[go: up one dir, main page]
More Web Proxy on the site http://driver.im/

CN105112146B - A kind of automotive trim seat uses noise reduction wax and preparation method thereof - Google Patents

A kind of automotive trim seat uses noise reduction wax and preparation method thereof Download PDF

Info

Publication number
CN105112146B
CN105112146B CN201510555225.8A CN201510555225A CN105112146B CN 105112146 B CN105112146 B CN 105112146B CN 201510555225 A CN201510555225 A CN 201510555225A CN 105112146 B CN105112146 B CN 105112146B
Authority
CN
China
Prior art keywords
parts
noise reduction
water
sorbester
paraffin
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Active
Application number
CN201510555225.8A
Other languages
Chinese (zh)
Other versions
CN105112146A (en
Inventor
李有刚
李林
蒋乔波
陈胜明
冉忠祥
魏星耀
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Chongqing Zhongke Litai polymer material Co.,Ltd.
Original Assignee
Ke Litai Macromolecular Material Limited-Liability Co In Chongqing
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Ke Litai Macromolecular Material Limited-Liability Co In Chongqing filed Critical Ke Litai Macromolecular Material Limited-Liability Co In Chongqing
Priority to CN201510555225.8A priority Critical patent/CN105112146B/en
Publication of CN105112146A publication Critical patent/CN105112146A/en
Application granted granted Critical
Publication of CN105112146B publication Critical patent/CN105112146B/en
Active legal-status Critical Current
Anticipated expiration legal-status Critical

Abstract

The invention discloses a kind of automotive trim seat using noise reduction wax and preparation method thereof, noise reduction wax is composed of the following components by weight, 3~4 parts of paraffin, 1~2 part of microwax;1~2 part of Tissuemat E;2~5 parts of silicone grease;2~3 parts of polyethylene glycol;1 part of paraffin emulsifier GR 200B;0~1 part of sorbester p18;1 part of sorbester p17;163 1~2 parts of white oil emulsifying agent;8~10 parts of white oil;50~80 parts of water, formula is reasonable, and preparation method is simple, and because the formula uses water as lubricant, nontoxic, low-carbon emission, security is good, and obtained noise reduction wax meets national VOC standards, can be used in a kind of lubricant used in automotive trim seat.

Description

A kind of automotive trim seat uses noise reduction wax and preparation method thereof
Technical field
The invention belongs to chemical field, and in particular to a kind of automotive trim seat uses noise reduction wax, further relates to the noise reduction wax Preparation method.
Background technology
Paraffin is one kind of refinery products, is one kind of mineral wax, is also one kind of pertroleum wax.Paraffin is that solid-state is high The mixture of level alkane, the molecular formula of main component is CnH2n+2, wherein n=17~35.Key component is linear paraffin, also There is the monocyclic naphthenes of a small amount of alkane with indivedual side chains and belt length side chain;It is mainly n-docosane in linear paraffin (C22H46) and positive octacosane (C28H58).It is from the lube cut obtained by crude distillation through solvent refining, solvent dewaxing or Be made slack wax through wax freezing and crystallizing, squeezing dewaxing, then through solvent deoiling, it is refined obtained by sheet or acicular crystal.According to whether Poisonous to be divided into food-grade (food-grade and packaging level, the former is excellent) and technical grade, food-grade is nontoxic, and edible, technical grade is not edible With, but purposes is wide, available for higher fatty acids processed, higher alcohol, match, candle, waterproofing agent, ointment, electrically insulating material, lubricant Deng.
White oil, alias paraffin oil, white oil, mineral oil are, by the mixture of refining liquid hydrocarbon obtained by oil, predominantly to satisfy The cycloalkane and alkane mixture of sum, crude oil are obtained through normal pressure and vacuum fractionation, solvent extraction and dewaxing, hydrofinishing. Food industry can be used as fruit glaze agent, China《Food additives use sanitary standard》(GB2760-2014) provided in:White oil can use In other candies in addition to gel-based candy, fresh egg, maximum usage amount is 5.0g/kg;Other use reference:It is stripped as bread Agent, baking plate corrosivity is small, and offending smell is not produced;As food machinery lubricant, not etching mechanism;In addition also it can use To extend water fruits and vegetables, the Storage period of can.
Silicone grease is the oily thick inorganic thickening agent based on refining artificial oil, and is added added with structural stabilizing agent, anticorrosion Agent is refined to be formed, and with good waterproof seal, waterproof, solvent resistance and creep resistance energy, does not corrode metal, has with rubber Well adapting to property, for bathing device, sealing ring, the waterproof sealing of electric industry and lubrication.
Paraffin, white oil and silicone grease can be used as lubricant, such as noise reduction wax, can be reduced froth pulp and be rubbed with metallic framework The abnormal sound of wiping, therefore widely used in automotive trim.But the noise reduction wax on existing market is typically dissolved using organic solvent, Volatilization produces harmful components.As the improvement of people's living standards, to vapour environment inside car requirement also more and more higher, country also puts into effect Corresponding VOC emission standard and requirement.In order to meet the VOC standards and low-carbon emission of customer and country, it is badly in need of exploitation one Plant water-based lubricant, the water-based emulsion made by paraffin white oil and silicone grease etc..
The content of the invention
In view of this, an object of the present invention is that providing a kind of automotive trim seat uses noise reduction wax;The present invention's The second purpose is to provide the preparation method that automotive trim seat uses noise reduction wax.
For achieving the above object, the present invention provides following technical scheme:
1st, a kind of automotive trim seat uses noise reduction wax, composed of the following components by weight, 3~4 parts of paraffin;Crystallite 1~2 part of wax;1~2 part of Tissuemat E;2~5 parts of silicone grease;2~3 parts of polyethylene glycol;1 part of paraffin emulsifier GR-200B;Sapn 60 0~1 part;1 part of sorbester p17;163 1~2 parts of white oil emulsifying agent;8~10 parts of white oil;50~80 parts of water.
2nd, automotive trim seat uses the preparation method of noise reduction wax, comprises the following steps:By paraffin, microwax, polyethylene Wax, silicone grease and white oil input reactor, 80~90 DEG C of fusings, are stirred and evenly mixed, and polyethylene glycol are then put at 80~90 DEG C, white Emulsifier 163, paraffin emulsifier GR-200B, sorbester p18 and sorbester p17, are stirred and evenly mixed;Then put under agitation equivalent to The temperature that water always adds quality 15% is 85~95 DEG C of water, is stirred, and it is 85~95 DEG C to be eventually adding remaining temperature Water, cools down blowing, obtains automotive trim seat and uses noise reduction wax.
It is preferred that, comprise the following steps:Paraffin, microwax, Tissuemat E, silicone grease and white oil are put into reactor, heating To 85 DEG C fusing, after melt under the conditions of 200~300r/min stir 30 minutes, then 85 DEG C put into polyethylene glycol, in vain Emulsifier 163, paraffin emulsifier GR-200B, sorbester p18 and sorbester p17, and keeping temperature is 85 DEG C, in 200~300r/min Under the conditions of stir 30 minutes, then it is 90 DEG C of water that the lower input of 1000r/min stirrings, which always adds the temperature of quality 15% equivalent to water, 30min is stirred, the water that remaining temperature is 90 DEG C is eventually adding, cools down blowing, automotive trim seat is obtained and uses noise reduction wax.
The beneficial effects of the present invention are:Noise reduction wax is used the invention discloses a kind of automotive trim seat, formula is environmentally friendly, It is aqueous wax emulsion using water as lubricant, therefore low-carbon emission in use, meet national VOC emission standard.
Embodiment
The preferred embodiments of the present invention will be described in detail below.The experiment of unreceipted actual conditions in embodiment Method, generally according to normal condition or according to the condition proposed by manufacturer.
In the present invention, paraffin is purchased from Fushun Dong Ke Fine Chemical Co., Ltd;Microwax is purchased from Wei Jia Chemical Co., Ltd.s; Tissuemat E is enough from Qingdao Sai Nuo new materials Co., Ltd;Silicone grease is purchased from Shanghai Hui Pu silicone grease Co., Ltd;Polyethylene glycol is purchased from Jiangsu Jia Feng chemistry limited company;Sorbester p18 and sorbester p17 are purchased from the chemical limited company of Shandong Bock;Emulsification of Paraffin Agent GR-200B is purchased from Shanghai Ge Running Chemical Industry Science Co., Ltd;White oil emulsifying agent 163 is purchased from Jiangsu Province Hai'an petrochemical industry Factory;White oil is purchased from Fushun Sheng Wei petrochemical industry Co., Ltd.
Embodiment 1
A kind of automotive trim seat uses noise reduction wax, composed of the following components by weight, 4 parts of paraffin, microwax 2 Part;2 parts of Tissuemat E;5 parts of silicone grease;3 parts of polyethylene glycol;1 part of paraffin emulsifier GR-200B;1 part of sorbester p18;Sorbester p17 1 Part;163 2 parts of white oil emulsifying agent;10 parts of white oil;80 parts of water.
Its preparation method is:Paraffin, microwax, Tissuemat E, silicone grease and white oil are put into reactor, 85 DEG C is warming up to and melts Change, stirred after having melted under the conditions of 250r/min 30 minutes, then put into polyethylene glycol, white oil emulsifying agent 163, stone at 85 DEG C Wax emulsifying agent GR-200B, sorbester p18 and sorbester p17, and keeping temperature is 85 DEG C, stirring 30 minutes under the conditions of 250r/min, then It is 90 DEG C of water stirring 30min that the lower input of 1000r/min stirrings, which always adds the temperature of quality 15% equivalent to water, is eventually adding surplus Remaining temperature is 90 DEG C of water, cools down blowing, obtains automotive trim seat and uses noise reduction wax.
Embodiment 2
A kind of automotive trim seat uses noise reduction wax, composed of the following components by weight, 3 parts of paraffin, microwax 1 Part;1 part of Tissuemat E;2 parts of silicone grease;2 parts of polyethylene glycol;1 part of paraffin emulsifier GR-200B;1 part of sorbester p17;White oil is emulsified 163 1 parts of agent;8 parts of white oil;50 parts of water.
Its preparation method is:Paraffin, microwax, Tissuemat E, silicone grease and white oil are put into reactor, 90 DEG C is warming up to and melts Change, stirred after having melted under the conditions of 300r/min 30 minutes, then put into polyethylene glycol, white oil emulsifying agent 163, stone at 90 DEG C Wax emulsifying agent GR-200B, sorbester p18 and sorbester p17, and keeping temperature is 90 DEG C, stirring 30 minutes under the conditions of 300r/min, then It is 95 DEG C of water stirring 30min that the lower input of 1000r/min stirrings, which always adds the temperature of quality 15% equivalent to water, is eventually adding surplus Remaining temperature is 95 DEG C of water, cools down blowing, obtains automotive trim seat and uses noise reduction wax.
Embodiment 3
A kind of automotive trim seat uses noise reduction wax, composed of the following components by weight, 3.5 parts of paraffin, microwax 1.5 part;1.5 parts of Tissuemat E;4 parts of silicone grease;2.5 parts of polyethylene glycol;1 part of paraffin emulsifier GR-200B;0.5 part of sorbester p17; 163 1.5 parts of white oil emulsifying agent;9 parts of white oil;68 parts of water.
Its preparation method is:Paraffin, microwax, Tissuemat E, silicone grease and white oil are put into reactor, 80 DEG C is warming up to and melts Change, stirred after having melted under the conditions of 200r/min 30 minutes, then put into polyethylene glycol, white oil emulsifying agent 163, stone at 80 DEG C Wax emulsifying agent GR-200B, sorbester p18 and sorbester p17, and keeping temperature is 80 DEG C, stirring 30 minutes under the conditions of 200r/min, then It is 85 DEG C of water stirring 30min that the lower input of 1000r/min stirrings, which always adds the temperature of quality 15% equivalent to water, is eventually adding surplus Remaining temperature is 55 DEG C of water, cools down blowing, obtains automotive trim seat and uses noise reduction wax.
Noise reduction wax made from above-described embodiment 1~3 can accomplish the solid content of the different gradients within 10~50%;Product After drying, into paste between -20~35 DEG C, adhere to beneficial to product in foam surface, without producing stream because of gravitional force Hang;And existing products in markets is generally liquid under similarity condition, easy sagging.In addition noise reduction wax produced by the present invention is at -20 DEG C Under the conditions of, product is solid, but still has lubrication between metal and foam, and on smell, this product is in standard It is 3 grades that smell is measured under conditions of PV3900-2000, and existing products in markets is more than 4 grades;And the product is in solid content Closed-cell foam surface is sprayed at when 10%, uniform droplet can be formed without reuniting in foam surface, but the existing production in market Product are sprayed at foam surface under conditions of same solid content can form uneven drop, there is agglomeration.
Finally illustrate, preferred embodiment above is merely illustrative of the technical solution of the present invention and unrestricted, although logical Cross above preferred embodiment the present invention is described in detail, it is to be understood by those skilled in the art that can be Various changes are made to it in form and in details, without departing from claims of the present invention limited range.

Claims (3)

1. a kind of automotive trim seat uses noise reduction wax, it is characterised in that:It is composed of the following components by weight, paraffin 3~4 Part;1~2 part of microwax;1~2 part of Tissuemat E;2~5 parts of silicone grease;2~3 parts of polyethylene glycol;Paraffin emulsifier GR-200B 1 Part;0~1 part of sorbester p18;1 part of sorbester p17;163 1~2 parts of white oil emulsifying agent;8~10 parts of white oil;50~80 parts of water.
2. automotive trim seat described in claim 1 uses the preparation method of noise reduction wax, it is characterised in that comprise the following steps: Paraffin, microwax, Tissuemat E, silicone grease and white oil are put into reactor, 80~90 DEG C of fusings are stirred and evenly mixed, then 80~ Polyethylene glycol, white oil emulsifying agent 163, paraffin emulsifier GR-200B, sorbester p18 and sorbester p17 are put at 90 DEG C, is stirred and evenly mixed;So It is 85~95 DEG C of water to put under agitation afterwards and the temperature of quality 15% is always added equivalent to water, stirs, is eventually adding surplus Remaining temperature is 85~95 DEG C of water, cools down blowing, obtains automotive trim seat and uses noise reduction wax.
3. automotive trim seat uses the preparation method of noise reduction wax according to claim 2, it is characterised in that including following step Suddenly:Paraffin, microwax, Tissuemat E, silicone grease and white oil are put into reactor, 85 DEG C of fusings are warming up to, after having melted 200~ Stirred under the conditions of 300r/min 30 minutes, then put into polyethylene glycol, white oil emulsifying agent 163, paraffin emulsifier GR- at 85 DEG C 200B, sorbester p18 and sorbester p17, and keeping temperature is 85 DEG C, stirring 30 minutes under the conditions of 200~300r/min, It is 90 DEG C of water stirring 30min that the lower input of 1000r/min stirrings, which always adds the temperature of quality 15% equivalent to water, is eventually adding surplus Remaining temperature is 90 DEG C of water, cools down blowing, obtains automotive trim seat and uses noise reduction wax.
CN201510555225.8A 2015-09-02 2015-09-02 A kind of automotive trim seat uses noise reduction wax and preparation method thereof Active CN105112146B (en)