[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

CN106436373A - Pigment printing technology of cotton ramie fabric - Google Patents

Pigment printing technology of cotton ramie fabric Download PDF

Info

Publication number
CN106436373A
CN106436373A CN201610769235.6A CN201610769235A CN106436373A CN 106436373 A CN106436373 A CN 106436373A CN 201610769235 A CN201610769235 A CN 201610769235A CN 106436373 A CN106436373 A CN 106436373A
Authority
CN
China
Prior art keywords
pigment
printing
cotton
cotton fibriia
pigment printing
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Pending
Application number
CN201610769235.6A
Other languages
Chinese (zh)
Inventor
温明华
陶建玉
尹寿虎
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Jiangsu Boboxiong Textiles Co.,Ltd.
Original Assignee
Suzhou Hengxin Knitting Printing & Dyeing Co Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Suzhou Hengxin Knitting Printing & Dyeing Co Ltd filed Critical Suzhou Hengxin Knitting Printing & Dyeing Co Ltd
Priority to CN201610769235.6A priority Critical patent/CN106436373A/en
Publication of CN106436373A publication Critical patent/CN106436373A/en
Pending legal-status Critical Current

Abstract

The invention discloses a pigment printing technology of a cotton ramie fabric. The pigment printing technology of the cotton ramie fabric adopts a technological process of biological enzyme modifying pretreatment, bleaching pretreatment, washing, printing pretreatment, printing, steaming fixation, afterfinish and washing drying. The technological process comprises the steps of conducting firstly the biological enzyme modifying pretreatment before the printing, conducting modifying treatment on the cotton ramie fabric, and then conducting bleaching pretreatment technology, which, on the one hand, overcomes the disadvantage that the dyeing keynote of the cotton ramie fabric is dark, on the other hand, effectively increases the color fastness of the printing of the cotton ramie fabric; in addition, specially made pigment printing paste is adopted to conduct printing and warm water washing and hot wind drying are adopted in the washing technology so as to stimulate chemical tolerance of the pigment and strengthen washing resistance performance and the sorption rate of the pigment. The pigment printing technology of cotton ramie fabric has the advantages of having fluent printing, bright color, proper color depth, high rub resistance fastness after the print, proper color and luster vividness, simple technology and the like.

Description

A kind of pigment printing technique of cotton fibriia fabric
Technical field
The present invention relates to the processing method of fabric, more particularly, to a kind of pigment printing technique of cotton fibriia fabric.
Background technology
Pigment printing is to be used macromolecular compound as adhesive, mechanical for pigment is adhered on fabric, postmenstruation Process to obtain and have certain elastic, wear-resisting, resistance to hand rubbing, the printing method of the transparent resin decorative pattern of resistance to fold, coating bone in fiber On mechanism to anchor at mechanism on fiber with other dyestuffs different, it is to form prison, colourless on fabric by adhesive Bright film, paint machine is covered on fabric, therefore, is applied to most of fibers with pigment printing, and process is simple, print Effect processed is preferable.
But on the one hand due to cotton fibriia fabric fabric itself, the pigment printing for cotton fibriia fabric exists But do not reach expected effect in practical application, there are a lot of problems, such as after printing, its fastness to rubbing is not high, bright in colour Spend inadequate problem, thus limit the development of pigment printing.
Accordingly, it would be desirable to a kind of new technology solves the above problems.
Content of the invention
Goal of the invention:In order to solve the problems of prior art, the invention provides a kind of printing quality is smooth, on Color depth is suitable, the pigment printing technique of the cotton fibriia fabric that after printing, fastness to rubbing is high, colour brightness is suitable.
Technical scheme:For reaching above-mentioned purpose, the present invention employs the following technical solutions:A kind of coating of cotton fibriia fabric Printing technology, comprises the following steps:
(1) enzyme modified pre-treatment:Cotton fibriia fabric is carried out enzyme modified pre-treatment, bath raio 1:6-1:9, make Biology enzyme is acidic cellulase, protease, amylase three 3:1:1 mixture, biological enzyme dosage 0.7-1.2g/L, Process time 25-35min, pH is adjusted to 4-5;
(2) bleach pre-treatment:Carry out bleaching, bath raio 1 by carrying out the cotton fibriia fabric after enzyme modified process: 6-1:9, add sodium metasilicate, the mixed bleach agent of 5-9g/L of 2-4g/L, bleaching is carried out using cold pad--batch single bath process technique;
(3) wash:Ramie cotton fabric warm water after bleaching is washed to be dehydrated after 2 times and does to 8 one-tenth;
(4) stamp pre-treatment:First preliminary drying process is carried out to ramie cotton fabric before stamp, combined using hypo-hyperthermia-low-temperature phase Mode, specifically 50-60 DEG C first low temperature preliminary drying 5-8min, be warming up to 100-110 DEG C of high temperature preliminary drying 5-8min, then be cooled to 50-60 DEG C of low temperature preliminary drying 3-6min;
(5) stamp:Prepare paint-printing colour size, the preparation of described paint-printing colour size is entered by weight according to formula as below Row is prepared:Inorganic color pigment 15-25%, filler 5-10%, nano material 2-4%, dispersant 2-4%, shitosan 2-4%, The vinyl monomer 3-5% of amide-containing, crosslinking agent 3-6%, textile binding agent 6-13%, thickener 3-5%, mineral element 0.2-0.5%, pH adjusting agent 0.2-3%, the water of surplus;Adopt pigment printing equipment using above-mentioned coating print paste to preliminary drying Cotton fibriia fabric afterwards carries out stamp process;
(6) vapour steaming colour fixing:After above-mentioned fabrics are carried out low temperature individual composition 10-15min at 55-75 DEG C, temperature is increased to 115-125 DEG C carries out fixation treatment;
(7) Final finishing:Final finishing is carried out using high temperature heat setting process;
(8) washing is dried:Cotton fibriia fabric through Final finishing is adopted hot-air seasoning after warm water washing.
Further, in step (2), bleaching temperature is 50-60 DEG C.
Further, in step (2), the bleaching time is 30-40min.
Further, mixed bleach agent described in step (2) is alkyl two phenolic ether disulfonate surfactants, secondary chlorine Sour sodium, hydrogen peroxide mass ratio are 1:2:2 mixture.
Further, inorganic color pigment described in step (5) has selected from green grass or young crops, fuchsin, Huang, indigo plant, green, red, orange, purple Colour with brown.
Further, crosslinking agent described in step (5) is resinae crosslinking agent.
Further, textile binding agent described in step (5) is aqueous polyurethane adhesive and acetates adhesive Mass ratio is 1:1 mixture.
Further, thickener described in step (5) is lignin sulfonic acid sodium salt and stearic acid mass ratio is 3:1 mixed Compound.
Further, filler described in step (5) is titanium dioxide.
Further, the temperature washing the warm water of use described in step (8) is 45-55 DEG C, and wash time is 12- 20min, 2-3 rear 70-75 DEG C of hot-air seasoning of washing.
Beneficial effect:A kind of pigment printing technique of cotton fibriia fabric provided by the present invention, using enzyme modified The technique that pre-treatment → bleaching pre-treatment → washing → stamp pre-treatment → stamp → vapour steaming colour fixing → Final finishing → washing is dried Flow process, has carried out processing before enzyme modified before stamp first, cotton fibriia is modified process, then before being bleached Handling process, on the one hand improves the partially dark shortcoming of cotton fibriia textile dyeing keynote, is on the other hand effectively increased cotton fibriia The color fastness of textile printing, carries out stamp using special paint-printing colour size in addition, and washing process adopts warm water washing+hot blast Dry, stimulate the chemical resistance of coating, strengthen its wash durability and sorption rate;The present invention has that stamp is smooth, color is fresh Gorgeous, colouring appropriate depth, print after fastness to rubbing is high, colour brightness is suitable, process is simple the advantages of.
Specific embodiment
With reference to specific embodiment, the present invention is further described:
Embodiment 1:
A kind of pigment printing technique of cotton fibriia fabric, comprises the following steps:
(1) enzyme modified pre-treatment:Cotton fibriia fabric is carried out enzyme modified pre-treatment, bath raio 1:6, use Biology enzyme is acidic cellulase, protease, amylase three 3:1:1 mixture, biological enzyme dosage 0.7g/L, process time 25min, pH are adjusted to 4;
(2) bleach pre-treatment:Carry out bleaching, bath raio 1 by carrying out the cotton fibriia fabric after enzyme modified process: 6, add sodium metasilicate, the mixed bleach agent of 5g/L of 2g/L, bleaching, treatment temperature are carried out using cold pad--batch single bath process technique For 50 DEG C, process time is 30min, and mixed bleach agent is alkyl two phenolic ether disulfonate surfactants, sodium hypochlorite, dioxygen Water quality is than for 1:2:2 mixture;
(3) wash:Ramie cotton fabric warm water after bleaching is washed to be dehydrated after 2 times and does to 8 one-tenth;
(4) stamp pre-treatment:First preliminary drying process is carried out to ramie cotton fabric before stamp, combined using hypo-hyperthermia-low-temperature phase Mode, specifically 50 DEG C first low temperature preliminary drying 5min, be warming up to 100 DEG C of high temperature preliminary drying 5min, then be cooled to 50 DEG C of low temperature preliminary dryings 3min;
(5) stamp:Prepare paint-printing colour size, the preparation of described paint-printing colour size is entered by weight according to formula as below Row is prepared:Inorganic color pigment 15%, filler 5%, nano material 2%, dispersant 2%, shitosan 2%, the second of amide-containing Alkenyl monomer 3%, crosslinking agent 3%, textile binding agent 6%, thickener 3%, mineral element 0.2%, pH adjusting agent 0.2%, remaining The water of amount;Pre-baked cotton fibriia fabric is carried out at stamp using pigment printing equipment using above-mentioned coating print paste Reason;Wherein, described inorganic color pigment have selected from green grass or young crops, fuchsin, Huang, indigo plant, green, red, orange, purple and brown colour;Described friendship Connection agent is resinae crosslinking agent;Described textile binding agent is aqueous polyurethane adhesive is 1 with acetates adhesive mass ratio: 1 mixture;Described thickener is lignin sulfonic acid sodium salt is 3 with stearic acid mass ratio:1 mixture;Described filler is titanium White powder;
(6) vapour steaming colour fixing:After above-mentioned fabrics are carried out low temperature individual composition 10min at 55-75 DEG C, temperature is increased to 115 DEG C carry out fixation treatment;
(7) Final finishing:Final finishing is carried out using high temperature heat setting process;
(8) washing is dried:Cotton fibriia fabric through Final finishing is adopted hot-air seasoning after warm water washing, washing uses Warm water temperature be 45 DEG C, wash time be 12min, washing 2 times after 70 DEG C of hot-air seasonings.Embodiment 2:
A kind of pigment printing technique of cotton fibriia fabric, comprises the following steps:
(1) enzyme modified pre-treatment:Cotton fibriia fabric is carried out enzyme modified pre-treatment, bath raio 1:9, use Biology enzyme is acidic cellulase, protease, amylase three 3:1:1 mixture, biological enzyme dosage 1.2g/L, process time 35min, pH are adjusted to 5;
(2) bleach pre-treatment:Carry out bleaching, bath raio 1 by carrying out the cotton fibriia fabric after enzyme modified process: 9, add sodium metasilicate, the mixed bleach agent of 9g/L of 4g/L, bleaching, treatment temperature are carried out using cold pad--batch single bath process technique For 60 DEG C, process time is 40min, and mixed bleach agent is alkyl two phenolic ether disulfonate surfactants, sodium hypochlorite, dioxygen Water quality is than for 1:2:2 mixture;
(3) wash:Ramie cotton fabric warm water after bleaching is washed to be dehydrated after 2 times and does to 8 one-tenth;
(4) stamp pre-treatment:First preliminary drying process is carried out to ramie cotton fabric before stamp, combined using hypo-hyperthermia-low-temperature phase Mode, specifically 60 DEG C first low temperature preliminary drying 8min, be warming up to 110 DEG C of high temperature preliminary drying 8min, then be cooled to 60 DEG C of low temperature preliminary dryings 6min;
(5) stamp:Prepare paint-printing colour size, the preparation of described paint-printing colour size is entered by weight according to formula as below Row is prepared:Inorganic color pigment 25%, filler 10%, nano material 4%, dispersant 4%, shitosan 4%, the second of amide-containing Alkenyl monomer 5%, crosslinking agent 6%, textile binding agent 13%, thickener 5%, mineral element 0.5%, pH adjusting agent 3%, surplus Water;Using above-mentioned coating print paste, stamp process is carried out to pre-baked cotton fibriia fabric using pigment printing equipment; Wherein, described inorganic color pigment have selected from green grass or young crops, fuchsin, Huang, indigo plant, green, red, orange, purple and brown colour;Described crosslinking agent For resinae crosslinking agent;Described textile binding agent is aqueous polyurethane adhesive is 1 with acetates adhesive mass ratio:1 Mixture;Described thickener is lignin sulfonic acid sodium salt is 3 with stearic acid mass ratio:1 mixture;Described filler is titanium white Powder;
(6) vapour steaming colour fixing:Above-mentioned fabrics are carried out at 75 DEG C temperature after low temperature individual composition 15min and be increased to 125 DEG C Carry out fixation treatment;
(7) Final finishing:Final finishing is carried out using high temperature heat setting process;
(8) washing is dried:Cotton fibriia fabric through Final finishing is adopted hot-air seasoning after warm water washing, washing uses Warm water temperature be 55 DEG C, wash time be 20min, washing 3 times after 75 DEG C of hot-air seasonings.Embodiment 3:
A kind of pigment printing technique of cotton fibriia fabric, comprises the following steps:
(1) enzyme modified pre-treatment:Cotton fibriia fabric is carried out enzyme modified pre-treatment, bath raio 1:7, use Biology enzyme is acidic cellulase, protease, amylase three 3:1:1 mixture, biological enzyme dosage 0.9g/L, process time 30min, pH are adjusted to 4.5;
(2) bleach pre-treatment:Carry out bleaching, bath raio 1 by carrying out the cotton fibriia fabric after enzyme modified process: 8, add sodium metasilicate, the mixed bleach agent of 7g/L of 3g/L, bleaching, treatment temperature are carried out using cold pad--batch single bath process technique For 55 DEG C, process time is 35min, and mixed bleach agent is alkyl two phenolic ether disulfonate surfactants, sodium hypochlorite, dioxygen Water quality is than for 1:2:2 mixture;
(3) wash:Ramie cotton fabric warm water after bleaching is washed to be dehydrated after 2 times and does to 8 one-tenth;
(4) stamp pre-treatment:First preliminary drying process is carried out to ramie cotton fabric before stamp, combined using hypo-hyperthermia-low-temperature phase Mode, specifically 55 DEG C first low temperature preliminary drying 6min, be warming up to 105 DEG C of high temperature preliminary drying 7min, then be cooled to 55 DEG C of low temperature preliminary dryings 5min;
(5) stamp:Prepare paint-printing colour size, the preparation of described paint-printing colour size is entered by weight according to formula as below Row is prepared:Inorganic color pigment 20%, filler 8%, nano material 3%, dispersant 3%, shitosan 3%, the second of amide-containing Alkenyl monomer 4%, crosslinking agent 5%, textile binding agent 10%, thickener 4%, mineral element 0.4%, pH adjusting agent 1.4%, remaining The water of amount;Pre-baked cotton fibriia fabric is carried out at stamp using pigment printing equipment using above-mentioned coating print paste Reason;Wherein, described inorganic color pigment have selected from green grass or young crops, fuchsin, Huang, indigo plant, green, red, orange, purple and brown colour;Described friendship Connection agent is resinae crosslinking agent;Described textile binding agent is aqueous polyurethane adhesive is 1 with acetates adhesive mass ratio: 1 mixture;Described thickener is lignin sulfonic acid sodium salt is 3 with stearic acid mass ratio:1 mixture;Described filler is titanium White powder;
(6) vapour steaming colour fixing:Above-mentioned fabrics are carried out at 65 DEG C temperature after low temperature individual composition 13min and be increased to 120 DEG C Carry out fixation treatment;
(7) Final finishing:Final finishing is carried out using high temperature heat setting process;
(8) washing is dried:Cotton fibriia fabric through Final finishing is adopted hot-air seasoning after warm water washing, washing uses Warm water temperature be 50 DEG C, wash time be 18min, washing 2 times after 73 DEG C of hot-air seasonings.
Take and above-mentioned complete each 20cm × 20cm of cotton fibriia article that pigment printing obtains, using ISO105C06: 1994+Corl:2002 method, under the conditions of 25 DEG C, machine washing nature dries, and tests water-fastness grade, test result such as following table institute Show:
Physical index Embodiment 1 Embodiment 2 Embodiment 3 Traditional handicraft
Water-fastness grade 4-5 5 4-5 3-4
Can be seen that from upper table data, using the pigment printing cotton fibriia fabric made by embodiment 1-3, compared with prior art Compare, there is significantly water-fastness advantage, and printing quality is smooth, paint appropriate depth, not fugitive color.
It should be pointed out that above specific embodiment is only illustrative of the invention and is not intended to limit the scope of the invention, After having read the present invention, the modification of the various equivalent form of values to the present invention for the those skilled in the art all falls within power appended by the application Profit requires limited range.

Claims (10)

1. a kind of pigment printing technique of cotton fibriia fabric is it is characterised in that comprise the following steps:
(1) enzyme modified pre-treatment:Cotton fibriia fabric is carried out enzyme modified pre-treatment, bath raio 1:6-1:9, use Biology enzyme is acidic cellulase, protease, amylase three 3:1:1 mixture, biological enzyme dosage 0.7-1.2g/L, process Time 25-35min, pH are adjusted to 4-5;
(2) bleach pre-treatment:Carry out bleaching, bath raio 1 by carrying out the cotton fibriia fabric after enzyme modified process:6-1: 9, add sodium metasilicate, the mixed bleach agent of 5-9g/L of 2-4g/L, bleaching is carried out using cold pad--batch single bath process technique;
(3) wash:Ramie cotton fabric warm water after bleaching is washed to be dehydrated after 2 times and does to 8 one-tenth;
(4) stamp pre-treatment:First preliminary drying process is carried out to ramie cotton fabric before stamp, the side combining using hypo-hyperthermia-low-temperature phase Formula, specifically 50-60 DEG C first low temperature preliminary drying 5-8min, it is warming up to 100-110 DEG C of high temperature preliminary drying 5-8min, then be cooled to 50-60 DEG C low temperature preliminary drying 3-6min;
(5) stamp:Prepare paint-printing colour size, the preparation of described paint-printing colour size is joined by weight according to formula as below System:Inorganic color pigment 15-25%, filler 5-10%, nano material 2-4%, dispersant 2-4%, shitosan 2-4%, contain acyl The vinyl monomer 3-5% of amido, crosslinking agent 3-6%, textile binding agent 6-13%, thickener 3-5%, mineral element 0.2- 0.5%th, the water of pH adjusting agent 0.2-3%, surplus;Adopt pigment printing equipment using above-mentioned coating print paste to pre-baked Cotton fibriia fabric carries out stamp process;
(6) vapour steaming colour fixing:After above-mentioned fabrics are carried out low temperature individual composition 10-15min at 55-75 DEG C, temperature is increased to 115- 125 DEG C carry out fixation treatment;
(7) Final finishing:Final finishing is carried out using high temperature heat setting process;
(8) washing is dried:Cotton fibriia fabric through Final finishing is adopted hot-air seasoning after warm water washing.
2. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Bleaching in step (2) Treatment temperature is 50-60 DEG C.
3. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Bleaching in step (2) Process time is 30-40min.
4. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Described in step (2) Mixed bleach agent is alkyl two phenolic ether disulfonate surfactants, sodium hypochlorite, hydrogen peroxide mass ratio are 1:2:2 mixing Thing.
5. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Described in step (5) Inorganic color pigment have selected from green grass or young crops, fuchsin, Huang, indigo plant, green, red, orange, purple and brown colour.
6. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Described in step (5) Crosslinking agent is resinae crosslinking agent.
7. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Described in step (5) Textile binding agent is aqueous polyurethane adhesive is 1 with acetates adhesive mass ratio:1 mixture.
8. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Described in step (5) Thickener is lignin sulfonic acid sodium salt is 3 with stearic acid mass ratio:1 mixture.
9. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Described in step (5) Filler is titanium dioxide.
10. cotton fibriia fabric according to claim 1 pigment printing technique it is characterised in that:Described in step (8) The temperature of the warm water that washing uses is 45-55 DEG C, and wash time is 12-20min, 70-75 DEG C of hot-air seasoning after washing 2-3 time.
CN201610769235.6A 2016-08-30 2016-08-30 Pigment printing technology of cotton ramie fabric Pending CN106436373A (en)