CN103834288A - Spraying paint formula and spraying process thereof - Google Patents

Spraying paint formula and spraying process thereof Download PDF

Info

Publication number
CN103834288A
CN103834288A CN201410088125.4A CN201410088125A CN103834288A CN 103834288 A CN103834288 A CN 103834288A CN 201410088125 A CN201410088125 A CN 201410088125A CN 103834288 A CN103834288 A CN 103834288A
Authority
CN
China
Prior art keywords
spraying
paint
polyurethane
coating process
mixing according
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201410088125.4A
Other languages
Chinese (zh)
Inventor
杨晓宇
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
NANTONG JIALONG PLASTIC Co Ltd
Original Assignee
NANTONG JIALONG PLASTIC Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by NANTONG JIALONG PLASTIC Co Ltd filed Critical NANTONG JIALONG PLASTIC Co Ltd
Priority to CN201410088125.4A priority Critical patent/CN103834288A/en
Publication of CN103834288A publication Critical patent/CN103834288A/en
Pending legal-status Critical Current

Abstract

The invention discloses a spraying paint formula and a spraying process thereof. The spraying paint comprises polyurethane primer, colored paint, polyurethane lacquer and Aksu lacquer. The spraying process comprises the steps: diluting the polyurethane primer and a curing agent by 40-50 percent after mixing according to weight ratio of 8:1, diluting the colored paint by 20-30 percent, diluting the polyurethane lacquer by 30-35 percent after mixing according to a weight ratio of 2:1, diluting to 1-1.2 after mixing according to a weight ratio of 2:1, and sequentially spraying according to an order of the primer, the colored paint and the lacquer. The paint disclosed by the invention is reasonable in formula, simple in process steps, convenient to operate, and high in efficiency, and the enterprise cost is greatly lowered, and the production efficiency is increased.

Description

A kind of spray paint formula and spraying coating process
 
Technical field
The present invention relates to a kind of spray paint formula and spraying coating process.
Background technology
Spray paint of the prior art batching is complicated, and making takes time and effort, and complex manufacturing technology, inconvenient operation, thereby has reduced working efficiency, has improved enterprise's production cost.
Summary of the invention
Goal of the invention: the present invention is directed to deficiency, propose a kind of working efficiency high and the rational spray paint formula of paint formulation and spraying coating process.
Technical scheme: a kind of spray paint formula of the present invention, described paint comprises polyurethane primer, colored paint, polyurethane lacquer and Aksu varnish, described polyurethane primer dilutes 40%~50% after mixing according to mass ratio 8:1 with solidifying agent, colored paint dilution 20%~30%, polyurethane lacquer dilutes 30%~35% after mixing according to mass ratio 2:1, and described Aksu varnish dilutes 1~1.2 after mixing according to mass ratio 2:1.
The invention also discloses a kind of spraying coating process, it is characterized in that: comprise following several step:
(1) upper part, and spray priming paint;
(2) toast;
(3) dust removal process is carried out on priming paint part surface;
(4) spraying colored paint, and carry out levelling;
(5) spraying varnish, and toast;
(6) examination and test of products;
(7) polished finish;
(8) product dress device, dispatches from the factory.
As preferably, described in step (2), baking time is 20~40 minutes.
As preferably, described in step (4), flow time is 5~15 minutes.
As preferably, described in step (5), baking time is 40~50 minutes.
Beneficial effect: paint formulation of the present invention is reasonable, processing step is simple, easy to operate, and this process efficiency is high, greatly reduces enterprise cost, has improved production efficiency.
Embodiment
Below in conjunction with specific embodiment, the invention will be further described:
Embodiment 1
A kind of spray paint formula, paint comprises polyurethane primer, colored paint, polyurethane lacquer and Aksu varnish, polyurethane primer dilutes 40%~50% after mixing according to mass ratio 8:1 with solidifying agent, viscosity is 14~15, colored paint dilution 20%~30%, viscosity 16~18, polyurethane lacquer dilutes 30%~35% after mixing according to mass ratio 2:1, viscosity is 14~15, and described Aksu varnish dilutes 1~1.2 after mixing according to mass ratio 2:1, and viscosity is 14~15.
The spraying coating process of above-mentioned spray paint, comprises following several step:
(1) upper part, and spray priming paint;
(2) toast, baking time is 20~40 minutes;
(3) dust removal process is carried out on priming paint part surface;
(4) spraying colored paint, and carry out levelling, flow time is 5~15 minutes;
(5) spraying varnish, and toast, baking time is 40~50 minutes;
(6) examination and test of products;
(7) polished finish;
(8) product dress device, dispatches from the factory.

Claims (5)

1. a spray paint formula, it is characterized in that: described paint comprises polyurethane primer, colored paint, polyurethane lacquer and Aksu varnish, described polyurethane primer dilutes 40%~50% after mixing according to mass ratio 8:1 with solidifying agent, colored paint dilution 20%~30%, polyurethane lacquer dilutes 30%~35% after mixing according to mass ratio 2:1, and described Aksu varnish dilutes 1~1.2 after mixing according to mass ratio 2:1.
2. a spraying coating process, is characterized in that: comprise following several step:
(1) upper part, and spray priming paint;
(2) toast;
(3) dust removal process is carried out on priming paint part surface;
(4) spraying colored paint, and carry out levelling;
(5) spraying varnish, and toast;
(6) examination and test of products;
(7) polished finish;
(8) product dress device, dispatches from the factory.
3. a kind of spraying coating process according to claim 2, is characterized in that: described in step (2), baking time is 20~40 minutes.
4. a kind of spraying coating process according to claim 2, is characterized in that: described in step (4), flow time is 5~15 minutes.
5. a kind of spraying coating process according to claim 2, is characterized in that: described in step (5), baking time is 40~50 minutes.
CN201410088125.4A 2014-03-12 2014-03-12 Spraying paint formula and spraying process thereof Pending CN103834288A (en)