CN105644176B - A kind of processing method of glitter powder bat printing film - Google Patents
A kind of processing method of glitter powder bat printing film Download PDFInfo
- Publication number
- CN105644176B CN105644176B CN201610019451.9A CN201610019451A CN105644176B CN 105644176 B CN105644176 B CN 105644176B CN 201610019451 A CN201610019451 A CN 201610019451A CN 105644176 B CN105644176 B CN 105644176B
- Authority
- CN
- China
- Prior art keywords
- glitter powder
- silicon oil
- primer
- membranes
- pet silicon
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Active
Abstract
The invention discloses a kind of processing method of glitter powder bat printing film, feature is first to modulate base oil, then by base oil and open profit in mass ratio be 3:2 ratio uniform mixing, obtain primer, then tune machine is carried out to screen process press, primer is coated by screen process press to one side PET silicon oil membranes again, after the completion of coating, passed through toward the one side with primer artificial or tremble powder machine and uniformly spread glitter powder, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces, finally dries the one side PET silicon oil membranes of one side dusting, obtains glitter powder bat printing film;It is covered in as long as advantage is the glitter powder bat printing film for processing to obtain by this method on the printing surface of printed article, can be by glitter powder bat printing to printed article by heating pressurization, make printed article that there is stronger visual effect, particularly suitable for the glitter powder bat printing for the printing paper printed to non-aqueous inks, it is easy to operate and pad printing method is simple, without special equipment, it is adapted to a small amount of processing such as personalized customization, and cost is relatively low.
Description
Technical field
The present invention relates to glitter powder printing, more particularly to a kind of processing method of glitter powder bat printing film.
Background technology
Glitter powder is also gold and silver piece, diamante, flashlight powder etc., is passed through by the plating material of the high different-thickness of smart brightness
Accurate cutting forms.The treatment material unique as a kind of effect, glitter powder are widely used in christmas crafts product, candle work
Skill, cosmetics, silk-screen printing industry, ornament materials etc., for strengthening the visual effect of product, decorative parts bumps are made to have layer
It is secondary, more third dimension.At present, glitter powder is printed on the materials such as paper, cloth, metal and generally required by special equipment, and must
Batch production that need be certain, and for some draw a design making or personalized customization, then cost is very high, causes its application by very
Big limitation.
The content of the invention
The technical problems to be solved by the invention be to provide one kind can meet personalized customization etc. on a small quantity processing and cost compared with
The processing method of glitter powder bat printing film low, without special equipment.
Technical scheme is used by the present invention solves above-mentioned technical problem:A kind of processing method of glitter powder bat printing film,
Including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 30~37%, polyvinyl chloride 20~
23%th, calcium carbonate 17~18%, unsaturated oleic acid 5~10%, phthalic anhydride 7~8%, antimony oxide 6~8%, O-phthalic
Sour didecyl 0.4~0.6%, dibasic calcium stearate 0.6~0.9%, trioctyl phosphate 0.4~0.8%, Tissuemat E 0.6~
1.2%th, tristerin 0.2~0.3%, alkyl phthalates 0.5~0.7%, carbon black 0.5~0.6%, acrylic acid copolymer
The above each component of thing 4~6% uniformly mixes at normal temperatures, obtains base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The net of 250~300 mesh, 3 layers of photosensitive layer is installed on screen process press
Version, take the soft-slab that hardness is 75HRC or 90HRC to be used as scraper plate, during installation, control the gradient of scraper plate and tool rest as 35~40 °;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >=
230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen
Printed edge is retracted 3~7mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into list by screen process press
On the silicone oil face of face PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine
Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
Compared with prior art, as long as it is an advantage of the invention that the glitter powder bat printing film for processing to obtain by this method covers
On the printing surface of printed article, it on glitter powder bat printing to printed article, can will make printed article with stronger by heating pressurization
Visual effect, particularly suitable for the glitter powder bat printing for the printing paper printed to non-aqueous inks, and pad printing method is simple,
It is easy to operate, without special equipment, it is adapted to a small amount of processing such as personalized customization, and cost is relatively low.
Embodiment
The present invention is described in further detail with reference to embodiments.
Embodiment one:A kind of processing method of glitter powder bat printing film, including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 30%, polyvinyl chloride 23%, calcium carbonate
17%th, unsaturated oleic acid 8%, phthalic anhydride 7.5%, antimony oxide 6%, didecyl phthalate 0.4%, dibasic are hard
Resin acid calcium 0.6%, trioctyl phosphate 0.8%, Tissuemat E 1.2%, tristerin 0.3%, alkyl phthalates 0.7%,
Carbon black 0.5%, the above each component of acrylic copolymer 4% uniformly mix at normal temperatures, obtain base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The half tone of 300 mesh, 3 layers of photosensitive layer is installed on screen process press, taken hard
Soft-slab for 75HRC is spent as scraper plate, and during installation, it is 35 ° to control the gradient of scraper plate and tool rest;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >=
230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen
Printed edge is retracted 5mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side by screen process press
On the silicone oil face of PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine
Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
Embodiment two:A kind of processing method of glitter powder bat printing film, including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 35%, polyvinyl chloride 20%, calcium carbonate
17.8%th, unsaturated oleic acid 5%, phthalic anhydride 7.5%, antimony oxide 6.5%, didecyl phthalate 0.6%, disalt
Base calcium stearate 0.9%, trioctyl phosphate 0.4%, Tissuemat E 1.0%, tristerin 0.2%, alkyl phthalates
0.5%th, carbon black 0.6%, the above each component of acrylic copolymer 4% uniformly mix at normal temperatures, obtain base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The half tone of 250 mesh, 3 layers of photosensitive layer is installed on screen process press, taken hard
Soft-slab for 90HRC is spent as scraper plate, and during installation, it is 35 ° to control the gradient of scraper plate and tool rest;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >=
230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen
Printed edge is retracted 7mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side by screen process press
On the silicone oil face of PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine
Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
Embodiment three:A kind of processing method of glitter powder bat printing film, including step in detail below:
(1), modulation base oil:It is by weight/mass percentage composition:Cyclomethicone 32%, polyvinyl chloride 20.5%, carbonic acid
Calcium 17.5%, unsaturated oleic acid 6.2%, phthalic anhydride 8%, antimony oxide 7%, didecyl phthalate 0.5%, disalt
Base calcium stearate 0.7%, trioctyl phosphate 0.6%, Tissuemat E 0.7%, tristerin 0.2%, alkyl phthalates
0.6%th, carbon black 0.5%, the above each component of acrylic copolymer 5% uniformly mix at normal temperatures, obtain base oil;
(2), by the above-mentioned base oil modulated and open profit in mass ratio be 3:2 ratio uniform mixing, obtains primer;
(3), tune machine is carried out to screen process press:The half tone of 300 mesh, 3 layers of photosensitive layer is installed on screen process press, taken hard
Soft-slab for 75HRC is spent as scraper plate, and during installation, it is 40 ° to control the gradient of scraper plate and tool rest;
(4), choose PET silicon oil membranes:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >=
230N/m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk screen
Printed edge is retracted 3mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side by screen process press
On the silicone oil face of PET silicon oil membranes;
(6), after the completion of primer coating, remove one side PET silicon oil membranes, pass through toward the one side with primer artificial or tremble powder machine
Glitter powder uniformly is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.
The glitter powder bat printing film for processing to obtain by the above method, golden green onion is carried out to the printing paper of non-aqueous inks printing
The concrete operations of powder bat printing are:Glitter powder bat printing film is covered on the printing surface of printing paper, passes through roller or other simple
Equipment is heated to glitter powder bat printing film and pressurizeed, and heating-up temperature is 120~150 DEG C, and pressure is 5~10MPa, heating pressurization 2~3 seconds
Afterwards, glitter powder bat printing film is taken away, printing paper, which moves up, is printed on glitter powder pattern.
Claims (1)
1. a kind of processing method of glitter powder bat printing film, it is characterised in that including step in detail below:
(1) base oil, is modulated:It is by weight/mass percentage composition:Cyclomethicone 30~37%, polyvinyl chloride 20~23%,
Calcium carbonate 17~18%, unsaturated oleic acid 5~10%, phthalic anhydride 7~8%, antimony oxide 6~8%, O-phthalic
Sour didecyl 0.4~0.6%, dibasic calcium stearate 0.6~0.9%, trioctyl phosphate 0.4~0.8%, Tissuemat E 0.6
~1.2%, tristerin 0.2~0.3%, alkyl phthalates 0.5~0.7%, carbon black 0.5~0.6%, propylene
The above each component of acid copolymer 4~6% uniformly mixes at normal temperatures, obtains base oil;
(2) it is, 3 in mass ratio with opening profit by the above-mentioned base oil modulated:2 ratio uniform mixing, obtains primer;
(3) tune machine, is carried out to screen process press:The half tone of 250~300 mesh, 3 layers of photosensitive layer is installed on screen process press, taken
The soft-slab that hardness is 75HRC or 90HRC is used as scraper plate, during installation, controls the gradient of scraper plate and tool rest as 35~40 °;
(4) PET silicon oil membranes, are chosen:Take one side PET silicon oil membranes, and in one side PET silicon oil membranes silicone oil peel strength >=230N/
m;
(5), one side PET silicon oil membranes coating primer:One side PET silicon oil membranes are fitted into screen process press, and control silk-screen printing
Edge is retracted 3~7mm than the edge of one side PET silicon oil membranes, and primer then is coated uniformly on into one side PET by screen process press
On the silicone oil face of silicon oil membrane;
(6), after the completion of primer coating, one side PET silicon oil membranes are removed, are passed through toward the one side with primer artificial or to tremble powder machine uniform
Glitter powder is spread, after glitter powder sticks primer, bullet falls the glitter powder of one side PET silicon oil membrane excess surfaces;
(7), the one side PET silicon oil membranes of one side dusting are dried, obtain glitter powder bat printing film.