:配加的钙盐为碳酸钙或氧化钙,其配加量为矿石量的5-15%,根据矿石成分调整加量。
3、根据权利要求1所述的方法,其特征在于:物料球磨在润湿式球磨机中进行,物料的含水率为3~10%,球磨料制粒的球粒直径为3-12mm。
4、根据权利要求1所述的方法,其特征在于:焙烧是在沸腾炉中或在回转窑中进行,焙烧温度700-1000℃,焙烧时间2-5小时。
5、根据权利要求1所述的方法,其特征在于:焙烧出炉料随即溜入水槽混合进入湿式球磨机浆化球磨,温度50-100℃,加水量为:料∶水=1∶3-5;湿磨料浆送机械搅拌槽浸出,温度35-100℃,加碳酸盐量为矿石量的5-10%,调整溶液PH值为7.5-9.0,浸出时间为1-4小时。
6、根据权利要求1所述的方法,其特征在于:可以将焙烧中的部分烟气鼓入浸出槽而利用其中的二氧化碳和热量。
7、根据权利要求1所述的方法,其特征在于:浸出矿浆放入重力沉降池,自然沉降2小时以上,重力沉降池的上清液送贮液池冷却到50℃以下,沉降池的底部浓泥送流态化洗涤槽,浓泥从上部中心加入,洗水从底部旋流向上,洗水量为渣量的2~3倍,洗水温度50-100℃,渣∶水=1∶2-3;洗涤槽的上部溢流液送湿球磨,底部排渣送堆渣池,渣在池中堆放72小时以上,重力挤压使渣含水从50%以上降到25%左右,水返回使用,渣中不含酸、碱和其它任何有害离子。
8、根据权利要求1所述的方法,其特征在于:贮液池中冷却到50℃以下的含钒溶液送到阴离子交换树脂柱吸附钒,排出液再送到阳离子交换树脂柱吸附铵和其它阳离子,两次吸附后的排出水已较纯净,可以返回使用或向外排放。
9、根据权利要求1所述的方法,其特征在于:吸附饱和钒的阴离子树脂用NaCl+NH4Cl的混合液脱洗,得到钒酸铵和钒酸钠的浓溶液,钒酸铵钠溶液送到沉钒池中加入NH4Cl,沉淀出偏钒酸铵结晶,偏钒酸铵经洗涤、甩干后,在400-550℃下热解得到99%以上的V205产品。