CN103114226A - 义齿合金材料 - Google Patents

义齿合金材料 Download PDF

Info

Publication number
CN103114226A
CN103114226A CN2013100482175A CN201310048217A CN103114226A CN 103114226 A CN103114226 A CN 103114226A CN 2013100482175 A CN2013100482175 A CN 2013100482175A CN 201310048217 A CN201310048217 A CN 201310048217A CN 103114226 A CN103114226 A CN 103114226A
Authority
CN
China
Prior art keywords
alloy material
cochrome
false tooth
tooth
cost
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN2013100482175A
Other languages
English (en)
Inventor
刘嘉
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
AI JIA DENTAL LAB Co Ltd
Original Assignee
AI JIA DENTAL LAB Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by AI JIA DENTAL LAB Co Ltd filed Critical AI JIA DENTAL LAB Co Ltd
Priority to CN2013100482175A priority Critical patent/CN103114226A/zh
Publication of CN103114226A publication Critical patent/CN103114226A/zh
Pending legal-status Critical Current

Abstract

一种义齿合金材料,以质量百分数计,包括以下组分:Co58.00-63.00%、Cr22.00-26%、W6.00-10.00%、Mo2.30-2.80%、Nb0.80-1.10%、Mn0.80-1.10%、Si0.80-1.10%、Fe0.80-1.10%。本发明的钴铬合金避免使用价格高昂的贵金属原料,摒弃了对人体有害的Be元素,以价格低廉、安全无毒的Co、Cr、W、Mo、Nb、Mn、Si和Fe元素为原料,制得的钴铬合金成本低,安全无毒,耐腐蚀性强,抗拉强度大,线膨胀系数小,硬度大,屈服强度大,是一种制作烤瓷牙优秀材料。

Description

义齿合金材料
技术领域
本发明涉及牙科修复领域,特别是涉及义齿合金材料。
背景技术
牙病是一种常见的病患,发病率很高。牙体缺损、牙列缺失则在牙病中的十分常见,通常采用义齿进行修复。
烤瓷牙是一种常用的义齿,一般采用合金材料制作烤瓷牙,制作烤瓷牙的合金必须满足以下条件:(1)生物相容性好,对人体无毒无害;(2)化学性能稳定,必须要有优秀的抗氧化及耐腐蚀性;(3)物理性能稳定,必须要有很高的强度。
一般的烤瓷牙分为贵金属烤瓷牙和非贵金属烤瓷牙,贵金属烤瓷牙是性能最好的烤瓷牙,以黄金烤瓷牙为例,生物相容性最好,其他相关性能也特别优秀,但贵金属材料价格昂贵,因此贵金属烤瓷牙价格高昂,一般患者难以承担。非贵金属烤瓷牙的合金材料中一般都含有Be元素,Be元素对人体有毒性作用,会危害使用者的健康。
发明内容
基于此,有必要针对贵金属材料价格昂贵和非贵金属合金材料对人体造成危害的问题,提供一种价格低廉、安全、性能优秀的义齿合金材料。
一种义齿合金材料,以质量百分数计,包括以下组分:Co58.00-63.00%、Cr22.00-26%、W6.00-10.00%、Mo2.30-2.80%、Nb0.80-1.10%、Mn0.80-1.10%、Si0.80-1.10%、Fe0.80-1.10%。
在其中一些实施例中,所述义齿合金材料包括以下组分:Co60.00-62.00%、Cr23.00-25%、W7.00-9.00%、Mo2.40-2.75%、Nb0.90-1.05%、Mn0.90-1.05%、Si0.90-1.05%、Fe0.90-1.05%。
在其中一个实施例中,所述义齿合金材料包括以下组分:Co61.00%、Cr24.00%、W8.00%、Mo2.50%、Nb1.00%、Mn1.00%、Si1.00%、Fe1.00%。
本发明的义齿合金材料包含Co、Cr、W、Mo、Nb、Mn、Si和Fe元素。各元素的功效如下:
Co元素坚硬、延展性好,能够提高钴铬合金的硬度和强度。
Cr能够在钴铬合金表面形成致密的Cr2O3保护膜,提高钴铬合金的抗氧化和耐腐蚀性。
W元素熔点高,化学性质稳定,能够提高钴铬合金对酸的耐受力。
Mo是固溶强化元素,能提高钴铬合金在硫酸、盐酸等还原酸以及氢氟酸气体中的耐腐蚀性。
Nb能够稳定钴铬合金组织,使钴铬合金不容易产生晶面腐蚀。
Mn的加入使钴铬合金坚硬而富有韧性。
Si不溶于硝酸和盐酸,可以提高钴铬合金对酸的耐腐蚀性。
Fe的主要作用是提高钴铬合金的硬度和屈服强度,并促进钴铬合金与瓷粉的结合能力。
本发明的钴铬合金避免使用价格高昂的贵金属原料,摒弃了对人体有害的Be元素,以价格低廉、安全无毒的Co、Cr、W、Mo、Nb、Mn、Si和Fe元素为原料,制得的钴铬合金成本低,安全无毒,耐腐蚀性强,抗拉强度大,线膨胀系数小,硬度大,屈服强度大,是一种制作烤瓷牙优秀材料。
具体实施方式
以下结合具体实施例对本发明做进一步的阐述。
实施例1钴铬合金
本实施例的义齿合金材料,以质量百分数计,包括以下组分:Co58.00%、Cr26.00%、W9.50%、Mo2.50%、Nb1.10%、Mn1.10%、Si0.80%、Fe1.00%。
实施例2钴铬合金
本实施例的义齿合金材料,以质量百分数计,包括以下组分:Co62.00%、Cr23.00%、W8.50%、Mo2.70%、Nb0.95%、Mn0.90%、Si1.05%、Fe0.90%。
实施例3钴铬合金
本实施例的义齿合金材料,以质量百分数计,包括以下组分:Co61.00%、Cr24.00%、W8.50%、Mo2.50%、Nb1.00%、Mn1.00%、Si1.00%、Fe1.00%。
实施例4钴铬合金力学性能测试
对实施例1、2、3的钴铬合金的抗拉强度、热膨胀系数、洛氏硬度、屈服强度进行检测。检测结果如表1。
表1钴铬合金力学性能测试结果表
Figure BSA00000853666000041
从表1可看出实施例1、2、3的钴铬合金的抗拉强度大,线膨胀系数小,洛氏硬度大,屈服强度大。
实施例5耐腐性测试
取实施倒1、2、3的钴铬合金进行人工唾液腐蚀失重实验,考察上述钴铬合金的耐腐蚀性。结果如表2所示。
表2钴铬合金耐腐蚀性测试结果表
Figure BSA00000853666000051
从表2可看出实施例1、2、3的钴铬合金具有优秀的耐腐蚀性。
实施例6成本核算
本发明实施例1、2、3的钴铬合金(1Kg)的成本分别如表3、4、5所示。
表3实施例1的钴铬合金(1Kg)的成本
组分 价格(元/kg) 处方含量(g) 处方成本(元)
Co 212 580 122.96
Cr 62 260 16.12
W 260 95 24.7
Mo 72 25 1.8
Nb 100 11 1.1
Mn 150 11 1.65
Si 34 8 0.27
Fe 15 10 0.15
合计 1000 168.75
表4实施例2的钴铬合金(1Kg)的成本
组分 价格(元/kg) 处方含量(g) 处方成本(元)
Co 212 620 131.44
Cr 62 230 14.26
W 260 85 22.1
Mo 72 27 1.94
Nb 100 9.5 0.95
Mn 150 9 1.35
Si 34 10.5 0.36
Fe 15 9 0.14
合计 1000 172.54
表5实施例3的钴铬合金(1Kg)的成本
组分 价格(元/kg) 处方含量(g) 处方成本(元)
Co 212 610 129.32
Cr 62 240 14.88
W 260 85 22.1
Mo 72 25 1.8
Nb 100 10 1
Mn 150 10 1.5
Si 34 10 0.34
Fe 15 10 0.15
合计 1000 171.09
本发明实施例1、2、3的钴铬合金与贵金属合金的成本对比如表6所示。
表6实施例1、2、3的钴铬合金与贵金属合金的成本对比
Figure BSA00000853666000071
由表6可知,本发明实施例1、2、3的钴铬合金相比贵金属合金有很大的价格优势,成本低很多,易于被患者接受。
以上所述实施例仅表达了本发明的几种实施方式,其描述较为具体和详细,但并不能因此而理解为对本发明专利范围的限制。应当指出的是,对于本领域的普通技术人员来说,在不脱离本发明构思的前提下,还可以做出若干变形和改进,这些都属于本发明的保护范围。因此,本发明专利的保护范围应以所附权利要求为准。

Claims (3)

1.一种义齿合金材料,其特征在于,以质量百分数计,包括以下组分:Co58.00-63.00%、Cr22.00-26%、W6.00-10.00%、Mo2.30-2.80%、Nb0.80-1.10%、Mn0.80-1.10%、Si0.80-1.10%、Fe0.80-1.10%。
2.根据权利要求1所述的义齿合金材料,其特征在于,包括以下组分:Co60.00-62,00%、Cr23.00-25%、W7.00-9.00%、Mo2.40-2.75%、Nb0.90-1.05%、Mn0.90-1,05%、Si0.90-1.05%、Fe0.90-1.05%。
3.根据权利要求2所述的义齿合金材料,其特征在于,包括以下组分:Co61.00%、Cr24.00%、W8.50%、Mo2.50%、Nb1.00%、Mn1.00%、Si1.00%、Fe1.00%。
CN2013100482175A 2013-02-05 2013-02-05 义齿合金材料 Pending CN103114226A (zh)